A method for preparing high-stability filler from red bed soft rock

By washing and compounding the red bed soft rock, combined with the use of solidifying agents such as steel slag powder, fly ash and quicklime, the construction problems caused by its instability were solved and the compressive strength and stability of the red bed soft rock were improved. It achieves efficient utilization of resources and improvement of construction performance.

CN118515459BActive Publication Date: 2024-10-11HUNAN RENJIAN DRY POWDER MORTAR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410977458.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-11
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

Due to its instability, the red layer soft rock is prone to cracking and mudification, which leads to problems such as settlement deformation and slope collapse during roadbed filling construction. It is difficult to effectively improve its stability and construction performance with existing technology, resulting in a waste of resources and increased construction. cost.

Method used

By washing the red bed soft rock and treating it with composite coal gangue powder, steel slag powder, graded particle size fly ash, quicklime and microsilica powder are used as curing agents to prepare high-stability fillers to improve its compressive strength and stability. .

Benefits of technology

It effectively improves the mechanical properties and stability of red layer soft rock, extends its application life, reduces environmental damage and construction costs, and expands its application scope in roadbed fillers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention provides a method for preparing high-stability filler from red-bed soft rock, and relates to the technical field of construction materials. The method for preparing high-stability filler from red-bed soft rock mainly comprises first washing the red-bed soft rock with water and then mixing it with coal gangue powder, then stirring it at high speed, and then continuing to mix steel slag powder, fly ash with graded particle size, quicklime and microsilica powder, and then adding water to configure it into a fluid material, and controlling the content of each component to obtain the final red-bed soft rock material. The present invention overcomes the shortcomings of the prior art, and produces a material with high stability by processing red-bed mud and sand and compounding multiple components. While effectively improving the overall mechanical properties of the material, the stability of the material is further improved, and the red-bed soft rock is efficiently utilized to reduce damage to the environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of construction materials, and in particular to a method for preparing high-stability filler from red layer soft rock. Background Art

[0002] Red-bed soft rock is mainly distributed in southern my country, including red-bed mudstone, red-bed sandstone, red-bed mudstone, etc. Its structural manifestations are mostly granular debris structure and mud cemented structure. Due to different structural composition and weathering degree, there are significant differences in its bearing capacity. The nature of red-bed soft rock is extremely unstable. It is very easy to crack and muddy when in contact with air, causing significant changes in the mechanical properties of the structure. Red-bed soft rock can generally be used as roadbed filling, slope, mine pit and cave backfill material. Using red-bed soft rock as roadbed filling is prone to cause different degrees of roadbed and pavement damage, mainly manifested as settlement deformation, slope collapse, etc.

[0003] At present, in order to ensure the quality of the project, many areas have abandoned red soft rock as roadbed material in road construction projects. However, in actual construction, if the red soft rock is completely abandoned, it will inevitably cause damage to the natural environment, lead to serious waste of resources, and significantly increase the cost of project construction. Therefore, it is of great practical significance to strengthen the structural characteristics of red soft rock as filler to achieve good road or construction performance. Summary of the invention

[0004] In view of the shortcomings of the prior art, the present invention provides a method for preparing high-stability fillers from red bed soft rock. By processing the red bed mud and sand and preparing the material in a fluid state through multi-component compounding, the overall mechanical properties of the material are effectively improved while further improving the stability of the material, thereby making efficient use of the red bed soft rock and reducing damage to the environment.

[0005] To achieve the above objectives, the technical solution of the present invention is implemented through the following technical solutions:

[0006] A method for preparing high-stability filler from red bed soft rock, the preparation method comprising the following steps:

[0007] S1. After crushing the red layer soft rock, wash and filter it, add coal gangue powder and mix it, self-compact and let it stand to obtain a preliminary mixture for use;

[0008] S2, stirring the above preliminary mixture to loosen it, and then crushing it through a 20-mesh sieve to obtain a crushed slurry for standby use;

[0009] S3, mixing the above-mentioned crushed slurry with steel slag powder and fly ash of graded particle size, stirring evenly, and then continuing to mix at an ash-water ratio of 1:0.5-2 to obtain a premix for standby use;

[0010] S4. Add quicklime, microsilica powder and high-efficiency water reducing agent to the above premix, continue to stir evenly and then grind through a 2-mesh sieve to obtain a high-stability filler.

[0011] Preferably, in step S1, the method of washing and filtering the red layer soft rock after crushing is to add 2-5 times the volume of clean water to the red layer soft rock, stir for 10-20 minutes and then filter.

[0012] Preferably, the amount of coal gangue added in step S1 is 1-5% of the mass of the red bed soft rock.

