A cerium oxide @ ZIF-8 composite abrasive, preparation method and application thereof

By growing the ZIF-8 shell layer on the cerium oxide abrasive particles, the poor dispersion and scratching of the commercially available abrasive particles are solved, and the polishing efficiency and accuracy of the large-size display glass substrate is improved. Higher material removal rates and lower surface roughness are achieved.

CN116285891BActive Publication Date: 2024-11-26SHANGHAI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211088718.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-07
Publication Date
2024-11-26
Estimated Expiration
2042-09-07

AI Technical Summary

Technical Problem

The commercially available cerium oxide abrasive particles have poor dispersion stability, which easily causes scratches, resulting in high surface roughness after polishing, which cannot meet the high-efficiency removal rate requirements of large-size display glass substrates.

Method used

Using the preparation method of cerium oxide @ZIF-8 composite abrasive particles, cerium oxide is modified by γ-aminopropyltriethoxysilane and glutaric anhydride, combined with zinc nitrate hexahydrate and dimethylimidazole to grow under hydrothermal conditions. ZIF-8 shell layer forms catalytic cerium oxide @ZIF-8 composite abrasive particles for chemical mechanical polishing of TFT-LCD substrate glass.

Benefits of technology

It significantly improves the material removal rate, up to 26%, reduces the surface roughness after polishing, improves polishing efficiency and accuracy, and reduces hard damage such as scratches.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116285891B_ABST
    Figure CN116285891B_ABST
Patent Text Reader

Abstract

The invention discloses a cerium oxide @ ZIF-8 composite abrasive, a preparation method thereof and an application thereof. The cerium oxide @ ZIF-8 composite abrasive is a micron-sized cerium oxide-metal organic framework material composite particle with irregular morphology. The preparation method thereof is to use γ-aminopropyltriethoxysilane and glutaric anhydride to carboxyl-modify cerium oxide, and then use a hydrothermal method to grow a layer of zeolite imidazolate framework material (ZIF-8) outside the carboxyl-modified cerium oxide core using zinc nitrate hexahydrate and dimethylimidazole to obtain a cerium oxide @ ZIF-8 composite abrasive with catalytic properties. Compared with conventional commercially available cerium oxide abrasives, the new cerium oxide @ ZIF-8 composite abrasive of the invention can increase the material removal rate of TFT-LCD substrate glass by up to 26%, and can effectively reduce the surface roughness after polishing to meet the requirements of TFT-LCD substrate glass surface processing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a micron-sized abrasive grain with irregular morphology and a preparation method thereof, in particular to a cerium oxide @ ZIF-8 composite abrasive grain used in the polishing process of a thin film transistor liquid crystal display substrate glass, belonging to the field of surface polishing technology. Background Art

[0002] Thin-film transistor (TFT) technology was born in the 1990s. It mainly forms various films necessary for manufacturing circuits on non-single-chip wafers such as glass or plastic substrates (or on wafers) through sputtering and chemical deposition processes. The films are then processed and finally laminated by the substrate and the film, and filled with liquid crystal to form a thin-film transistor liquid crystal display (TFT-LCD). TFT-LCD substrate glass is an alkali-free glass with a high strain point, good chemical stability and low thermal expansion coefficient, and is widely used in the electronic information display industry. As the production line evolves along the direction of Nishimura's law and the era of large screens arrives, the size of glass substrates becomes larger and larger, which also puts higher requirements on the thinning process of substrate glass. While removing surface defects such as micro-bumps and corrosion pits after chemical etching of substrate glass, the material removal rate of substrate glass is maximized.

