A method for preparing ZnO@CuO reinforced silver-based composite materials by powder metallurgy

ZnO@CuO reinforced silver-based composite materials were prepared by powder metallurgy, which improved the interfacial wettability and solved the problem of poor interfacial wettability of Ag/ZnO electrical contact materials during arc erosion, thereby improving the arc extinguishing performance and electrical life of the materials.

CN118531250BActive Publication Date: 2026-11-17NANCHONG FUHAI MATERIAL TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410598270.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-15
Publication Date
2026-11-17
Estimated Expiration
2044-05-15

AI Technical Summary

Technical Problem

Ag/ZnO electrical contact materials exhibit poor interfacial wettability during arc erosion, resulting in poor arc extinguishing performance and insufficient electrical life.

Method used

ZnO@CuO reinforced silver-based composite material was prepared by powder metallurgy. CuO was used as the interface between ZnO and Ag to improve the interface wettability and enhance the bonding force. ZnO@CuO powder was prepared by a combination of electrolysis and sintering, and then ball-milled, pressed into shape and sintered to form a core-shell structure.

Benefits of technology

It improves the physical properties and arc erosion resistance of silver-based composite materials, and has good arc extinguishing performance and long electrical life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118531250B_ABST
    Figure CN118531250B_ABST
Patent Text Reader

Abstract

This invention relates to the field of composite material technology and discloses a method for preparing ZnO@CuO reinforced silver-based composite materials using powder metallurgy. The method includes the following steps: S1, using ZnO powder as raw material, ZnO@CuO powder is obtained through a combination of electrolysis and sintering; S2, the ZnO@CuO powder obtained in step S1 is mixed with Ag powder in a certain proportion and then ball-milled to obtain a composite powder; S3, the composite powder obtained in step S2 is pressed into shape in a mold and sintered in a sintering furnace to form a ZnO@CuO reinforced silver-based composite material sintered blank; the sintered blank is then densified, extruded, and drawn into wire. This invention uses the CuO shell as the interface between ZnO and Ag, improving the interfacial wettability and interfacial bonding force, thus obtaining a ZnO@CuO core-shell structure metal oxide reinforced silver-based composite material. This improves the physical properties and arc erosion resistance of the silver-based composite material, resulting in good arc extinguishing performance, high electrical lifetime, and excellent resistance to material transfer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of composite material technology, specifically a method for preparing ZnO@CuO reinforced silver-based composite materials using powder metallurgy. Background Technology

[0002] Ag / ZnO is widely used as an electrical contact material in air circuit breakers, residual current circuit breakers, and miniature circuit breakers due to its properties such as resistance to burn-through, good resistance to welding, resistance to electrical abrasion, and low and stable contact resistance. Especially in the current range of 3000–5000A, Ag / ZnO electrical contact material exhibits excellent resistance to arc erosion during breaking, making it the preferred material for low-voltage electrical appliances with breaking currents of 3000–5000A, and particularly suitable for manufacturing larger contact sizes.

[0003] However, Ag and ZnO have poor interfacial wettability, which can easily cause splashing during arc erosion, resulting in poor arc extinguishing performance, poor electrical lifetime, and poor resistance to material transfer. Summary of the Invention

[0004] The purpose of this invention is to provide a method for preparing ZnO@CuO reinforced silver-based composite materials by powder metallurgy, so as to solve the problems mentioned in the background art.

[0005] To achieve the above objectives, the present invention provides the following technical solution:

[0006] A method for preparing ZnO@CuO reinforced silver-based composite materials by powder metallurgy includes the following steps:

[0007] S1. Using ZnO powder as raw material, ZnO@CuO powder is obtained through a combination of electrolysis and sintering.

[0008] S2. The ZnO@CuO powder obtained in step S1 is mixed with Ag powder in a certain proportion and then ball-milled to obtain composite powder.

[0009] S3. Press the composite powder obtained in step S2 into a mold; sinter it in a sintering furnace to form a ZnO@CuO reinforced silver matrix composite sintered blank; then densify the sintered blank, extrude it, and draw it into wire or roll it into strip. Since CuO is between ZnO and Ag, which have poor interfacial wettability, it improves the interfacial bonding force between the reinforcing phase and the silver matrix, and ultimately improves the mechanical properties and electrical contact properties of the metal oxide reinforced silver matrix composite.

[0010] As a further aspect of the present invention: in step S1, the specific preparation method of ZnO@CuO powder is as follows:

[0011] S11. Electrolysis is carried out in an electrolyte with a copper plate as the anode and a graphite electrode as the cathode until the copper plate at the anode is completely electrolyzed and disappears in the electrolyte.

