A chemical mechanical polishing liquid

By adding abrasive particles, anionic surfactant, complexing agent and other components to the CMP polishing liquid, the problems in the prior art that the Cu film removal rate, the selectivity of the blocking material and the static etching rate are difficult to meet at the same time, and high efficiency is achieved , low defect polishing effect.

CN118516045BActive Publication Date: 2024-11-29QIXINWEI (SHAOXING) ELECTRONIC MATERIALS TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410970119.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-29
Estimated Expiration
2044-07-19

AI Technical Summary

Technical Problem

During the manufacturing process of copper interconnect structures, existing CMP polishing liquids are difficult to meet the requirements of high Cu film removal rate, high selectivity for barrier materials and low Cu static etching rate, and are prone to defects such as disc grooves and scratches. mark.

Method used

Using a chemical mechanical polishing liquid, including abrasive particles, anionic surfactant, complexing agent, oxidant, corrosion inhibitor, o-diamine salt and water, by adjusting the content of each component, a stable solution is formed and Cu is improved. Polishing rate, suppresses the polishing rate of the blocking material, and reduces the occurrence of defects during the polishing process.

Benefits of technology

High Cu removal rate and low Cu static etch rate are achieved, which suppresses the polishing rate of the blocking material, reduces the generation of defects during the polishing process, and meets the needs of advanced node copper and through-silicon CMP applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_4
    Figure SMS_4
  • Figure SMS_5
    Figure SMS_5
Patent Text Reader

Abstract

The invention discloses a chemical mechanical polishing liquid, comprising silicon dioxide abrasive particles, anionic surfactant, complexing agent, oxidant, corrosion inhibitor, ortho-diamine salt and water. The chemical mechanical polishing liquid of the invention can improve the polishing rate of Cu film, inhibit the polishing rate of barrier material, and reduce the generation of defects such as dished grooves and scratches during the polishing process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polishing liquid, and in particular to a chemical mechanical polishing liquid. Background Art

[0002] With the rapid development of semiconductor technology, the integration and performance requirements of integrated circuits are constantly increasing, making the manufacturing process of semiconductor wafers increasingly complex and sophisticated. Among them, copper (Cu), as an ideal interconnect material, has been widely used in advanced integrated circuit manufacturing due to its low resistivity, high reliability and scalability. However, in the manufacturing process of copper interconnect structures, the copper chemical mechanical planarization (CMP) process is a key step to ensure the surface flatness of the copper layer and remove excess copper layers.

[0003] As technology nodes continue to shrink, the performance requirements for CMP polishing liquids are getting higher and higher. Although some CMP polishing liquids have tried to meet the above requirements by adding different additive components, these methods often have some problems. For example, although some polishing liquids have a high Cu film removal rate, they have poor selectivity for barrier materials and are prone to material loss; while other polishing liquids have good selectivity for barrier materials, but have a high Cu static etching rate, which is prone to over-etching and copper ion contamination.

[0004] Therefore, how to develop a new type of CMP polishing liquid that can meet the requirements of high Cu film removal rate, high selectivity to barrier materials and low Cu static etching rate while maintaining low defect rate has become an urgent problem to be solved in the current semiconductor manufacturing field. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the present invention provides a chemical mechanical polishing solution, which can improve the polishing rate of the Cu film, inhibit the polishing rate of the barrier material, and reduce the generation of defects such as dishing grooves and scratches during the polishing process.

[0006] To achieve the above object, the embodiments of the present invention adopt the following technical solutions:

[0007] A chemical mechanical polishing liquid comprises abrasive particles, anionic surfactant, complexing agent, oxidant, corrosion inhibitor, ortho-diamine salt and water.

[0008] According to one aspect of the present invention, the chemical mechanical polishing liquid includes 0.5%-3% by mass of abrasive particles, 0.05%-4.0% by mass of anionic surfactant, 0.05%-8% by mass of complexing agent, 0.5%-3% by mass of oxidant, 0.05%-1% by mass of corrosion inhibitor, 0.005%-2% by mass of o-diamine salt and pH regulator, and the balance is water.

[0009] According to one aspect of the present invention, the molecular structure of the ortho-diamine salt is: , where anion Y - Selected from one or more of bicarbonate, hydroxide, p-toluenesulfonate and / or bitartrate; n is 1 or 2.