[0013] Preferably, the self-compacting standing time in step S1 is 10-20 hours, and the humidity of the mixture is maintained at 60-80% during the standing period.

[0014] Preferably, the stirring speed in step S2 is 120-160 r / min, and the stirring time is 10-20 min.

[0015] Preferably, in step S3, the steel slag powder is sieved through a 120-mesh sieve, and the amount of steel slag powder added is 2-4% of the total mass of the red bed soft rock.

[0016] Preferably, in step S3, the fly ash with a particle size distribution of 200-300 μm accounts for 40-60% of the total amount, the fly ash with a particle size of 80-150 μm accounts for 20-30% of the total amount, and the remaining fly ash has a particle size range of ≤45 μm.

[0017] Preferably, the amount of fly ash of graded particle size added in step S3 is 3-6% of the total mass of the red bed soft rock.

[0018] Preferably, in step S4, the amount of quicklime added is 1-3% of the total mass of the red bed soft rock, the amount of microsilica powder added is 0.8-2% of the total mass of the red bed soft rock, and the amount of high-efficiency water reducer added is 0-1% of the total mass of the red bed soft rock.

[0019] Preferably, the particle size of the microsilica powder in step S4 is 0.1-0.3 μm.

[0020] The present invention provides a method for preparing high-stability filler from red bed soft rock, which has the following advantages compared with the prior art:

[0021] The present invention prepares a fluid material by washing the red-bed soft rock with water and modifying it by high-speed stirring with composite coal gangue powder, and then combining steel slag powder, fly ash with graded particle size, quicklime and microsilica powder. The fluid material uses steel slag powder, fly ash with graded particle size, quicklime and microsilica powder as components of the curing agent, which effectively improves the compressive strength and stability of the red-bed soft rock after subsequent curing, improves the construction performance of the red-bed soft rock, enables road construction, further reduces the waste of environmental resources, ensures the full utilization of materials, reduces construction costs, and ensures construction safety. DETAILED DESCRIPTION

[0022] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention is clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] The raw materials in the following examples and comparative examples are:

[0024] 1. The main chemical composition of red bed soft rock is shown in Table 1:

[0025] Table 1

[0026]

[0027] 2. The main chemical composition of coal gangue powder is shown in Table 2:

[0028] Table 2

[0029]

[0030] 3. The main chemical composition of steel slag powder (passing 120 mesh sieve) is shown in Table 3 below:

[0031] Table 3

[0032]

[0033] 4. The main chemical components of fly ash are shown in Table 4 below:

[0034] Table 4

[0035]

[0036] The fly ash particle size is screened and reserved in three intervals: 200-300 μm, 80-150 μm, and less than or equal to 45 μm;

[0037] 5. The particle size of microsilica powder is 0.1-0.3μm, and the silicon content is greater than 80%.

[0038] Embodiment 1:

[0039] Preparation of red bed soft rock materials:

[0040] (1) After crushing the red soft rock, add 3 times the volume of clean water, stir for 15 minutes, filter, add coal gangue powder and mix, keep the humidity at 70%, self-compact and let stand for 15 hours to obtain the preliminary mixture for use;

[0041] (2) After the preliminary mixture is stirred loosely, it is stirred in a mixer at 160 r / min for 20 minutes, and then crushed through a 20-mesh sieve to obtain a crushed slurry for use;

[0042] (3) The above-mentioned crushed slurry is mixed with steel slag powder and fly ash (the fly ash with a particle size distribution of 200-300 μm accounts for 50% of the total amount, the fly ash with a particle size distribution of 80-150 μm accounts for 25% of the total amount, and the remaining fly ash particle size range is ≤45 μm) and stirred evenly to obtain a premix for use;

[0043] (4) Add quicklime, microsilica powder and polycarboxylic acid water reducer CP1801X to the above premix, continue to stir evenly and then continue to mix evenly according to the lime-water ratio of 1:1 to obtain red layer soft rock material.

[0044] And taking the red layer soft rock before crushing as a reference, the addition combination of each component shown in Table 5 below is set:

[0045] Table 5

[0046]

[0047] Comparative Example 1:

[0048] Preparation of red bed soft rock materials:

[0049] The red bed soft rock material was prepared according to the preparation method of the above-mentioned Example 1 and the raw material ratio of the experimental group 3, and the particle size range of the fly ash was controlled as shown in Table 6:

[0050] Table 6

[0051]

[0052] Comparative Example 2:

[0053] Preparation of red bed soft rock material (using the raw material ratio of experimental group 3 in the above embodiment 1):

[0054] (1) Crush the red soft rock and add coal gangue powder to mix, adjust the humidity to 70% and maintain it, self-compact and let it stand for 15 hours to obtain the preliminary mixture for use;