[0003] At present, chemical mechanical polishing technology is a general processing technology for auxiliary grinding of substrate glass to achieve global flatness. Polishing liquid is the most important consumable in chemical mechanical polishing, and abrasive particles are a vital component of polishing liquid. Rare earth cerium oxide materials have become the most widely used abrasive particles in substrate glass polishing due to their low price, moderate hardness, and high removal rate for glass materials. In view of the current situation that rare earth polishing materials for high-generation large-size display glass substrates for new displays are completely dependent on imports, we hope to develop cerium oxide abrasive particles with higher material removal rates to meet the growing industrial needs. Summary of the invention

[0004] In order to solve the existing technical problems that commercially available cerium oxide abrasives have poor dispersion stability and are easy to cause scratches, the purpose of the present invention is to overcome the shortcomings of the existing technology and provide a cerium oxide @ ZIF-8 composite abrasive, a preparation method and application thereof, to increase the material removal rate, effectively reduce the surface roughness after polishing, and improve the polishing efficiency and polishing quality.

[0005] In order to achieve the above object, the present invention adopts the following technical scheme:

[0006] A method for preparing cerium oxide @ ZIF-8 composite abrasive particles comprises the following steps:

[0007] S01: Add γ-aminopropyltriethoxysilane to N,N-dimethylformamide (DMF), stir to mix, then add glutaric anhydride, and stir at room temperature not less than 25°C for at least 3 hours to obtain a clear solution;

[0008] S02: dissolving cerium oxide with an average particle size of 1 micron in an N,N-dimethylformamide aqueous solution, and ultrasonicating for at least 10 minutes to obtain a cerium oxide suspension;

[0009] S03: adding the cerium oxide suspension obtained in step S02 to the clarified solution obtained in step S01, so that the mass ratio of the cerium oxide suspension and the clarified solution is 32:25, and continuously stirring at room temperature of 25°C for at least 5 hours to obtain a reactant mixed solution; then centrifuging the reactant mixed solution at a speed of not less than 5000 rpm for at least 5 minutes to precipitate, and then washing the precipitate with water and ethanol at least twice each, and then drying at not less than 60°C for at least 8 hours to obtain a carboxyl-modified cerium oxide powder;

[0010] S04: Add the carboxyl-modified cerium oxide powder obtained in step S03 to the zinc nitrate hexahydrate aqueous solution, stir until uniformly dispersed, and heat in a water bath at not less than 70° C. for at least 30 minutes, then quickly add a dimethylimidazole aqueous solution with a molar concentration of not less than 0.389 M, and after the dimethylimidazole solution is added, continue stirring for at least 20 minutes and cool to room temperature, and then centrifuge at a speed of not less than 5000 rpm for at least 5 minutes to precipitate, and then wash the precipitate with water and ethanol at least twice each, and then dry at not less than 80° C. for at least 8 hours to obtain cerium oxide @ ZIF-8 composite abrasive.

[0011] Preferably, in step S01, the mass ratio of γ-aminopropyltriethoxysilane, N,N-dimethylformamide and glutaric anhydride is 5:120:3.

[0012] Preferably, in step S02, the mass ratio of cerium oxide, N,N-dimethylformamide and water is 2:2:1.

[0013] Preferably, in step S04, the molar concentration of the zinc nitrate hexahydrate aqueous solution is 0.019-0.146M.

[0014] Preferably, in step S04, the mass ratio of the zinc nitrate hexahydrate aqueous solution, the carboxyl-modified cerium oxide, and the dimethylimidazole aqueous solution is 25:2:75.

[0015] Preferably, in the step S04, the mass percentage content of ZIF-8 in the prepared cerium oxide@ZIF-8 composite abrasive is 5.35-41.31 wt.%.

[0016] A cerium oxide @ ZIF-8 composite abrasive grain is prepared by using the preparation method of the cerium oxide @ ZIF-8 composite abrasive grain of the present invention.

[0017] An application of the cerium oxide @ ZIF-8 composite abrasive grains of the present invention is to prepare a polishing liquid using the cerium oxide @ ZIF-8 composite abrasive grains, and to apply the polishing liquid to a TFT-LCD substrate glass.

[0018] Compared with the prior art, the present invention has the following obvious outstanding substantive features and significant advantages:

[0019] 1. The present invention prepares cerium oxide @ ZIF-8 composite abrasive by hydrothermal method under mild conditions; Zn with positive charge in aqueous solution 2+ The cerium oxide@ZIF-8 composite abrasive is prepared by adsorbing on negatively charged CeO2-COOH and then coordinating with N in dimethylimidazole to grow a ZIF-8 shell outside the CeO2-COOH core. The novel abrasive preparation method is simple and can be scaled up for industrial production.

