A hard carbon microsphere negative electrode material and its preparation method and application

By embedding carbon dots and doping boron elements in hard carbon microspheres, the problems of poor thermal stability of starch and structural melting and foaming are solved, and the electrochemical performance and capacity performance of hard carbon microsphere anode materials are improved.

CN118538913BActive Publication Date: 2024-10-18GUOKE TANMEI NEW MATERIALS (HUZHOU) CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411002066.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-10-18
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

In the existing technology, problems such as poor thermal stability of starch and structural melting and foaming lead to poor electrochemical performance of hard carbon microsphere anode materials in batteries and low carbon yield, which affects the transmission and diffusion of ions and electrons.

Method used

The carbon dots are uniformly embedded in the disordered carbon structure and doped with boron element to form a stable carbon skeleton, reduce the activation energy of the conversion of amorphous carbon to crystalline carbon, enhance the interconnection of carbon dots, and improve the ion adsorption and diffusion rate.

Benefits of technology

It improves the Coulombic efficiency and cycle stability of the hard carbon microsphere anode material, while taking into account its capacity performance, forming a continuous conductive path in the disordered matrix, and solving the thermal stability and structural problems of starch.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118538913B_ABST
    Figure CN118538913B_ABST
Patent Text Reader

Abstract

The present invention provides a hard carbon microsphere negative electrode material and a preparation method and application thereof, belonging to the technical field of battery materials, wherein the hard carbon microsphere negative electrode material comprises a disordered carbon matrix and carbon dots embedded in the disordered carbon matrix; the hard carbon microsphere negative electrode material is doped with boron. The present invention uniformly embeds carbon dots in the disordered carbon structure and simultaneously performs boron doping, which not only forms a stable carbon skeleton, solves the problems of poor thermal stability of starch, structural melting and foaming, but also effectively reduces the activation energy of the transformation of amorphous carbon to crystalline carbon, enhances the interconnection of carbon dots with fewer defects and higher degree of graphitization in the matrix, forms a continuous conductive path in the disordered matrix, and the doping of boron effectively improves the ion adsorption and diffusion rate, which helps the hard carbon microsphere negative electrode material to maintain high coulomb efficiency and cycle stability while taking into account its capacity performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of battery materials, and specifically relates to a hard carbon microsphere negative electrode material and a preparation method and application thereof. Background Art

[0002] At present, the development of new energy has become a hot topic. One of the core technologies of new energy lies in the breakthrough of battery technology. However, the lithium-ion batteries with rising costs and increasingly scarce resources can no longer meet the growing demand in the energy field. Therefore, it is imperative to develop sodium-ion batteries with low costs, abundant resources and high safety. Hard carbon, as the only negative electrode material for sodium-ion batteries that can be commercialized, has received widespread attention.

[0003] Hard carbon is mainly produced by high-molecular polymers, coal or petroleum asphalt, biomass and other raw materials through high-temperature carbonization. Among them, biomass has become a high-quality precursor for the preparation of advanced carbon materials due to its advantages such as wide sources, low cost, high carbon content and diversified structure. However, due to the complexity of the original biomass components, during the carbonization process, different components decompose through their own specific pathways and kinetics, and affect each other, resulting in the inability of directly carbonizing biomass to give hard carbon a controllable structure and ideal properties. Starch, as a natural high-molecular polymer with high purity and spherical structure, is widely used in the synthesis of hard carbon materials due to its low cost, green and renewable, high carbon content and other advantages. In the prior art, patent CN103647082A discloses a method for preparing hard carbon microspheres for lithium-ion secondary batteries, that is, starch is used as a raw material, and hard carbon microspheres are prepared through stabilization and carbonization processes under reduced pressure conditions. Although the above method effectively suppresses the foaming and agglomeration problems of starch particles during the carbonization process and maintains the good sphericity and dispersibility of starch-based hard carbon, the method requires a long-term heating and stabilization treatment of starch at a relatively low temperature, resulting in a long preparation time for hard carbon microspheres. Patent CN106006603A discloses a method for preparing a negative electrode material for lithium-ion battery hard carbon microspheres, using a fluidized bed reactor as a stabilization or carbonization treatment device for starch raw materials, and heating and stabilizing or carbonizing natural starch in a fluidized state, which greatly improves the preparation efficiency of hard carbon microspheres. However, in this method, starch has a typical polysaccharide structure with poor thermal stability. When directly carbonized at high temperature, the structure will melt and foam and produce a large number of volatile small molecules. These volatile small molecules may pass through the bed in a large bubble state, resulting in poor contact between the flue gas and the starch raw material, uneven heat exchange, and low carbonization efficiency. Patent CN111204731A discloses a method for preparing hard carbon microspheres, firstly, starch is mixed with oligophenolic resin and then cured to obtain a starch-based hard carbon precursor with a surface-coated polymer, and then hard carbon microspheres are obtained by pyrolysis. When used as the negative electrode of a lithium-ion battery, the first discharge specific capacity is higher than 300mAh / g. However, due to the poor thermal stability of starch, a large amount of volatile matter is produced during the preparation of carbon materials, making the final carbon yield generally low. More importantly, the escape of small molecules during the pyrolysis process leads to the formation of a large number of defects and holes in the carbon structure. These defects and holes will cause the arrangement of discontinuous and dislocated graphite microdomains inside the hard carbon material, affecting the transmission and diffusion of ions and electrons, and ultimately affecting the sodium storage performance of the material.

