Composite film sprayed with nano-diamond, shell and lithium ion battery

By applying nanodiamond composite coating on the film and shell of the lithium-ion battery, the problem of rising internal temperature of the fast-charge lithium-ion battery is solved, extending the battery's cycle life and improving safety, and achieving heat transfer Improvement.

CN119029431APending Publication Date: 2024-11-26GUANGDONG TECHN COLLEGE OF WATER RESOURCES & ELECTRIC ENG +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410875089.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art methods of reducing the internal temperature of fast charging lithium-ion batteries have limited effects and may consume battery power or require changes in the battery structure.

Method used

Using a composite film and shell sprayed with nanodiamond, the nanodiamond composite coating is applied to the film and shell of the lithium-ion battery to improve heat transfer between the core package and the shell and reduce the internal temperature of the battery.

Benefits of technology

It effectively reduces the internal temperature of the battery, extends the cycle life of the battery, improves the safety and thermal management capabilities of the battery, and does not affect the production process and performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119029431A_ABST
    Figure CN119029431A_ABST
Patent Text Reader

Abstract

The invention relates to a composite film sprayed with nano-diamond, which comprises a film sprayed with a composite coating, and the material of the composite coating comprises nano-diamond particles. The invention also relates to a shell and a lithium ion battery. The characteristic that the diamond material has the highest heat conductivity coefficient is utilized, so that heat transfer between the core package and the lithium ion battery shell can be improved, the temperature of the core package during fast charging is reduced, and the cycle life of a battery cell is prolonged; the preparation method can improve the puncture resistance strength of the film and the insulativity between the core package and the shell, reduce the sensitivity of the battery to foreign matters in the production process and the corrosion risk of the battery shell, and improve the safety of the battery, and belongs to the manufacturing technology of the lithium ion battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a lithium ion battery manufacturing technology, and in particular to a composite film sprayed with nano-diamond, a shell and a lithium ion battery. Background Art

[0002] Capacity / energy, energy density and charging speed are the three core technical indicators of lithium-ion batteries, and are also the key factors in whether electric vehicles can replace fuel vehicles. In recent years, fast-charging lithium-ion batteries have continued to develop, and the charging time required for batteries to charge from 10-80% SOC has been gradually shortened from about 60 minutes to about 10 minutes, greatly alleviating potential consumer users' anxiety about the battery life and energy replenishment of battery vehicles. However, according to the heat generation formula P = I 2 *R, under the condition that the battery internal resistance R does not change much, the increase of current I will exponentially increase the heat generation power P of the battery, causing the internal temperature of the fast-charging battery to be much higher than that of conventional batteries. The upper limit of the temperature safety window of lithium-ion batteries is generally 60°C. Exceeding this temperature will not only accelerate battery aging and shorten the battery life, but may also bring safety risks. Therefore, reducing the internal temperature of the battery is one of the important tasks in the development and use of fast-charging lithium-ion batteries.

[0003] There are currently two main ways to reduce the internal temperature of fast-charging batteries: First, optimize the battery structure and chemical system to reduce heat generation by reducing the battery internal resistance R. Battery structure optimization includes the width of the pole ear, the lead-out method of the pole ear, the grouping method of the pole piece, etc. Chemical system optimization includes the use of low-viscosity electrolytes, the selection of suitable film-forming additives to reduce the charge transfer impedance of the positive and negative SEI films, and the optimization of electrode formulations. However, the internal resistance of fast-charging lithium-ion batteries is currently about 0.3-0.5mΩ, and the internal resistance of the battery is already very low, so there is relatively limited room for further optimization and improvement. Secondly, according to the heat generation formula P=I 2 *R, the heat generation power P and the battery internal resistance R have a linear relationship, and the heat generation power P and the current I have a quadratic relationship. The contribution of reducing the battery internal resistance R to reducing the heat generation power is far from offsetting the negative impact of the increase in the charging rate. 2. Improve the thermal management capability at the system level, and reduce the internal temperature of the battery by improving the heat dissipation capability, including increasing the coolant cooling power, increasing the battery-coolant pipe contact area, etc. However, increasing the coolant cooling power will inevitably consume battery power, thereby reducing the mileage of the vehicle. In addition, increasing the battery-coolant pipe contact area requires changing the way the batteries are grouped in the vehicle, which increases the complexity of the system design.