[0020] 2. The cerium oxide @ ZIF-8 composite abrasive polishing liquid of the present invention is applied to chemical mechanical polishing of TFT-LCD substrate glass, which can effectively reduce the surface roughness of the substrate glass. Compared with conventional commercially available cerium oxide abrasives, the polishing rate of the cerium oxide @ ZIF-8 composite abrasive can be increased by 26% at most;

[0021] 3. Compared with conventional commercially available cerium oxide abrasives, the cerium oxide @ ZIF-8 composite abrasive with catalytic properties of the present invention has rounded surface edges, which is beneficial to reduce hard damage such as scratches, and the pore characteristics of ZIF-8 with high specific surface area can improve solid-phase chemical reactions, thereby achieving efficient processing purposes. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a field emission scanning electron microscope image of the cerium oxide @ ZIF-8 composite abrasive in Example 1 of the present invention. DETAILED DESCRIPTION

[0023] In order to make the objectives, technical solutions and advantages of the present invention more clear, the specific implementation modes of the present invention are further described in detail below with reference to the accompanying drawings.

[0024] A method for preparing cerium oxide @ ZIF-8 composite abrasive particles comprises the following steps:

[0025] S01: Add γ-aminopropyltriethoxysilane to N,N-dimethylformamide (DMF), stir and mix, then add glutaric anhydride, and stir at room temperature not less than 25°C for at least 3 hours to obtain a clear solution; wherein the mass ratio of γ-aminopropyltriethoxysilane, N,N-dimethylformamide, and glutaric anhydride is 5:120:3;

[0026] S02: dissolving cerium oxide with an average particle size of 1 micron in an N,N-dimethylformamide aqueous solution, and ultrasonicating for at least 10 minutes to obtain a cerium oxide suspension; wherein the mass ratio of cerium oxide, N,N-dimethylformamide, and water is 2:2:1;

[0027] S03: adding the cerium oxide suspension obtained in step S02 to the clarified solution obtained in step S01, so that the mass ratio of the cerium oxide suspension and the clarified solution is 32:25, and continuously stirring at room temperature of 25°C for at least 5 hours to obtain a reactant mixed solution; then centrifuging the reactant mixed solution at a speed of not less than 5000 rpm for at least 5 minutes to precipitate, and then washing the precipitate with water and ethanol at least twice each, and then drying at not less than 60°C for at least 8 hours to obtain a carboxyl-modified cerium oxide powder;

[0028] S04: Add the carboxyl-modified cerium oxide powder obtained in step S03 to the zinc nitrate hexahydrate aqueous solution, stir until uniformly dispersed, and heat in a water bath at not less than 70°C for at least 30 minutes, then quickly add a dimethylimidazole aqueous solution with a molar concentration of not less than 0.389M, and after the dimethylimidazole solution is added, continue stirring for at least 20 minutes and cool to room temperature, then centrifuge at a speed of not less than 5000 rpm for at least 5 minutes to precipitate, then wash the precipitate with water and ethanol at least twice each, and then dry at not less than 80°C for at least 8 hours to obtain cerium oxide @ ZIF-8 composite abrasive. Wherein, the mass ratio of the zinc nitrate hexahydrate aqueous solution, the carboxyl-modified cerium oxide, and the dimethylimidazole aqueous solution is 25:2:75. The molar concentration of the zinc nitrate hexahydrate aqueous solution is 0.019-0.146M; by using zinc nitrate hexahydrate solutions with different molar concentrations, cerium oxide @ ZIF-8 composite abrasive particles with a ZIF-8 content between 5.35 and 41.31wt.% can be prepared.