[0004] In summary, how to solve the problems of poor thermal stability of starch and structural melting and foaming in order to improve the electrochemical performance of hard carbon microsphere negative electrode materials in batteries is a hot research direction at present. Summary of the invention

[0005] In view of the deficiencies of the prior art, the purpose of the present invention is to provide a hard carbon microsphere negative electrode material and its preparation method and application. The present invention uniformly embeds carbon dots in a disordered carbon structure and simultaneously performs boron doping, which not only forms a stable carbon skeleton, solves the problems of poor thermal stability of starch, structural melting and foaming, but also effectively reduces the activation energy of the transformation of amorphous carbon to crystalline carbon, enhances the interconnection of carbon dots with fewer defects and higher degree of graphitization in the matrix, forms a continuous conductive path in the disordered matrix, and boron doping effectively improves the ion adsorption and diffusion rate, which helps the hard carbon microsphere negative electrode material to maintain high coulomb efficiency and cycle stability while taking into account its capacity performance.

[0006] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0007] In a first aspect, the present invention provides a hard carbon microsphere negative electrode material, the hard carbon microsphere negative electrode material comprising a disordered carbon matrix and carbon dots embedded in the disordered carbon matrix;

[0008] The hard carbon microsphere negative electrode material is doped with boron.

[0009] The present invention evenly embeds carbon dots in a disordered carbon structure and simultaneously performs boron doping, which not only forms a stable carbon skeleton and solves the problems of poor thermal stability of starch and structural melting and foaming, but also effectively reduces the activation energy of the transformation of amorphous carbon to crystalline carbon, enhances the interconnection of carbon dots with fewer defects and a higher degree of graphitization in the matrix, forms a continuous conductive path in the disordered matrix, and boron doping effectively improves the ion adsorption and diffusion rate, which helps the hard carbon microsphere negative electrode material to maintain high coulomb efficiency and cycle stability while taking into account its capacity performance.

[0010] It should be noted that disordered carbon matrix refers to the carbon atoms not having a periodic stacking structure, which is composed of sp 2 and sp 3 Amorphous carbon materials are formed by random bonding of hybrid carbon atoms.

[0011] It should be noted that carbon dots, also known as carbon quantum dots or carbon nanodots, are a type of zero-dimensional carbon nanomaterials with significant fluorescence properties. They are composed of ultrafine, dispersed, quasi-spherical carbon nanoparticles with a size of less than 10nm.

[0012] As a preferred technical solution of the present invention, the doping amount of the boron element is 1-15wt%, for example, it can be 1wt%, 3wt%, 5wt%, 7wt%, 9wt%, 11wt%, 13wt% or 15wt%.

[0013] Boron, as an electron acceptor, is more inclined to act as a potential-philic site or Lewis acid due to its unique structure that is missing one electron compared to carbon atoms, causing the Fermi level to shift negatively relative to the Dirac energy. Therefore, doping boron in the hard carbon microsphere negative electrode material can act as an electron acceptor to passivate unstable electron pairs, and by adjusting the electron density of boron-doped carbon, the electrode electrochemical interface can be stabilized. In the present invention, if the doping amount of boron element is too small, the active hydroxyl groups in the starch molecules cannot be fully consumed, resulting in the inability to effectively fix the carbon skeleton; if the doping amount of boron element is too much, the boron source cannot be dispersed at the molecular level in the starch, and in the subsequent carbonization process, B2O3 crystals tend to aggregate and grow to form a larger pore structure.

[0014] Preferably, the interlayer spacing of the hard carbon microsphere negative electrode material is 0.37-0.4 nm, for example, 0.37 nm, 0.38 nm, 0.39 nm or 0.4 nm.

[0015] Preferably, the diameter of the hard carbon microsphere negative electrode material is 5-30 μm, for example, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm or 30 μm.

[0016] Preferably, the specific surface area of ​​the hard carbon microsphere negative electrode material is 1-20 m 2 / g, for example, 1m 2 / g, 5m 2 / g, 10m 2 / g, 15m 2 / g or 20m 2 / g, etc.

[0017] Preferably, the carbon yield of the hard carbon microsphere negative electrode material is 28-50wt%, for example, it can be 28wt%, 30wt%, 35wt%, 40wt%, 45wt% or 50wt%.

