Strong and tough cast polypropylene film and preparation method thereof
By using polyurethane-coated titanium dioxide particles and amino-terminated dendrimers to modify carbon fibers in the core layer and heat-sealing layer of the cast polypropylene film to form a cross-linked network structure, the problem of insufficient toughness of the polypropylene film is solved and significantly improved Its impact resistance and strength.
Patent Information
- Application Number
- CN202410590530.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-13
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-05-13
AI Technical Summary
The toughness of cast polypropylene film is insufficient. Existing toughening agents cause a large loss of material strength and poor interfacial compatibility, resulting in poor impact and impact resistance.
The carbon fiber modified by polyurethane-coated titanium dioxide particles and amino-terminated dendrimers is used to form a cross-linked network structure in the core layer and heat-sealing layer. Through the cross-linking of polyurethane and epoxidized polypropylene and the uniform dispersion of titanium dioxide particles, the reinforcement Film toughness and impact resistance.
Significantly improves the toughness and impact resistance of polypropylene films, reduces crack expansion, enhances the elastic modulus and strength of the material, while reducing the agglomeration of titanium dioxide particles and improving crystal orientation.
Smart Images

Figure BDA0004837128860000101 
Figure BDA0004837128860000111
Abstract
Description
Technical Field
[0001] The present application relates to the field of film technology, and more specifically, to a strong and tough cast polypropylene film and a preparation method thereof. Background Art
[0002] Cast polypropylene film (CPP film) is a non-stretched, non-directional flat extruded film produced by single-layer or multi-layer co-extrusion melt casting and quenching of polypropylene resin. Compared with blown film, it has the characteristics of fast production speed, high output, good film transparency, glossiness, thickness uniformity, and excellent balance of various properties. At the same time, because it is a flat extruded film, subsequent processes such as printing and lamination are extremely convenient, so it is widely used in the packaging of textiles, flowers, food, and daily necessities.
[0003] However, since polypropylene is a semi-crystalline polymer, its structural characteristics lead to low notched impact strength of the resin, easy brittle fracture at low temperatures, large shrinkage, and poor creep resistance. People improve the toughness of polypropylene films by adding toughening agents to polypropylene, but elastomer toughening causes a large loss in material strength, inorganic particle toughening has a general effect and poor interface compatibility, large toughening particle size can easily lead to defects inside the polymer matrix, small particle size is easy to agglomerate, and adding a large amount can easily cause microcracks in the matrix after impact, and adding a small amount cannot effectively disperse the load. The matrix is still the main bearer of the load, and the improvement of toughness and impact resistance is limited, resulting in the toughness of the cast polypropylene film formed by it not being well improved.
[0004] Therefore, how to effectively improve the toughness of cast polypropylene film is of great significance to its use and development. Summary of the invention
[0005] In order to improve the toughness of a cast polypropylene film, the present application provides a strong and tough cast polypropylene film and a preparation method thereof.
[0006] In the first aspect, the present application provides a tough cast polypropylene film, which adopts the following technical solution:
[0007] A strong and tough cast polypropylene film comprises, from top to bottom, a heat sealing layer, a core layer and a corona layer; the core layer comprises the following raw materials in parts by weight: 100 parts of polypropylene, 10-25 parts of epoxidized polypropylene, and 20-24 parts of fillers, wherein the fillers comprise polyurethane-coated titanium dioxide particles; the heat sealing layer comprises the following raw materials in parts by weight: 70-80 parts of polypropylene, 15-25 parts of polyolefin elastomer, 1-5 parts of lubricant, and 2-5 parts of polyurethane-coated titanium dioxide particles.