[0055] (2) After the preliminary mixture is stirred loosely, it is stirred in a mixer at 160 r / min for 20 minutes, and then crushed through a 20-mesh sieve to obtain a crushed slurry for use;

[0056] (3) The above-mentioned crushed slurry is mixed with steel slag powder and fly ash (the fly ash with a particle size distribution of 200-300 μm accounts for 50% of the total amount, the fly ash with a particle size distribution of 80-150 μm accounts for 25% of the total amount, and the remaining fly ash particle size range is ≤45 μm) and stirred evenly to obtain a premix for use;

[0057] (4) Add quicklime and microsilica powder to the above premix, continue to stir evenly, and then continue to mix evenly according to the lime-water ratio of 1:1 to obtain red layer soft rock material.

[0058] Comparative Example 3:

[0059] Preparation of red bed soft rock material (using the raw material ratio of experimental group 3 in the above embodiment 1):

[0060] (1) Add the red bed soft rock to the coal gangue powder and mix them, then crush them through a 20-mesh sieve to obtain crushed material;

[0061] (2) The above crushed materials are mixed with steel slag powder and fly ash (the fly ash with a particle size distribution of 200-300 μm accounts for 50% of the total amount, the fly ash with a particle size distribution of 80-150 μm accounts for 25% of the total amount, and the remaining fly ash particle size range is ≤45 μm) and stirred evenly to obtain a premix for use;

[0062] (3) Add quicklime and microsilica powder to the above premix, continue to stir evenly, and then continue to mix evenly according to the lime-water ratio of 1:1 to obtain red layer soft rock material.

[0063] Detection:

[0064] The red-layer soft rock materials prepared in the above experimental groups 1-6 and comparative examples 2-3 were tested as follows, with the red-layer soft rock as the control group:

[0065] 1. Refer to the requirements of "Testing Procedures for Stabilized Materials of Inorganic Binders for Highway Engineering" (JTG E51-2009) and "Soil Stabilization Admixtures" (CJ / T 486-2015) to test the unconfined compressive strength, shear strength and shrinkage performance of each group of red layer soft rock materials or red layer soft rock:

[0066] (1) Unconfined compressive strength test:

[0067] Set up samples: each group of red layer soft rock materials is loaded into the mold in layers, vibrated evenly by hand, and then left to stand for 24 hours for solidification. The solidified red sandstone slag is a cylindrical sample of Φ=39.1 mm, h=80 mm. Three parallel samples are set for each group of samples. After standing and demoulding, the samples are wrapped with plastic wrap to remove air and sealed. They are placed in a curing box at a constant temperature of 20±2℃ and a humidity of 90-95% for curing for 7 days. After that, they are taken out and the unconfined compressive strength of each group of specimens is tested using a YYW-2 strain-controlled unconfined pressure instrument.

[0068] (2) Shear strength test:

[0069] Set up samples: each group of red layer soft rock materials are loaded into the mold in layers and vibrated evenly by hand, then left to stand for 24 hours for solidification, and the solidified red sandstone slag is made into a cake-shaped sample with a size of Φ=61.8 mm and h=20 mm. Three parallel samples are set up for each group of samples. After standing and demoulding, the samples are wrapped with plastic wrap to remove air and sealed, placed in a curing box at a constant temperature of 20±2℃ and controlled to have a humidity of 90-95% for curing for 7 days, and then taken out; a ZJ strain-controlled direct shear apparatus is used to conduct a shear strength test on the specimens (the vertical pressure is set to 300 kPa);

[0070] (3) Shrinkage performance test:

[0071] Set up samples: put each group of red layer soft rock materials into the mold in layers and vibrate them evenly, then let them stand for 24 hours to solidify. Make the solidified red sandstone slag into cylindrical samples with Φ=150mm and h1=120mm. Set up 3 parallel samples for each group of samples. After standing and demoulding, wrap the samples with plastic wrap to remove air and seal them. Place them in a curing box and control the humidity to 90-95% at a constant temperature of 20±2℃ for 7 days. Then take them out and immerse each specimen in clean water. Control the clean water level to be 3-5cm higher than the specimen. Let them stand at room temperature at 20±2℃ for 5 days. Then take them out and measure the height of the specimen, recorded as h2. Calculate the shrinkage rate. The shrinkage rate is calculated as follows:

[0072] Shrinkage % = (h1-h2) / h1×100%;

[0073] The specific results are shown in Table 7 below:

[0074] Table 7

[0075]

[0076] 2. Test the stability and durability of each group of red bed soft rock materials:

[0077] (1) Water stability test:

