Antioxidant copper powder, preparation method and application thereof

By forming a dense coating layer of hydrated calcium silicate crystals and amorphous calcium silicate on the surface of the copper powder, the problem of oxidation resistance and sintering shrinkage matching of the copper powder in the LTCC substrate is solved, and high-performance LTCC is realized Conductive materials.

CN118527652BActive Publication Date: 2024-10-25EAST CHINA UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411010196.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-25
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

In the existing technology, copper powder has poor oxidation resistance in the LTCC substrate, causing the copper paste to oxidize during the debinding process, and has poor matching with the sintering shrinkage of the LTCC substrate, resulting in poor product quality.

Method used

The copper powder is coated with a dense coating layer composed of hydrated calcium silicate crystals and amorphous calcium silicate, and a core-shell structure is formed through ultrasonic treatment and hydrothermal treatment to improve the oxidation resistance and sintering shrinkage matching of the copper powder.

Benefits of technology

It achieves good oxidation resistance of copper powder and good sintering matching with LTCC substrate, ensures high density and low-cost production of conductive paste, and reduces process complexity and environmental risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118527652B_ABST
    Figure CN118527652B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of electronic packaging, and relates to an antioxidant copper powder, a preparation method and an application thereof. The antioxidant copper powder comprises copper powder and a coating layer located on the surface thereof; the coating layer is composed of hydrated calcium silicate crystals and amorphous calcium silicate, the hydrated calcium silicate crystals exist in the coating layer in a fibrous state, and the amorphous calcium silicate exists in the coating layer in an amorphous state; the preparation method: pre-treating the copper powder to obtain pre-treated copper powder; at the same time, mixing TEOS and calcium salt in a solvent, stirring and heating to obtain a sol; after the pre-treated copper powder and the sol are evenly mixed, evaporation concentration and drying are performed in sequence to obtain a gel-coated copper powder; after preparing a reaction mixture containing gel-coated copper powder, water and calcium hydroxide at the same time, hydrothermal treatment is performed, and antioxidant copper powder is obtained by post-treatment; application: used for preparing conductive slurry for LTCC. The antioxidant copper powder prepared by the present invention has excellent antioxidant properties and good matching with the sintering shrinkage of the LTCC substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of electronic packaging and relates to an oxidation-resistant copper powder, a preparation method and application thereof. Background Art

[0002] LTCC (Low Temperature Co-fired Ceramics) has been widely used in high-frequency and higher-transmission-rate communications, sensor technology and other fields due to its advantages such as high conductivity and low dielectric loss. Precious metal materials such as gold and silver that are maturely used for LTCC conductors are expensive, and silver has the phenomenon of electromigration, which greatly limits the application and promotion of gold and silver pastes in LTCC materials. In order to further reduce the impact of silver migration on the electrical properties of LTCC substrate materials and reduce production costs, base metal pastes have become a new research direction. Copper powder has become an ideal substitute for silver powder due to its low cost, excellent conductivity and low electrochemical mobility.

[0003] Traditional high-temperature sintered copper-based conductors are conductive pastes made of copper powder, glass powder, and organic carriers. They can form conductive lines with good conductivity by co-firing with LTCC in a protective atmosphere. However, copper's poor oxidation resistance may cause oxidation of the copper paste during the debonding process. At the same time, the copper powder has a low shrinkage starting temperature and poor matching with the sintering shrinkage of the LTCC substrate, which may cause severe warping and cracking, ultimately resulting in poor product quality.

[0004] To solve the above problems, patent application CN106205855A discloses a solution for customized matching of silver-coated copper electrode paste with LTCC film strip. The coating layer on the copper surface is silver, which can make copper have good oxidation resistance at high temperature, but it does not solve the problem of poor sintering shrinkage matching between copper powder and LTCC substrate. Patent application CN105957642A discloses a method for preparing silica-coated copper electronic paste for LTCC substrate, which solves the problems of uneven distribution of glass phase, high preparation temperature, complicated process, and unfavorable environmental protection. However, the copper paste prepared by the invention needs to be sintered in nitrogen atmosphere during sintering and debinding, which fails to solve the problem of poor oxidation resistance of copper. Patent application JP2013064191A discloses a type of copper nanoparticles coated with collagen peptides for low-temperature curing slurries at 100-350°C. These copper nanoparticles have excellent oxidation resistance and dispersion stability, but the coating layer formed by the collagen peptide will completely decompose above 500°C, making it difficult to solve the problem of poor sintering shrinkage matching between copper powder and LTCC substrates.

[0005] Therefore, it is necessary to provide an oxidation resistant copper powder having excellent oxidation resistance and good matching with the sintering shrinkage of the LTCC substrate, so as to produce an LTCC with excellent comprehensive performance. Summary of the invention

[0006] The purpose of the present invention is to solve the problems existing in the prior art and provide an oxidation-resistant copper powder, a preparation method and an application thereof.

[0007] To achieve the above object, the technical solution adopted by the present invention is as follows:

[0008] An antioxidant copper powder comprises copper powder and a coating layer on the surface of the copper powder; the coating layer is composed of hydrated calcium silicate crystals and amorphous calcium silicate, the hydrated calcium silicate crystals exist in the coating layer in a fibrous state, and the amorphous calcium silicate exists in the coating layer in an amorphous state; the coating layer is dense.

[0009] The calcium silicate hydrate in the coating layer of the antioxidant copper powder of the present invention is an ideal coating material. On the one hand, the calcium silicate hydrate has good stability and oxidation resistance as a coating layer. On the other hand, the calcium silicate hydrate has a similar chemical composition to the crystalline phase α-CaSiO3 and β-CaSiO3 in the common calcium borosilicate LTCC substrate. It has good sintering shrinkage matching performance for the common LTCC substrate and will not introduce additional impurities.

[0010] As the preferred technical solution:

[0011] The antioxidant copper powder as described above is spherical copper or plate-like copper, the particle size of the spherical copper is 0.85-5 μm, and the particle size of the plate-like copper is 1.43-10.58 μm; in the antioxidant copper powder, the content of the coating layer is 3-20wt%; and the content of calcium silicate hydrate crystals in the coating layer is 20-50wt%.

[0012] The present invention also provides a method for preparing an antioxidant copper powder as described in any one of the above items, comprising the following steps:

[0013] (1) Pre-treating the copper powder to remove the surface passivation layer to obtain pre-treated copper powder; at the same time, mixing TEOS (tetraethyl orthosilicate) and calcium salt in a solvent, stirring and heating until TEOS is fully hydrolyzed to obtain a sol. During the hydrolysis process, the tetraethyl orthosilicate is hydrolyzed to form a three-dimensional network structure, and calcium ions enter the gaps in the network structure;

[0014] (2) The pretreated copper powder and the sol are mixed evenly by ultrasonic treatment and stirring, and then evaporated, concentrated, and dried in sequence to obtain gel-coated copper powder. During the evaporation and concentration process, the sol is converted into gel and adsorbed on the surface of the copper powder to form a core-shell structure;

[0015] (3) After preparing a reaction mixture containing gel-coated copper powder, water, calcium hydroxide and an antioxidant, a hydrothermal treatment is performed. During the hydrothermal process, calcium ions play a promoting role. Calcium hydroxide reacts with the gel layer on the surface of the copper powder to form hydrated calcium silicate crystals and amorphous calcium silicate. After post-treatment (washing and drying), an antioxidant copper powder is obtained.

[0016] As the preferred technical solution:

[0017] In the method as described above, in step (1), the copper powder is pretreated, that is, the copper powder is sequentially washed with an acid wash solution, washed with an organic solvent, washed by centrifugation, and dried;

[0018] The components and contents of the pickling solution are: 30-50wt% 1M hydrochloric acid solution, 20-30wt% 1M nitric acid solution, 0-10wt% acetone, and the balance ethanol; the temperature of the pickling solution is 40-60°C, and the cleaning time is 10-120min;

[0019] The components and contents of the organic solvent are: acetone 50-90wt%, ethanol 8-48wt%, and xylene as the remainder; the temperature of the organic solvent cleaning is 20-70°C, and the time is 10-120min.