[0008] By adopting the above technical solution, adding a certain amount of epoxidized polypropylene to the core layer can improve the toughness of the polypropylene film. A certain mass of polyurethane-coated titanium dioxide particles are added to the core layer and the heat-sealing layer, and the polyurethane can be well dispersed in the polypropylene system, while reducing the agglomeration of the titanium dioxide particles. The polyurethane-coated titanium dioxide particles are evenly dispersed in the polypropylene system. The polyurethane-coated titanium dioxide particles dispersed in the core layer can be cross-linked with the epoxidized polypropylene to form a network structure to better disperse stress. On the other hand, the polyurethane-coated titanium dioxide particles dispersed in the heat-sealing layer and the epoxidized polypropylene in the core layer strengthen the connection strength between the core layer and the heat-sealing layer, and further conduct the stress. At this mass, the yield deformation zones of the core layer and the heat-sealing layer are connected to each other, and the polypropylene film undergoes a brittle-to-tough transition. Because the elasticity of titanium dioxide particles, polyurethane, polypropylene, and epoxidized polypropylene has the characteristic of gradually increasing, when the polypropylene film is deformed by external force, the polyurethane-coated titanium dioxide particles serve as stress concentration points, and the polyurethane produces silver streaks and shear bands to absorb part of the stress, and also generates three-dimensional stress around the titanium dioxide particles, and then the interface between the titanium dioxide particles and the polyurethane, polypropylene, and epoxy polypropylene matrix is debonded, and the voids caused by the debonding of the polyurethane cause the stress state around the particles to change from plane strain to plane stress, and induce shear deformation of the polypropylene film, thereby dissipating a large amount of energy, and the obtained polypropylene film is under the joint action of the conduction of the cross-linked network structure and the consumption of the stress by the polyurethane-coated titanium dioxide particles as stress concentration points, and the cracks end around the titanium dioxide particles and are not easy to expand, and have high toughness and impact resistance. The present application conducts stress by adding polyurethane-coated titanium dioxide particles to the percolation channel connected to the core layer and the heat-sealing layer and the epoxidized polypropylene, and the added particles have a small volume fraction, and have both high toughness and low microcracks and plastic deformation. Under the joint action of each component, the obtained polypropylene film is strong and tough and impact-resistant. By coating the titanium dioxide particles with polyurethane, the agglomeration of the titanium dioxide particles is reduced, more crystal nuclei are formed in the polypropylene film, the polypropylene grains are finer and more uniform, and the orientation of the polypropylene crystals is improved. When the material is impacted, the polypropylene film can produce greater yield and dissipate stress, further improving the toughness and elastic modulus of the polypropylene film.
[0009] In a specific embodiment, the preparation method of aminosilane-modified polyurethane-coated titanium dioxide particles comprises the following steps: activating titanium dioxide particles at high temperature under the protection of nitrogen to obtain activated titanium dioxide, adding the activated titanium dioxide into a mixed solution of polyether polyol, catalyst, and toluene diisocyanate, ultrasonically dispersing, introducing nitrogen, stirring at 65-70°C for 0.5-1.5 hours, reacting, continuing nitrogen protection, slowly adding aminosilane coupling agent, stirring at 60-65°C for 0.5-1.5 hours, reacting, vacuum filtering, and drying to obtain the polyurethane-coated titanium dioxide particles.
[0010] In a specific embodiment, the high temperature activation temperature is 240-260° C. and the time is 4.5-5.5 hours.
[0011] By adopting the above scheme, under the above activation conditions, the degree of particle activation is moderate, the bonding strength between titanium dioxide particles and polyurethane is appropriate, and after co-extrusion, the particles are not too tightly bonded so that the polypropylene film cannot debond when subjected to stress, nor are they too loose so that too much stress cannot be consumed, and the toughness of the obtained polypropylene film is improved effectively. The amino grafting rate of the obtained polyurethane-coated titanium dioxide particles modified with aminosilane is appropriate, and a good cross-linking effect is formed with epoxidized polypropylene.
[0012] In a specific embodiment, the core layer filler further comprises the following raw materials: amino-terminated dendritic macromolecule-modified carbon fibers, wherein the fiber diameter of the amino-terminated dendritic macromolecule-modified carbon fibers is 5-12 μm.
[0013] Dendritic macromolecules have flexible long chains, which can buffer external forces when impacted, increase the toughness of polypropylene film, improve the fluidity of the solution, improve the dispersion of polyurethane coated with titanium dioxide particles on the core layer, and further improve the toughness of polypropylene film. After the amino-terminated dendritic macromolecules are modified on the carbon fiber, the active functional groups on the surface of the carbon fiber are increased, which improves its compatibility with polypropylene, so that the strength of the carbon fiber can be better applied to the polypropylene film. The terminal amino group undergoes a cross-linking reaction with the epoxy group of epoxidized polypropylene, and the dendritic macromolecules form a network with cross-linked amino groups as nodes. The dendritic cross-linked network forms an effective tethered chain, which is interspersed between two or more lamellae, thereby reducing the crystallization ability of polypropylene, reducing the deflection of the bending of the polypropylene lamellae, and increasing the stress required for the bending and breaking of the lamellae, further improving the strength and toughness of the polypropylene film. The terminal amino group dendritic macromolecules modified carbon fiber and the polyurethane-coated carbon nanoparticles participate in cross-linking to form a network interspersed, and the cracks in the obtained polypropylene film are less likely to expand, and the toughness performance is better. Experiments show that the present application has better performance in improving toughness than using any of the above modification alone through the joint use of terminal amino group dendritic macromolecules modified carbon fiber and polyurethane-coated carbon nanoparticles.