[0018] Preferably, the hard carbon microsphere negative electrode material is a porous structure, and the pore size of the hard carbon microsphere negative electrode material is 0.4-1.5 nm, for example, it can be 0.4 nm, 0.6 nm, 0.8 nm, 1 nm, 1.2 nm or 1.5 nm.

[0019] The hard carbon microsphere negative electrode material provided by the invention has ultra-low specific surface area, abundant closed pores, large interlayer spacing and high degree of graphitization.

[0020] In a second aspect, the present invention provides a method for preparing the hard carbon microsphere negative electrode material as described in the first aspect, the preparation method comprising the following steps:

[0021] (1) Pre-treating the starch raw material, and then adding a boron source and mixing to obtain a mixture;

[0022] (2) drying the mixture to obtain composite precursor microspheres, and then performing a reduction reaction to obtain composite microsphere intermediates;

[0023] (3) Carbonizing the composite microsphere intermediate to obtain the hard carbon microsphere negative electrode material.

[0024] In the preparation method provided by the present invention, the boron source reacts with the free active hydroxyl groups in the starch molecules to undergo a dehydration reaction, thereby uniformly grafting the small molecular boron source into the starch molecules. Combined with the reduction reaction, the oxygen content of the cross-linked starch is effectively regulated while maintaining the structural stability of the cross-linked starch. This strategy promotes the rearrangement and fixation of carbon during the carbonization process and the uniform embedding of carbon dots in the disordered carbon matrix. At the same time, the introduction of covalent grafted bonds in the starch molecules greatly enhances the disorder of the carbonized product and expands its interlayer spacing and the number of closed pores.

[0025] The preparation method provided by the invention has simple equipment, easy-to-control operation process, stable product performance, and can realize large-scale production.

[0026] As a preferred technical solution of the present invention, the specific steps of the pre-treatment in step (1) include:

[0027] The starch raw material is dispersed in water to obtain starch milk, and then alkali solution is added to adjust the pH value to obtain alkaline emulsion.

[0028] In the present invention, the purpose of preparing the alkaline emulsion is to promote the dispersion effect of the boron source in the starch and achieve a uniform reaction between the two.

[0029] Preferably, the starch raw material includes at least one of wheat starch, sorghum starch, corn starch, mung bean starch, potato starch, sweet potato starch, water chestnut starch, lotus root starch, water chestnut starch, arrowroot starch, cassava starch and crystal starch.

[0030] Preferably, the alkali solution includes at least one of sodium hydroxide solution, potassium hydroxide solution and ammonia water.

[0031] Preferably, the pH value is 9-11, for example, 9, 10 or 11.

[0032] As a preferred technical solution of the present invention, the boron source in step (1) includes boric acid and / or terephthalic acid.

[0033] Preferably, the mass ratio of the alkaline emulsion and the boron source is (1-10):(10-1), wherein the selection range of the alkaline emulsion "1-10" can be, for example, 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10, and the selection range of the boron source "1-10" can be, for example, 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10, etc.

[0034] Preferably, the mixing method in step (1) includes ultrasonic dispersion.

[0035] Preferably, the ultrasonic dispersion time is 10-120 min, for example, it can be 10 min, 20 min, 40 min, 60 min, 80 min, 100 min or 120 min, etc., and the ultrasonic power of the ultrasonic dispersion is 100-800 W, for example, it can be 100 W, 200 W, 300 W, 400 W, 500 W, 600 W, 700 W or 800 W, etc.

[0036] As a preferred technical solution of the present invention, the specific steps of drying in step (2) include: sucking the mixture into a spray dryer using a peristaltic pump and atomizing it into droplets.

[0037] Preferably, the drying temperature in step (2) is 150-250°C, for example, 150°C, 180°C, 200°C, 220°C or 250°C.

[0038] Preferably, the feeding frequency of the peristaltic pump is 30-100 mL / min, for example, 30 mL / min, 30 mL / min, 50 mL / min, 70 mL / min or 90 mL / min.

[0039] Preferably, the reduction reaction in step (2) is carried out in a working atmosphere, and the gas in the working atmosphere includes reducing gas and inert gas.

[0040] Preferably, the reducing gas includes at least one of hydrogen, methane, ammonia, ethylene and acetylene.

[0041] Preferably, the inert gas comprises argon.

[0042] Preferably, the volume flow ratio of the reducing gas to the inert gas is (1-5):5, for example, it can be 1:5, 2:5, 3:5, 4:5 or 5:5, etc.

[0043] Preferably, the temperature of the reduction reaction in step (2) is 200-600°C, for example, 200°C, 300°C, 400°C, 500°C or 600°C, and the time of the reduction reaction is 0.5-6h, for example, 0.5h, 1h, 2h, 3h, 4h, 5h or 6h.