[0029] The application of the zeolite imidazolate-cerium oxide composite abrasive of the present invention uses the above cerium oxide @ ZIF-8 composite abrasive to prepare a polishing liquid, which is applied to the polishing of TFT-LCD substrate glass, can significantly improve the polishing rate and polishing accuracy, achieving a "high efficiency, high precision" polishing effect.

[0030] The above scheme is further described below in conjunction with specific implementation examples. The preferred embodiments of the present invention are described in detail as follows:

[0031] Example 1

[0032] In this embodiment, a method for preparing cerium oxide @ ZIF-8 composite abrasive particles is provided, wherein zeolite imidazolate-cerium oxide composite abrasive particles are prepared by a simple and easy hydrothermal method, and the method steps are as follows:

[0033] (1) Add 5 g of γ-aminopropyltriethoxysilane to 120 g of N,N-dimethylformamide (DMF), stir to mix, then add 3 g of glutaric anhydride, and stir at room temperature of 25°C for 3 h to obtain a clear solution;

[0034] (2) dissolving 40 g of cerium oxide having an average particle size of 1 μm in 60 g of N,N-dimethylformamide aqueous solution (DMF:H2O mass ratio = 2:1), and ultrasonicating for 10 min to obtain a cerium oxide suspension;

[0035] (3) adding 100 g of the cerium oxide suspension obtained in (2) to 128 g of the clear solution obtained in (1), and stirring continuously at room temperature of 25° C. for 5 h; finally, the collected reaction solution was centrifuged at 5000 rpm for 5 min, the precipitate was washed twice with water and ethanol, and dried at 60° C. for 8 h to obtain carboxyl-modified cerium oxide powder (CeO2-COOH);

[0036] (4) Add 10 g of carboxyl-modified cerium oxide powder to 125 g of 0.019 M zinc nitrate hexahydrate aqueous solution, stir until uniformly dispersed, and heat in a water bath at 70° C. for 30 min; then quickly add 375 g of 0.389 M dimethylimidazole aqueous solution, and after the dimethylimidazole solution is added, continue stirring for 20 min and cool to room temperature; finally, the collected reaction solution is centrifuged at 5000 rpm for 5 min, the precipitate is washed twice with water and ethanol, and dried at 80° C. for 8 h to obtain a cerium oxide@ZIF-8 composite abrasive with a ZIF-8 content of 5.35 wt.%;

[0037] The cerium oxide @ ZIF-8 composite abrasive obtained above was added with deionized water to prepare a cerium oxide @ ZIF-8 composite abrasive polishing liquid with a solid mass fraction of 2 wt.%, thereby obtaining the polishing liquid of Example 1.

[0038] The polishing effect of the polishing liquid of this embodiment on the substrate glass is shown in Table 1.

[0039] Example 2

[0040] This embodiment is basically the same as Embodiment 1, except that:

[0041] In this embodiment, the steps and amounts are the same as those of embodiment 1, except that the molar concentration of the zinc nitrate hexahydrate aqueous solution in step (4) is changed to 0.076 M, to obtain a cerium oxide @ ZIF-8 composite abrasive having a ZIF-8 content of 21.42 wt.%.

[0042] Similarly, deionized water was added to prepare a cerium oxide @ ZIF-8 composite abrasive polishing liquid with a solid mass fraction of 2 wt.%.

[0043] The polishing effect of the polishing liquid of Example 2 on the substrate glass is shown in Table 1.

[0044] Example 3

[0045] This embodiment is basically the same as the above embodiment, with the following features:

[0046] In this embodiment, the steps and amounts are the same as those of embodiment 1, except that the molar concentration of the zinc nitrate hexahydrate aqueous solution in step (4) is changed to 0.146 M, to obtain a cerium oxide @ ZIF-8 composite abrasive having a ZIF-8 content of 41.31 wt.%.

[0047] Similarly, deionized water was added to prepare a cerium oxide @ ZIF-8 composite abrasive polishing liquid with a solid mass fraction of 2 wt.%.

[0048] The polishing effect of the polishing liquid of Example 3 on the substrate glass is shown in Table 1.