[0014] In a specific embodiment, the diameter of the carbon fiber in the amino-terminated dendrimer-modified carbon fiber is 5-12 μm.
[0015] Dendritic macromolecules are sensitive to steric hindrance. By limiting the size of carbon fibers, amino-terminated dendritic macromolecules modified carbon fibers and polyurethane coated with titanium dioxide are evenly dispersed in the polypropylene matrix, and the formed cross-linked network is more uniform with fewer defects. The resulting polypropylene film is stronger and tougher. The network of amino-terminated dendritic macromolecules modified carbon fibers and the network of polyurethane coated titanium dioxide particles have good cross-distribution. The resulting polypropylene film has a smooth surface, no bubbles or weld marks, good stress dissipation effect, small non-uniform tension, and is stronger, tougher and more stable.
[0016] In a specific embodiment, the particle size of the titanium dioxide particles in the polyurethane-coated titanium dioxide particles is 1-20 nm.
[0017] By adopting the above technical solution, the debonding effect of the interface between titanium dioxide particles and polyurethane is more obvious, the formed polypropylene grains are fine, and the dispersion is still relatively uniform after adding the amino-terminated dendritic macromolecule modified carbon fiber to the polypropylene system.
[0018] In a specific embodiment, the mass ratio of the amino-terminated dendritic macromolecule modified carbon fibers and the polyurethane-coated titanium dioxide particles in the core layer is (5-6):1.
[0019] By adopting the above technical solution, the formed cross-linked network is more uniform and has fewer defects, the yield deformation zones are interconnected, and the obtained polypropylene film is stronger and tougher. Therefore, the modification of the polypropylene film within the above range can achieve the best toughness effect.
[0020] In a specific embodiment, the polypropylene is a random copolymer polypropylene.
[0021] By adopting the above technical scheme, the obtained polypropylene film has good mechanical properties, the ethylene segments of the random copolymerized polypropylene are randomly dispersed in the propylene segments, which hinders the crystallization of the polypropylene segments, and the obtained polypropylene film has better toughness.
[0022] In a specific embodiment, the preparation method of amino-terminated dendritic macromolecule modified carbon fiber includes the following steps: putting the carbon fiber into a strong oxidizing acid for acidification to obtain acidified carbon fiber, putting the acidified carbon fiber into an amino-terminated dendritic macromolecule solution for reaction to obtain amino-terminated dendritic macromolecule modified carbon fiber.
[0023] By adopting the above technical scheme, the obtained terminal amino dendritic macromolecule modified carbon fiber has a three-dimensional structure, the terminal amino group activity is relatively high, it is easy to cross-link, the core layer has a low viscosity, unique rheological properties, and good film-forming properties, and the obtained dendritic macromolecule modified carbon fiber has a large number of functional groups and stable bonding.
[0024] Preferably, the polyurethane is polyether polyurethane.
[0025] The ether bond has low cohesive energy and is easy to rotate. The polypropylene film made by adding polyether polyurethane has higher toughness, the raw material system has lower viscosity, and the titanium dioxide particles are more evenly distributed, further improving the toughness of the polypropylene film.
[0026] In a second aspect, the present application provides a method for preparing a tough cast polypropylene film, using the following technical solution:
[0027] A method for preparing a tough cast polypropylene film comprises the following steps:
[0028] (1) weighing the raw materials of the heat seal layer, the core layer and the corona layer in corresponding weight portions according to the formula, co-extruding and cooling to shape;
[0029] (2) performing corona treatment on the surface of the corona layer of the film after cooling and setting to obtain the tough cast polypropylene film.
[0030] By adopting the above technical solution, the preparation method is simple, the obtained polypropylene cast film has a uniform structure, each layer is tightly combined, and is relatively strong.
[0031] In summary, this application has the following beneficial effects:
[0032] 1. The present application adds a certain mass of epoxidized polypropylene to the core layer and a certain mass of polyurethane-coated titanium dioxide particles to the core layer and the heat-sealing layer, so that a force is formed in the core layer and between the core layer and the heat-sealing layer to transmit stress, and the stress is consumed by debonding at the interface of titanium dioxide and polyurethane, which have different elasticity from the matrix, and the crystallization of polypropylene is adjusted by tiny titanium dioxide, so that the obtained polypropylene film is strong and tough, and cracks do not expand.