[0004] In summary, existing methods for reducing the internal temperature of fast-charging batteries have limited effects, consume battery power or require changes to the battery structure. Summary of the invention

[0005] In view of the technical problems existing in the prior art, the purpose of the present invention is to provide a composite film sprayed with nano-diamonds, and apply the composite film to lithium-ion batteries to solve the problems that the existing methods of reducing the internal temperature of fast-charging batteries have limited effects, consume battery power or require changes to the battery structure.

[0006] Another object of the present invention is to provide a shell, which is applied to a lithium-ion battery to solve the problems that existing methods for reducing the internal temperature of fast-charging batteries have limited effects, consume battery power or require changes in battery structure.

[0007] Another object of the present invention is to provide a lithium-ion battery that can solve the problems that existing methods for reducing the internal temperature of fast-charging batteries have limited effects, consume battery power or require changes in battery structure.

[0008] In order to achieve the above object, the present invention adopts the following technical solution:

[0009] A composite film sprayed with nano-diamond comprises a film sprayed with a composite coating, wherein the material of the composite coating comprises nano-diamond particles.

[0010] As a preference, the film is any one of polyethylene, polypropylene, polyurethane, polycarbonate, polyethylene terephthalate, polymethyl methacrylate, polyvinyl chloride, and triacetyl cellulose.

[0011] As a preferred method, the preparation method of the composite coating is: nano diamond particles with a diameter of 20-500nm, an adhesive and a dispersant are mixed in a mass ratio of 85-90%: 2-10%: 0.2-2% to form a mixed material, pure water is added to the mixed material to obtain a composite slurry, the composite slurry is sprayed on all surfaces except the two sides of the film, and then dried to obtain a composite coating.

[0012] As a preference, the adhesive is any one of polyvinylidene fluoride and polymethyl methacrylate or a mixture of the two.

[0013] As a preference, the dispersant is any one of sodium carboxymethyl cellulose and lithium carboxymethyl cellulose or a mixture of the two.

[0014] As a preference, the film has a thickness of 10-500 μm.

[0015] As a preferred embodiment, the thickness of the composite coating is 10-200 μm and the surface density is 50-800 g / m 2 .

[0016] A shell comprises a shell body sprayed with a composite coating, wherein the composite coating is coated on the inner wall of the shell body, and the composite coating is a composite coating coated on a film.

[0017] A lithium ion battery comprises a film, a shell and a core package. The film is a composite film, the outer surface of the core package is wrapped with the film, the inner wall of the shell is coated with a composite coating, the composite coating is a composite coating coated on the film, and the core package is arranged on the inner side of the shell.

[0018] In general, the present invention has the following advantages:

[0019] The composite film of the present invention has a simple structure, low cost, and is compatible with the existing production process of lithium-ion batteries without affecting the performance of the battery. It can improve the heat transfer between the core pack and the lithium-ion battery shell, reduce the core pack temperature during fast charging, and improve the cycle life of the battery core; it can improve the puncture resistance of the film and the insulation between the core pack and the shell, reduce the sensitivity of the battery to foreign matter in the production process and the risk of battery shell corrosion, and improve the safety of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The process flow chart for preparing spray-coated nano-diamond composite films.

[0021] Figure 2 This is the assembly drawing of the membrane, shell and core package.

[0022] Figure 3 This is a bar chart comparing the temperatures at different positions of the battery when directly charged to the upper limit voltage at a 3C rate in Example 1.

[0023] Figure 4 The figure is a comparison curve of the battery capacity retention rate during normal temperature cycling in Example 1.

[0024] Figure 5 This is a bar chart comparing the temperatures at different positions of the battery when directly charged to the upper voltage limit at a 3C rate in Example 2.

[0025] Figure 6 This is a comparison curve of the battery capacity retention rate during normal temperature cycling in Example 2.

[0026] Figure 7 This is a bar chart comparing the temperatures at different positions of the battery when directly charged to the upper limit voltage at a 3C rate in Example 3.