[0012] S12. Add ZnO powder to the electrolyte at a ratio of 10-80 g / L and stir for 3-15 min; after centrifuging the electrolyte, wash it 3-6 times with deionized water at a volume ratio of 10:1; preferably, the ratio of ZnO powder to electrolyte is 50 g / L, stir for 6 min, and wash 4 times.

[0013] S13. Dry in a drying oven at 60-140℃ for 5-20 hours, then grind and pass through a 200-900 mesh sieve to obtain Cu(OH)2 powder; preferably, dry in a drying oven at 100℃ for 10 hours and grind and pass through a 200 mesh sieve.

[0014] S14. Sintering is carried out sequentially at 50-100℃ and held for 1-3 hours, at 350-450℃ and held for 1-4 hours, and at 750-850℃ and held for 1-2 hours to prepare ZnO@CuO powder; preferably, the holding temperature is 100℃ for 1 hour, 400℃ for 3 hours, and 800℃ for 2 hours.

[0015] As a further aspect of the present invention: in step S11, the electrolyte is prepared by dissolving NH4Cl in deionized water; and the current density during the electrolysis process is 0.2–0.8 A / cm². 2 The preferred current density is 0.6 A / cm². 2 .

[0016] As a further embodiment of the present invention: the particle size of the ZnO powder is 50-800 nm, the purity is ≥99.9%, and the sphericity is ≥0.9; the particle size of the ZnO powder is preferably 400 nm; the particle size of the ZnO@CuO powder is 60-900 nm, and the sphericity is ≥0.9; the particle size of the ZnO@CuO powder is preferably 550 nm.

[0017] As a further embodiment of the present invention: in step S2, the Ag powder has a particle size of 10-50 μm and a purity of ≥99.9%, and the mass percentage of ZnO@CuO powder to Ag powder is 7%-18%; preferably, the Ag powder has a particle size of 30 μm, and preferably the mass percentage of ZnO@CuO powder to Ag powder is 14%; the ball milling process has a rotation speed of 150-800 r / min and a time of 0.5-2 h; preferably, the ball milling process has a rotation speed of 400 r / min and a time of 1 h.

[0018] As a further embodiment of the present invention: in step S3, the pressure during the pressing process is 200-800 MPa; preferably 600 MPa; the sintering process adopts a multi-stage sintering method, and the sintering temperature is 100-900℃; preferably, the multi-stage sintering method is sintering at 300℃ and holding for 1 hour, sintering at 500℃ and holding for 1 hour, and sintering at 850℃ and holding for 2 hours; the extrusion temperature is 300-900℃, and the extrusion pressure is 200-800 MPa; preferably, the extrusion temperature is 820℃, and the extrusion pressure is 600 MPa.

[0019] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0020] This invention uses CuO as the interface between ZnO and Ag to improve the interfacial wettability of ZnO and Ag, thereby increasing their interfacial bonding force and obtaining a ZnO@CuO core-shell structure metal oxide reinforced silver-based composite material. This improves the physical properties and arc erosion resistance of the silver-based composite material, thus giving it good arc extinguishing performance, long electrical lifetime, and excellent resistance to material transfer. Attached Figure Description

[0021] Figure 1 This is a schematic flowchart of a method for preparing ZnO@CuO reinforced silver-based composite materials using powder metallurgy. Detailed Implementation

[0022] Example 1

[0023] Please see Figure 1 In this embodiment of the invention, a method for preparing ZnO@CuO reinforced silver-based composite materials by powder metallurgy includes the following steps:

[0024] S1. An electrolyte is prepared by dissolving NH4Cl in deionized water. A copper plate is used as the anode and a graphite electrode as the cathode. The electrolyte is then charged at a current of 0.6 A / cm. 2 Electrolysis was performed at a current density until all the copper plate at the anode disappeared into the electrolyte. ZnO powder with a particle size of 400 nm, a purity of 99.9%, and a sphericity of 0.9 was then added to the electrolyte at a ratio of 50 g / L and stirred for 6 min. After centrifugation, the electrolyte was washed four times with deionized water at a volume ratio of 10:1. Then, it was dried in a drying oven at 100℃ for 10 h, ground, and passed through a 200-mesh sieve to obtain Cu(OH)₂ powder. Finally, the powder was sintered sequentially at 100℃ for 1 h, 400℃ for 3 h, and 800℃ for 2 h to prepare ZnO@CuO powder with a particle size of 550 nm and a sphericity of 0.9.