[0033] 2. This application adds amino-terminated dendritic macromolecules to modify carbon fibers in the core layer, further participates in the interlacing of the cross-linked network and polyurethane-coated titanium dioxide particles, and improves the toughness of the film through the combined action of epoxy polypropylene, amino-terminated dendritic macromolecules to modify carbon fibers, and polyurethane-coated titanium dioxide particles. By limiting the specifications of carbon fibers and titanium dioxide, the obtained polypropylene film is smoother and more flexible. DETAILED DESCRIPTION
[0034] The following is a more specific description of the technical solution of the present invention in combination with several specific implementation examples. The embodiments are only partial embodiments of the present invention, not all of them. The following specific embodiments can be combined with each other, and the same or similar concepts or processes therein may not be repeated in some embodiments.
[0035] Unless otherwise specified, the experimental reagents in the preparation examples, embodiments and comparative examples are conventional commercial brands or obtained through conventional preparation processes.
[0036] In the preparation examples, embodiments and comparative examples: the random copolymer polypropylene is ExxonMobil 9074MED; the polyurethane is Lubrizol ECO D12T90E; the carbon fiber in Preparation Example 2 and Preparation Example 8 is Mitsubishi TR 50S12L, and the carbon fiber in Preparation Example 3 is purchased from Jinchuan Carbon Fiber; the lubricant is purchased from Deyin Chemical DY-9238; the polyolefin elastomer is Dow ENGAGE TM 8400; aminosilane coupling agent is kh-550.
[0037] Preparation Example 1: Preparation Example of Epoxidized Polypropylene
[0038] 100g of propylene was added to gasoline, and then 20g of allyl glycidyl ether was added. After mixing, catalysts titanium trichloride and (C2H5)3Al were added. The temperature and pressure were raised to 60°C, and the reaction was carried out at 600kPa for 5h. The solvent was removed from the material to obtain epoxidized polypropylene.
[0039] Dendritic macromolecule modified carbon fiber is obtained by conventional preparation process:
[0040] Preparation Example 2: Preparation Example of Dendritic Macromolecule Modified Carbon Fiber
[0041] S1: 100g of carbon fiber was put into 1000g of 50wt% sulfuric acid, ultrasonically dispersed for 25 minutes at a frequency of 80KHz, heated under reflux at 80°C for 2h, washed twice with deionized water, and dried to obtain acidified carbon fiber;
[0042] S2: Add 70g of terminal amino hyperbranched polyether into methanol and stir evenly, then add 100g of the acidified carbon fiber prepared in S1, stir, ultrasonically disperse at 35KHz for 15 minutes, heat to 65°C, react, and after 20 minutes, wash alternately with methanol and deionized water for 4 times, and then dry at 50°C and vacuum degree of -0.1Mpa for 1 hour to obtain dendritic macromolecular modified carbon fiber.
[0043] The diameter of the carbon fiber filaments in this preparation example is 7 μm.
[0044] Preparation Example 3: Preparation Example of Dendritic Macromolecule Modified Carbon Fiber:
[0045] The only difference between this preparation example and preparation example 2 is that the diameter of the carbon fiber filaments is 15 μm.
[0046] Preparation Example 4: Preparation Example of Aminosilane-modified Polyurethane-coated Titanium Dioxide Particles:
[0047] S1: Place 150 g of titanium dioxide in a sand bath, introduce nitrogen protection, and activate at 250° C. for 5 hours to obtain activated titanium dioxide;
[0048] S2: Add 150g of the activated titanium dioxide prepared in S1 into a mixed solution of 350g of polyether polyol, 15g of N,N-dimethylcyclohexylamine, and 1200g of toluene diisocyanate, and disperse it ultrasonically at 25KHz for 1 hour. Then introduce nitrogen, stir at 70°C for 1 hour, react, continue nitrogen protection, slowly add 170g of aminosilane coupling agent, stir at 60°C for 1 hour, react, vacuum filter, and dry to obtain the aminosilane-modified polyurethane-coated titanium dioxide particles.
[0049] The particle size of the titanium dioxide particles in this preparation example is 10 nm.
[0050] Preparation Example 5: Preparation Example of Aminosilane-modified Polyurethane-coated Titanium Dioxide Particles:
[0051] The only difference between this preparation example and preparation example 4 is that the particle size of the titanium dioxide particles is 30 nm.
[0052] Preparation Example 6: Preparation Example of Aminosilane-modified Polyurethane-coated Titanium Dioxide Particles:
[0053] The only difference between this preparation example and preparation example 4 is that the particle size of the titanium dioxide particles is 0.1 nm.
[0054] Preparation Example 7: Preparation Example of Aminosilane-modified Polyurethane-coated Titanium Dioxide Particles:
[0055] The only difference between this preparation example and preparation example 4 is that the high temperature activation temperature is 220°C.