[0020] In the method as described above, in step (1), the calcium salt is calcium chloride and / or calcium nitrate; the solvent is one or more of ethanol, ethylene glycol and triethanolamine; the molar ratio of TEOS to calcium salt is 1-2:1, and the concentration of TEOS in the solvent is 9 g / L.

[0021] In the method as described above, in step (2), the mass ratio of the pretreated copper powder to the sol is 1:20-160; the power of the ultrasonic treatment is 50-500 W, the stirring speed is 40-100 rpm, and the time is 5-20 min.

[0022] In the method as described above, in step (3), water is deionized water or ultrapure water; the mass ratio of the gel-coated copper powder, water, and calcium hydroxide is 1-10:50-100:0.01-3; the temperature of the hydrothermal treatment is 160-200°C, and the time is 8-24h.

[0023] In the method as described above, the antioxidant is one or more of ethylene glycol, ascorbic acid, citric acid, oleylamine and oleic acid; and the mass ratio of the antioxidant to the gel-coated copper powder is 0.002-0.05:1.

[0024] The present invention also provides a use of the anti-oxidation copper powder as described in any one of the above items, wherein the anti-oxidation copper powder is used as a conductive agent to prepare a conductive paste for LTCC.

[0025] As the preferred technical solution:

[0026] For the application described above, the components and contents of the conductive paste for LTCC are: 70-85wt% antioxidant copper powder, 0-10wt% glass powder, and the balance organic carrier.

[0027] In the application as described above, the organic carrier is composed of 5-15wt% of resin and the balance of organic solvent; the resin is ethyl cellulose, cellulose acetate butyrate or acrylic resin; the organic solvent is acetone, turpentine, terpineol, dihydroterpineol, ethylene glycol butyl ether, diethylene glycol butyl ether, diethylene glycol butyl ether acetate, tributyl citrate or dibutyl phthalate.

[0028] As described above, the conductive paste for LTCC is printed on the surface of the LTCC substrate, and then dried and co-fired to obtain LTCC.

[0029] For the application as described above, the drying temperature is 100-150°C and the drying time is 10-30min; the co-firing process is: first, in an air atmosphere, the temperature is increased to 300°C at a heating rate of 1-10°C / min and then kept warm for 30min-1h; then, in a dry nitrogen atmosphere, the temperature is increased to 450-600°C at a heating rate of 1-10°C / min and then kept warm for 2-3h, or in a wet nitrogen atmosphere (vapor pressure partial pressure is 12kPa) The atmosphere is heated to 450-600°C at a heating rate of 1-10°C / min and then kept warm for 3-6h, and finally in a dry nitrogen atmosphere or a weak reducing atmosphere, the temperature is increased to 850-900°C at a heating rate of 5-15°C / min and then kept warm for 20-40min, and the weak reducing atmosphere is composed of 2%V / V hydrogen and the balance argon.

[0030] As described above, LTCC is composed of a copper film and a LTCC substrate. The copper film has no warping or cracking, and the average square resistance of the copper film is 3-20.3 mΩ / square (i.e., 3-20.3 milliohms per square). The tensile force between the copper film and the LTCC substrate is 20-49N.

[0031] Principle of the invention:

[0032] The anti-oxidation copper powder prepared by the present invention is a powder with a core-shell structure, and its coating layer is composed of hydrated calcium silicate crystals and amorphous calcium silicate. The hydrated calcium silicate crystals exist in the coating layer in a fibrous state, and the amorphous calcium silicate exists in the coating layer in an amorphous state, and the two together constitute a dense coating layer.

[0033] Among them, calcium silicate hydrate crystals can inhibit the shrinkage of copper powder during the sintering process, and can effectively avoid the warping and cracking of LTCC substrate caused by different shrinkage starting temperatures during the sintering process of copper paste and LTCC. The specific principle is: the microscopic essence of the shrinkage of copper powder during the sintering process is that the centers of two particles are close to each other and merged into a large particle. The grain grows, and the calcium silicate hydrate crystals block the contact between the two particles, slowing down the grain growth process;

[0034] Amorphous calcium silicate can soften to form a liquid phase, wet the copper powder and the LTCC substrate, so that the sintered copper film and the LTCC substrate have good bonding strength.

[0035] In addition, the dense coating layer formed can provide copper powder with good oxidation resistance. The copper paste prepared by using oxidation-resistant copper powder can be debonded at low temperature in air atmosphere.

[0036] The glass powder added to the conductive paste for LTCC of the present invention can help reduce the wetting angle between amorphous calcium silicate and the LTCC substrate, improve the acid resistance of the paste after sintering, control the thermal expansion coefficient of the copper paste, and at the same time, can effectively reduce the liquefaction temperature of the amorphous calcium silicate, promote the densification process of the paste during sintering, reduce the sintering time, and reduce energy consumption.

[0037] The copper paste prepared in the present invention can be co-fired with the LTCC substrate to form a dense conductive pattern, and has a strong bonding force with the LTCC substrate. The LTCC device prepared in the present invention has the advantages of high sintering densification and high electroplating pass rate, and the internal stress distribution of the chip device after sintering is uniform and moderate, the square resistance is small, and the solder resistance is strong. The pass rate of reliability tests such as heating aging and accelerated life is high.

[0038] Beneficial effects:

[0039] The present invention forms a coating layer composed of hydrated calcium silicate crystals and amorphous calcium silicate on the surface of copper powder to obtain an antioxidant copper powder, which has excellent antioxidant properties and good matching with the sintering shrinkage of the LTCC substrate.

[0040] The conductive paste for LTCC formed by uniformly mixing the prepared anti-oxidation copper powder with an organic carrier and glass powder (glass powder may not be added) can be debonded during the co-firing process, and the conductive paste for LTCC can form an LTCC substrate with excellent comprehensive performance after being co-fired with the LTCC substrate;

[0041] The preparation cost of the invention is low, the process is simple, and it is non-toxic and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 The SEM morphology images of the oxidation-resistant copper powder and the copper film of LTCC prepared in different embodiments; wherein, Figure 1 a is the SEM morphology of the oxidation-resistant copper powder of Example 1, Figure 1 b is the SEM morphology of the oxidation-resistant copper powder of Example 2, Figure 1 Figure c is the SEM morphology of the antioxidant copper powder of Example 3. Figure 1 Figure d is the SEM morphology of the copper film of the LTCC of Example 1. Figure 1Figure e is a SEM morphology of the copper film of the LTCC of Example 2. Figure 1 Fig. f is the SEM morphology of the copper film of the LTCC of Example 3;

[0043] Figure 2 This is a TEM morphology of the oxidation-resistant copper powder prepared in Example 1; wherein, Figure 2 Figure a is the structural diagram of the antioxidant copper powder. Figure 2 Figure b is the EDS Ca and Cu element distribution diagram of the antioxidant copper powder. Figure 2 Figure c is the EDS Si element distribution diagram of the oxidation-resistant copper powder. Figure 2 Figure d is the HAADF diagram of the oxidation-resistant copper powder. Figure 2 e is the EDS O element distribution diagram of the oxidation-resistant copper powder. Figure 2 f in the figure is the electron diffraction pattern of the oxidation-resistant copper powder;

[0044] Figure 3 This is a process flow chart for preparing coated copper powder for LTCC in Example 1 and preparing LTCC using antioxidant copper powder. DETAILED DESCRIPTION

[0045] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0046] The following are the test methods for the relevant performance indicators in each embodiment and comparative example:

[0047] Average square resistance: Use ST2258C digital four-probe to test the square resistance of the copper film of the sintered LTCC. Adjust the four-probe measurement mode to the square resistance mode, place the sintered LTCC on the test bench, make the probe face the center of the copper film surface and press down slowly at the same time, after the copper film is completely pressed, close the loop and get the square resistance value. Test and calculate 10 samples (i.e. LTCC) under the same preparation conditions to get the average square resistance.

[0048] Tensile force between copper film and LTCC substrate: Tested with reference to standard GB / T 17473.4-2008 (Test method for precious metal paste for microelectronics technology - Adhesion determination). Solder 0.8mm tinned copper wire to the copper film of LTCC, bend the copper wire 90° perpendicular to the substrate surface, and place it on a tensile tester (universal tensile tester CMT4204). Pull the lead off the substrate at a constant speed of 20mm / min, and use the average force when the lead is pulled off to represent the adhesion of the paste.