[0025] S2. The ZnO@CuO powder obtained in step S1 is mixed with Ag powder with a particle size of 30μm and a purity of 99.9% at a mass percentage of 14%, and then ball-milled at a speed of 400r / min for 1h to obtain composite powder.

[0026] S3. The composite powder obtained in step S2 is pressed into shape in a mold under a pressure of 600 MPa; and sintered in a sintering furnace at 300℃ and held for 1 hour, 500℃ and held for 1 hour, and 850℃ and held for 2 hours to obtain a ZnO@CuO reinforced silver-based composite sintered blank; then the sintered blank is densified, extruded at a temperature of 820℃ and a pressure of 600 MPa, and drawn into wire.

[0027] Example 2

[0028] Please see Figure 1 In this embodiment of the invention, a method for preparing ZnO@CuO reinforced silver-based composite materials by powder metallurgy includes the following steps:

[0029] S1. An electrolyte is prepared by dissolving NH4Cl in deionized water. A copper plate is used as the anode and a graphite electrode as the cathode. The electrolyte is then charged at a current of 0.5 A / cm. 2 Electrolysis was performed at a current density until all the copper plate at the anode disappeared into the electrolyte. ZnO powder with a particle size of 500 nm, a purity of 99.9%, and a sphericity of 0.9 was then added to the electrolyte at a ratio of 50 g / L and stirred for 5 min. After centrifugation, the electrolyte was washed five times with deionized water at a volume ratio of 10:1. Then, it was dried in a drying oven at 110℃ for 5 h, ground, and passed through a 300-mesh sieve to obtain Cu(OH)₂ powder. Finally, it was sintered sequentially at 60℃ for 1 h, 400℃ for 2 h, and 800℃ for 2 h to prepare ZnO@CuO powder. ZnO@CuO powder with a particle size of 650 nm and a sphericity of 0.9 was obtained.

[0030] S2. The ZnO@CuO powder obtained in step S1 is mixed with Ag powder with a particle size of 50μm and a purity of 99.9% at a mass percentage of 13%, and then ball-milled at a speed of 500r / min for 1h to obtain composite powder.

[0031] S3. The composite powder obtained in step S2 is pressed into shape in a mold under a pressure of 200-800 MPa; and sintered in a sintering furnace at 300℃ and held for 1 hour, 450℃ and held for 3 hours, and 850℃ and held for 3 hours to obtain a ZnO@CuO reinforced silver-based composite material sintered blank; then the sintered blank is densified, extruded at a temperature of 750℃ and a pressure of 550 MPa, and drawn into wire.

[0032] Example 3

[0033] Please see Figure 1 In this embodiment of the invention, a method for preparing ZnO@CuO reinforced silver-based composite materials by powder metallurgy includes the following steps:

[0034] S1. An electrolyte is prepared by dissolving NH4Cl in deionized water. A copper plate is used as the anode and a graphite electrode as the cathode. The electrolyte is then charged at a current of 0.6 A / cm. 2 Electrolysis was performed at a current density until all the copper plate at the anode disappeared into the electrolyte. ZnO powder with a particle size of 200 nm, a purity of 99.9%, and a sphericity of 0.9 was then added to the electrolyte at a ratio of 60 g / L and stirred for 6 min. After centrifugation, the electrolyte was washed three times with deionized water at a volume ratio of 10:1. Then, it was dried in a drying oven at 110℃ for 5 h, ground, and passed through a 200-mesh sieve to obtain Cu(OH)₂ powder. Finally, it was sintered sequentially at 80℃ for 1.5 h, 400℃ for 1 h, and 820℃ for 2 h to prepare ZnO@CuO powder. ZnO@CuO powder with a particle size of 300 nm and a sphericity of 0.9 was obtained.

[0035] S2. The ZnO@CuO powder obtained in step S1 is mixed with Ag powder with a particle size of 45μm and a purity of 99.9% at a mass percentage of 10%, and then ball-milled at a speed of 300r / min for 0.5h to obtain composite powder.

[0036] S3. The composite powder obtained in step S2 is pressed into shape in a mold under a pressure of 550 MPa; and sintered in a sintering furnace at 200℃ and held for 2 hours, 450℃ and held for 2 hours, 600℃ and held for 2 hours, and 850℃ and held for 2 hours to obtain a ZnO@CuO reinforced silver-based composite material sintered blank; then the sintered blank is densified, extruded at a temperature of 700℃ and a pressure of 650 MPa, and drawn into wire.