[0056] Preparation Example 8: Preparation Example of Silane-modified Carbon Fiber:
[0057] 30 g of silane coupling agent KH550 was added to 2000 g of ethanol, and the mixture was stirred evenly to obtain a mixed solution. 100 g of carbon fiber was added to the mixed solution, and the mixture was stirred for 2 hours at a stirring speed of 300 rpm. The mixture was filtered and dried to obtain silane-modified carbon fiber.
[0058] The diameter of the carbon fiber filaments in this preparation example is 7 μm.
[0059] Preparation Example 9: Preparation Example of Polyurethane-coated Titanium Dioxide Particles:
[0060] S1: Place 150g of titanium dioxide in a sand bath, introduce nitrogen protection, and activate at 250°C for 5 hours to obtain activated titanium dioxide; S2: Add 150g of the activated titanium dioxide prepared in S1 into a mixed solution of 350g of polyether polyol, 15g of N,N-dimethylcyclohexylamine, and 1200g of toluene diisocyanate, ultrasonically disperse at 25KHz for 1 hour, introduce nitrogen, stir at 70°C for 1 hour, react, vacuum filter, and dry to obtain the polyurethane-coated titanium dioxide particles.
[0061] Example
[0062] Example 1
[0063] In this embodiment, the tough cast polypropylene film is cast by three extruder heads of a melt extruder in a three-layer co-extrusion manner, and includes a heat sealing layer, a core layer and a corona layer from top to bottom.
[0064] The heat seal layer includes the following components: 70 kg of random copolymer polypropylene, 25 kg of polyolefin elastomer, 5 kg of lubricant, and 3 kg of aminosilane-modified polyurethane-coated titanium dioxide particles prepared in Preparation Example 4;
[0065] The core layer includes the following components: 100 kg of polypropylene, 12 kg of epoxidized polypropylene prepared in Preparation Example 1, and 22 kg of aminosilane-modified polyurethane-coated titanium dioxide particles prepared in Preparation Example 4;
[0066] The component of the corona layer is 100 kg of random copolymer polypropylene.
[0067] In this embodiment, the tough cast polypropylene film is prepared according to the following steps:
[0068] (1) The raw materials of the heat sealing layer, the core layer and the corona layer are weighed according to the formula and placed in an extruder, and after co-extrusion, they are cast and cooled to shape; wherein the temperatures of the three barrels of the extruder are evenly divided into the upper end, and the temperatures of each section are as follows: 220° C. for the first section, 255° C. for the second section, and 250° C. for the third section, and the die head temperature of the extruder is 240° C.; the surface temperature of the casting roll used in the casting is 15° C., the air knife is 90 cm away from the cooling roll, and the air knife forms an angle of 45° with the cooling roll, that is, the air knife forms an angle of 45° on the surface of the cooling roll and the vertical plane, and the air knife pressure is 5 mbar;
[0069] (2) The surface of the corona layer of the film after cast forming is subjected to corona treatment to form a strong and tough polypropylene film with a bottom thickness of 60 μm; wherein the power of the corona treatment is 8 kW, the pressure of the corona roller is 3 bar, the thickness of the heat sealing layer is 12 μm, the thickness of the core layer is 36 μm, and the thickness of the corona layer is 12 μm.
[0070] Example 2
[0071] The difference between this embodiment and embodiment 1 is that, in this embodiment,
[0072] The heat seal layer includes the following components: 80 kg of random copolymer polypropylene, 15 kg of polyolefin elastomer, 4 kg of lubricant, and 3 kg of aminosilane-modified polyurethane-coated titanium dioxide particles prepared in Preparation Example 4;
[0073] The core layer includes the following components: 100 kg of polypropylene, 25 kg of epoxidized polypropylene prepared in Preparation Example 1, and 20 kg of aminosilane-modified polyurethane-coated titanium dioxide particles prepared in Preparation Example 4;
[0074] The component of the corona layer is 100 kg of random copolymer polypropylene.
[0075] Example 3
[0076] The difference between this embodiment and embodiment 1 is that, in this embodiment,
[0077] The heat seal layer includes the following components: 75 kg of random copolymer polypropylene, 20 kg of polyolefin elastomer, 4 kg of lubricant, and 4 kg of aminosilane-modified polyurethane-coated titanium dioxide particles prepared in Preparation Example 4;
[0078] The core layer includes the following components: 100 kg of polypropylene, 20 kg of epoxidized polypropylene prepared in Preparation Example 1, and 24 kg of aminosilane-modified polyurethane-coated titanium dioxide particles prepared in Preparation Example 4;
[0079] The component of the corona layer is 100 kg of random copolymer polypropylene.
