An N-type back-contact photovoltaic module resistant to potential induced degradation

By using high resistivity N-type silicon wafer material and SiNx/SiO2 stacked passivation layer in photovoltaic modules, combined with the improved packaging structure, the potential-induced attenuation problem of photovoltaic modules is solved, improving the photoelectric conversion efficiency and reducing costs.

CN118538832BActive Publication Date: 2024-11-08JIANGSU FUTULA NEW ENERGY GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410816663.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-11-08
Estimated Expiration
2044-06-24

AI Technical Summary

Technical Problem

During use, photovoltaic modules are prone to potential-induced attenuation effects, resulting in a decrease in output power, existing protective measures are costly and increase safety risks, and the problem cannot be solved from the source.

Method used

Using high resistivity N-type silicon wafer material, the front and back emitters are formed through synchronous diffusion, and a layered passivation layer of SiNx and SiO2 is deposited on the battery surface, simplifying the process flow, improving the component packaging structure, and adding flexible insulating components to Improve insulation performance.

Benefits of technology

It effectively reduces the potential-induced attenuation effect, improves the photoelectric conversion efficiency, enhances the components' anti-PID capability, simplifies the process flow and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118538832B_ABST
    Figure CN118538832B_ABST
Patent Text Reader

Abstract

The present invention provides an N-type back-contact photovoltaic module with resistance to potential induced degradation, which comprises a solar cell string encapsulated in the middle of the module, a glass substrate located on the outside, an EVA layer that seals the solar cell string and the glass substrate, a back plate located on the rear side, and a frame encapsulated at the edge of the module; the front surface and back emitters are formed by synchronous diffusion on the frame and the module edge silicon substrate, and boron diffusion is used to form a borosilicate glass layer and a SiO2 layer as a passivation layer, thereby eliminating the oxidation and passivation steps of the existing process and simplifying the process flow; a high-resistivity silicon wafer material is selected, and a SiNx film and SiO2 are deposited on the front surface of the battery to form a laminated passivation layer, which can effectively play an anti-PID effect; the prepared battery has relatively large open-circuit voltage and short-circuit current, thereby ensuring a high photoelectric conversion efficiency of the back-contact solar cell; the packaging structure of the module, including the module frame, is improved, the insulation performance of the packaging structure is significantly improved, and the ability to resist the PID effect is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solar photovoltaic power generation, and in particular to an N-type back-contact photovoltaic component resistant to potential induced degradation. Background Art

[0002] The photovoltaic power generation system is a power generation system that directly converts solar energy into electrical energy. It can take into account both economic development and ecological protection while generating clean electricity. It is currently widely used in a variety of scenarios. It is one of the important clean energy sources to replace traditional fossil energy and has broad development prospects.

[0003] Photovoltaic power generation system is to connect photovoltaic modules through cables to form a module array, and then directly provide the electricity generated by photovoltaic modules to the power load or connect it to the power grid through branch lines, busbars, DC / AC conversion. Since crystalline silicon solar cells and modules are the most mature and low-cost, and with the continuous improvement of technology and processes, the photoelectric conversion efficiency of crystalline silicon modules is getting higher and higher, so in the current photovoltaic power generation system, crystalline silicon modules are still the main type of modules used; and as the difference between the power generation cost of crystalline silicon modules and the cost per kilowatt-hour of thermal power generation continues to narrow, it can be foreseen that they will still occupy the vast majority of the market share at present and for a considerable period of time in the future.

[0004] Photovoltaic cells and photovoltaic modules based on photovoltaic cells are the main components of photovoltaic power generation systems. The power generation efficiency of photovoltaic power generation systems is mainly determined by the photoelectric conversion efficiency of photovoltaic cells, and is also affected by photovoltaic modules. For photovoltaic cells, increasing the effective light-receiving area of ​​the cell is always one of the important factors to improve the photoelectric conversion efficiency of photovoltaic cells. Since the electrode structure of back-contact solar cells is on the backlight side of the cell, there is no electrode blocking the light-facing side. Therefore, it has higher short-circuit current and photoelectric conversion efficiency, and is one of the important development directions of high-efficiency solar cells.

