A filling composition for improving the wear resistance of PE materials and its preparation method and application
By modifying SEBS elastomer and composite whiskers, a filler composition with excellent compatibility was prepared, which solved the problems of insufficient wear resistance and chemical resistance of polyethylene materials and achieved performance improvement of polyethylene materials.
Patent Information
- Application Number
- CN202410943417.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-15
AI Technical Summary
In the prior art, the filler composition has poor compatibility with polyethylene material, making it difficult to effectively improve the wear resistance and chemical resistance of polyethylene material, affecting its performance and processability, and failing to meet process and environmental requirements.
A modified SEBS elastomer and composite whiskers were used. The SEBS elastomer was grafted with acryloyloxypropyltrimethoxysilane and the potassium titanate whiskers were wet-processed with magnesium hexafluorosilicate to prepare a filler composition with excellent compatibility. Accelerators, antioxidants and fillers were added to improve the wear resistance and chemical resistance of PE materials.
It significantly improves the wear resistance and chemical stability of polyethylene materials, enhances their mechanical properties and service life, improves compatibility with polyethylene materials, and improves overall performance.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a filling composition for improving the wear resistance of PE materials, and a preparation method and application thereof. Background Art
[0002] PE material is a thermoplastic resin made from ethylene monomers through polymerization. This material is odorless and non-toxic, feels like wax, and exhibits excellent low-temperature resistance, with a minimum operating temperature of -100~-70°C. Polyethylene has very good chemical stability and can withstand the erosion of most acids and alkalis (not resistant to acids with oxidizing properties). At room temperature, polyethylene is insoluble in general solvents, has low water absorption, and has excellent electrical insulation. Due to its unique physical and chemical properties, polyethylene has a wide range of uses, mainly used to make films, packaging materials, containers, pipes, monofilaments, wires and cables, daily necessities, etc., and can be used as high-frequency insulation materials for televisions, radars, etc.
[0003] Polyethylene can be divided into many types according to different polymerization methods and molecular structures, including linear low-density polyethylene (LLDPE), low-density polyethylene (LDPE), high-density polyethylene (HDPE), etc. These different types of polyethylene differ in structure, performance and application. For example, LLDPE has a narrower molecular weight distribution and linear structure than general LDPE, which makes it have excellent resistance to environmental stress cracking, low-temperature impact resistance and warping resistance, and is suitable for pipe, sheet extrusion and all molding applications. HDPE has good thermal, electrical and mechanical properties, as well as good heat resistance and corrosion resistance, and is suitable for films, pipes, injection daily necessities and other fields.
[0004] However, with the development of science and technology, the demand for mechanical and chemical properties of polyethylene materials is also increasing. Therefore, various filler compositions are often added to polyethylene in the prior art to improve the various properties of polyethylene.
[0005] However, the filler compositions in the prior art have poor compatibility with polyethylene materials and are difficult to be effectively compounded in polyethylene materials. Not only can they not effectively improve the performance of polyethylene materials, but they will affect their own performance and processability. In addition, the filler compositions in the prior art have limited effect on improving the wear resistance and chemical resistance of polyethylene materials and cannot meet the requirements of various processes and environments.
[0006] Therefore, there is an urgent need for a filling composition that can effectively improve the wear resistance and chemical resistance of polyethylene materials and has excellent compatibility with polyethylene materials. Summary of the invention
[0007] In view of the defects of the prior art, the purpose of the present invention is to provide a filling composition for improving the wear resistance of polyethylene materials, which can effectively improve the wear resistance and chemical resistance of polyethylene materials and has excellent compatibility with polyethylene materials, and a preparation method and application thereof.
[0008] A filling composition for improving the wear resistance of PE materials comprises a modified SEBS elastomer, a composite whisker, a accelerator, an antioxidant and a filler; the modified SEBS elastomer is prepared by grafting acryloxypropyltrimethoxysilane onto the SEBS elastomer; and the composite whisker is prepared by wet-process modification of potassium titanate whiskers and magnesium hexafluorosilicate.
[0009] The SEBS elastomer in the present invention has good compatibility with PE materials. By using the modified SEBS elastomer as the main component, the filling composition can be effectively compounded in the PE material, thereby improving various properties of the PE material. In addition, based on the excellent weather resistance, high and low temperature resistance and easy processing performance of the SEBS elastomer, the mechanical properties and chemical properties of the PE material can be significantly improved.
[0010] Furthermore, the modified SEBS elastomer is prepared by the following steps: adding acryloxypropyltrimethoxysilane, an initiator and an organic solvent into a reactor, adding SEBS elastomer after stirring and mixing evenly, transferring to a twin-screw extruder, and performing extrusion granulation to obtain the modified SEBS elastomer.