[0080] Example 4
[0081] The difference between this embodiment and embodiment 1 is that, in this embodiment,
[0082] The heat seal layer includes the following components: 75 kg of random copolymer polypropylene, 20 kg of polyolefin elastomer, 4 kg of lubricant, and 4 kg of aminosilane-modified polyurethane-coated titanium dioxide particles prepared in Preparation Example 4;
[0083] The core layer includes the following components: 100 kg of polypropylene, 20 kg of epoxidized polypropylene prepared in Preparation Example 1, and 24 kg of aminosilane-modified polyurethane-coated titanium dioxide particles prepared in Preparation Example 5;
[0084] The component of the corona layer is 100 kg of random copolymer polypropylene.
[0085] Example 5
[0086] The difference between this embodiment and embodiment 1 is that, in this embodiment,
[0087] The heat seal layer includes the following components: 75 kg of random copolymer polypropylene, 20 kg of polyolefin elastomer, 4 kg of lubricant, and 4 kg of aminosilane-modified polyurethane-coated titanium dioxide particles prepared in Preparation Example 4;
[0088] The core layer includes the following components: 100 kg of polypropylene, 20 kg of epoxidized polypropylene prepared in Preparation Example 1, and 24 kg of aminosilane-modified polyurethane-coated titanium dioxide particles prepared in Preparation Example 6;
[0089] The component of the corona layer is 100 kg of random copolymer polypropylene.
[0090] Example 6
[0091] The difference between this embodiment and embodiment 1 is that, in this embodiment,
[0092] The heat seal layer includes the following components: 75 kg of random copolymer polypropylene, 20 kg of polyolefin elastomer, 4 kg of lubricant, and 4 kg of aminosilane-modified polyurethane-coated titanium dioxide particles prepared in Preparation Example 4;
[0093] The core layer includes the following components: 100 kg of polypropylene, 20 kg of epoxidized polypropylene prepared in Preparation Example 1, and 24 kg of aminosilane-modified polyurethane-coated titanium dioxide particles prepared in Preparation Example 7;
[0094] The component of the corona layer is 100 kg of random copolymer polypropylene.
[0095] Example 7
[0096] The difference between this embodiment and embodiment 1 is that, in this embodiment,
[0097] The heat seal layer includes the following components: 75 kg of random copolymer polypropylene, 20 kg of polyolefin elastomer, 4 kg of lubricant, and 4 kg of aminosilane-modified polyurethane-coated titanium dioxide particles prepared in Preparation Example 4;
[0098] The core layer includes the following components: 100 kg of polypropylene, 20 kg of epoxidized polypropylene prepared in Preparation Example 1, 4 kg of aminosilane-modified polyurethane-coated titanium dioxide particles prepared in Preparation Example 4, and 20 kg of dendritic macromolecular modified carbon fibers prepared in Preparation Example 2; the component of the corona layer is 100 kg of random copolymer polypropylene.
[0099] Example 8
[0100] The difference between this embodiment and embodiment 1 is that, in this embodiment,
[0101] The heat seal layer includes the following components: 75 kg of random copolymer polypropylene, 20 kg of polyolefin elastomer, 4 kg of lubricant, and 4 kg of aminosilane-modified polyurethane-coated titanium dioxide particles prepared in Preparation Example 4;
[0102] The core layer includes the following components: 100 kg of polypropylene, 20 kg of epoxidized polypropylene prepared in Preparation Example 1, 4 kg of aminosilane-modified polyurethane-coated titanium dioxide particles prepared in Preparation Example 4, and 20 kg of dendritic macromolecular modified carbon fibers prepared in Preparation Example 3; the component of the corona layer is 100 kg of random copolymer polypropylene.
[0103] Example 9
[0104] The difference between this embodiment and embodiment 1 is that, in this embodiment,
[0105] The heat seal layer includes the following components: 75 kg of random copolymer polypropylene, 20 kg of polyolefin elastomer, 4 kg of lubricant, and 4 kg of aminosilane-modified polyurethane-coated titanium dioxide particles prepared in Preparation Example 4;
[0106] The core layer includes the following components: 100 kg of polypropylene, 20 kg of epoxidized polypropylene prepared in Preparation Example 1, 6 kg of aminosilane-modified polyurethane-coated titanium dioxide particles prepared in Preparation Example 4, and 18 kg of dendritic macromolecular modified carbon fibers prepared in Preparation Example 2; the component of the corona layer is 100 kg of random copolymer polypropylene.