[0005] Potential induced degradation (PID) is the power loss of photovoltaic modules due to leakage current under high voltage conditions. During the use of photovoltaic modules, the high potential of the modules to the ground will cause leakage, which will cause the performance of the photovoltaic modules to decline. This is mainly because the modules are under high voltage for a long time, which makes leakage current between the cells, glass and packaging material layers. A large amount of charge accumulates on the surface of the cells, causing the passivation effect of the solar cell to deteriorate. The minority carriers recombine seriously on the surface of the silicon wafer, resulting in a decrease in its open circuit voltage, short circuit current and fill factor, and a significant decrease in output power. This is the so-called potential induced degradation effect. According to usage surveys, the maximum attenuation of photovoltaic modules during use can exceed 30%.

[0006] The potential induced degradation (PID) effect was first discovered in N-type back-contact cells, that is, when an N-type solar cell generates a positive potential to the ground, its output power will continue to decline, which shows that the influence of the potential on the base material of the solar cell causes the solar cell efficiency to decline. The base material of the N-type solar cell is an N-type silicon wafer, and a layer of silicon nitride film and silicon oxide film are deposited on the surface of the silicon wafer, which is mainly to achieve the effect of anti-reflection passivation. When the N-type solar cell / cell module generates a positive potential to the ground, due to the grounding of the metal frame of the module, a high voltage is generated between the solar cell and the metal frame, which will form a leakage current from the solar cell through the frame to the ground, and induce negative charges in the silicon nitride film. When the density of negative charges gradually increases and eventually exceeds the density of the original positive charge of the film, it will cause the energy band to bend upward, attracting photogenerated minority carriers to the surface, exacerbating the surface recombination of minority carriers. Due to the large ratio of the surface area (effective light receiving area) to the volume of the back-contact solar cell, the surface recombination will be more serious, which will significantly reduce the minority carrier lifetime and the open circuit voltage of the battery, thereby affecting the conversion efficiency of the battery.

[0007] Therefore, how to reduce or avoid the potential induced degradation effect of photovoltaic cells and photovoltaic modules is an issue that battery manufacturers, module manufacturers and photovoltaic system builders need to pay attention to. The current measures to prevent potential induced degradation are mainly focused on components and systems, such as reverse bias recovery: using an additional voltage device to apply a positive voltage to the negative electrode of the component at night to perform reverse bias recovery to repair PID; or grounding the negative electrode of the component through a high resistance to keep the negative electrode at a low potential to suppress PID; or using an additional device to raise the negative electrode potential or neutral point potential to achieve the effect of negative electrode grounding, thereby suppressing PID. These measures can solve some problems of potential induced degradation, but each has its own defects. The main one is that additional equipment needs to be added to the system. One is that the cost of photovoltaic power generation systems is high, and adding electrical equipment will also increase safety risks; in addition, these measures cannot solve the problem of potential induced degradation of photovoltaic modules from the source. Summary of the invention

[0008] The purpose of the present invention is to address the problem of potential induced degradation in existing photovoltaic modules and to propose an N-type back-contact photovoltaic module that is resistant to potential induced degradation. Multiple PID protections are performed at the cell level and the module level, so that the photovoltaic module still has a high photoelectric conversion efficiency when used for a long time.

[0009] To achieve the above object, the present invention adopts the following technical solutions:

[0010] An N-type back-contact photovoltaic module with resistance to potential induced degradation comprises a solar cell string encapsulated in the middle of the module, a glass substrate located outside the solar cell string, an EVA layer hermetically encapsulating the solar cell string and the glass substrate, a back plate located at the rear side, and a frame encapsulating the edge of the module composed of the solar cell string, the glass substrate, the EVA layer and the back plate; a flexible insulating component is arranged between the frame and the module edge; the preparation process of the N-type back-contact photovoltaic module is as follows:

[0011] S1. Battery preparation, using N-type silicon wafer as the base material, the resistivity of the silicon wafer base material is 15~20Ω·cm, and the preparation process includes the following steps:

[0012] S11: Cleaning and texturing of the damaged layer on the surface of the silicon wafer: The cut silicon wafer is cleaned in ozone water, and then the surface is corroded and texturized with an alkaline solution with a concentration of about 20% to form a velvet structure on the surface of the silicon wafer;