[0044] In the present invention, if the temperature of the reduction reaction is too low, the excess oxygen in the precursor cannot be effectively removed, which is not conducive to the closure of open pores during high-temperature carbonization, and is not conducive to the directional arrangement of the derived hard carbon layer, forming a local ordered microcrystalline structure and reducing the defect concentration; if the temperature of the reduction reaction is too high, excessive deoxidation will introduce new defects such as vacancies, hindering the improvement of order.

[0045] Preferably, the heating rate of the reduction reaction in step (2) is 1-5°C / min, for example, 1°C / min, 2°C / min, 3°C / min, 4°C / min or 5°C / min.

[0046] Preferably, after the reduction reaction in step (2) is completed, cooling, washing, filtering and freeze-drying steps are further performed.

[0047] Preferably, the detergent used in the washing comprises alkali solution, organic solvent and water.

[0048] Preferably, the concentration of the alkali solution is 0.5-3 mol / L, for example, it can be 0.5 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L or 3 mol / L.

[0049] Preferably, the alkali solution includes any one of potassium hydroxide solution, sodium hydroxide solution, lithium hydroxide solution or ammonia water, or a combination of at least two of them.

[0050] Preferably, the organic solvent includes any one of acetone, anhydrous ethanol or isopropanol, or a combination of at least two of them.

[0051] Preferably, the washing time is 1-10 h, for example, it can be 1 h, 2 h, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h or 10 h.

[0052] Preferably, the freeze-drying temperature is minus 20°C to minus 50°C, for example, minus 20°C, minus 30°C, minus 40°C or minus 50°C.

[0053] Preferably, the freeze-drying time is 4-12 h, for example, 4 h, 6 h, 8 h, 10 h or 12 h.

[0054] As a preferred technical solution of the present invention, the carbonization treatment in step (3) is carried out in an inert atmosphere.

[0055] It should be noted that the present invention does not limit the type of gas in the inert atmosphere, and it may be, for example, argon or nitrogen.

[0056] Preferably, the temperature of the carbonization treatment in step (3) is 900-1600°C, for example, it can be 900°C, 1000°C, 1100°C, 1200°C, 1300°C, 1400°C, 1500°C or 1600°C, and the time of the carbonization treatment is 0.5-8h, for example, it can be 0.5h, 1h, 2h, 3h, 4h, 5h, 6h, 7h or 8h, etc.

[0057] In the present invention, if the temperature of the carbonization treatment is too low, the open pores cannot be effectively closed, and sufficient closed pores cannot be formed, which is not conducive to the improvement of the platform capacity; if the carbonization temperature is too high, although it is conducive to the formation of new closed pores, the migration, accumulation and growth of the graphite layer will cause the closed pores to shrink and the spacing to decrease, hindering the diffusion of sodium ions into the closed pores, thereby reducing the platform capacity.

[0058] Preferably, the heating rate of the carbonization treatment in step (3) is 1-10°C / min, for example, it can be 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min or 10°C / min, etc.

[0059] Preferably, after the carbonization treatment, washing and drying steps are also performed, and the washing includes acid washing, anhydrous ethanol washing and water washing performed in sequence. The washing time is 1-10h, for example, it can be 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h or 10h, etc., and the washing temperature is 40-95°C, for example, it can be 40°C, 50°C, 60°C, 70°C, 80°C or 90°C, etc.

[0060] Preferably, in the acid washing, the concentration of the acid is 0.5-3 mol / L, for example, it can be 0.5 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L or 3 mol / L, etc., and the acid includes any one of hydrochloric acid, sulfuric acid, nitric acid or acetic acid, or a combination of at least two of them.

[0061] As a preferred technical solution of the present invention, the preparation method comprises the following steps:

[0062] (1) Dispersing the starch raw material in deionized water, stirring evenly to obtain starch emulsion, and then adding alkali solution to adjust the pH value to 9-11 to obtain alkaline emulsion;

[0063] (2) placing the alkaline emulsion and the boron source in a cell crusher at a mass ratio of (1-10):(10-1), and performing ultrasonic dispersion to obtain a mixed solution;

[0064] The ultrasonic dispersion time is 10-120 min, and the ultrasonic power of the ultrasonic dispersion is 100-800 W;

[0065] (3) The mixed liquid is sucked into a spray dryer through a peristaltic pump with a feeding frequency of 30-100 mL / min, atomized into droplets, and then heat exchanged with hot air to obtain composite precursor microspheres;

[0066] (4) placing the composite precursor microsphere in a tube furnace under working atmosphere conditions, and heating the temperature to 200-600°C at a heating rate of 1-5°C / min, and performing a reduction reaction at a constant temperature for 0.5-6h. After the reaction is completed, cooling to room temperature to obtain a cooling product, and then washing the cooling product with an alkali solution with a concentration of 0.5-3mol / L, an organic solvent and water for 1-10h, filtering and freeze-drying to obtain a composite microsphere intermediate;