[0107] Example 10
[0108] The difference between this embodiment and embodiment 1 is that, in this embodiment,
[0109] The heat seal layer includes the following components: 75 kg of random copolymer polypropylene, 20 kg of polyolefin elastomer, 4 kg of lubricant, and 4 kg of aminosilane-modified polyurethane-coated titanium dioxide particles prepared in Preparation Example 4;
[0110] The core layer includes the following components: 100 kg of polypropylene, 20 kg of epoxidized polypropylene prepared in Preparation Example 1, 4 kg of aminosilane-modified polyurethane-coated titanium dioxide particles prepared in Preparation Example 4, and 20 kg of silane-modified carbon fibers prepared in Preparation Example 8;
[0111] The component of the corona layer is 100 kg of random copolymer polypropylene.
[0112] Embodiment 11
[0113] The difference between this embodiment and embodiment 1 is that, in this embodiment,
[0114] The heat seal layer includes the following components: 75 kg of random copolymer polypropylene, 20 kg of polyolefin elastomer, 4 kg of lubricant, and 4 kg of aminosilane-modified polyurethane-coated titanium dioxide particles prepared in Preparation Example 4;
[0115] The core layer includes the following components: 100 kg of polypropylene, 20 kg of epoxidized polypropylene prepared in Preparation Example 1, 4 kg of aminosilane-modified polyurethane-coated titanium dioxide particles prepared in Preparation Example 4, and 20 kg of carbon fiber;
[0116] The component of the corona layer is 100 kg of random copolymer polypropylene.
[0117] Comparative Example
[0118] Comparative Example 1
[0119] The difference between this comparative example and Example 3 is that, in this example,
[0120] The heat seal layer includes the following components: 75 kg of random copolymer polypropylene, 20 kg of polyolefin elastomer, 4 kg of lubricant, and 4 kg of aminosilane-modified polyurethane-coated titanium dioxide particles prepared in Preparation Example 4;
[0121] The core layer includes the following components: 120 kg of polypropylene, 24 kg of aminosilane-modified polyurethane-coated titanium dioxide particles obtained in Preparation Example 4;
[0122] The component of the corona layer is 100 kg of random copolymer polypropylene.
[0123] Comparative Example 2
[0124] The difference between this comparative example and Example 3 is that, in this example,
[0125] The heat seal layer includes the following components: 75 kg of random copolymer polypropylene, 20 kg of polyolefin elastomer, 4 kg of lubricant, and 4 kg of aminosilane-modified polyurethane-coated titanium dioxide particles prepared in Preparation Example 4;
[0126] The core layer includes the following components: 100 kg of polypropylene, 20 kg of epoxidized polypropylene obtained in Preparation Example 1, 12 kg of polyurethane, and 12 kg of titanium dioxide;
[0127] The component of the corona layer is 100 kg of random copolymer polypropylene.
[0128] Comparative Example 3
[0129] The difference between this comparative example and Example 3 is that, in this example,
[0130] The heat seal layer includes the following components: 75 kg of random copolymer polypropylene, 20 kg of polyolefin elastomer, 5 kg of lubricant, and 3 kg of aminosilane-modified polyurethane-coated titanium dioxide particles prepared in Preparation Example 4;
[0131] The core layer includes the following components: 100 kg of polypropylene, 12 kg of epoxidized polypropylene prepared in Preparation Example 1, and 24 kg of polyurethane-coated titanium dioxide particles prepared in Preparation Example 9;
[0132] The component of the corona layer is 100 kg of random copolymer polypropylene.
[0133] Comparative Example 4
[0134] The difference between this comparative example and Example 3 is that, in this example,
[0135] The heat seal layer includes the following components: 75 kg of random copolymer polypropylene, 20 kg of polyolefin elastomer, 4 kg of lubricant, and 4 kg of aminosilane-modified polyurethane-coated titanium dioxide particles prepared in Preparation Example 4;
[0136] The core layer includes the following components: 100 kg of polypropylene, 20 kg of epoxidized polypropylene obtained in Preparation Example 1, and 24 kg of polyurethane;
[0137] The component of the corona layer is 100 kg of random copolymer polypropylene.
[0138] Performance testing methods
[0139] 1. Tensile properties
[0140] The tensile strength of the polypropylene films of the embodiments and comparative examples was tested according to "GB / T 13022-1991 Test method for tensile properties of plastic films". The test results are shown in Table 1.
[0141] 2. Falling dart impact strength
[0142] According to GB9639.1-2008 Test method for impact resistance of plastic films and sheets, the falling dart impact strength of the polypropylene films of the embodiments and comparative examples was measured at 23°C. The test results are shown in Table 1.