[0010] According to one aspect of the present invention, the ortho-diamine salt includes but is not limited to the following optical isomers and mixtures thereof: R, R configuration, S, S configuration, R, S configuration and / or S, R configuration.

[0011] According to one aspect of the present invention, the complexing agent is one or a combination of glycine, D-alanine, L-alanine, DL-alanine, β-alanine, N,N-dihydroxyethylglycine, tri(hydroxymethyl)methylglycine, sarcosine, valine, leucine, isoleucine, proline, serine, threonine, tyrosine, glutamine, asparagine, tryptophan, histidine, arginine, lysine, methionine, cysteine ​​and / or iminodiacetic acid.

[0012] According to one aspect of the present invention, the optical configuration of the complexing agent is D configuration, L configuration or DL ​​racemate.

[0013] According to one aspect of the present invention, the anionic surfactant is an anionic polymer or its aqueous solution, and the anionic polymer is one of dodecylbenzenesulfonic acid, dodecylsulfonic acid, methylenebisnaphthalenesulfonic acid, alkyl phosphate diethanolamine salt, alkyl phosphate triethanolamine salt, polyol phosphate, glycerol polyoxypropylene ether phosphate triethanolamine salt, acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer, polyacrylic acid and / or anionic polyacrylamide, or a combination thereof.

[0014] According to one aspect of the present invention, the corrosion inhibitor is one or a combination of 1,2,4-triazole, aminotriazole (or 3-amino-1,2,4-triazole), 3,5-diimino-1,2,4-triazole, benzotriazole or benzotriazole derivatives, tetrazole or tetrazole derivatives, imidazole or imidazole derivatives, benzimidazole or benzimidazole derivatives, pyrazole or pyrazole derivatives and / or tetrazole or tetrazole derivatives.

[0015] According to one aspect of the present invention, the oxidant is one or a combination of periodic acid, hydrogen peroxide, peracetic acid, potassium iodate, potassium periodate, ammonium persulfate, ammonium molybdate, ammonium nitrate, nitric acid, potassium nitrate, and organic peroxides.

[0016] According to one aspect of the present invention, the abrasive particles are silicon dioxide, and the average particle size of the abrasive particles is 50-300 nanometers, and the average grain size is 20-150 nanometers.

[0017] According to one aspect of the present invention, the pH adjusting agent is an inorganic acid, an organic acid, an alkali solution or a combination thereof. Specifically, the inorganic acid may be nitric acid, hydrochloric acid, sulfuric acid and / or phosphoric acid. The alkali solution is an inorganic base, such as sodium hydroxide, potassium hydroxide, ammonium hydroxide and / or ammonia water.

[0018] According to one aspect of the present invention, the pH value of the chemical mechanical polishing solution is 5-10.

[0019] According to one aspect of the present invention, the chemical mechanical polishing solution further includes an antibacterial agent and / or a viscosity regulator.

[0020] Advantages of the present invention: The chemical mechanical polishing solution uses a complexing agent to react with copper ions to form a compound, thereby accelerating the copper polishing rate. At the same time, an anionic surfactant can be used to reduce the metal etching rate to obtain a flatter surface, and is compounded with an ortho-diamine salt to form a passivation layer during the chemical mechanical polishing process. By adjusting the content of each substance, a stable solution is formed to meet the high Cu removal rate and low Cu static etching rate required for advanced node copper and silicon through hole CMP applications, inhibit the polishing rate of the blocking material, and reduce the generation of defects such as dishing grooves and scratches during the polishing process. DETAILED DESCRIPTION

[0021] The technical solutions in the embodiments of the present invention are described clearly and completely. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] A chemical mechanical polishing liquid comprises abrasive particles, anionic surfactants, complexing agents, oxidants, corrosion inhibitors, ortho-diamine salts and water. Specifically, the chemical mechanical polishing liquid comprises 0.5%-3% by mass of abrasive particles, 0.05%-4.0% by mass of anionic surfactants, 0.05%-8% by mass of complexing agents, 0.5%-3% by mass of oxidants, 0.05%-1% by mass of corrosion inhibitors, 0.005%-2% by mass of ortho-diamine salts and pH regulators, and the balance is water.