[0011] The present invention grafts and modifies SEBS elastomer by acryloxypropyltrimethoxysilane, and the siloxane structure can be cross-linked inside the SEBS elastomer to form a network siloxane structure with excellent stability, which can not only be used as a filler to significantly improve the wear resistance of PE materials, but also improve the overall chemical resistance of PE materials.
[0012] Furthermore, the number average molecular weight of the SEBS elastomer is 400,000-600,000; the initiator is selected from one of azobisisobutyronitrile, azobisisoheptanenitrile or benzoyl peroxide; and the mass ratio of acryloxypropyltrimethoxysilane to SEBS elastomer is 3-5:15.
[0013] Furthermore, the screw feeding section temperature of the twin-screw extruder is 170-190°C, the conveying section temperature is 190-195°C, the melting section temperature is 200-210°C, the die head temperature is 200-205°C, and the screw speed is 200-240r / min.
[0014] Furthermore, the composite whisker is prepared by the following steps: adding magnesium hexafluorosilicate and deionized water into a reactor, stirring and dissolving, then adding potassium titanate whisker, heating to 60-70°C, stirring and reacting at 120-140 r / min for 2-3 hours, cooling, filtering, washing and drying to obtain the composite whisker.
[0015] The invention can further improve the chemical resistance and wear resistance of the PE material based on the excellent chemical stability and mechanical properties of the potassium titanate whisker.
[0016] The present invention wet-modifies potassium titanate whiskers by magnesium hexafluorosilicate. On the one hand, magnesium hexafluorosilicate with polyfluorosilicon branches can improve the dispersibility of potassium titanate whiskers and avoid agglomeration of fine potassium titanate whiskers to affect overall performance. On the other hand, the chemical stability of potassium titanate whiskers can be improved by the fluorine-silicon bonds in magnesium hexafluorosilicate, so that the filling composition can further improve the chemical resistance of PE materials and extend the service life of the device.
[0017] Furthermore, the mass ratio of the potassium titanate whiskers to the magnesium hexafluorosilicate is 6-8:1.
[0018] Furthermore, the promoter is selected from one of triethanolamine, triethylenediamine or dibutyltin dilaurate; the antioxidant is selected from one of antioxidant 1010, antioxidant BHT or sodium metabisulfite; and the filler is selected from one of kaolin, diatomaceous earth or talc.
[0019] Furthermore, based on the total mass fraction being 100%, the mass percentage of each component is:
[0020] Modified SEBS elastomer 25-30%
[0021] Composite whisker 8-12%
[0022] Accelerator 3-5%
[0023] Antioxidant 1-3%
[0024] The balance is filler.
[0025] The preparation method of any of the above-mentioned filling compositions for improving the wear resistance of PE materials comprises the following steps: adding a modified SEBS elastomer, a accelerator, an antioxidant and a filler into a reactor, stirring evenly and heating to 50-60°C, adding composite whiskers, and shearing at 1200-1500 r / min for 1-2 hours to obtain the filling composition for improving the wear resistance of PE materials.
[0026] Application of any one of the above-mentioned filling compositions for improving the wear resistance of PE materials in PE materials.
[0027] Beneficial effects: (1) The filler composition for improving the wear resistance of PE materials provided by the present invention is prepared by adding a modified SEBS elastomer and a composite whisker with excellent wear resistance and a promoter, an antioxidant and a filler. The filler composition has good compatibility with PE materials, can not only improve the wear resistance and anti-aging ability of PE materials, but also enhance the chemical stability of PE materials and increase the service life. The filler composition can be widely used in the field of PE materials.
[0028] (2) The present invention provides a filling composition for improving the wear resistance of PE materials. The SEBS elastomer has good compatibility with the PE material. By using the modified SEBS elastomer as the main component, the filling composition can be effectively compounded in the PE material, thereby improving various properties of the PE material. In addition, based on the excellent weather resistance, high and low temperature resistance and easy processing performance of the SEBS elastomer, the mechanical properties and chemical properties of the PE material can be significantly improved.
[0029] (3) The present invention provides a filler composition for improving the wear resistance of PE materials. SEBS elastomer is grafted with acryloxypropyltrimethoxysilane, and its siloxane structure can be cross-linked inside the SEBS elastomer to form a network siloxane structure with excellent stability. It can not only be used as a filler to significantly improve the wear resistance of PE materials, but also improve the overall chemical resistance of PE materials.