[0143] Table 1
[0144]
[0145]
[0146] In combination with Examples 1-3, Comparative Examples 1-4 and Table 1, the tough cast polypropylene film prepared in the present application has high tensile strength and good impact resistance.
[0147] In combination with Examples 3-5 and Table 1, the present application further improves the tensile strength and impact resistance of the obtained strong cast polypropylene film by limiting the particle size of the titanium dioxide particles.
[0148] In combination with Examples 3 and 6 and Table 1, the present application further improves the tensile strength and impact resistance of the obtained tough cast polypropylene film by limiting the activation temperature of the titanium dioxide particles.
[0149] In combination with Examples 3, 7, 10-11 and Table 1, the present application adds a certain mass of amino-terminated dendritic macromolecule-modified carbon fiber to the core layer, and through the combined effect of the carbon fiber and the polyurethane-coated titanium dioxide, the tensile strength and impact resistance of the obtained strong cast polypropylene film are greatly improved.
[0150] In combination with Examples 3 and 8 and Table 1, the present application improves the tensile strength and impact resistance of the obtained strong and tough cast polypropylene film to a limited extent by limiting the wire diameter of the carbon fiber.
[0151] In combination with Examples 3, 7, 9 and Table 1, the present application further improves the tensile strength and impact resistance of the obtained tough cast polypropylene film by limiting the mass ratio of the amino-terminated dendritic macromolecule modified carbon fiber and the polyurethane-coated titanium dioxide particles in the core layer.
[0152] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A tough cast polypropylene film, characterized in that: The invention comprises a heat-sealing layer, a core layer and a corona layer from top to bottom; the core layer comprises the following raw materials in parts by weight: 100 parts of polypropylene, 10-25 parts of epoxidized polypropylene, and 20-24 parts of fillers, wherein the fillers comprise polyurethane-coated titanium dioxide particles; the heat-sealing layer comprises the following raw materials in parts by weight: 70-80 parts of polypropylene, 15-25 parts of polyolefin elastomer, 1-5 parts of lubricant, and 2-5 parts of polyurethane-coated titanium dioxide particles; the polyurethane-coated titanium dioxide particles in the core layer and the heat-sealing layer are both modified with aminosilane; the preparation method of the polyurethane-coated titanium dioxide particles The method comprises the following steps: activating titanium dioxide particles at high temperature under the protection of nitrogen to obtain activated titanium dioxide, adding the activated titanium dioxide into a mixed solution of polyether polyol, catalyst and toluene diisocyanate, ultrasonically dispersing, introducing nitrogen, stirring at 65-70°C for 0.5-1.5 hours, reacting, continuing nitrogen protection, slowly adding an aminosilane coupling agent, stirring at 60-65°C for 0.5-1.5 hours, reacting, vacuum filtering, and drying to obtain the polyurethane-coated titanium dioxide particles; the high-temperature activation temperature is 240-260°C, and the activation time is 4.5-5.5 hours.
2. The tough cast polypropylene film according to claim 1, characterized in that: The core layer filler also includes: amino-terminated dendritic macromolecule modified carbon fiber.
3. The tough cast polypropylene film according to claim 2, characterized in that: The fiber diameter of the carbon fiber in the amino-terminated dendritic macromolecule modified carbon fiber is 5-12 μm.
4. The tough cast polypropylene film according to claim 2, characterized in that: The particle size of the titanium dioxide particles in the polyurethane-coated titanium dioxide particles is 1-20 nm.
5. The tough cast polypropylene film according to claim 2, characterized in that: The mass ratio of the amino-terminated dendritic macromolecule modified carbon fibers and the polyurethane-coated titanium dioxide particles in the core layer is (5-6):
1.
6. The tough cast polypropylene film according to claim 2, characterized in that: The preparation method of amino-terminated dendritic macromolecule modified carbon fiber comprises the following steps: putting carbon fiber into strong oxidizing acid for acidification to obtain acidified carbon fiber, putting acidified carbon fiber into amino-terminated dendritic macromolecule solution for reaction to obtain amino-terminated dendritic macromolecule modified carbon fiber.
7. The tough cast polypropylene film according to claim 1, characterized in that: The polypropylene is random copolymer polypropylene.
8. The method for preparing a tough cast polypropylene film according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: S1: weighing raw materials of a heat-sealing layer, a core layer and a corona layer in corresponding weight portions according to a formula, co-extruding, casting, cooling and shaping; S2: performing corona treatment on the surface of the corona layer of the film after casting, cooling and shaping to obtain the tough cast polypropylene film.
Citation Information
Cited By
Tape-casting polypropylene film and preparation method thereof
CN120329586A
A cast polypropylene film and a method for producing the same
CN120329586B