[0049] Example 1

[0050] A method for preparing an oxidation-resistant copper powder, the preparation process is as follows Figure 3 As shown, the specific steps are as follows:

[0051] (1) Preparation of raw materials;

[0052] Copper powder: spherical copper, the manufacturer is Ningbo Guangxin Nanomaterial Co., Ltd., the specification is Cu-GB0501, the particle size is 0.85-3μm;

[0053] TEOS;

[0054] Calcium salt: calcium chloride;

[0055] Solvent: ethanol;

[0056] Hydrochloric acid aqueous solution: concentration is 1M;

[0057] Nitric acid aqueous solution: concentration is 1M;

[0058] acetone;

[0059] Ethanol;

[0060] Xylene;

[0061] Water: deionized water;

[0062] Antioxidant: Ethylene glycol;

[0063] Calcium hydroxide;

[0064] (2) washing the copper powder with an acid solution, washing with an organic solvent, washing with a centrifuge, and drying in sequence to remove the surface passivation layer to obtain a pretreated copper powder; at the same time, mixing TEOS and calcium salt in a molar ratio of 1:1 in a solvent (the concentration of TEOS in the solvent is 9 g / L), stirring, and heating until TEOS is fully hydrolyzed to obtain a sol;

[0065] The components and contents of the pickling solution are as follows: 30wt% hydrochloric acid aqueous solution, 20wt% nitric acid aqueous solution, 10wt% acetone, and the balance ethanol; the pickling solution is cleaned at a temperature of 40°C and for 30 minutes;

[0066] The components and contents of the organic solvent are: acetone 50wt%, ethanol 48wt%, and xylene as the balance; the organic solvent cleaning temperature is 40°C and the time is 60min;

[0067] (3) The pretreated copper powder and the sol in a mass ratio of 1:40 were mixed evenly by ultrasonic treatment (power of 500 W) and stirring (speed of 100 rpm, time of 20 min), and then evaporated, concentrated and dried in sequence to obtain gel-coated copper powder;

[0068] (4) After preparing a reaction mixture containing gel-coated copper powder, water, an antioxidant and calcium hydroxide, a hydrothermal treatment is performed, and after post-treatment, an antioxidant copper powder is obtained; wherein the mass ratio of the gel-coated copper powder, water and calcium hydroxide is 10:50:0.15, and the mass ratio of the antioxidant to the gel-coated copper powder is 0.04:1; the temperature of the hydrothermal treatment is 180° C., and the time is 16 hours.

[0069] The SEM morphology of the finally obtained oxidation-resistant copper powder is as follows: Figure 1 As shown in a, the TEM structure diagram is as follows Figure 2 As shown in a, the TEM EDS Ca and Cu element distribution map is as follows Figure 2 As shown in b, the TEM EDS Si element distribution map is as follows Figure 2 As shown in c, the TEMHAADF diagram is as follows Figure 2 As shown in (d), the TEM EDS O element distribution map is as follows Figure 2 As shown in e, the TEM electron diffraction pattern is as follows Figure 2 As shown in f; the antioxidant copper powder is composed of copper powder and a coating layer located on the surface thereof; the coating layer is composed of hydrated calcium silicate crystals and amorphous calcium silicate, the hydrated calcium silicate crystals exist in the coating layer in a fibrous state, and the amorphous calcium silicate exists in the coating layer in an amorphous state; in the antioxidant copper powder, the content of the coating layer is 5wt%; the content of the hydrated calcium silicate crystals in the coating layer is 50wt%.

[0070] An application of an oxidation resistant copper powder, such as Figure 3 As shown, the antioxidant copper powder prepared in this embodiment is mixed with glass powder (prepared by melt quenching method, the molar percentage of each component is: SiO2 8%, Al2O3 8%, B2O3 44%, BaO 40%; the particle size after ball milling is 3.1-4.5μm) and an organic carrier by a centrifugal mixer and a three-roll mill to prepare a conductive paste for LTCC, and then the conductive paste for LTCC is printed on the surface of a LTCC substrate (manufacturer is Ferro Company, model A6M-E), and then dried and co-fired in sequence to prepare LTCC;

[0071] The contents of the components in the conductive paste for LTCC are as follows: 85wt% of antioxidant copper powder, 5wt% of glass powder, and the balance of organic carrier; the organic carrier is composed of 15wt% of resin and the balance of organic solvent; the resin is acrylic resin (manufacturer is Mitsubishi Group, model BR105); the organic solvent is pine alcohol;

[0072] The drying temperature is 120℃ and the time is 15min. The co-firing process is as follows: first, in an air atmosphere, the temperature is increased to 300℃ at a heating rate of 5℃ / min and then kept warm for 30min. Then, in a wet nitrogen (vapor pressure partial pressure is 12kPa) atmosphere, the temperature is increased to 600℃ at a heating rate of 10℃ / min and then kept warm for 3h. Finally, in a weak reducing atmosphere, the temperature is increased to 870℃ at a heating rate of 15℃ / min and then kept warm for 30min. The weak reducing atmosphere consists of 2%V / V hydrogen and the balance argon.

[0073] The final LTCC is made of copper film (SEM morphology as shown in Figure 1 The copper film has no warping or cracking, the average square resistance of the copper film is 3mΩ / square, and the tensile force between the copper film and the LTCC substrate is 49N.

[0074] Comparative Example 1

[0075] A method for preparing an antioxidant copper powder is basically the same as that of Example 1, except that in step (4), no antioxidant is added when preparing the reaction mixture.

[0076] The application of an antioxidant copper powder is basically the same as that of Example 1, except that the antioxidant copper powder used in preparing the conductive paste for LTCC is the antioxidant copper powder prepared in this comparative example.

[0077] The final LTCC is composed of a copper film and a LTCC substrate. The copper film has no warping or cracking, the average square resistance of the copper film is 600mΩ / square, and the tensile force between the copper film and the LTCC substrate is 5N.

[0078] Compared with Example 1, the comprehensive performance of LTCC in Comparative Example 1 is significantly reduced. This is mainly because in Comparative Example 1, the reaction vessel contains oxygen during the hydrothermal treatment stage, which causes the copper powder to oxidize in the absence of effective antioxidant protection, generating a large amount of cuprous oxide. The cuprous oxide not only destroys the core-shell structure of the copper powder, but also prevents the copper particles from forming a dense connection during the sintering process, thereby increasing the resistance of the sintered copper film and weakening the bonding force with the LTCC substrate.

[0079] Example 2

[0080] A method for preparing an oxidation-resistant copper powder, the specific steps are as follows:

[0081] (1) Preparation of raw materials;

[0082] Copper powder: spherical copper, the manufacturer is Ningbo Guangxin Nanomaterial Co., Ltd., the specification is Cu-GB0501, the particle size is 0.85-3μm;

[0083] TEOS;

[0084] Calcium salts: calcium nitrate;

[0085] Solvent: a mixture of ethanol and ethylene glycol in a molar ratio of 1:1;

[0086] Hydrochloric acid aqueous solution: concentration is 1M;

[0087] Nitric acid aqueous solution: concentration is 1M;

[0088] acetone;

[0089] Ethanol;

[0090] Xylene;

[0091] Water: deionized water;

[0092] Antioxidant: a mixture of ethylene glycol and oleylamine in a mass ratio of 1:1;

[0093] Calcium hydroxide;

[0094] (2) washing the copper powder with an acid solution, washing with an organic solvent, washing with a centrifuge, and drying in sequence to remove the surface passivation layer to obtain a pretreated copper powder; at the same time, mixing TEOS and calcium salt in a molar ratio of 1:1 in a solvent (the concentration of TEOS in the solvent is 9 g / L), stirring, and heating until TEOS is fully hydrolyzed to obtain a sol;

[0095] The components and contents of the pickling solution are as follows: 50wt% hydrochloric acid aqueous solution, 20wt% nitric acid aqueous solution, 5wt% acetone, and the balance ethanol; the pickling solution is cleaned at a temperature of 50°C and for 10 minutes;

[0096] The components and contents of the organic solvent are: acetone 60wt%, ethanol 10wt%, and xylene as the balance; the organic solvent washing temperature is 50°C and the time is 80min;

[0097] (3) The pretreated copper powder and the sol in a mass ratio of 1:40 were mixed evenly by ultrasonic treatment (power of 500 W) and stirring (speed of 40 rpm, time of 15 min), and then evaporated, concentrated and dried in sequence to obtain gel-coated copper powder;

[0098] (4) After preparing a reaction mixture containing gel-coated copper powder, water, an antioxidant and calcium hydroxide, a hydrothermal treatment is performed, and after post-treatment, an antioxidant copper powder is obtained; wherein the mass ratio of the gel-coated copper powder, water and calcium hydroxide is 10:100:3, and the mass ratio of the antioxidant to the gel-coated copper powder is 0.002:1; the temperature of the hydrothermal treatment is 160° C., and the time is 16 hours.