[0023] In practical applications, the chemical mechanical polishing liquid can significantly increase the polishing rate of silica abrasive particles on Cu, inhibit the polishing rate of barrier materials (such as Ta, TaN, Ti, TiN and SiN), and avoid or reduce the generation of defects such as dishing grooves and scratches during the polishing process.

[0024] In practical applications, the molecular structure of the ortho-diamine salt is: , where anion Y -Selected from one or more of bicarbonate, hydroxide, p-toluenesulfonate and / or bitartrate; n is 1 or 2.

[0025] In practical applications, the complexing agent is one or a combination of glycine, D-alanine, L-alanine, DL-alanine, β-alanine, N,N-dihydroxyethylglycine, tri(hydroxymethyl)methylglycine, sarcosine, valine, leucine, isoleucine, proline, serine, threonine, tyrosine, glutamine, asparagine, tryptophan, histidine, arginine, lysine, methionine, cysteine ​​and / or iminodiacetic acid. The complexing agent is D configuration, L configuration or DL ​​racemate.

[0026] In practical applications, the anionic surfactant is an anionic polymer or its aqueous solution, and the anionic polymer is one of dodecylbenzenesulfonic acid, dodecylsulfonic acid, methylenebisnaphthalenesulfonic acid, alkyl phosphate diethanolamine salt, alkyl phosphate triethanolamine salt, polyol phosphate, glycerol polyoxypropylene ether phosphate triethanolamine salt, acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer, polyacrylic acid and / or anionic polyacrylamide, or a combination thereof.

[0027] In practical applications, the corrosion inhibitor is one or a combination of 1,2,4-triazole, aminotriazole (or 3-amino-1,2,4-triazole), 3,5-diimino-1,2,4-triazole, benzotriazole or benzotriazole derivatives, tetrazole or tetrazole derivatives, imidazole or imidazole derivatives, benzimidazole or benzimidazole derivatives, pyrazole or pyrazole derivatives and / or tetrazole or tetrazole derivatives.

[0028] In practical applications, the oxidant is one or a combination of periodic acid, hydrogen peroxide, peracetic acid, potassium iodate, potassium periodate, ammonium persulfate, ammonium molybdate, ammonium nitrate, nitric acid, potassium nitrate and / or organic peroxides.

[0029] In practical applications, the abrasive particles are silicon dioxide, the average particle size of the abrasive particles is 50-300 nanometers, and the average grain size is 20-150 nanometers.

[0030] In practical applications, the pH adjuster is an inorganic acid, an organic acid, an alkali solution or a combination thereof. Specifically, the inorganic acid may be nitric acid, hydrochloric acid, sulfuric acid and / or phosphoric acid. Alternatively, the alkali solution is an inorganic base, such as sodium hydroxide, potassium hydroxide, ammonium hydroxide and / or ammonia water.

[0031] In practical applications, the pH value of the chemical mechanical polishing solution is 5-10, preferably 5-9.

[0032] In practical applications, the chemical mechanical polishing liquid further includes an antibacterial agent and / or a viscosity regulator. Specifically, the antibacterial agent and viscosity regulator can be selected from conventional antibacterial agent and viscosity regulator products on the market.

[0033] The advantages of the present invention are further described below through more specific embodiments, but the protection scope of the present invention is not limited to the following embodiments.

[0034] Table 1 shows the formula of Examples 1 to 39 and Comparative Examples 1 to 9 of the chemical mechanical polishing solution of the present invention. According to the formula given in the table, the other components except the oxidant are mixed evenly, and the mass percentage is supplemented with water to 100%. Ammonia water or nitric acid is used to adjust the pH value to the required value. Hydrogen peroxide is added before use and mixed evenly.

[0035] Table 1

[0036]

[0037]

[0038]

[0039]

[0040] In order to verify the use effect of the chemical mechanical polishing liquid of the present invention, effect verification example 1, effect verification example 2 and effect verification example 3 are set for illustration.