[0049] Comparative Example

[0050] Unmodified pure cerium oxide is used as a comparative example for comparison. In the comparative example, a method for preparing a cerium oxide polishing liquid is as follows:

[0051] (1) Weigh 10 g of cerium oxide powder with an average particle size of 1 μm and dissolve it in deionized water to prepare a cerium oxide polishing liquid with a mass fraction of 2 wt.%.

[0052] The polishing effect of the polishing liquid of Comparative Example 1 on the substrate glass is shown in Table 1.

[0053] The polishing liquids of Examples 1-3 and Comparative Example 1 were used to perform a polishing test on a glass substrate under certain polishing conditions.

[0054] The polishing conditions of the polishing test are as follows:

[0055] Polishing machine: UNIPOL-1000s automatic pressure grinding and polishing machine;

[0056] Workpiece: TFT-LCD substrate glass sheet with a diameter of 50mm and a thickness of 0.7mm;

[0057] Polishing pad: polyurethane polishing pad;

[0058] Polishing pressure: 3kg;

[0059] Upper plate speed: 30rpm;

[0060] Lower plate speed: 60rpm;

[0061] Polishing time: 1h;

[0062] After polishing, the substrate glass piece is washed and dried in the order of cleaning liquid, deionized water, and ethanol, and the mass of the substrate glass piece before and after polishing is weighed with a precision analytical balance to calculate the material removal rate MRR. In addition, the surface roughness Ra of the substrate glass piece before and after polishing measured by the 3D surface profiler has a step accuracy of 0.5%, a step repeatability of 0.1%, a vertical resolution of 0.1nm, a maximum lateral resolution of 0.14nm, and a Z-direction scanning range of 0.1nm-34mm.

[0063] The polishing effects of the polishing liquids with a mass fraction of abrasive particles of about 2 wt.% on the substrate glass sheet in each embodiment are shown in Table 1. As can be seen from Table 1, compared with the polishing liquids with the same solid content in the comparative example, the material removal rate of the polishing liquids in each embodiment is significantly increased, and the surface roughness is significantly reduced. The cerium oxide @ ZIF-8 composite abrasive in Example 2 has a material removal rate increased by 26% and a roughness reduction of 35% compared with the commercially available cerium oxide abrasive in Comparative Example 1.

[0064] Table 1. Polishing effect of the polishing liquids of the embodiments of the present invention and the comparative examples on the substrate glass

[0065] Example 1 Example 2 Example 3 Comparative Example 1 Content of ZIF-8 in abrasive particles (%) 5.35 21.42 41.31 0 Polishing rate MRR (μm / h) 19.24 22.2 18.24 17.6 Ra(nm) 120.6 100.4 121.3 154.9

[0066] Note: The ZIF-8 content in Table 1 refers to the ratio of the mass of ZIF-8 to the total mass of cerium oxide @ ZIF-8 composite abrasive.

[0067] In summary, compared with conventional commercially available cerium oxide abrasives, the surface of the cerium oxide @ ZIF-8 composite abrasive of the present invention is rougher and the edges are blunted. For polishing of substrate glass, since the ZIF-8 on the surface of the composite abrasive has a pore structure and a large specific surface area, it can promote the chemical reaction during the chemical mechanical polishing process, significantly improve the material removal rate, and effectively improve the surface accuracy after polishing. The cerium oxide @ ZIF-8 composite abrasive of the above embodiment of the present invention is a micron-sized cerium oxide-metal organic framework material composite particle with irregular morphology. The cerium oxide is carboxyl-modified using γ-aminopropyltriethoxysilane and glutaric anhydride, and then a layer of zeolite imidazole framework material (ZIF-8) is grown outside the carboxyl-modified cerium oxide core using zinc nitrate hexahydrate and dimethylimidazole by a hydrothermal method to obtain cerium oxide @ ZIF-8 composite abrasive. Compared with conventional commercially available cerium oxide abrasives, the novel cerium oxide@ZIF-8 composite abrasives of the above embodiment of the present invention can increase the material removal rate of TFT-LCD substrate glass by up to 26%, and can effectively reduce the surface roughness after polishing.