[0013] S12, Phosphorus diffusion: The pressure in the diffusion furnace is set at 10~25Kpa, and the reaction temperature is first controlled at about 795℃. A mixed gas of N2 and O2 carrying POCl3 is pre-deposited on the surface of the silicon wafer to form a phosphorus silicon glass layer, and the deposition reaction time is controlled at about 15min; then the temperature is raised to about 945℃, and the reaction time does not exceed 15min. At high temperature, the phosphorus dopant is diffused into the silicon wafer to form a back field layer on the surface of the silicon wafer;

[0014] S13, depositing a silicon nitride mask and forming a p+ doping window by laser ablation: after phosphorus diffusion, use tubular PECVD to deposit SiNx to form a mask layer, and then use high-energy laser ablation to form a specific pattern on the back of the battery according to the designed pattern, and etch the SiNx film formed in the step to form a p+ doping window;

[0015] S14, secondary cleaning, removing the phosphorus dopant on the front surface of the silicon wafer and the n+ doping at the groove on the back surface, to obtain a silicon wafer with a clean surface;

[0016] S15, using furnace tube thermal diffusion to diffuse boron tribromide on both sides of the silicon wafer after texturing, forming a floating emitter on the front surface and an emitter in the grooved area on the back; the diffusion process is to first deposit a layer of borosilicate glass on the surface of the silicon wafer at 890-910°C, and then perform high-temperature oxidation at 980°C-1000°C in an oxygen atmosphere, and produce a SiO2 layer between the borosilicate glass layer formed in the diffusion process and the doped silicon interface in a high-temperature oxygen atmosphere; then, through the HF acid solution corrosion process, the borosilicate glass layer formed on the surface of the silicon wafer during the boron diffusion process is thinned to make the surface smooth;

[0017] S16, double-sided deposition of silicon nitride film: through tubular PECVD to stimulate SiH4 and NH3 to react to form SiNx film, forming SiO2 / SiNx stacked passivation anti-reflection film on the surface of the cell;

[0018] S17: printing electrodes and sintering, first printing fine grid lines, then printing insulating paste to form an isolation layer, and finally printing main grid line paste, the main grid line and the fine grid line have multiple connection points for current collection; then a solar cell is formed through a sintering process;

[0019] S18: Perform quality inspection and efficiency test on the finished cells, and classify and manage cells with the same conversion efficiency as cells for preparing photovoltaic modules;

[0020] S2, component preparation, which includes the following steps:

[0021] S21. Frame preparation:

[0022] Select appropriate aluminum alloy materials and form the frame profile according to the product design structure; then clean the frame profile to remove surface grease, dirt and oxides, etc.;

[0023] Soak the cleaned frame in the pretreatment solution to remove residual impurities and surface oxides;

[0024] The pre-treated frame is used as an anode and placed in an electrolytic cell, and powered by a DC power supply to form an oxide film on the surface of the aluminum alloy;

[0025] The anodized frame is placed in a high temperature environment to close the pores in the oxide film and form a dense aluminum oxide insulating layer on the surface of the frame;

[0026] S22, arranging the battery cells according to specifications to form a battery string;

[0027] S23, laminating the backplane, the EVA layer, the battery cell and the glass substrate and performing hot pressing;

[0028] S24, installing the hot-pressed module on a frame, and setting a flexible insulating component between the frame and the edge of the module.

[0029] Preferably, the above-mentioned preparation process further includes the step of installing a photovoltaic junction box on the back side of the component after the frame is installed.

[0030] More preferably, in the above preparation process, it also includes connecting a grounding component to the component frame.

[0031] More preferably, in the step S11, a step of cleaning the silicon wafer with ozone water is further included after the textured structure is formed.

[0032] More preferably, in the above step S15, the thickness of SiO2 grown in a high temperature oxygen atmosphere is controlled to be 20±3 nm, and the thickness of the borosilicate glass layer is controlled to be 4-8 nm.

[0033] More preferably, in step S16, the thickness of the formed SiNx and SiO2 stacked passivation layer is controlled to be 50±5 nm.