[0099] The final oxidation-resistant copper powder (SEM morphology as shown in Figure 1(as shown in b) is composed of copper powder and a coating layer located on its surface; the coating layer is composed of hydrated calcium silicate crystals and amorphous calcium silicate, the hydrated calcium silicate crystals exist in the coating layer in a fibrous state, and the amorphous calcium silicate exists in the coating layer in an amorphous state; in the antioxidant copper powder, the content of the coating layer is 5wt%; the content of the hydrated calcium silicate crystals in the coating layer is 30wt%.

[0100] An application of an antioxidant copper powder, wherein the antioxidant copper powder prepared in this embodiment is mixed with an organic carrier by a centrifugal mixer and a three-roll mill to prepare a conductive paste for LTCC, and then the conductive paste for LTCC is printed on the surface of a LTCC substrate (manufacturer: Ferro Company, model: A6M-E), and then dried and co-fired in sequence to prepare LTCC;

[0101] The contents of the components in the conductive paste for LTCC are as follows: 85wt% of antioxidant copper powder and the balance of organic carrier; the organic carrier is composed of 15wt% of resin and the balance of organic solvent; the resin is acrylic resin (manufacturer is Mitsubishi Group, model BR105); the organic solvent is turpentine;

[0102] The drying temperature is 120℃ and the time is 10min; the co-firing process is as follows: first, in an air atmosphere, the temperature is increased to 300℃ at a heating rate of 5℃ / min and then kept for 45min, then in a dry atmosphere, the temperature is increased to 450℃ at a heating rate of 1℃ / min and then kept for 6h, and finally in a dry nitrogen atmosphere, the temperature is increased to 850℃ at a heating rate of 5℃ / min and then kept for 20min.

[0103] The final LTCC is made of copper film (SEM morphology as shown in Figure 1 The copper film has no warping or cracking, the average square resistance of the copper film is 4.7mΩ / square, and the tensile force between the copper film and the LTCC substrate is 34N.

[0104] Example 3

[0105] A method for preparing an oxidation-resistant copper powder, the specific steps are as follows:

[0106] (1) Preparation of raw materials;

[0107] Copper powder: spherical copper, the manufacturer is Ningbo Guangxin Nanomaterial Co., Ltd., the specification is Cu-GB0501, the particle size is 0.85-3μm;

[0108] TEOS;

[0109] Calcium salt: calcium chloride;

[0110] Solvent: ethylene glycol;

[0111] Hydrochloric acid aqueous solution: concentration is 1M;

[0112] Nitric acid aqueous solution: concentration is 1M;

[0113] acetone;

[0114] Ethanol;

[0115] Xylene;

[0116] Water: deionized water;

[0117] Antioxidants: Ascorbic acid;

[0118] Calcium hydroxide;

[0119] (2) washing the copper powder with an acid solution, washing with an organic solvent, washing with a centrifuge, and drying in sequence to remove the surface passivation layer to obtain a pretreated copper powder; at the same time, mixing TEOS and calcium salt in a molar ratio of 1:1 in a solvent (the concentration of TEOS in the solvent is 9 g / L), stirring, and heating until TEOS is fully hydrolyzed to obtain a sol;

[0120] The components and contents of the pickling solution are as follows: 30 wt% hydrochloric acid aqueous solution, 30 wt% nitric acid aqueous solution, and the balance ethanol; the pickling solution is cleaned at a temperature of 60°C and for 10 minutes;

[0121] The components and contents of the organic solvent are: acetone 75wt%, ethanol 10wt%, and xylene as the balance; the organic solvent cleaning temperature is 60°C and the cleaning time is 100min;

[0122] (3) The pretreated copper powder and the sol in a mass ratio of 1:40 were mixed evenly by ultrasonic treatment (power of 200 W) and stirring (speed of 60 rpm, time of 10 min), and then evaporated, concentrated and dried in sequence to obtain gel-coated copper powder;

[0123] (4) After preparing a reaction mixture containing gel-coated copper powder, water, an antioxidant and calcium hydroxide, a hydrothermal treatment is performed, and after post-treatment, an antioxidant copper powder is obtained; wherein the mass ratio of the gel-coated copper powder, water and calcium hydroxide is 1:50:0.01, and the mass ratio of the antioxidant to the gel-coated copper powder is 0.05:1; the temperature of the hydrothermal treatment is 200°C, and the time is 8 hours.

[0124] The final oxidation-resistant copper powder (SEM morphology as shown in Figure 1 (as shown in c) is composed of copper powder and a coating layer located on its surface; the coating layer is composed of hydrated calcium silicate crystals and amorphous calcium silicate, the hydrated calcium silicate crystals exist in the coating layer in a fibrous state, and the amorphous calcium silicate exists in the coating layer in an amorphous state; in the antioxidant copper powder, the content of the coating layer is 5wt%; the content of the hydrated calcium silicate crystals in the coating layer is 20wt%.

[0125] An application of an antioxidant copper powder, wherein the antioxidant copper powder prepared in this embodiment is mixed with glass powder (prepared by melt quenching method, the molar percentage of each component is: SiO2 13%, Al2O3 9%, B2O3 35%, BaO 10%, CaO 33%; the particle size after ball milling is 3.5-4.1 μm) and an organic carrier through a centrifugal mixer and a three-roll mill to prepare a conductive paste for LTCC, and then the conductive paste for LTCC is printed on the surface of a LTCC substrate (manufacturer is Ferro Company, model A6M-E), and then dried and co-fired in sequence to prepare LTCC;

[0126] The contents of the components in the conductive paste for LTCC are as follows: 85wt% of antioxidant copper powder, 10wt% of glass powder, and the balance of organic carrier; the organic carrier is composed of 5wt% of resin and the balance of organic solvent; the resin is acrylic resin (manufacturer is Mitsubishi Group, model BR105); the organic solvent is dibutyl phthalate;

[0127] The drying temperature is 120°C and the time is 15 minutes. The co-firing process is as follows: first, in an air atmosphere, the temperature is increased to 300°C at a heating rate of 1°C / min and then kept warm for 30 minutes. Then, in a dry atmosphere, the temperature is increased to 500°C at a heating rate of 5°C / min and then kept warm for 2 hours. Finally, in a dry nitrogen atmosphere, the temperature is increased to 860°C at a heating rate of 8°C / min and then kept warm for 25 minutes.

[0128] The final LTCC is made of copper film (SEM morphology as shown in Figure 1 The copper film has no warping or cracking, the average square resistance of the copper film is 13.2mΩ / square, and the tensile force between the copper film and the LTCC substrate is 35N.