[0027] Figure 8 This is a comparison curve of the battery capacity retention rate during normal temperature cycling in Example 3. DETAILED DESCRIPTION

[0028] The present invention will be further described in detail below in conjunction with specific implementation methods.

[0029] Mylar films include polyethylene, polypropylene, polyurethane, polycarbonate, polyethylene terephthalate, polymethyl methacrylate, polyvinyl chloride, and triacetyl cellulose. The films in the following embodiments use any one of the Mylar films.

[0030] Embodiment 1:

[0031] The method for preparing a composite slurry containing nano-diamond particles is as follows: nano-diamond particles with a diameter of 20-500nm, polyvinylidene fluoride (PVDF) and sodium carboxymethyl cellulose are mixed in a mass ratio of 94%:5%:1% to obtain a mixed material, and then an appropriate amount of pure water is added and stirred evenly to obtain a composite slurry. The final composite slurry has a viscosity of 3500mPa·s and a solid content of 45%.

[0032] Spraying method of composite slurry: A polyethylene terephthalate polymer film with a thickness of 100 μm was selected as the Mylar-like film, and an aluminum shell was selected as the shell. In order to facilitate comparison, the control group did not spray on the Mylar-like film and the shell; the experimental group was divided into three types, namely, spraying composite slurry only on the two outer large surfaces and outer bottom surface of the Mylar-like film, spraying composite slurry only on the two inner large surfaces and inner bottom surface of the aluminum shell, and spraying composite slurry on both the outer surface of the Mylar-like film and the inner surface of the shell. Figure 2 After spraying, the film coated with the composite slurry was placed in a dry environment at 60°C for 1.5 hours. The sprayed composite slurry coating had a thickness of 50 μm and a surface density of 200 g / m 2 .

[0033] Assembly method of core package, Mylar film and aluminum shell: Wrap the Mylar film sprayed with composite slurry on the surface of the core package, then put the core package into the aluminum shell, and continue other subsequent processes until the lithium-ion battery production is completed. The assembly process makes the outer surface (two outer large surfaces and outer bottom surface) of the Mylar film sprayed with composite slurry correspond to the inner surface (two inner large surfaces and inner bottom surface) of the shell sprayed with composite slurry.

[0034] Application effect: Figure 3As shown, the temperature at the center of the conventional battery 3C fast charging core pack is as high as 50°C, the temperature of the large surface of the aluminum shell is 35°C, and the temperature difference between the inside and the large surface of the battery is 15°C; spraying the composite slurry only on the outer surface of the Mylar film or the inner surface of the shell can have a certain heat dissipation effect, but the heat dissipation effect is weaker than spraying the composite slurry on the outer surface of the Mylar film and the inner surface of the shell at the same time. The center of the battery core pack sprayed with composite slurry is 45°C, the temperature of the large surface of the aluminum shell is 39°C, and the temperature of the inside and large surface of the battery is only 6°C. This result shows that the nano-diamond composite coating sprayed on the outer surface of the polyethylene terephthalate polymer film and the inner surface of the aluminum shell in this embodiment effectively improves the heat transfer between the core pack and the shell, and reduces the temperature difference between the inside and outside of the battery. Excessive internal temperature of the battery will aggravate the degree of side reactions and the consumption of electrolyte, and affect the performance of the battery. Figure 4 By comparing the capacity retention rates of conventional batteries and the batteries of this embodiment under normal temperature cycles, it can be seen that the conventional battery experienced rapid capacity decay at 600 weeks, and the capacity retention rate was only 75% at 900 weeks; spraying the composite slurry only on the outer surface of the Mylar-type film or the inner surface of the shell had no obvious effect on improving the cycle; while the battery in which the composite slurry was sprayed on both the outer surface of the Mylar-type film and the inner surface of the shell simultaneously delayed the rapid capacity decay until 800 weeks, and the capacity retention rate was still 82.3% at 1200 weeks, greatly extending the cycle life of the battery.