[0067] The gas in the working atmosphere includes a reducing gas and an inert gas at a volume flow ratio of (1-5):5, the reducing gas includes at least one of hydrogen, methane, ammonia, ethylene and acetylene, and the inert gas includes argon;

[0068] (5) placing the composite microsphere intermediate in a carbonization furnace under an inert atmosphere, heating the temperature to 900-1600°C at a heating rate of 1-10°C / min, and carbonizing the composite microsphere intermediate at a constant temperature for 0.5-8h. After the carbonization treatment, washing the composite microsphere intermediate with an acid solution with a concentration of 0.5-3mol / L, anhydrous ethanol and water at 40-95°C for 1-10h in sequence, and drying to obtain the hard carbon microsphere negative electrode material.

[0069] In a third aspect, the present invention provides a sodium ion battery, wherein the negative electrode of the sodium ion battery comprises the hard carbon microsphere negative electrode material as described in the first aspect.

[0070] In a fourth aspect, the present invention provides a use of the hard carbon microsphere negative electrode material as described in the first aspect in a lithium ion battery and / or a potassium ion battery.

[0071] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0072] Compared with the prior art, the present invention has the following beneficial effects:

[0073] (1) The present invention uniformly embeds carbon dots in a disordered carbon structure and simultaneously performs boron doping, which not only forms a stable carbon skeleton and solves the problems of poor thermal stability of starch and structural melting and foaming, but also effectively reduces the activation energy of the transformation of amorphous carbon to crystalline carbon, enhances the interconnection of carbon dots with fewer defects and higher degree of graphitization in the matrix, forms a continuous conductive path in the disordered matrix, and boron doping effectively improves the ion adsorption and diffusion rate, which helps the hard carbon microsphere negative electrode material to maintain high Coulomb efficiency and cycle stability while taking into account its capacity performance.

[0074] (2) In the preparation method provided by the present invention, the boron source reacts with the free active hydroxyl groups in the starch molecules to undergo a dehydration reaction, and the small molecular boron source is uniformly grafted into the starch molecules. Combined with the reduction reaction, the oxygen content of the cross-linked starch is effectively regulated while maintaining the structural stability of the cross-linked starch. This strategy promotes the rearrangement and fixation of carbon during the carbonization process and the uniform embedding of carbon dots in the disordered carbon matrix. At the same time, the introduction of covalent grafting bonds in the precursor greatly enhances the disorder of the carbonized product and expands its interlayer spacing and the number of closed pores.

[0075] (3) The preparation method provided by the present invention has simple equipment, easy-to-control operation process, stable product performance, and can be mass-produced. BRIEF DESCRIPTION OF THE DRAWINGS

[0076] Figure 1 This is a TEM image of the hard carbon microsphere negative electrode material prepared in Example 3 of the present invention.

[0077] Figure 2 This is a rate performance diagram of the hard carbon microsphere negative electrode material prepared in Example 3 of the present invention.

[0078] Figure 3 This is the charge and discharge curve of the hard carbon microsphere negative electrode material prepared in Example 3 of the present invention. DETAILED DESCRIPTION

[0079] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0080] It should be noted that the room temperature below refers to 25°C.

[0081] Example 1

[0082] This embodiment provides a hard carbon microsphere negative electrode material, the hard carbon microsphere negative electrode material comprising a disordered carbon matrix and carbon dots embedded in the disordered carbon matrix;

[0083] The hard carbon microsphere negative electrode material is doped with boron, and the doping amount of the boron element is 15wt%;

[0084] The graphite interlayer spacing of the hard carbon microsphere negative electrode material is 0.384nm; the diameter of the hard carbon microsphere negative electrode material is 5μm; the specific surface area of ​​the hard carbon microsphere negative electrode material is 10m 2 / g; the carbon yield of the hard carbon microsphere negative electrode material is 50wt%;

[0085] The hard carbon microsphere negative electrode material has a porous structure, and the pore size of the hard carbon microsphere negative electrode material is 0.4 nm.

[0086] This embodiment also provides a method for preparing the hard carbon microsphere negative electrode material, the preparation method comprising the following steps:

[0087] (1) Dispersing wheat starch in deionized water, stirring evenly to obtain starch emulsion, and then adding 0.5 mL of sodium hydroxide solution to adjust the pH value to 9 to obtain an alkaline emulsion;

[0088] (2) placing the alkaline emulsion and terephthaloyl boric acid in a cell crusher at a mass ratio of 1:10, and ultrasonically dispersing them to obtain a uniformly dispersed mixed solution;

[0089] The ultrasonic dispersion time was 120 min, and the ultrasonic power was 100 W.