[0030] (4) The present invention provides a filler composition for improving the wear resistance of PE materials, which can further improve the chemical resistance and wear resistance of PE materials based on the excellent chemical stability and mechanical properties of potassium titanate whiskers;
[0031] (5) The present invention provides a filling composition for improving the wear resistance of PE materials. Potassium titanate whiskers are wet-modified by magnesium hexafluorosilicate. On the one hand, magnesium hexafluorosilicate with polyfluorosilicon branches can improve the dispersibility of potassium titanate whiskers and avoid agglomeration of fine potassium titanate whiskers, which affects the overall performance. On the other hand, the fluorine-silicon bonds in magnesium hexafluorosilicate can improve the chemical stability of potassium titanate whiskers, thereby enabling the filling composition to further improve the chemical resistance of PE materials and extend the service life of the device. DETAILED DESCRIPTION
[0032] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0033] The commercially available wear-resistant additive was American Solvay POLYMIST® PTFE XPP 545 purchased from Guangzhou Jiushun New Materials Co., Ltd.; the remaining reagents and equipment were conventional reagents and equipment in the technical field.
[0034] Preparation of modified SEBS elastomer-1
[0035] Modified SEBS elastomer-1 was prepared by the following steps:
[0036] In the reactor, 4 g of acryloxypropyltrimethoxysilane, 0.3 g of azobisisobutyronitrile and 100 mL of butanone were added, and 15 g of SEBS elastomer was added after stirring and mixed evenly. The mixture was transferred to a twin-screw extruder, and extrusion granulation was carried out under the conditions of a feeding section temperature of 180° C., a conveying section temperature of 195° C., a melting section temperature of 210° C., a die head temperature of 200° C., and a screw speed of 240 r / min to obtain the modified SEBS elastomer-1.
[0037] Preparation of modified SEBS elastomer-2
[0038] The preparation method is basically the same as that of modified SEBS elastomer-1, except that acryloxypropyltrimethoxysilane is replaced by an equal amount of maleic anhydride.
[0039] Preparation of composite whiskers-1
[0040] Composite whisker-1 was prepared by the following steps:
[0041] In a reactor, 1 part of magnesium hexafluorosilicate and deionized water were added by weight, and 8 parts of potassium titanate whiskers were added after stirring to dissolve. The temperature was raised to 70° C., and the reaction was stirred at 130 r / min for 3 hours. After cooling, filtering, washing and drying, the composite whisker-1 was obtained.
[0042] Preparation of composite whiskers-2
[0043] The preparation is basically the same as that of composite whisker-1, except that magnesium hexafluorosilicate is replaced by an equal amount of magnesium silicate.
[0044] Example 1
[0045] The filling composition for improving the wear resistance of PE material is prepared by the following steps:
[0046] In a reactor, a modified SEBS elastomer, triethanolamine, antioxidant 1010 and kaolin are added, stirred evenly and then heated to 60° C., composite whisker-1 is added, and sheared at 1400 r / min for 2 hours to obtain the filler composition for improving the wear resistance of PE materials;
[0047] Taking the total mass fraction as 100%, the mass percentage of each component is:
[0048] Modified SEBS elastomer-1 30%
[0049] Composite Whiskers -1 10%
[0050] Triethanolamine 4%
[0051] Antioxidant 1010 2%
[0052] The balance is kaolin.
[0053] Example 2
[0054] The same as Example 1, except that, based on the total mass fraction being 100%, the components and their mass percentages are as follows:
[0055] Modified SEBS elastomer-1 25%
[0056] Composite Whisker-1 12%
[0057] Triethylenediamine 5%
[0058] Antioxidant BHT 1%
[0059] The balance is talc.
[0060] Example 3
[0061] The same as Example 1, except that, based on the total mass fraction being 100%, the components and their mass percentages are as follows:
[0062] Modified SEBS elastomer-1 28%
[0063] Composite Whiskers -1 8%
[0064] Dibutyltin dilaurate 3%
[0065] Sodium metabisulfite 3%
[0066] The balance was diatomaceous earth.
[0067] Comparative Example 1
[0068] Commercially available anti-wear additives.
[0069] Comparative Example 2
[0070] The method is basically the same as Example 1, except that the modified SEBS elastomer-1 is replaced by an equal amount of SEBS elastomer.
[0071] Comparative Example 3
[0072] The method is basically the same as Example 1, except that the modified SEBS elastomer-1 is replaced by an equal amount of modified SEBS elastomer-2.
[0073] Comparative Example 4
[0074] The method is basically the same as Example 1, except that the composite whisker-1 is replaced with an equal amount of filler.
[0075] Comparative Example 5
[0076] The method is basically the same as Example 1, except that the composite whisker-1 is replaced by an equal amount of composite whisker-2.