[0035] Embodiment 2:

[0036] The method for preparing a composite slurry containing nano-diamond particles is as follows: nano-diamond particles with a diameter of 20-500 nm, methyl methacrylate (PMMA) and sodium carboxymethyl cellulose are mixed in a mass ratio of 92%:7%:1%, and then an appropriate amount of pure water is added and stirred to obtain a composite slurry. The final composite slurry has a viscosity of 5000 mPa·s and a solid content of 45%.

[0037] Spraying method of composite slurry: A polypropylene film with a thickness of 100μm is selected as the Mylar-type film, and an aluminum shell is selected as the shell. In order to facilitate comparison, the control group does not spray on the Mylar-type film and the shell; the experimental group is divided into three types, namely, spraying the composite slurry only on the two outer large surfaces and the outer bottom surface of the Mylar-type film, spraying the composite slurry only on the two inner large surfaces and the inner bottom surface of the aluminum shell, and spraying the composite slurry on both the Mylar-type film and the shell. After spraying, the coated film is placed in a dry environment at 60°C for 1.5 hours. The sprayed composite slurry coating has a thickness of 40μm and a surface density of 200g / m 2 .

[0038] Assembly method of core pack, polypropylene film and aluminum shell: Wrap the Mylar film sprayed with composite slurry on the surface of the core pack, then put the core pack into the aluminum shell, and continue other subsequent processes until the battery production is completed. The assembly process makes the outer surface (two outer large surfaces and outer bottom surface) of the polypropylene film sprayed with composite slurry correspond to the inner surface (two inner large surfaces and inner bottom surface) of the shell sprayed with composite slurry.

[0039] Application effect: Figure 5 As shown, the temperature at the center of the conventional battery 3C fast charging core pack is as high as 50°C, the temperature of the large surface of the aluminum shell is 35°C, and the temperature difference between the inside and the large surface of the battery is 15°C; spraying the composite slurry only on the outer surface of the Mylar film or the inner surface of the shell can achieve a certain heat dissipation effect, but the heat dissipation effect is significantly weaker than spraying the composite slurry on the outer surface of the Mylar film and the inner surface of the shell at the same time. The center of the battery core pack sprayed with composite slurry is 43°C, the temperature of the large surface of the aluminum shell is 40°C, and the temperature of the inside and large surface of the battery is only 3°C. This result shows that the nano-diamond-containing composite coating sprayed on the outer surface of the polypropylene film and the inner surface of the aluminum shell in this embodiment effectively improves the heat transfer between the core pack and the shell, and reduces the temperature difference between the inside and outside of the battery. Figure 6 By comparing the capacity retention rates of conventional batteries and the batteries of this embodiment under normal temperature cycles, it can be seen that the capacity of conventional batteries rapidly decayed after 600 cycles, and the capacity retention rate was only 75% after 900 cycles; spraying the composite slurry only on the outer surface of the Mylar-type film or the inner surface of the shell has limited effect on cycle improvement; while the battery with the composite slurry sprayed on both the outer surface of the Mylar-type film and the inner surface of the shell simultaneously showed linear decay throughout 1200 weeks, and the capacity retention rate was still 90% after 1200 weeks, and the cycle life of the battery was significantly improved.

[0040] Embodiment three:

[0041] The method for preparing a composite slurry containing nano-diamond particles is as follows: nano-diamond particles with a diameter of 20-500 nm, polyvinylidene fluoride (PVDF), methyl methacrylate (PMMA) and sodium carboxymethyl cellulose are mixed in a mass ratio of 92%:4%:3%:1%, and then an appropriate amount of pure water is added and stirred to obtain a composite slurry. The final composite slurry has a viscosity of 4500 mPa·s and a solid content of 45%.

[0042] Spraying method of composite slurry: A polypropylene film with a thickness of 100μm is selected as the Mylar-type film, and an aluminum shell is selected as the shell. In order to facilitate comparison, the control group does not spray on the Mylar-type film and the shell; the experimental group is divided into three types, namely, spraying the composite slurry only on the two outer large surfaces and the outer bottom surface of the Mylar-type film, spraying the composite slurry only on the two inner large surfaces and the inner bottom surface of the aluminum shell, and spraying the composite slurry on both the Mylar-type film and the shell. After spraying, the coated film is placed in a dry environment at 60°C for 1.5 hours. The sprayed composite slurry coating has a thickness of 50μm and a surface density of 180g / m 2 .