[0037] Example 4

[0038] Please see Figure 1 In this embodiment of the invention, a method for preparing ZnO@CuO reinforced silver-based composite materials by powder metallurgy includes the following steps:

[0039] S1. An electrolyte is prepared by dissolving NH4Cl in deionized water. A copper plate is used as the anode and a graphite electrode as the cathode. The electrolyte is then charged at a current of 0.8 A / cm. 2Electrolysis was performed at a current density until all the copper plate at the anode disappeared into the electrolyte. ZnO powder with a particle size of 800 nm, a purity of 99.9%, and a sphericity of 0.9 was then added to the electrolyte at a ratio of 40 g / L and stirred for 6 min. After centrifugation, the electrolyte was washed three times with deionized water at a volume ratio of 10:1. Then, it was dried in a drying oven at 100℃ for 15 h, ground, and passed through a 700-mesh sieve to obtain Cu(OH)₂ powder. Finally, it was sintered sequentially at 100℃ for 1 h, 400℃ for 2 h, and 820℃ for 2 h to prepare ZnO@CuO powder. ZnO@CuO powder with a particle size of 900 nm and a sphericity of 0.9 was obtained.

[0040] S2. The ZnO@CuO powder obtained in step S1 is mixed with Ag powder with a particle size of 20μm and a purity of 99.9% at a mass percentage of 15%, and then ball-milled at a speed of 600r / min for 1h to obtain composite powder.

[0041] S3. The composite powder obtained in step S2 is pressed into shape in a mold under a pressure of 700 MPa; and sintered in a sintering furnace at 100℃ and held for 1 h, 300℃ and held for 2.5 h, 450℃ and held for 2 h, and 850℃ and held for 3 h to obtain a ZnO@CuO reinforced silver-based composite sintered blank; then the sintered blank is densified, extruded at a temperature of 800℃ and a pressure of 600 MPa, and drawn into wire.

[0042] Example 5

[0043] Please see Figure 1 In this embodiment of the invention, a method for preparing ZnO@CuO reinforced silver-based composite materials by powder metallurgy includes the following steps:

[0044] S1. An electrolyte is prepared by dissolving NH4Cl in deionized water. A copper plate is used as the anode and a graphite electrode as the cathode. The electrolyte is then charged at a current of 0.8 A / cm. 2Electrolysis was performed at a current density until all the copper plate at the anode disappeared into the electrolyte. ZnO powder with a particle size of 80 nm, a purity of 99.9%, and a sphericity of 0.9 was then added to the electrolyte at a ratio of 40 g / L and stirred for 10 min. After centrifugation, the electrolyte was washed three times with deionized water at a volume ratio of 10:1. Then, it was dried in an oven at 80℃ for 15 h, ground, and passed through a 600-mesh sieve to obtain Cu(OH)₂ powder. Finally, the powder was sintered sequentially at 80℃ for 2.5 h, 400℃ for 3 h, and 800℃ for 2 h to prepare ZnO@CuO powder. ZnO@CuO powder with a particle size of 100 nm and a sphericity of 0.9 was obtained.

[0045] S2. The ZnO@CuO powder obtained in step S1 is mixed with Ag powder with a particle size of 20μm and a purity of 99.9% at a mass percentage of 8%, and then ball-milled at a speed of 700r / min for 2h to obtain composite powder.

[0046] S3. The composite powder obtained in step S2 is pressed into shape in a mold under a pressure of 800 MPa; and sintered in a sintering furnace at 100℃ and held for 2 hours, 350℃ and held for 2 hours, 450℃ and held for 2 hours, 650℃ and held for 2 hours, and 850℃ and held for 2 hours to obtain a ZnO@CuO reinforced silver-based composite material sintered blank; then the sintered blank is densified, extruded at a temperature of 780℃ and a pressure of 550 MPa, and drawn into wire.

[0047] To better illustrate the technical effects of the present invention, the following experiments are conducted:

[0048] Example 1 of the preparation method of silver-zinc oxide composite material disclosed on the patent website (publication date 2010-02-03, publication number CN101638732A) is used as comparative example 1.

[0049] I. Composite material samples prepared in Examples 1-5 and Comparative Example 1 (Example 1) were used as contacts, with a diameter of 4 mm and a weight of 5 ± 0.1 g. These were used as the positive and negative electrodes, respectively, for electro-erosion experiments. The test conditions were: test voltage 20 VDC, test current 20 A, purely resistive load; static contact pressure 1 N, opening and closing frequency 100 times / min, and opening distance 2 mm. After 150,000 breaking operations, the losses of the positive and negative electrodes were measured and recorded in Table 1 below.