[0068] The embodiments of the present invention are described above in conjunction with the accompanying drawings, but the present invention is not limited to the above embodiments. Various changes can be made according to the purpose of the invention of the present invention. Any changes, modifications, substitutions, combinations or simplifications made according to the spirit and principle of the technical solution of the present invention should be equivalent replacement methods. As long as they meet the purpose of the invention of the present invention and do not deviate from the technical principles and inventive concepts of the present invention, they belong to the protection scope of the present invention.

Claims

1. A method for preparing cerium oxide @ ZIF-8 composite abrasive, characterized in that: The steps include: S01: Add γ-aminopropyltriethoxysilane to N,N-dimethylformamide (DMF), stir to mix, then add glutaric anhydride, and stir at room temperature not less than 25°C for at least 3 hours to obtain a clear solution; S02: dissolving cerium oxide with an average particle size of 1 micron in an N,N-dimethylformamide aqueous solution, and ultrasonicating for at least 10 minutes to obtain a cerium oxide suspension; S03: adding the cerium oxide suspension obtained in step S02 to the clarified solution obtained in step S01, so that the mass ratio of the cerium oxide suspension and the clarified solution is 32:25, and continuously stirring at room temperature of 25°C for at least 5 hours to obtain a reactant mixed solution; then centrifuging the reactant mixed solution at a speed of not less than 5000 rpm for at least 5 minutes to precipitate, and then washing the precipitate with water and ethanol at least twice each, and then drying at not less than 60°C for at least 8 hours to obtain a carboxyl-modified cerium oxide powder; S04: Add the carboxyl-modified cerium oxide powder obtained in step S03 to the zinc nitrate hexahydrate aqueous solution, stir until uniformly dispersed, and heat in a water bath at not less than 70° C. for at least 30 minutes, and then quickly add a dimethylimidazole aqueous solution having a molar concentration of not less than 0.389 M. After the dimethylimidazole solution is added, stirring is continued for at least 20 minutes and cooled to room temperature, and then centrifuged at a speed of not less than 5000 rpm for at least 5 minutes to precipitate, and then the precipitate is washed with water and ethanol at least twice each, and then dried at not less than 80° C. for at least 8 hours to obtain cerium oxide @ ZIF-8 composite abrasive.

2. The method for preparing the cerium oxide @ ZIF-8 composite abrasive according to claim 1, characterized in that: In the step S01, the mass ratio of γ-aminopropyltriethoxysilane, N,N-dimethylformamide, and glutaric anhydride is 5:120:

3.

3. The method for preparing the cerium oxide @ ZIF-8 composite abrasive according to claim 1, characterized in that: In step S02, the mass ratio of cerium oxide, N,N-dimethylformamide and water is 2:2:

1.

4. The method for preparing the cerium oxide @ ZIF-8 composite abrasive according to claim 1, characterized in that: In the step S04, the molar concentration of the zinc nitrate hexahydrate aqueous solution is 0.019-0.146M.

5. The method for preparing the cerium oxide @ ZIF-8 composite abrasive according to claim 1, characterized in that: In the step S04, the mass ratio of the zinc nitrate hexahydrate aqueous solution, the carboxyl-modified cerium oxide, and the dimethylimidazole aqueous solution is 25:2:

75.

6. The method for preparing the cerium oxide @ ZIF-8 composite abrasive according to claim 1, characterized in that: In the step S04, the mass percentage content of ZIF-8 in the prepared cerium oxide@ZIF-8 composite abrasive is 5.35-41.31 wt.%.

7. A cerium oxide @ ZIF-8 composite abrasive, characterized in that: The composite abrasive is prepared by the preparation method of cerium oxide @ ZIF-8 composite abrasive according to claim 1.

8. An application of the cerium oxide @ ZIF-8 composite abrasive according to claim 7, characterized in that: The polishing liquid was prepared by using cerium oxide @ ZIF-8 composite abrasive and applied to the polishing process of TFT-LCD substrate glass.