[0129] Example 4

[0130] A method for preparing an oxidation-resistant copper powder, the specific steps are as follows:

[0131] (1) Preparation of raw materials;

[0132] Copper powder: spherical copper, the manufacturer is Ningbo Guangxin Nanomaterials Co., Ltd., the specification is Cu-GB1001, the particle size is 1.5-5μm;

[0133] TEOS;

[0134] Calcium salts: calcium nitrate;

[0135] Solvent: ethanol;

[0136] Hydrochloric acid aqueous solution: concentration is 1M;

[0137] Nitric acid aqueous solution: concentration is 1M;

[0138] acetone;

[0139] Ethanol;

[0140] Xylene;

[0141] Water: deionized water;

[0142] Antioxidant: Oleic acid;

[0143] Calcium hydroxide;

[0144] (2) washing the copper powder with an acid solution, washing with an organic solvent, washing with a centrifuge, and drying in sequence to remove the surface passivation layer to obtain a pretreated copper powder; at the same time, mixing TEOS and calcium salt in a molar ratio of 1:1 in a solvent (the concentration of TEOS in the solvent is 9 g / L), stirring, and heating until TEOS is fully hydrolyzed to obtain a sol;

[0145] The components and contents of the pickling solution are as follows: 40wt% hydrochloric acid aqueous solution, 20wt% nitric acid aqueous solution, and the balance ethanol; the pickling solution is cleaned at a temperature of 40°C and for 60 minutes;

[0146] The components and contents of the organic solvent are: 90wt% acetone, 8wt% ethanol, and the remainder xylene; the temperature of the organic solvent cleaning is 70°C, and the time is 120min;

[0147] (3) The pretreated copper powder and the sol in a mass ratio of 1:40 were mixed evenly by ultrasonic treatment (power of 50 W) and stirring (speed of 80 rpm, time of 5 min), and then evaporated, concentrated and dried in sequence to obtain gel-coated copper powder;

[0148] (4) After preparing a reaction mixture containing gel-coated copper powder, water, an antioxidant and calcium hydroxide, a hydrothermal treatment is performed, and after post-treatment, an antioxidant copper powder is obtained; wherein the mass ratio of the gel-coated copper powder, water and calcium hydroxide is 10:100:0.3, and the mass ratio of the antioxidant to the gel-coated copper powder is 0.01:1; the temperature of the hydrothermal treatment is 180° C., and the time is 24 hours.

[0149] The finally obtained antioxidant copper powder consists of copper powder and a coating layer located on the surface thereof; the coating layer consists of hydrated calcium silicate crystals and amorphous calcium silicate, the hydrated calcium silicate crystals exist in the coating layer in a fibrous state, and the amorphous calcium silicate exists in the coating layer in an amorphous state; in the antioxidant copper powder, the content of the coating layer is 5wt%; and the content of the hydrated calcium silicate crystals in the coating layer is 50wt%.

[0150] An application of an antioxidant copper powder, wherein the antioxidant copper powder prepared in this embodiment is mixed with glass powder (prepared by melt quenching method, the molar percentage of each component is: SiO2 12%, Al2O3 10%, B2O3 36%, BaO 9%, CaO 29%, Na2O4%; the particle size after ball milling is 6.5-8.7 μm) and an organic carrier through a centrifugal mixer and a three-roll mill to prepare a conductive paste for LTCC, and then the conductive paste for LTCC is printed on the surface of a LTCC substrate (manufactured by DuPont, model 9K7), and then dried and co-fired in sequence to prepare LTCC;

[0151] The contents of the components in the conductive paste for LTCC are as follows: 70wt% of antioxidant copper powder, 10wt% of glass powder, and the balance of organic carrier; the organic carrier is composed of 15wt% of resin and the balance of organic solvent; the resin is acrylic resin (manufacturer is Mitsubishi Group, model BR105); the organic solvent is dihydropinene alcohol;

[0152] The drying temperature is 120°C and the time is 30 minutes. The co-firing process is as follows: first, in an air atmosphere, the temperature is increased to 300°C at a heating rate of 2°C / min and then kept warm for 45 minutes. Then, in a dry atmosphere, the temperature is increased to 450°C at a heating rate of 10°C / min and then kept warm for 3 hours. Finally, in a dry nitrogen atmosphere, the temperature is increased to 870°C at a heating rate of 7°C / min and then kept warm for 30 minutes.

[0153] The final LTCC is composed of a copper film and a LTCC substrate. The copper film has no warping or cracking, the average square resistance of the copper film is 7.6mΩ / square, and the tensile force between the copper film and the LTCC substrate is 24N.

[0154] Example 5

[0155] A method for preparing an oxidation-resistant copper powder, the specific steps are as follows:

[0156] (1) Preparation of raw materials;

[0157] Copper powder: spherical copper, the manufacturer is Ningbo Guangxin Nanomaterials Co., Ltd., the specification is Cu-GB1001, the particle size is 1.5-5μm;

[0158] TEOS;

[0159] Calcium salt: calcium chloride;

[0160] Solvent: triethanolamine;

[0161] Hydrochloric acid aqueous solution: concentration is 1M;

[0162] Nitric acid aqueous solution: concentration is 1M;

[0163] acetone;

[0164] Ethanol;

[0165] Xylene;

[0166] Water: ultrapure water;

[0167] Antioxidant: Citric acid;

[0168] Calcium hydroxide;

[0169] (2) washing the copper powder with an acid solution, washing with an organic solvent, washing with a centrifuge, and drying in sequence to remove the surface passivation layer to obtain a pretreated copper powder; at the same time, mixing TEOS and calcium salt in a molar ratio of 1:1 in a solvent (the concentration of TEOS in the solvent is 9 g / L), stirring, and heating until TEOS is fully hydrolyzed to obtain a sol;

[0170] The components and contents of the pickling solution are as follows: 30 wt% hydrochloric acid aqueous solution, 20 wt% nitric acid aqueous solution, and the balance ethanol; the pickling solution cleaning temperature is 40°C and the cleaning time is 100 min;

[0171] The components and contents of the organic solvent are: acetone 70wt%, ethanol 10wt%, and xylene as the balance; the organic solvent washing temperature is 20°C and the washing time is 10min;

[0172] (3) The pretreated copper powder and the sol in a mass ratio of 1:40 were mixed evenly by ultrasonic treatment (power of 300 W) and stirring (speed of 100 rpm, time of 20 min), and then evaporated, concentrated and dried in sequence to obtain gel-coated copper powder;

[0173] (4) After preparing a reaction mixture containing gel-coated copper powder, water, an antioxidant and calcium hydroxide, a hydrothermal treatment is performed, and after post-treatment, an antioxidant copper powder is obtained; wherein the mass ratio of the gel-coated copper powder, water and calcium hydroxide is 5:100:0.3, and the mass ratio of the antioxidant to the gel-coated copper powder is 0.03:1; the temperature of the hydrothermal treatment is 180° C., and the time is 16 hours.

[0174] The finally obtained antioxidant copper powder consists of copper powder and a coating layer located on the surface thereof; the coating layer consists of hydrated calcium silicate crystals and amorphous calcium silicate, the hydrated calcium silicate crystals exist in the coating layer in a fibrous state, and the amorphous calcium silicate exists in the coating layer in an amorphous state; in the antioxidant copper powder, the content of the coating layer is 5wt%; and the content of the hydrated calcium silicate crystals in the coating layer is 20wt%.

[0175] An application of an antioxidant copper powder, wherein the antioxidant copper powder prepared in this embodiment is mixed with glass powder (prepared by melt quenching method, the molar percentage of each component is: SiO2 12%, Al2O3 10%, B2O3 30%, BaO 9%, CaO 29%, Na2O4%, Y2O3 6%; the particle size after ball milling is 3.6-5.1 μm) and an organic carrier through a centrifugal mixer and a three-roll mill to prepare a conductive paste for LTCC, and then the conductive paste for LTCC is printed on the surface of a LTCC substrate (manufacturer is DuPont, model 951), and then dried and co-fired in sequence to prepare LTCC;

[0176] The contents of the components in the conductive paste for LTCC are as follows: 80wt% of antioxidant copper powder, 5wt% of glass powder, and the balance of organic carrier; the organic carrier is composed of 5wt% of resin and the balance of organic solvent; the resin is ethyl cellulose (manufacturer is Shanghai Yuanye Biotechnology Co., Ltd., model number is S14026); the organic solvent is ethylene glycol butyl ether;

[0177] The drying temperature is 120℃ and the time is 20min; the co-firing process is as follows: first, in an air atmosphere, the temperature is increased to 300℃ at a heating rate of 8℃ / min and then kept warm for 30min; then, in a dry atmosphere, the temperature is increased to 600℃ at a heating rate of 10℃ / min and then kept warm for 3h; finally, in a dry nitrogen atmosphere, the temperature is increased to 880℃ at a heating rate of 10℃ / min and then kept warm for 35min.

[0178] The final LTCC is composed of a copper film and a LTCC substrate. The copper film has no warping or cracking, the average square resistance of the copper film is 15.5mΩ / square, and the tensile force between the copper film and the LTCC substrate is 37N.