[0041] Effect verification example 1:

[0042] The polishing liquids of comparative examples 1-3 and the polishing liquids of embodiments 34-36 of the present invention were used to perform polishing experiments on blank copper sheets, and the static corrosion rate, removal rate and static corrosion rate of copper in the polishing liquid were measured. At the same time, the patterned copper wafer was polished, and after polishing, the butterfly depression value of the 80um*80um copper block on the patterned copper wafer was measured using an XE-300P atomic force microscope. The details are as follows:

[0043] Polishing conditions for blank wafers: copper wafer: down pressure 3Psi / 1Psi; polishing disc and polishing head speed 70 / 80rpm, polishing pad PPG MX710, polishing liquid flow rate 100mL / min, polishing machine is LogitechPM5 Polisher.

[0044] Static corrosion rate test conditions: copper wafers were immersed in polishing liquid at room temperature and 50°C, respectively, and the immersion time was 30 minutes at room temperature and 5 minutes at 50°C.

[0045] The industrial conditions for polishing the patterned copper wafer are: 3 psi down pressure, polishing the patterned copper wafer until the residual copper is about 2000A, then lowering the residual copper by 1 psi and over-polishing for 30 seconds. The polishing disc and polishing head speed are 70 / 80 rpm, the polishing pad is PPG MX710, the polishing liquid flow rate is 100 mL / min, and the polishing machine is Logitech PM5 Polisher. After polishing, the butterfly depression value of the 80um*80um copper block on the patterned copper wafer is measured using an XE-300P atomic force microscope.

[0046] The copper removal rate, static corrosion rate, and butterfly depression value were calculated and are shown in Table 2.

[0047] Table 2

[0048]

[0049] As can be seen from Table 2, compared with Comparative Examples 1-3 without the addition of anionic surfactant, the polishing liquids of Examples 34 to 36 contain anionic surfactants, which can suppress the removal rate of copper at low pressure, which is beneficial to reducing the depression on the patterned copper wafer, and can maintain a high copper removal rate under high pressure without affecting the production capacity. Furthermore, the anionic surfactant can effectively suppress the static corrosion rate of copper at room temperature and polishing temperature (such as 50°C), which is beneficial to reducing defects and butterfly depressions generated during the polishing process.

[0050] Effect verification example 2:

[0051] The blank copper (Cu) was polished using the polishing liquids of Comparative Examples 4-6 and the polishing liquids of Examples 37-39 of the present invention, and the static corrosion rate, removal rate and static corrosion rate of copper in the polishing liquid were measured. The details are as follows:

[0052] Polishing conditions for blank wafers: copper wafer: down pressure 3Psi / 1Psi; polishing disc and polishing head speed 70 / 80rpm, polishing pad PPG MX710, polishing liquid flow rate 100mL / min, polishing machine is LogitechPM5 Polisher.

[0053] Static corrosion rate test conditions: copper wafers were immersed in polishing liquid at room temperature and 50°C, respectively, and the immersion time was 30 minutes at room temperature and 5 minutes at 50°C.

[0054] The removal rate and static corrosion rate of copper are shown in Table 3.

[0055] Table 3

[0056]

[0057] As shown in Table 3, compared with Comparative Examples 4-6 without adding o-diamine salt, Examples 37-39 added o-diamine salt, which can increase the removal rate of copper at high pressure and improve production capacity. It has little effect on the removal rate of copper at low pressure, which is beneficial to maintain the flatness of the patterned copper wafer after polishing.

[0058] Effect verification example 3:

[0059] The polishing liquids of Comparative Examples 7-9 and the polishing liquids of Examples 37-39 of the present invention were used to perform polishing experiments on blank copper (Cu), blank Ta and blank SiN, and the removal rates (Å / min) were measured respectively. The details are as follows:

[0060] Polishing experiments were performed using 50Å thick blanket Cu wafers, 2500Å thick Ta and SiN blanket wafers. The blanket wafers were purchased from Silicon Valley Microelectronics.

[0061] Polishing conditions for blank wafers: downward pressure 2.5 Psi; polishing disc and polishing head rotation speed 70 / 80 rpm, polishing pad PPG MX710, polishing liquid flow rate 100 mL / min, polishing machine is Logitech PM5 Polisher.

[0062] The Cu removal rate (Å / min), Ta removal rate (Å / min), and SiN removal rate (Å / min) were calculated and are shown in Table 4.