[0034] The N-type back-contact photovoltaic module with resistance to potential induced degradation of the present invention, when preparing the battery, synchronously diffuses on the N-type silicon substrate to form the front surface and the back emitter, and uses boron diffusion to form a borosilicate glass layer and a SiO2 layer as a passivation layer, eliminating the oxidation and passivation steps of the existing process and simplifying the process flow; selects high-resistivity silicon wafer materials, and deposits SiNx film and SiO2 on the front surface of the battery to form a laminated passivation layer, which can effectively play an anti-PID effect; the prepared battery has a relatively large open-circuit voltage and short-circuit current, ensuring a high photoelectric conversion efficiency of the back-contact solar cell; the packaging structure of the component, including the component frame, is improved, the insulation performance of the packaging structure is significantly improved, and the ability to resist the PID effect is further improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0036] Figure 1 Shown is a schematic diagram of a half-section structure of an N-type back-contact photovoltaic module resistant to potential induced degradation of the present invention;

[0037] Figure 2 Shown is a schematic diagram of the production process flow of the cell of the N-type back-contact photovoltaic module resistant to potential induced degradation of the present invention. DETAILED DESCRIPTION

[0038] In order to provide a further understanding of the purpose, structure, features, and functions of the present invention, the following detailed description is given in conjunction with the embodiments.

[0039] In the description of the present invention, it should be noted that the terms "center", "up", "down", "left", "right", "vertical", "horizontal", "inside", "outside", etc. indicate directions or positional relationships based on the directions or positional relationships shown in the accompanying drawings. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction. Therefore, they cannot be understood as limitations on the present invention.

[0040] Reference Figure 1 As shown, according to the purpose of the present invention, an N-type back contact photovoltaic module with resistance to potential induced degradation of the present invention comprises a solar cell string 10 encapsulated in the middle of the module, a glass substrate 12 located outside the solar cell string 10, an EVA layer 14 that seals the solar cell string 10 and the glass substrate 12, a back plate 16 located at the rear side, and a frame 20 that encapsulates the edge of the module composed of the solar cell string 10, the glass substrate 12, the EVA layer 14 and the back plate 16; a flexible insulating component 22 is arranged between the frame 20 and the edge of the module; the preparation process of the N-type back contact photovoltaic module is as follows:

[0041] S1. Preparation of battery: N-type Cz silicon wafer is used as substrate material. Since the resistivity of silicon wafer will have a certain influence on the PID effect of N-type solar cell, the greater the resistivity, the better the anti-PID effect. Therefore, the resistivity of silicon wafer substrate material of the present invention is 15~20Ω·cm, combined with Figure 2 As shown, the battery preparation process includes the following steps:

[0042] S11: Cleaning and texturing of the damaged layer on the surface of silicon wafers: Since a damaged layer will be formed on the surface of the silicon wafer during the cutting process, there are a large number of defects and recombination centers, which have a great impact on the conversion efficiency and yield of the battery. Therefore, it is necessary to clean the surface of the silicon wafer to remove the damaged layer first; specifically, the silicon wafer is first thoroughly cleaned in ozone water, and then the surface is corroded and texturized by an alkaline solution with a concentration of about 20%, such as KOH or NaOH, to form a pyramid structure on the surface of the silicon wafer, namely the so-called velvet structure to increase the light-receiving surface of the silicon wafer; in a preferred embodiment, after the velvet structure is formed, it can be cleaned once with ozone water. Since ozone water is obtained by passing ozone gas into high-purity water, a silicon wafer with a clean surface can be obtained by cleaning with ozone water, which is convenient for subsequent processes;

[0043] S12: Phosphorus diffusion, doping on the surface of the silicon wafer to form a back field (n+ layer). Specifically, the reaction temperature is first controlled at about 795°C, and a mixed gas of N2 and O2 carrying POCl3 is pre-deposited on the surface of the silicon wafer to form a phosphorus silicon glass layer, and the deposition reaction time is controlled at about 15 minutes; then the temperature is raised to about 945°C, and the reaction time does not exceed 15 minutes. At high temperature, the phosphorus dopant is diffused into the silicon wafer to form a back field layer on the surface of the silicon wafer;