[0090] (3) The mixed liquid is sucked into a spray dryer through a peristaltic pump with a feeding frequency of 100 mL / min, atomized into droplets, and then heat exchanged with hot air at 150° C. to obtain composite precursor microspheres;

[0091] (4) placing the composite precursor microsphere in a tube furnace under working atmosphere conditions, and heating the temperature to 200°C at a heating rate of 1°C / min, and performing a reduction reaction at a constant temperature for 2 hours. After the reaction is completed, cooling to room temperature to obtain a cooling product, and then washing the cooling product with a 1.5 mol / L sodium hydroxide solution, acetone and deionized water for 6 hours, filtering and freeze-drying at -30°C for 8 hours to obtain a composite microsphere intermediate;

[0092] The gas in the working atmosphere includes hydrogen and argon with a volume flow ratio of 1:5;

[0093] (5) Placing the composite microsphere intermediate in a carbonization furnace under an argon atmosphere, heating the temperature to 900°C at a heating rate of 5°C / min, and carbonizing the composite microsphere intermediate at a constant temperature for 8 hours. After the carbonization, washing the composite microsphere intermediate with 0.5 mol / L hydrochloric acid, anhydrous ethanol and deionized water at 70°C for 5 hours in sequence, and drying to obtain the hard carbon microsphere negative electrode material.

[0094] Example 2

[0095] This embodiment provides a hard carbon microsphere negative electrode material, the hard carbon microsphere negative electrode material comprising a disordered carbon matrix and carbon dots embedded in the disordered carbon matrix;

[0096] The hard carbon microsphere negative electrode material is doped with boron, and the doping amount of the boron element is 1wt%;

[0097] The graphite interlayer spacing of the hard carbon microsphere negative electrode material is 0.384nm; the diameter of the hard carbon microsphere negative electrode material is 25μm; the specific surface area of ​​the hard carbon microsphere negative electrode material is 1.5m 2 / g; the carbon yield of the hard carbon microsphere negative electrode material is 28wt%;

[0098] The hard carbon microsphere negative electrode material has a porous structure, and the pore size of the hard carbon microsphere negative electrode material is 1 nm.

[0099] This embodiment also provides a method for preparing the hard carbon microsphere negative electrode material, the preparation method comprising the following steps:

[0100] (1) Dispersing potato starch in deionized water, stirring evenly to obtain starch emulsion, and then adding 10 mL of sodium hydroxide solution to adjust the pH value to 11 to obtain an alkaline emulsion;

[0101] (2) placing the alkaline emulsion and terephthaloyl boric acid in a cell crusher at a mass ratio of 10:1, and dispersing them by ultrasonication to obtain a uniformly dispersed mixed solution;

[0102] The ultrasonic dispersion time was 10 min, and the ultrasonic power was 800 W.

[0103] (3) The mixed liquid is sucked into a spray dryer through a peristaltic pump with a feeding frequency of 30 mL / min, atomized into droplets, and then heat exchanged with hot air at 180° C. to obtain composite precursor microspheres;

[0104] (4) placing the composite precursor microsphere in a tube furnace under working atmosphere conditions, and heating the temperature to 200°C at a heating rate of 5°C / min, and performing a reduction reaction at a constant temperature for 6 hours. After the reaction is completed, cooling to room temperature to obtain a cooling product, and then washing the cooling product with a 1.5 mol / L sodium hydroxide solution, acetone and deionized water for 6 hours, filtering and freeze-drying at -30°C for 8 hours to obtain a composite microsphere intermediate;

[0105] The gas in the working atmosphere includes hydrogen and argon with a volume flow ratio of 5:5;

[0106] (5) Placing the composite microsphere intermediate in a carbonization furnace under an argon atmosphere, heating the temperature to 1600°C at a heating rate of 10°C / min, and carbonizing the composite microsphere intermediate at a constant temperature for 0.5 h. After the carbonization, washing the composite microsphere intermediate with 3 mol / L hydrochloric acid, anhydrous ethanol and deionized water at 95°C for 10 h in sequence, and drying the composite microsphere intermediate to obtain the hard carbon microsphere negative electrode material.

[0107] Example 3

[0108] This embodiment provides a hard carbon microsphere negative electrode material, the hard carbon microsphere negative electrode material comprising a disordered carbon matrix and carbon dots embedded in the disordered carbon matrix;

[0109] The hard carbon microsphere negative electrode material is doped with boron, and the doping amount of the boron element is 8wt%;

[0110] The graphite interlayer spacing of the hard carbon microsphere negative electrode material is 0.382nm; the diameter of the hard carbon microsphere negative electrode material is 10μm; the specific surface area of ​​the hard carbon microsphere negative electrode material is 2.3m 2 / g; the carbon yield of the hard carbon microsphere negative electrode material is 40wt%;

[0111] The hard carbon microsphere negative electrode material has a porous structure, and the pore size of the hard carbon microsphere negative electrode material is 0.75 nm.