[0043] Assembly method of core pack, polypropylene film and aluminum shell: Wrap the Mylar film sprayed with composite slurry on the surface of the core pack, then put the core pack into the aluminum shell, and continue other subsequent processes until the battery production is completed. The assembly process makes the outer surface (two outer large surfaces and outer bottom surface) of the polypropylene film sprayed with composite slurry correspond to the inner surface (two inner large surfaces and inner bottom surface) of the shell sprayed with composite slurry.

[0044] Application effect: Figure 7 As shown in the figure, the temperature at the center of the conventional battery 3C fast charging core pack is as high as 50°C, the temperature of the large surface of the aluminum shell is 35°C, and the temperature difference between the inside and the large surface of the battery is 15°C; the battery sprayed with composite slurry has the best effect, the center of the battery core pack is 40°C, the temperature of the large surface of the aluminum shell is 38°C, and the temperature of the inside and the large surface of the battery is only 2°C. This result shows that the nano-diamond-containing composite coating sprayed on the outer surface of the polypropylene film and the inner surface of the aluminum shell in this embodiment effectively improves the heat transfer between the core pack and the shell, and reduces the temperature difference between the inside and outside of the battery. Figure 8 By comparing the capacity retention rates of conventional batteries and the batteries of this embodiment under normal temperature cycles, it can be seen that the conventional battery experienced rapid capacity decay at 600 weeks, and the capacity retention rate was only 75% at 900 weeks; spraying the composite slurry only on the outer surface of the Mylar film or the inner surface of the shell improved the cycle, but the battery with the composite slurry sprayed on both the outer surface of the Mylar film and the inner surface of the shell had the best cycle improvement effect. It always showed linear decay in the first 1000 weeks, and the battery experienced rapid capacity decay at 1000 weeks. The capacity decay transition point was delayed by 400 weeks compared with the conventional battery, and the capacity retention rate was still 85.9% at 1200 weeks.

[0045] The battery in the above embodiment is a lithium ion battery.

[0046] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A composite film of sprayed nano-diamond, characterized in that: The invention comprises a film sprayed with a composite coating, wherein the material of the composite coating comprises nano-diamond particles.

2. The composite film of sprayed nano-diamond according to claim 1, characterized in that: The film is any one of polyethylene, polypropylene, polyurethane, polycarbonate, polyethylene terephthalate, polymethyl methacrylate, polyvinyl chloride, and triacetyl cellulose.

3. The composite film of sprayed nano-diamond according to claim 1, characterized in that: The preparation method of the composite coating is as follows: nano diamond particles with a diameter of 20-500nm, an adhesive and a dispersant are mixed in a mass ratio of 85-90%: 2-10%: 0.2-2% to form a mixed material, pure water is added to the mixed material to obtain a composite slurry, the composite slurry is sprayed on all surfaces except the two sides of the film, and then dried to obtain a composite coating.

4. The composite film of sprayed nano-diamond according to claim 3, characterized in that: The adhesive is either polyvinylidene fluoride or polymethyl methacrylate or a mixture of the two.

5. The composite film of sprayed nano-diamond according to claim 3, characterized in that: The dispersant is either sodium carboxymethyl cellulose or lithium carboxymethyl cellulose or a mixture of the two.

6. The composite film of sprayed nano-diamond according to claim 1, characterized in that: The thickness of the film is 10-500 μm.

7. The composite film of sprayed nano-diamond according to claim 1, characterized in that: The thickness of the composite coating is 10-200μm and the surface density is 50-800g / m 2 .

8. A housing, characterized in that: It comprises a shell body sprayed with a composite coating, wherein the composite coating is coated on the inner wall of the shell body, and the composite coating is the composite coating described in any one of claims 1-7.

9. A lithium ion battery, characterized in that: It includes a film, a shell and a core package, wherein the film is the composite film described in any one of claims 1 to 7, the outer surface of the core package is wrapped with the film, the inner wall of the shell is coated with a composite coating, the composite coating is a composite coating coated on the film, and the core package is arranged on the inner side of the shell.