[0063] Table 4

[0064]

[0065] It can be seen from Table 4 that compared with Comparative Examples 7-9 to which no chelating agent amino acid is added, chelating agent amino acid is added to Examples 37-39. The chelating agent amino acid can undergo a complex reaction with Cu, reduce the copper ions in the solution, promote the reaction process, greatly increase the copper removal rate, and improve production capacity, while having little effect on the removal rate of other barrier layers such as Ta and SiN, thereby ensuring the selectivity and uniformity of the polishing process.

[0066] In summary, the polishing liquid of the present invention can maintain a relatively high copper removal rate under high pressure, while improving the high selectivity of copper film relative to other barrier layers such as Ta and SiN; this type of low-k and ultra-low-k film.

[0067] Advantages of the present invention: The chemical mechanical polishing solution uses a complexing agent to react with copper ions to form a compound, thereby accelerating the copper polishing rate. At the same time, an anionic surfactant can be used to reduce the metal etching rate to obtain a flatter surface, and is compounded with an ortho-diamine salt to form a passivation layer during the chemical mechanical polishing process. By adjusting the content of each substance, a stable solution is formed to meet the high Cu removal rate and low Cu static etching rate required for advanced node copper and silicon through hole CMP applications, inhibit the polishing rate of the blocking material, and reduce the generation of defects such as dishing grooves and scratches during the polishing process.

[0068] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the art within the technical scope disclosed in the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.

Claims

1. A chemical mechanical polishing liquid, characterized in that: The invention comprises 0.5%-3% by mass of abrasive particles, 0.05%-4.0% by mass of anionic surfactant, 0.05%-8% by mass of complexing agent, 0.5%-3% by mass of oxidant, 0.05%-1% by mass of corrosion inhibitor, 0.005%-2% by mass of ortho-diamine salt and pH regulator, and the balance is water, wherein the complexing agent is one of glycine, D-alanine, L-alanine, DL-alanine, β-alanine, N,N-dihydroxyethylglycine, tri(hydroxymethyl)methylglycine, sarcosine, valine, leucine, isoleucine, proline, serine, threonine, tyrosine, glutamine, asparagine, tryptophan, histidine, arginine, lysine, methionine, cysteine ​​or iminodiacetic acid or a combination thereof, and the molecular structure of the ortho-diamine salt is: , where the anion Y - Selected from one or more of bicarbonate, hydroxide, p-toluenesulfonate and / or bitartrate; n is 1 or 2.

2. A chemical mechanical polishing solution according to claim 1, characterized in that: The ortho-diamine salt includes, but is not limited to, the following optical isomers and mixtures thereof: R, R configuration, S, S configuration, R, S configuration or S, R configuration.

3. A chemical mechanical polishing solution according to claim 1, characterized in that: The anionic surfactant is one of dodecylbenzene sulfonic acid, dodecyl sulfonic acid, methylenebisnaphthalene sulfonic acid, alkyl phosphate diethanolamine salt, alkyl phosphate triethanolamine salt, polyol phosphate, glycerol polyoxypropylene ether phosphate triethanolamine salt, acrylic acid-2-acrylamide-2-methylpropane sulfonic acid copolymer, polyacrylic acid and / or anionic polyacrylamide, or a combination thereof.

4. A chemical mechanical polishing solution according to claim 1, characterized in that: The corrosion inhibitor is one or a combination of 1,2,4-triazole, aminotriazole, 3,5-diimino-1,2,4-triazole, benzotriazole or benzotriazole derivatives, imidazole or imidazole derivatives, benzimidazole or benzimidazole derivatives, pyrazole or pyrazole derivatives and / or tetrazole or tetrazole derivatives.

5. A chemical mechanical polishing solution according to claim 1, characterized in that: The abrasive particles are silicon dioxide, the average particle size of the abrasive particles is 50-300 nanometers, and the average grain size is 20-150 nanometers.

6. A chemical mechanical polishing solution according to claim 1, characterized in that: The pH value of the chemical mechanical polishing liquid is 5-10.

7. A chemical mechanical polishing solution according to claim 1, characterized in that: The chemical mechanical polishing liquid also includes an antibacterial agent and / or a viscosity regulator.

Citation Information

Patent Citations

  • Polishing liquid

    US20080203354A1