[0179] Example 6

[0180] A method for preparing an oxidation-resistant copper powder, the specific steps are as follows:

[0181] (1) Preparation of raw materials;

[0182] Copper powder: copper flakes, the manufacturer is Ningbo Guangxin Nanomaterials Co., Ltd., the specification is CuF-GB1001, the particle size is 1.5-5.5μm;

[0183] TEOS;

[0184] Calcium salts: calcium nitrate;

[0185] Solvent: triethanolamine;

[0186] Hydrochloric acid aqueous solution: concentration is 1M;

[0187] Nitric acid aqueous solution: concentration is 1M;

[0188] acetone;

[0189] Ethanol;

[0190] Xylene;

[0191] Water: ultrapure water;

[0192] Antioxidants: Ascorbic acid;

[0193] Calcium hydroxide;

[0194] (2) washing the copper powder with an acid solution, washing with an organic solvent, washing with a centrifuge, and drying in sequence to remove the surface passivation layer to obtain a pretreated copper powder; at the same time, mixing TEOS and calcium salt in a molar ratio of 1.2:1 in a solvent (the concentration of TEOS in the solvent is 9 g / L), stirring, and heating until TEOS is fully hydrolyzed to obtain a sol;

[0195] The components and contents of the pickling solution are as follows: 30wt% hydrochloric acid aqueous solution, 20wt% nitric acid aqueous solution, and the balance ethanol; the pickling solution is cleaned at a temperature of 40°C and for 120 minutes;

[0196] The components and contents of the organic solvent are: acetone 50wt%, ethanol 45wt%, and xylene as the balance; the organic solvent washing temperature is 30°C and the time is 30min;

[0197] (3) The pretreated copper powder and the sol in a mass ratio of 1:24 were mixed evenly by ultrasonic treatment (power of 500 W) and stirring (speed of 80 rpm, time of 20 min), and then evaporated, concentrated and dried in sequence to obtain gel-coated copper powder;

[0198] (4) After preparing a reaction mixture containing gel-coated copper powder, water, an antioxidant and calcium hydroxide, a hydrothermal treatment is performed, and after post-treatment, an antioxidant copper powder is obtained; wherein the mass ratio of the gel-coated copper powder, water and calcium hydroxide is 10:50:0.05, and the mass ratio of the antioxidant to the gel-coated copper powder is 0.04:1; the temperature of the hydrothermal treatment is 180° C., and the time is 16 hours.

[0199] The finally obtained antioxidant copper powder consists of copper powder and a coating layer located on the surface thereof; the coating layer consists of hydrated calcium silicate crystals and amorphous calcium silicate, the hydrated calcium silicate crystals exist in the coating layer in a fibrous state, and the amorphous calcium silicate exists in the coating layer in an amorphous state; in the antioxidant copper powder, the content of the coating layer is 3wt%; and the content of the hydrated calcium silicate crystals in the coating layer is 40wt%.

[0200] An application of an antioxidant copper powder, wherein the antioxidant copper powder prepared in this embodiment is mixed with glass powder (manufacturer is AGC, model number is ASF-1700) and an organic carrier by a centrifugal mixer and a three-roll mill to prepare a conductive paste for LTCC, and then the conductive paste for LTCC is printed on the surface of a LTCC substrate (manufacturer is Kyocera, model number is GL330), and then dried and co-fired in sequence to prepare LTCC;

[0201] The contents of the components in the conductive paste for LTCC are as follows: 85wt% of antioxidant copper powder, 2wt% of glass powder, and the balance of organic carrier; the organic carrier is composed of 10wt% of resin and the balance of organic solvent; the resin is ethyl cellulose (manufacturer is Shanghai Yuanye Biotechnology Co., Ltd., model number is S14026); the organic solvent is diethylene glycol butyl ether;

[0202] The drying temperature is 100°C and the time is 10 min. The co-firing process is as follows: first, in an air atmosphere, the temperature is increased to 300°C at a heating rate of 10°C / min and then kept for 1 h. Then, in a dry atmosphere, the temperature is increased to 500°C at a heating rate of 10°C / min and then kept for 6 h. Finally, in a weak reducing atmosphere, the temperature is increased to 890°C at a heating rate of 15°C / min and then kept for 40 min. The weak reducing atmosphere consists of 2% V / V hydrogen and the balance argon.

[0203] The final LTCC is composed of a copper film and a LTCC substrate. The copper film has no warping or cracking, the average square resistance of the copper film is 16.2mΩ / square, and the tensile force between the copper film and the LTCC substrate is 25N.

[0204] Example 7

[0205] A method for preparing an oxidation-resistant copper powder, the specific steps are as follows:

[0206] (1) Preparation of raw materials;

[0207] Copper powder: copper flakes, manufactured by Zeyu New Materials Technology Co., Ltd., specification ZC-2000F, particle size 1.43-5.70μm;

[0208] TEOS;

[0209] Calcium salt: a mixture of calcium chloride and calcium nitrate in a mass ratio of 1:1;

[0210] Solvent: ethanol;

[0211] Hydrochloric acid aqueous solution: concentration is 1M;

[0212] Nitric acid aqueous solution: concentration is 1M;

[0213] acetone;

[0214] Ethanol;

[0215] Xylene;

[0216] Water: ultrapure water;

[0217] Antioxidant: Oleylamine;

[0218] Calcium hydroxide;

[0219] (2) washing the copper powder with an acid solution, washing with an organic solvent, washing with a centrifuge, and drying in sequence to remove the surface passivation layer to obtain a pretreated copper powder; at the same time, mixing TEOS and calcium salt in a solvent at a molar ratio of 1.5:1 (the concentration of TEOS in the solvent is 9 g / L), stirring, and heating until TEOS is fully hydrolyzed to obtain a sol;

[0220] The components and contents of the pickling solution are as follows: 50wt% hydrochloric acid aqueous solution, 20wt% nitric acid aqueous solution, 5wt% acetone, and the balance ethanol; the pickling solution is cleaned at a temperature of 40°C and for 30 minutes;

[0221] The components and contents of the organic solvent are: acetone 50wt%, ethanol 45wt%, and xylene as the balance; the organic solvent washing temperature is 30°C and the time is 30min;

[0222] (3) The pretreated copper powder and the sol in a mass ratio of 1:80 were mixed evenly by ultrasonic treatment (power of 50 W) and stirring (speed of 80 rpm, time of 20 min), and then evaporated, concentrated and dried in sequence to obtain gel-coated copper powder;

[0223] (4) After preparing a reaction mixture containing gel-coated copper powder, water, an antioxidant and calcium hydroxide, a hydrothermal treatment is performed, and after post-treatment, an antioxidant copper powder is obtained; wherein the mass ratio of the gel-coated copper powder, water and calcium hydroxide is 10:50:0.1, and the mass ratio of the antioxidant to the gel-coated copper powder is 0.04:1; the temperature of the hydrothermal treatment is 180°C, and the time is 16 hours.

[0224] The finally obtained antioxidant copper powder consists of copper powder and a coating layer located on the surface thereof; the coating layer consists of hydrated calcium silicate crystals and amorphous calcium silicate, the hydrated calcium silicate crystals exist in the coating layer in a fibrous state, and the amorphous calcium silicate exists in the coating layer in an amorphous state; in the antioxidant copper powder, the content of the coating layer is 10wt%; and the content of the hydrated calcium silicate crystals in the coating layer is 34wt%.

[0225] An application of an antioxidant copper powder, wherein the antioxidant copper powder prepared in this embodiment is mixed with glass powder (manufactured by AGC, model ASF-1780) and an organic carrier by a centrifugal mixer and a three-roll mill to prepare a conductive paste for LTCC, and then the conductive paste for LTCC is printed on the surface of a LTCC substrate (manufactured by Ferro, model A6M-E), and then dried and co-fired in sequence to prepare LTCC;

[0226] The contents of the components in the conductive paste for LTCC are as follows: 85wt% of antioxidant copper powder, 3wt% of glass powder, and the balance of organic carrier; the organic carrier is composed of 12wt% of resin and the balance of organic solvent; the resin is cellulose acetate butyrate (manufacturer is Shanghai Yuanye Biotechnology Co., Ltd., model number is S33470); the organic solvent is diethylene glycol butyl ether acetate;

[0227] The drying temperature is 130℃ and the time is 10min. The co-firing process is as follows: first, in an air atmosphere, the temperature is increased to 300℃ at a heating rate of 10℃ / min and then kept for 1h. Then, in a wet nitrogen (vapor pressure partial pressure is 12kPa) atmosphere, the temperature is increased to 450℃ at a heating rate of 5℃ / min and then kept for 3h. Finally, in a weak reducing atmosphere, the temperature is increased to 900℃ at a heating rate of 5℃ / min and then kept for 30min. The weak reducing atmosphere consists of 2%V / V hydrogen and the balance argon.