[0077] Performance Testing
[0078] By weight, 15 parts of the products of Examples 1-3 and Comparative Examples 1-5 were mixed with 85 parts of polyethylene material, and the modified polyethylene material was obtained after melt mixing and extrusion granulation in a twin-screw extruder.
[0079] Tensile strength test: According to the test standard of GB / T 1040-1992 Plastic tensile test method, the tensile strength of the modified polyethylene material prepared above was tested respectively.
[0080] Chemical resistance test: The modified polyethylene materials prepared above were placed in a xylene solution, and after standing for 72 hours, the tensile strength of the modified polyethylene materials was tested again according to the test standard of GB / T 1040-1992 Plastic Tensile Test Method.
[0081] Wear resistance test: According to the test standard of GB / T 3960-2016 Test method for sliding friction and wear of plastics, the volume wear of the modified polyethylene materials prepared above was tested respectively.
[0082] The test results are shown in the following table:
[0083]
[0084] According to the comparison of the test results of Examples 1-3 with those of Comparative Example 1, it can be seen that the filling composition provided by the present invention can more effectively improve the wear resistance and chemical resistance of the PE material than the wear-resistant additives in the prior art.
[0085] According to the comparison of the test results of Examples 1-3 and Comparative Examples 2-3, it can be seen that the modified SEBS elastomer in the filling composition provided by the present invention can effectively improve its compatibility with the PE material, and further can effectively enhance the wear resistance and chemical resistance of the PE material.
[0086] According to the comparison of the test results of Examples 1-3 and Comparative Examples 4-5, it can be seen that the composite whiskers in the filling composition provided by the present invention can further improve the wear resistance and chemical resistance of the PE material.
[0087] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A filling composition for improving the wear resistance of PE materials, characterized in that: Contains modified SEBS elastomer, composite whisker, accelerator, antioxidant and filler; The modified SEBS elastomer is prepared by grafting and modifying SEBS elastomer with acryloxypropyltrimethoxysilane; The composite whisker is prepared by wet modification of potassium titanate whisker and magnesium hexafluorosilicate; Taking the total mass fraction as 100%, the mass percentage of each component contained in the filling composition is: Modified SEBS elastomer 25-30% Composite whisker 8-12% Accelerator 3-5% Antioxidant 1-3% The balance is filler.
2. The filler composition for improving the wear resistance of PE material according to claim 1, characterized in that: The modified SEBS elastomer is prepared by the following steps: adding acryloxypropyltrimethoxysilane, an initiator and an organic solvent into a reactor, adding SEBS elastomer after stirring and mixing evenly, transferring to a twin-screw extruder, and performing extrusion granulation to obtain the modified SEBS elastomer.
3. The filler composition for improving the wear resistance of PE material according to claim 2, characterized in that: The number average molecular weight of the SEBS elastomer is 400,000-600,000; the initiator is selected from one of azobisisobutyronitrile, azobisisoheptanenitrile or benzoyl peroxide; the mass ratio of the acryloxypropyltrimethoxysilane to the SEBS elastomer is 3-5:
15.
4. The filler composition for improving the wear resistance of PE material according to claim 2, characterized in that: The twin-screw extruder has a screw feeding section temperature of 170-190°C, a conveying section temperature of 190-195°C, a melting section temperature of 200-210°C, a die head temperature of 200-205°C, and a screw speed of 200-240r / min.
5. The filler composition for improving the wear resistance of PE material according to claim 1, characterized in that: The composite whisker is prepared by the following steps: adding magnesium hexafluorosilicate and deionized water into a reactor, stirring and dissolving, then adding potassium titanate whisker, heating to 60-70° C., stirring and reacting at 120-140 r / min for 2-3 hours, cooling, filtering, washing and drying to obtain the composite whisker.
6. The filler composition for improving the wear resistance of PE material according to claim 5, characterized in that: The mass ratio of the potassium titanate whisker to the magnesium hexafluorosilicate is 6-8:
1.
7. The filler composition for improving the wear resistance of PE material according to claim 1, characterized in that: The accelerator is selected from one of triethanolamine, triethylenediamine or dibutyltin dilaurate; the antioxidant is selected from one of antioxidant 1010, antioxidant BHT or sodium pyrosulfite; the filler is selected from one of kaolin, diatomaceous earth or talc.
8. The method for preparing the filling composition for improving the wear resistance of PE material according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: adding modified SEBS elastomer, accelerator, antioxidant and filler into a reactor, stirring evenly and heating to 50-60°C, adding composite whisker and shearing for 1-2 hours at 1200-1500 r / min to obtain the filling composition for improving the wear resistance of PE material.
9. Use of the filling composition for improving the wear resistance of PE materials according to any one of claims 1 to 7 in PE materials.