[0078] Setting samples: each group of red layer soft rock materials were loaded into the mold in layers and vibrated evenly by hand, then left to solidify for 24 hours, and the solidified red sandstone slag was made into cylindrical samples of Φ=39.1 mm, h=80 mm. Six parallel samples were set for each group of samples. After standing and demoulding, the samples were wrapped with plastic wrap to remove air and sealed, and placed in a curing box at a constant temperature of 20±2℃ and humidity of 90-95% for curing for 6 days. Three samples in the same group continued to be cured for 1 day, and the other three samples were immersed in clean water for 1 day, and then taken out to test the unconfined compressive strength of the samples treated under different conditions in each group. The specific results are shown in Table 8 below:

[0079] Table 8

[0080]

[0081] It can be seen from the above table that due to the addition of a variety of ingredients with curing effects in the experimental group and the comparative example, after immersion in water, the moisture enhances the interaction between the red bed soft rock and the other components, and reacts thoroughly with water to form cementitious substances such as calcium silicate and calcium aluminate, thereby further improving the strength of the specimens.

[0082] (2) Dry-wet cycle performance test:

[0083] Set up samples: each group of red layer soft rock materials was loaded into the mold in layers and vibrated evenly by hand, then left to solidify for 24 hours. The solidified red sandstone slag was made into cylindrical samples with a diameter of Φ=39.1 mm and h=80 mm. Six parallel samples were set up for each group of samples. After standing and demoulding, the samples were wrapped with plastic wrap to remove air and sealed. They were placed in a curing box and maintained at a constant temperature of 20±2℃ and a humidity of 90-95% for 14 days. The samples were weighed and recorded as the initial weight. Three samples in the same group were taken out to directly test the unconfined compressive strength, and the other three samples were subjected to dry-wet cycle treatment. The dry-wet cycle method was to immerse the samples in clean water for 24 hours, then take them out and use a constant temperature drying oven at 45℃ to dry them to an initial weight error of ±2g. A total of 7 dry-wet cycles were performed, and the samples were taken out to test their unconfined compressive strength. The specific results are shown in Table 9 below:

[0084] Table 9

[0085]

[0086] From the above tests, it can be seen that the red layer soft rock materials prepared by experimental groups 1-3 can effectively improve the mechanical properties of the products, maintain the stability of the products, expand the application scope of red layer soft rock, and reduce the waste of resources.

[0087] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing high-stability filler from red bed soft rock, characterized in that: The preparation method comprises the following steps: S1. After crushing the red soft rock, wash and filter it, add coal gangue powder and mix it, self-compact and let it stand to obtain a preliminary mixture for use, and the amount of coal gangue added is 1-5% of the mass of the red soft rock; S2, stirring the above preliminary mixture until loose, and then crushing it through a 20-mesh sieve to obtain a crushed slurry for standby use; S3, mixing the above-mentioned crushed slurry with steel slag powder and graded particle size fly ash, stirring evenly, and then continuing to mix according to the ash-water ratio of 1:0.5-2 to obtain a premix for use, and the fly ash with a particle size distribution of 200-300 μm accounts for 40-60% of the total amount, the fly ash with a particle size of 80-150 μm accounts for 20-30% of the total amount, and the remaining fly ash particle size range is ≤45 μm, and the addition amount of steel slag powder is 2-4% of the total mass of the red bed soft rock, and the addition amount of graded particle size fly ash is 3-6% of the total mass of the red bed soft rock; S4. Add quicklime, microsilica powder and high-efficiency water reducing agent to the above premix, continue to stir evenly and then crush through a 2-mesh sieve to obtain a high-stability filler. The amount of quicklime added is 1-3% of the total mass of the red bed soft rock, the amount of microsilica powder added is 0.8-2% of the total mass of the red bed soft rock, and the amount of high-efficiency water reducing agent added is 0-1% of the total mass of the red bed soft rock.

2. The method for preparing high-stability filler from red bed soft rock according to claim 1, characterized in that: In the step S1, the red layer soft rock is crushed and then washed and filtered by adding 2-5 times the volume of clean water to the red layer soft rock, stirring for 10-20 minutes and then filtering.

3. The method for preparing high-stability filler from red bed soft rock according to claim 1, characterized in that: The self-compacting standing time in step S1 is 10-20 hours, and the humidity of the mixture is maintained at 60-80% during the standing time.

4. The method for preparing high-stability filler from red bed soft rock according to claim 1, characterized in that: The stirring speed in step S2 is 120-160 r / min, and the stirring time is 10-20 min.

5. The method for preparing high-stability filler from red bed soft rock according to claim 1, characterized in that: In the step S3, the steel slag powder is passed through a 120-mesh sieve.

6. The method for preparing high-stability filler from red bed soft rock according to claim 1, characterized in that: The particle size of the microsilica powder in step S4 is 0.1-0.3 μm.