[0228] The final LTCC is composed of a copper film and a LTCC substrate. The copper film has no warping or cracking, the average square resistance of the copper film is 14.7mΩ / square, and the tensile force between the copper film and the LTCC substrate is 21N.

[0229] Example 8

[0230] A method for preparing an oxidation-resistant copper powder, the specific steps are as follows:

[0231] (1) Preparation of raw materials;

[0232] Copper powder: copper flakes, manufactured by Zeyu New Materials Technology Co., Ltd., specification ZC-3000F, particle size 1.81-6.96μm;

[0233] TEOS;

[0234] Calcium salt: calcium chloride;

[0235] Solvent: ethanol;

[0236] Hydrochloric acid aqueous solution: concentration is 1M;

[0237] Nitric acid aqueous solution: concentration is 1M;

[0238] acetone;

[0239] Ethanol;

[0240] Xylene;

[0241] Water: ultrapure water;

[0242] Antioxidant: Citric acid;

[0243] Calcium hydroxide;

[0244] (2) washing the copper powder with an acid solution, washing with an organic solvent, washing with a centrifuge, and drying in sequence to remove the surface passivation layer to obtain a pretreated copper powder; at the same time, mixing TEOS and calcium salt in a solvent at a molar ratio of 1.8:1 (the concentration of TEOS in the solvent is 9 g / L), stirring, and heating until TEOS is fully hydrolyzed to obtain a sol;

[0245] The components and contents of the pickling solution are as follows: 30wt% hydrochloric acid aqueous solution, 20wt% nitric acid aqueous solution, 5wt% acetone, and the balance ethanol; the pickling solution is cleaned at a temperature of 40°C and for 30 minutes;

[0246] The components and contents of the organic solvent are: acetone 50wt%, ethanol 45wt%, and xylene as the balance; the organic solvent washing temperature is 30°C and the time is 30min;

[0247] (3) The pretreated copper powder and the sol in a mass ratio of 1:120 were mixed evenly by ultrasonic treatment (power of 200 W) and stirring (speed of 80 rpm, time of 20 min), and then evaporated, concentrated and dried in sequence to obtain gel-coated copper powder;

[0248] (4) After preparing a reaction mixture containing gel-coated copper powder, water, an antioxidant and calcium hydroxide, a hydrothermal treatment is performed, and after post-treatment, an antioxidant copper powder is obtained; wherein the mass ratio of the gel-coated copper powder, water and calcium hydroxide is 10:50:0.15, and the mass ratio of the antioxidant to the gel-coated copper powder is 0.04:1; the temperature of the hydrothermal treatment is 180° C., and the time is 16 hours.

[0249] The finally obtained antioxidant copper powder consists of copper powder and a coating layer located on the surface thereof; the coating layer consists of hydrated calcium silicate crystals and amorphous calcium silicate, the hydrated calcium silicate crystals exist in the coating layer in a fibrous state, and the amorphous calcium silicate exists in the coating layer in an amorphous state; in the antioxidant copper powder, the content of the coating layer is 15wt%; and the content of the hydrated calcium silicate crystals in the coating layer is 25wt%.

[0250] An application of an antioxidant copper powder, wherein the antioxidant copper powder prepared in this embodiment is mixed with glass powder (manufactured by Xi'an Xinzheng Materials Technology Co., Ltd., model PM-850) and an organic carrier by a centrifugal mixer and a three-roll mill to prepare a conductive paste for LTCC, and then the conductive paste for LTCC is printed on the surface of a LTCC substrate (manufactured by Ferro, model A6M-E), and then dried and co-fired in sequence to prepare LTCC;

[0251] The contents of the components in the conductive paste for LTCC are as follows: 85wt% of antioxidant copper powder, 4wt% of glass powder, and the balance of organic carrier; the organic carrier is composed of 13wt% of resin and the balance of organic solvent; the resin is cellulose acetate butyrate (manufacturer is Shanghai Yuanye Biotechnology Co., Ltd., model number is S33470); the organic solvent is tributyl citrate;

[0252] The drying temperature is 140℃ and the time is 10min. The co-firing process is as follows: first, in an air atmosphere, the temperature is increased to 300℃ at a heating rate of 10℃ / min and then kept for 1h. Then, in a wet nitrogen (vapor pressure partial pressure is 12kPa) atmosphere, the temperature is increased to 500℃ at a heating rate of 2℃ / min and then kept for 3h. Finally, in a weak reducing atmosphere, the temperature is increased to 900℃ at a heating rate of 5℃ / min and then kept for 30min. The weak reducing atmosphere consists of 2%V / V hydrogen and the balance argon.

[0253] The final LTCC is composed of a copper film and a LTCC substrate. The copper film has no warping or cracking, the average square resistance of the copper film is 14.5mΩ / square, and the tensile force between the copper film and the LTCC substrate is 22N.

[0254] Example 9

[0255] A method for preparing an oxidation-resistant copper powder, the specific steps are as follows:

[0256] (1) Preparation of raw materials;

[0257] Copper powder: copper flakes, manufactured by Zeyu New Materials Technology Co., Ltd., specification ZC-4000F, particle size 2.43-10.58μm;

[0258] TEOS;

[0259] Calcium salts: calcium nitrate;

[0260] Solvent: ethanol;

[0261] Hydrochloric acid aqueous solution: concentration is 1M;

[0262] Nitric acid aqueous solution: concentration is 1M;

[0263] acetone;

[0264] Ethanol;

[0265] Xylene;

[0266] Water: deionized water;

[0267] Antioxidant: Oleic acid;

[0268] Calcium hydroxide;

[0269] (2) washing the copper powder with an acid solution, washing with an organic solvent, washing with a centrifuge, and drying in sequence to remove the surface passivation layer to obtain a pretreated copper powder; at the same time, mixing TEOS and calcium salt in a molar ratio of 2:1 in a solvent (the concentration of TEOS in the solvent is 9 g / L), stirring, and heating until TEOS is fully hydrolyzed to obtain a sol;

[0270] The components and contents of the pickling solution are as follows: 30wt% hydrochloric acid aqueous solution, 20wt% nitric acid aqueous solution, 5wt% acetone, and the balance ethanol; the pickling solution is cleaned at a temperature of 40°C and for 30 minutes;

[0271] The components and contents of the organic solvent are: acetone 50wt%, ethanol 45wt%, and xylene as the balance; the organic solvent washing temperature is 30°C and the time is 30min;

[0272] (3) The pretreated copper powder and the sol in a mass ratio of 1:160 were mixed evenly by ultrasonic treatment (power of 500 W) and stirring (speed of 80 rpm, time of 20 min), and then evaporated, concentrated and dried in sequence to obtain gel-coated copper powder;

[0273] (4) After preparing a reaction mixture containing gel-coated copper powder, water, an antioxidant and calcium hydroxide, a hydrothermal treatment is performed, and after post-treatment, an antioxidant copper powder is obtained; wherein the mass ratio of the gel-coated copper powder, water and calcium hydroxide is 10:50:0.2, and the mass ratio of the antioxidant to the gel-coated copper powder is 0.04:1; the temperature of the hydrothermal treatment is 180° C., and the time is 16 hours.

[0274] The finally obtained antioxidant copper powder consists of copper powder and a coating layer located on the surface thereof; the coating layer consists of hydrated calcium silicate crystals and amorphous calcium silicate, the hydrated calcium silicate crystals exist in the coating layer in a fibrous state, and the amorphous calcium silicate exists in the coating layer in an amorphous state; in the antioxidant copper powder, the content of the coating layer is 20wt%; and the content of the hydrated calcium silicate crystals in the coating layer is 33wt%.