[0112] This embodiment also provides a method for preparing the hard carbon microsphere negative electrode material, the preparation method comprising the following steps:

[0113] (1) Dispersing corn starch in deionized water, stirring evenly to obtain starch emulsion, and then adding 2 mL of sodium hydroxide solution to adjust the pH value to 10 to obtain an alkaline emulsion;

[0114] (2) placing the alkaline emulsion and terephthaloyl boric acid in a cell crusher at a mass ratio of 5:5, and performing ultrasonic dispersion to obtain a uniformly dispersed mixed solution;

[0115] The ultrasonic dispersion time was 30 min, and the ultrasonic power was 500 W.

[0116] (3) The mixed liquid is sucked into a spray dryer through a peristaltic pump with a feeding frequency of 80 mL / min, atomized into droplets, and then heat exchanged with hot air at 220° C. to obtain composite precursor microspheres;

[0117] (4) placing the composite precursor microsphere in a tube furnace under working atmosphere conditions, and heating the temperature to 300°C at a heating rate of 3°C / min, and performing a reduction reaction at a constant temperature for 4 hours. After the reaction is completed, cooling to room temperature to obtain a cooling product, and then washing the cooling product with a 1.5 mol / L sodium hydroxide solution, acetone and deionized water for 6 hours, filtering and freeze-drying at -30°C for 8 hours to obtain a composite microsphere intermediate;

[0118] The gas in the working atmosphere includes hydrogen and argon with a volume flow ratio of 2:5;

[0119] (5) Placing the composite microsphere intermediate in a carbonization furnace under an argon atmosphere, heating the temperature to 1300°C at a heating rate of 5°C / min, and carbonizing the composite microsphere intermediate at a constant temperature for 4 hours. After the carbonization, washing the composite microsphere intermediate with 1 mol / L hydrochloric acid, anhydrous ethanol and deionized water at 40°C for 10 hours in sequence, and drying the composite microsphere intermediate to obtain the hard carbon microsphere negative electrode material.

[0120] Figure 1 The TEM image of the hard carbon microsphere negative electrode material prepared in this example is shown. It can be seen from the image that the prepared hard carbon microspheres exhibit typical hard carbon structural characteristics.

[0121] Figure 2 The rate performance diagram of the hard carbon microsphere negative electrode material prepared in this embodiment is shown. It can be seen from the figure that in the carbon ball structure prepared in this embodiment, the carbon dots are uniformly embedded in the disordered carbon matrix to form a continuous conductive path in the disordered matrix. At the same time, the in-situ uniform doping of boron induces the transformation of the material's electronic structure to an electron-deficient system, thereby effectively improving the adsorption and diffusion rate of sodium ions, so that it exhibits excellent rate performance.

[0122] Figure 3 The charge-discharge curve of the hard carbon microsphere negative electrode material prepared in this embodiment is shown. It can be seen from the figure that the charge-discharge curve of the hard carbon microsphere negative electrode prepared in this embodiment includes a high potential slope region (0.1-2V) and a low potential platform region (0-0.1V). The small molecule terephthaloyl diboric acid is uniformly grafted into the starch molecules, combined with low-temperature reduction, which greatly enhances the disorder of the carbonization product, expands its interlayer spacing and the number of closed pores, thereby improving the sodium storage capacity of the hard carbon microspheres.

[0123] Example 4

[0124] This embodiment provides a hard carbon microsphere negative electrode material, the hard carbon microsphere negative electrode material comprising a disordered carbon matrix and carbon dots embedded in the disordered carbon matrix;

[0125] The hard carbon microsphere negative electrode material is doped with boron, and the doping amount of the boron element is 5wt%;

[0126] The graphite interlayer spacing of the hard carbon microsphere negative electrode material is 0.387nm; the diameter of the hard carbon microsphere negative electrode material is 18μm; the specific surface area of ​​the hard carbon microsphere negative electrode material is 7.8m 2 / g; the carbon yield of the hard carbon microsphere negative electrode material is 35wt%;

[0127] The hard carbon microsphere negative electrode material has a porous structure, and the pore size of the hard carbon microsphere negative electrode material is 0.9 nm.

[0128] This embodiment also provides a method for preparing the hard carbon microsphere negative electrode material, the preparation method comprising the following steps:

[0129] (1) Dispersing corn starch in deionized water, stirring evenly to obtain starch emulsion, and then adding 1.5 mL of sodium hydroxide solution to adjust the pH value to 9 to obtain an alkaline emulsion;

[0130] (2) placing the alkaline emulsion and terephthaloyl boric acid in a cell crusher at a mass ratio of 5:5, and performing ultrasonic dispersion to obtain a uniformly dispersed mixed solution;

[0131] The ultrasonic dispersion time was 30 min, and the ultrasonic power was 500 W.