[0044] S13: Deposit a silicon nitride mask and form a p+ doping window by laser ablation. Since the emitter and back field of the back-contact solar cell are integrated on the back of the cell, two different dopings need to be performed on the same side of the cell. Therefore, after phosphorus diffusion, SiNx is deposited by tubular PECVD to form a mask layer. Using SiNx as a mask can better block the diffusion of the inversion layer; then high-energy laser ablation is used to form a specific pattern on the back of the cell according to the designed pattern, and the SiNx film formed in the step is etched to form a p+ doping window;

[0045] S14: Secondary cleaning. The cleaning process removes the phosphorus dopant on the front surface of the silicon wafer and the n+ doping at the groove on the back surface, making the surface of the silicon wafer clean;

[0046] S15: Use furnace tube thermal diffusion to diffuse boron tribromide on both sides of the silicon wafer after texturing, forming a floating emitter on the front surface and an emitter in the grooved area on the back; then use HF acid solution etching process to thin and smooth the silicon glass layer formed on the surface of the silicon wafer during the boron diffusion process;

[0047] S16: Double-sided deposition of silicon nitride film, i.e., forming SiNx film by exciting SiH4 and NH3 to react through tubular PECVD, and forming SiO2 / SiNx stacked passivation anti-reflection film on the surface of the cell;

[0048] S17: Printing electrodes and sintering. Since the electrodes (i.e., grid lines) of the back-contact solar cells are all arranged on the back of the cells, when printing the electrodes, the fine grid lines are printed first, then the insulating paste is printed to form an isolation layer, and finally the main grid line paste is printed. The main grid line and the fine grid line have multiple connection points for current collection; then the solar cell is formed through a sintering process;

[0049] S18: Perform quality inspection and efficiency test on the finished cells, and classify and manage cells with the same conversion efficiency as cells for preparing photovoltaic modules;

[0050] S2, component preparation, which includes the following steps:

[0051] S21. Frame preparation:

[0052] Select appropriate aluminum alloy materials and form the frame profile according to the product design structure; then clean the frame profile to remove surface grease, dirt and oxides. Mechanical cleaning, chemical cleaning or electrochemical cleaning can be used;

[0053] Soaking the cleaned frame in a pretreatment solution to remove residual impurities and surface oxides; the pretreatment solution may include an alkaline solution, an acidic solution or a composite solution;

[0054] The pre-treated frame is used as an anode and placed in an electrolytic cell, and powered by a DC power supply to form an oxide film on the surface of the aluminum alloy;

[0055] The anodized frame is placed in a high temperature environment to close the pores in the oxide film and form a dense aluminum oxide insulating layer on the surface of the frame;

[0056] S22, arranging the battery cells according to specifications to form a battery string;

[0057] S23, laminating the backplane, the EVA layer, the battery cell and the glass substrate and performing hot pressing;

[0058] S24, installing the hot-pressed module on a frame, and setting a flexible insulating component between the frame and the edge of the module.

[0059] The above-mentioned preparation process also includes the step of installing a photovoltaic junction box on the back of the component after the frame is installed.

[0060] The above-mentioned preparation process also includes connecting a grounding component 24 on the component frame.

[0061] The main reason for the power decline of photovoltaic modules due to the PID effect is that the induced charge causes the energy band of the semiconductor material to bend, the surface load of the carrier increases, and the battery efficiency decreases. The higher the resistivity of the silicon wafer, the weaker the PID effect will be. For N-type solar cells, the characteristics of the passivation film on the surface of the cell will have an important impact on the PID effect. The higher the inherent charge density of the passivation film, the denser the film, the stronger the charge capacity, and the smaller the impact on the PID effect.