[0275] An application of an antioxidant copper powder, wherein the antioxidant copper powder prepared in this embodiment is mixed with glass powder (manufacturer is Jiangsu Baifu Technology Co., Ltd., model number is SEAL-106) and an organic carrier by a centrifugal mixer and a three-roll mill to prepare a conductive paste for LTCC, and then the conductive paste for LTCC is printed on the surface of a LTCC substrate (manufacturer is Ferro, model number is A6M-E), and then dried and co-fired in sequence to prepare LTCC;

[0276] The contents of the components in the conductive paste for LTCC are as follows: 85wt% of antioxidant copper powder, 5wt% of glass powder, and the balance of organic carrier; the organic carrier is composed of 14wt% of resin and the balance of organic solvent; the resin is cellulose acetate butyrate (manufacturer is Shanghai Yuanye Biotechnology Co., Ltd., model number is S33470); the organic solvent is acetone;

[0277] The drying temperature is 150℃ and the time is 10min. The co-firing process is as follows: first, in an air atmosphere, the temperature is increased to 300℃ at a heating rate of 10℃ / min and then kept for 1h. Then, in a wet nitrogen (vapor pressure partial pressure is 12kPa) atmosphere, the temperature is increased to 600℃ at a heating rate of 3℃ / min and then kept for 3h. Finally, in a weak reducing atmosphere, the temperature is increased to 870℃ at a heating rate of 5℃ / min and then kept for 30min. The weak reducing atmosphere consists of 2%V / V hydrogen and the balance argon.

[0278] The final LTCC is composed of a copper film and a LTCC substrate. The copper film has no warping or cracking, the average square resistance of the copper film is 20.3mΩ / square, and the tensile force between the copper film and the LTCC substrate is 20N.

[0279] Comparative Example 2

[0280] A method for preparing an antioxidant copper powder is basically the same as that of Example 9, except that step (2) and step (3) are not performed, the gel-coated copper powder in step (4) is replaced by the copper powder in Example 9, and the mass of the copper powder added is the same as that of Example 9.

[0281] The application of an antioxidant copper powder is basically the same as that of Example 9, except that the antioxidant copper powder used in preparing the conductive paste for LTCC is the antioxidant copper powder prepared in this comparative example.

[0282] In comparative example 2, during the co-firing process, the copper powder was severely oxidized, the surface of the copper film was brown-black, and the sintering density was poor; the average square resistance of the copper film in the final LTCC was 16000 mΩ / square, and the tension between the copper film and the LTCC substrate was 6N.

[0283] Compared with Example 9, the comprehensive performance of the LTCC prepared in Comparative Example 2 is significantly reduced. This is because in Comparative Example 2, copper powder is directly used to replace the gel-coated copper powder in Example 9 when preparing the antioxidant copper powder. This copper powder does not have a core-shell structure and lacks a coating layer composed of hydrated calcium silicate crystals and amorphous calcium silicate. The copper powder is not effectively protected during the sintering process. Therefore, the copper powder is severely oxidized during the co-firing process, the surface of the copper film appears brown-black, and the sintering density is poor. This oxidation not only affects the conductivity of the copper film, but also reduces its bonding strength with the LTCC substrate.

[0284] Comparative Example 3

[0285] A method for preparing an antioxidant copper powder is basically the same as that of Example 9, except that: step (4) comprises preparing a reaction mixture containing gel-coated copper powder, water, an antioxidant and calcium hydroxide and placing the mixture in an alumina porcelain boat; heating the reaction mixture in a tube furnace at a rate of 5°C / min to 600°C under nitrogen protection and keeping the temperature for 2 hours; wherein the mass ratio of the gel-coated copper powder, water and calcium hydroxide is 10:50:0.2, and the mass ratio of the antioxidant to the gel-coated copper powder is 0.04:1.

[0286] The finally prepared anti-oxidation copper powder consists of copper powder and a coating layer on the surface of the copper powder; the coating layer is amorphous calcium silicate.

[0287] The application of an antioxidant copper powder is basically the same as that of Example 9, except that the antioxidant copper powder used in preparing the conductive paste for LTCC is the antioxidant copper powder prepared in this comparative example.

[0288] The average square resistance of the copper film in the final LTCC is 25mΩ / square.

[0289] Compared with Example 9, the average square resistance of LTCC in Comparative Example 3 is increased. This is because the oxidation-resistant copper powder used in Comparative Example 3 to prepare the conductive paste for LTCC is only composed of amorphous calcium silicate as a coating layer, and its density is poorer than that of the coating layer composed of hydrated calcium silicate crystals and amorphous calcium silicate, which leads to its insufficient antioxidant ability and is easily affected by oxidation, resulting in a decrease in the conductivity of the copper film and an increase in the average square resistance.

Claims

1. An oxidation resistant copper powder, characterized in that: The invention comprises copper powder and a coating layer on the surface of the copper powder; the coating layer is composed of hydrated calcium silicate crystals and amorphous calcium silicate, the hydrated calcium silicate crystals exist in the coating layer in a fibrous state, and the amorphous calcium silicate exists in the coating layer in an amorphous state; the copper powder is spherical copper or plate-like copper, the particle size of the spherical copper is 0.85-5μm, and the particle size of the plate-like copper is 1.43-10.58μm; in the antioxidant copper powder, the content of the coating layer is 3-20wt%; and the content of the hydrated calcium silicate crystals in the coating layer is 20-50wt%.

2. A method for preparing an oxidation resistant copper powder as claimed in claim 1, characterized in that: The following steps are involved: (1) Pre-treating the copper powder to remove the surface passivation layer to obtain pre-treated copper powder; at the same time, mixing TEOS and calcium salt in a solvent, stirring and heating until TEOS is fully hydrolyzed to obtain a sol; (2) After the pretreated copper powder and the sol are uniformly mixed, evaporation concentration and drying are performed in sequence to obtain gel-coated copper powder; (3) preparing a reaction mixture containing gel-coated copper powder, water, calcium hydroxide and an antioxidant, performing a hydrothermal treatment, and obtaining an antioxidant copper powder through post-treatment.

3. The method according to claim 2, characterized in that In step (1), the calcium salt is calcium chloride and / or calcium nitrate; the solvent is one or more of ethanol, ethylene glycol and triethanolamine; the molar ratio of TEOS to the calcium salt is 1-2:1, and the concentration of TEOS in the solvent is 9 g / L.

4. The method according to claim 2, characterized in that: In step (2), the mass ratio of the pretreated copper powder to the sol is 1:20-160.

5. The method according to claim 2, characterized in that: In step (3), water is deionized water or ultrapure water; the mass ratio of gel-coated copper powder, water, and calcium hydroxide is 1-10:50-100:0.01-3; the temperature of the hydrothermal treatment is 160-200° C., and the time is 8-24 hours.

6. The use of an oxidation-resistant copper powder as claimed in claim 1, characterized in that: The conductive paste for LTCC was prepared using the oxidation-resistant copper powder as a conductive agent.

7. The use according to claim 6, characterized in that: The components and contents of the conductive paste for LTCC are: 70-85wt% of antioxidant copper powder, 0-10wt% of glass powder, and the balance of organic carrier.

8. The use according to claim 6, characterized in that: The conductive paste for LTCC is also printed on the surface of the LTCC substrate, and then dried and co-fired in sequence to obtain LTCC.

9. The use according to claim 8, characterized in that: The drying temperature is 100-150°C and the time is 10-30min. The co-firing process is as follows: first, in an air atmosphere, the temperature is increased to 300°C at a heating rate of 1-10°C / min and then kept for 30min-1h. Then, in a dry nitrogen atmosphere, the temperature is increased to 450-600°C at a heating rate of 1-10°C / min and then kept for 2-3h. Alternatively, in a wet nitrogen atmosphere, the temperature is increased to 450-600°C at a heating rate of 1-10°C / min and then kept for 3-6h. Finally, in a dry nitrogen atmosphere or a weak reducing atmosphere, the temperature is increased to 850-900°C at a heating rate of 5-15°C / min and then kept for 20-40min. The weak reducing atmosphere is composed of 2%V / V hydrogen and the balance argon. LTCC is composed of copper film and LTCC substrate. The copper film has no warping or cracking. The average square resistance of the copper film is 3-20.3mΩ / square. The tensile force between the copper film and the LTCC substrate is 20-49N.