[0050] Table 1. Record of contact loss between positive and negative electrodes

[0051]

[0052]

[0053] Table 1 above shows that the positive and negative electrode losses of the contacts in Examples 1 to 5 are significantly less than those in Comparative Example 1; and the positive and negative electrode losses of the contacts in Example 1 are the smallest. Therefore, it can be concluded that the silver-based composite material prepared by the method of the present invention has excellent arc erosion performance.

[0054] II. Composite material samples prepared in Examples 1-5 and Comparative Example 1 (Example 1) were used as contacts, with a diameter of 4 mm and a length of 2 cm; their physical properties, including density (unit: g / cm³), were tested. 3 ), resistivity (unit: uΩ·cm) and hardness (unit: HV); and record them in Table 2 below.

[0055] Table 2 Analysis of Physical Properties of Composite Materials

[0056]

[0057] From Table 2 above, it can be concluded that the density and hardness of the composite materials in Examples 1 to 5 are significantly greater than those in Comparative Example 1, and the density and hardness of the composite material in Example 1 are the highest; the resistivity of the composite materials in Examples 1 to 5 are significantly lower than those in Comparative Example 1; and the resistivity of the composite material in Example 1 is the lowest; thus, it can be concluded that the silver-based composite material prepared by the method of the present invention has high density and hardness, low resistivity, and excellent physical properties.

[0058] The above description is merely a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.

Claims

1. A method for preparing ZnO@CuO reinforced silver-based composite materials by powder metallurgy, characterized in that, Includes the following steps: S1. Using ZnO powder as raw material, ZnO@CuO powder is obtained through a combination of electrolysis and sintering. S2. After mixing the ZnO@CuO powder obtained in step S1 with Ag powder at a mass ratio of 7% to 18%, the mixture is ball-milled to obtain the composite powder. S3. Press the composite powder obtained in step S2 into a mold; sinter it in a sintering furnace to form a ZnO@CuO reinforced silver-based composite sintered blank; then densify the sintered blank, extrude it, and draw it into wire. In step S1, the specific preparation method of ZnO@CuO powder is as follows: S11. Electrolysis is carried out in an electrolyte with a copper plate as the anode and a graphite electrode as the cathode until the copper plate at the anode is completely electrolyzed and disappears in the electrolyte. S12. Add ZnO powder to the electrolyte at a ratio of 10-80 g / L and stir for 3-15 min; after centrifuging the electrolyte, wash it 3-6 times with deionized water at a volume ratio of 10:

1. S13. Dry in a drying oven at 60-140℃ for 5-20 hours, then grind and pass through a 200-900 mesh sieve to obtain Cu(OH)2 powder; S14. Sintering is carried out sequentially at 50-100℃ and held for 1-3 hours, at 350-450℃ and held for 1-4 hours, and at 750-850℃ and held for 1-2 hours to prepare ZnO@CuO powder.

2. The method for preparing ZnO@CuO reinforced silver-based composite materials by powder metallurgy according to claim 1, characterized in that, In the S11 step, the electrolyte is formed by dissolving NH4Cl in deionized water; and the current density in the electrolysis process is 0.2-0.8 A / cm2 2 .

3. The method for preparing ZnO@CuO reinforced silver-based composite materials by powder metallurgy according to claim 1, characterized in that, The ZnO powder has a particle size of 50–800 nm, a purity of ≥99.9%, and a sphericity of ≥0.9; the ZnO@CuO powder has a particle size of 60–900 nm and a sphericity of ≥0.

9.

4. The method for preparing ZnO@CuO reinforced silver-based composite materials by powder metallurgy according to claim 1, characterized in that, In step S2, the Ag powder has a particle size of 10–50 µm and a purity of ≥99.9%, and the ball milling process is carried out at a speed of 150–800 r / min for 0.5–2 h.

5. The method for preparing ZnO@CuO reinforced silver-based composite materials by powder metallurgy according to claim 1, characterized in that, In step S3, the pressure during the pressing process is 200–800 MPa; the sintering process adopts a multi-stage sintering method, and the sintering temperature is 100–900℃; the extrusion temperature is 300–850℃, and the extrusion pressure is 200–800 MPa.

Citation Information

Patent Citations

  • Method for preparing silver zinc oxide composite material

    CN101638732A

  • Preparation method of silver-base electric contact material

    CN101000828A

  • Manufacturing process for silver zinc oxide copper oxide electrical contact and electrical contact product

    CN104201019A