[0062] In the above step S12, in the traditional silicon wafer processing process of solar cells, in order to form a good ohmic contact between the silicon surface of the emitter region and the metal grid line, and reduce the contact resistance and series resistance loss, the emitter region needs to be heavily doped, but heavy doping is prone to produce large surface recombination and a decrease in short-wave spectrum response, resulting in voltage and current losses. For silicon wafers used for back-contact solar cells, since the metal grid lines are all arranged on the back surface of the silicon wafer and there are no grid lines on the front surface, the preparation process of the present application, for silicon wafers used for back-contact solar cells, adopts a light doping process to reduce the recombination of minority carriers when P diffusion doping is performed on the surface of the silicon wafer. In a preferred embodiment, the pressure in the diffusion furnace is set at 10~25KPa, which can effectively ensure the uniformity and stability of the atmosphere in the furnace and improve the uniformity of diffusion on the surface of the silicon wafer; in addition, the silicon wafer preparation process of the present application adopts a low temperature in the initial stage of deposition, and controls the deposition time to about 15 minutes; a higher temperature and a shorter time are used in the advancement stage to increase the temperature difference between the two times, which can form a better concentration gradient distribution on the surface of the silicon wafer, obtain an ideal doping curve, and obtain a low-concentration emitter junction. The square resistance of the silicon wafer after diffusion can reach more than 180Ω / □; and the overall diffusion time of the silicon wafer can be shortened, thereby improving the production efficiency of the process.

[0063] In the boron tribromide diffusion process of step S15, according to the existing boron tribromide diffusion process, boron tribromide vapor is first mixed with oxygen to form B2O3 and bromine vapor, and then the B2O3 deposited on the surface of the silicon wafer reacts with the underlying silicon substrate layer to form boron atoms and SiO2. At the conventional deposition temperature (about 950°C), the vapor pressure of B2O3 is relatively low, and the liquid B2O3 condenses on the surface of the silicon wafer and inside the diffusion furnace. During the reaction process at this stage, a glass layer rich in B2O3, i.e., a borosilicate glass layer, is formed on the surface of the boron-doped silicon wafer. During the boron diffusion process, if the reaction atmosphere and temperature are not uniform, the thickness of the borosilicate glass layer inside the solar cell will be uneven. If the SiNx layer deposited directly on the borosilicate glass layer is combined with the borosilicate glass layer as a laminated passivation and anti-reflection film, it will lead to differences in properties between different regions of the cell, reducing the short-circuit current of the cell. Therefore, the current process requires first removing the BSG layer by pickling, first growing a passivation layer on the p+ doped surface, and then depositing the SiNx passivation layer. The process is relatively complicated, and the quality of the generated surface passivation layer cannot be guaranteed.

[0064] Therefore, in step S15 of the present invention, the boron diffusion process is to first deposit a layer of borosilicate glass on the surface of the silicon wafer at a low temperature (890-910°C), and then perform high temperature (980°C-1000°C) oxidation in an oxygen atmosphere. Under this process condition, the borosilicate glass layer is in a low viscosity state, oxygen and silicon react at the interface between the borosilicate glass layer and the doped silicon, and SiO2 is produced between the borosilicate glass layer and the doped silicon interface. When the concentration of B2O3 in the borosilicate glass layer is lower than a certain concentration, the growth of SiO2 stops, and SiO2 with a certain thickness is formed. Moreover, since the solubility of boron in SiO2 is higher than that of Si, this oxidation process also reduces the surface concentration of boron, forms boron doping in silicon dioxide, and avoids the formation of a surface boron-rich layer. In this oxidation process, the surface borosilicate glass layer will be relatively loose, which will affect the formation of the subsequent passivation layer. Therefore, after the boron is diffused, it is necessary to use HF acid solution to etch away the loose borosilicate glass layer of a certain thickness on the surface. In addition, according to the experimental results, when the thickness of the formed SiOx:B is small, its structure is not dense enough, and there are pores and induced defects. Only when it reaches a certain thickness can the external environment be effectively prevented from affecting the SiOx:B / Si interface. Compared with the thickness of SiO2 formed by the traditional wet chemical process, which generally does not exceed 10nm, the thickness of SiO2 grown in the high-temperature oxygen atmosphere of the present application can reach up to 30nm. Considering the overall performance and manufacturing process of the solar cell, the thickness of SiO2 grown in the high-temperature oxygen atmosphere of the present invention is preferably controlled at about 22nm (20±3nm), and the thickness of the borosilicate glass layer is controlled at 4-8nm. Therefore, compared with the existing diffusion process, the process steps of the present invention are simpler, the cost is low, and the passivation effect is excellent.

[0065] In step S16, the preparation process of the present invention deposits SiNx film and SiO2 on the front surface of the battery to form a laminated passivation layer, and the high-quality Si-SiO2 passivation layer formed in the diffusion process of step S16 can effectively reduce the silicon interface state density. The H atoms introduced when depositing the SiNx passivation anti-reflection film diffuse into the silicon wafer during the sintering process, which can saturate the silicon dangling bonds and passivate the silicon wafer body defects. In addition, the formed SiO2 / SiNx laminated passivation film has a higher fixed positive charge concentration than the single-layer SiO2 film, thereby playing a better field passivation role and can effectively play an anti-PID role. In a preferred embodiment, the thickness of the formed SiNx and SiO2 laminated passivation layer is controlled at 50±5nm.

[0066] In addition, according to research findings, the packaging materials of photovoltaic modules and the gaps between different materials are the main channels for leakage. The insulation properties of the packaging materials and the matching between different materials will affect the PID effect. After years of industrial development, the gaps between the laminated layers inside the component can basically be eliminated through the current mature preparation process. Therefore, in the present invention, on the one hand, the component frame is surface treated to form a dense oxide layer on the surface of the frame. Due to the large specific surface area, small dielectric constant and high dielectric strength of aluminum oxide, it can effectively prevent the flow of current; in addition, aluminum oxide also has excellent corrosion resistance, which can prevent the frame from being affected by rainy days, foggy days, seawater salt atmosphere and other environmental factors when used for a long time, causing material corrosion, so that water vapor enters the component to affect the internal sealing performance and thus have a more negative impact on the PID effect; in the present invention, further, when the frame is installed, a flexible insulating component, such as insulating rubber, is arranged between the edges of the laminated modules inside the frame component. On the one hand, the insulating performance of the component packaging material is further guaranteed, and the edge of the laminated module inside the component and the frame can be packaged more tightly, significantly reducing the gap inside the frame, avoiding water vapor from entering the frame and the component, and improving the anti-PID effect.

[0067] The N-type back-contact photovoltaic module with resistance to potential induced degradation of the present invention, when preparing the battery, synchronously diffuses on the N-type silicon substrate to form the front surface and the back emitter, and uses boron diffusion to form a borosilicate glass layer and a SiO2 layer as a passivation layer, eliminating the oxidation and passivation steps of the existing process and simplifying the process flow; selects high-resistivity silicon wafer materials, and deposits SiNx film and SiO2 on the front surface of the battery to form a laminated passivation layer, which can effectively play an anti-PID effect; the prepared battery has a relatively large open-circuit voltage and short-circuit current, ensuring a high photoelectric conversion efficiency of the back-contact solar cell; the packaging structure of the component, including the component frame, is improved, the insulation performance of the packaging structure is significantly improved, and the ability to resist the PID effect is further improved.

[0068] The present invention has been described by the above-mentioned relevant embodiments, however, the above-mentioned embodiments are only examples for implementing the present invention. It must be pointed out that the disclosed embodiments do not limit the scope of the present invention. On the contrary, changes and modifications made without departing from the spirit and scope of the present invention are all within the scope of patent protection of the present invention.

Claims

1. An N-type back-contact photovoltaic module resistant to potential induced degradation, characterized in that: The photovoltaic module comprises a solar cell string encapsulated in the middle of the module, a glass substrate located outside the solar cell string, an EVA layer hermetically encapsulating the solar cell string and the glass substrate, a backplane located at the rear side, and a frame encapsulating the edge of the module composed of the solar cell string, the glass substrate, the EVA layer and the backplane; a flexible insulating component is arranged between the frame and the edge of the module; the preparation process of the N-type back contact photovoltaic module is as follows: S1. Battery preparation, using N-type silicon wafer as the base material, the resistivity of the silicon wafer base material is 15~20Ω·cm, and the preparation process includes the following steps: S11: Cleaning and texturing of the damaged layer on the surface of the silicon wafer: The cut silicon wafer is cleaned in ozone water, and then the surface is corroded and texturized by an alkaline solution with a concentration of 20% to form a velvet structure on the surface of the silicon wafer; S12, Phosphorus diffusion: The pressure in the diffusion furnace is set at 10~25Kpa, the reaction temperature is first controlled at 795℃, and a mixed gas of N2 and O2 carrying POCl3 is pre-deposited on the surface of the silicon wafer to form a phosphorus silicon glass layer, and the deposition reaction time is controlled at 15min; then the temperature is raised to 945℃, and the reaction time does not exceed 15min, and the phosphorus dopant is diffused into the silicon wafer at high temperature to form a back field layer on the surface of the silicon wafer; S13, depositing a silicon nitride mask and forming a p+ doping window by laser ablation: after phosphorus diffusion, use tubular PECVD to deposit SiNx to form a mask layer, then use high-energy laser ablation to form a pattern on the back of the battery according to the designed pattern, and etch the formed SiNx mask layer to form a p+ doping window; S14, secondary cleaning, removing the phosphorus dopant on the front surface of the silicon wafer and the n+ doping at the groove on the back surface, to obtain a silicon wafer with a clean surface; S15, using furnace tube thermal diffusion to diffuse boron tribromide on both sides of the silicon wafer after texturing, forming a floating emitter on the front surface and an emitter in the grooved area on the back; the diffusion process is to first deposit a layer of borosilicate glass on the surface of the silicon wafer at 890-910°C, and then perform high-temperature oxidation at 980°C-1000°C in an oxygen atmosphere, and produce a SiO2 layer between the borosilicate glass layer formed in the diffusion process and the doped silicon interface in a high-temperature oxygen atmosphere; then, through the HF acid solution corrosion process, the borosilicate glass layer formed on the surface of the silicon wafer during the boron diffusion process is thinned to make the surface smooth; S16, double-sided deposition of silicon nitride film: through tubular PECVD, SiH4 and NH3 are stimulated to react to form SiNx film, and SiO2 / SiNx stacked passivation anti-reflection film is formed on the surface of the cell; S17: printing electrodes and sintering, first printing fine grid lines, then printing insulating paste to form an isolation layer, and finally printing main grid line paste, the main grid line and the fine grid line have multiple connection points for current collection; then a solar cell is formed through a sintering process; S18: Perform quality inspection and efficiency test on the finished cells, and classify and manage cells with the same conversion efficiency as cells for preparing photovoltaic modules; S2, component preparation, which includes the following steps: S21. Frame preparation: Select appropriate aluminum alloy materials and form the frame profile according to the product design structure; then clean the frame profile to remove surface grease, dirt and oxides; Soak the cleaned frame in the pretreatment solution to remove residual impurities and surface oxides; The pre-treated frame is used as an anode and placed in an electrolytic cell, and powered by a DC power supply to form an oxide film on the surface of the aluminum alloy; The anodized frame is placed in a high temperature environment to close the pores in the oxide film and form a dense aluminum oxide insulating layer on the surface of the frame; S22, arranging the battery cells according to specifications to form a battery string; S23, laminating the backplane, the EVA layer, the battery cell and the glass substrate and performing hot pressing; S24, installing the hot-pressed module on a frame, and setting a flexible insulating component between the frame and the edge of the module.

2. The N-type back-contact photovoltaic module with resistance to potential induced degradation according to claim 1, characterized in that: The step of installing and connecting a photovoltaic junction box on the back of the component after the frame is installed is also included.

3. An N-type back-contact photovoltaic module resistant to potential induced degradation as claimed in claim 1 or 2, characterized in that: Also included is connecting a grounding component to the component frame.

4. The N-type back-contact photovoltaic module with resistance to potential induced degradation according to claim 3, characterized in that: In the step S11, it also includes a step of cleaning the silicon wafer with ozone water after the textured structure is formed.

5. The N-type back-contact photovoltaic module with resistance to potential induced degradation according to claim 1, characterized in that: In step S15, the thickness of SiO2 grown in a high temperature oxygen atmosphere is controlled to be 20±3 nm, and the thickness of the borosilicate glass layer is controlled to be 4-8 nm.

6. The N-type back-contact photovoltaic module with resistance to potential induced degradation according to claim 5, characterized in that: In step S16, the thickness of the formed SiNx and SiO2 stacked passivation layer is controlled to be 50±5 nm.