[0132] (3) The mixed liquid is sucked into a spray dryer through a peristaltic pump with a feeding frequency of 60 mL / min, atomized into droplets, and then heat exchanged with hot air at 200° C. to obtain composite precursor microspheres;

[0133] (4) placing the composite precursor microsphere in a tube furnace under working atmosphere conditions, and heating the temperature to 300°C at a heating rate of 2°C / min, and performing a reduction reaction at a constant temperature for 2 hours. After the reaction is completed, cooling to room temperature to obtain a cooling product, and then washing the cooling product with a 1.5 mol / L sodium hydroxide solution, acetone and deionized water for 6 hours, filtering and freeze-drying at -30°C for 8 hours to obtain a composite microsphere intermediate;

[0134] The gas in the working atmosphere includes hydrogen and argon with a volume flow ratio of 1:5;

[0135] (5) Placing the composite microsphere intermediate in a carbonization furnace under an argon atmosphere, heating the temperature to 1100°C at a heating rate of 3°C / min, and carbonizing the composite microsphere intermediate at a constant temperature for 5 hours. After the carbonization, washing the composite microsphere intermediate with 1 mol / L hydrochloric acid, anhydrous ethanol and deionized water at 95°C for 1 hour in sequence, and drying the composite microsphere intermediate to obtain the hard carbon microsphere negative electrode material.

[0136] Example 5

[0137] This embodiment provides a hard carbon microsphere negative electrode material, the hard carbon microsphere negative electrode material comprising a disordered carbon matrix and carbon dots embedded in the disordered carbon matrix;

[0138] The hard carbon microsphere negative electrode material is doped with boron, and the doping amount of the boron element is 7wt%;

[0139] The graphite interlayer spacing of the hard carbon microsphere negative electrode material is 0.378nm; the diameter of the hard carbon microsphere negative electrode material is 15μm; the specific surface area of ​​the hard carbon microsphere negative electrode material is 1.8m 2 / g; the carbon yield of the hard carbon microsphere negative electrode material is 45wt%;

[0140] The hard carbon microsphere negative electrode material has a porous structure, and the pore size of the hard carbon microsphere negative electrode material is 0.8 nm.

[0141] This embodiment also provides a method for preparing the hard carbon microsphere negative electrode material, the preparation method comprising the following steps:

[0142] (1) Dispersing corn starch in deionized water, stirring evenly to obtain starch emulsion, and then adding 1.5 mL of sodium hydroxide solution to adjust the pH value to 10 to obtain an alkaline emulsion;

[0143] (2) placing the alkaline emulsion and terephthaloyl boric acid in a mass ratio of 3:7 in a cell crusher, and performing ultrasonic dispersion to obtain a uniformly dispersed mixed solution;

[0144] The ultrasonic dispersion time was 30 min, and the ultrasonic power was 500 W.

[0145] (3) The mixed liquid is sucked into a spray dryer through a peristaltic pump with a feeding frequency of 100 mL / min, atomized into droplets, and then heat exchanged with hot air at 250° C. to obtain composite precursor microspheres;

[0146] (4) placing the composite precursor microsphere in a tube furnace under working atmosphere conditions, and heating the temperature to 350°C at a heating rate of 1°C / min, and performing a reduction reaction at a constant temperature for 3 hours. After the reaction is completed, cooling to room temperature to obtain a cooling product, and then washing the cooling product with a 1.5 mol / L sodium hydroxide solution, acetone and deionized water for 6 hours, filtering and freeze-drying at -30°C for 8 hours to obtain a composite microsphere intermediate;

[0147] The gas in the working atmosphere includes hydrogen and argon with a volume flow ratio of 1:5;

[0148] (5) Placing the composite microsphere intermediate in a carbonization furnace under an argon atmosphere, heating the temperature to 1300°C at a heating rate of 5°C / min, and carbonizing the composite microsphere intermediate at a constant temperature for 5 hours. After the carbonization, washing the composite microsphere intermediate with 1 mol / L hydrochloric acid, anhydrous ethanol and deionized water at 95°C for 1 hour in sequence, and drying the composite microsphere intermediate to obtain the hard carbon microsphere negative electrode material.

[0149] Example 6

[0150] The difference between this embodiment and embodiment 1 is that in step (1), no sodium hydroxide solution is added to adjust the pH value, but starch milk and terephthalic acid are directly mixed.

[0151] The rest of the preparation methods and parameters were the same as those in Example 1.

[0152] Example 7

[0153] The difference between this embodiment and embodiment 1 is that the mass ratio of the alkaline emulsion and terephthaloyl diboric acid in step (2) is adjusted so that the doping amount of the boron element is 0.5 wt %.

[0154] The rest of the preparation methods and parameters were the same as those in Example 1.

[0155] Example 8

[0156] The difference between this embodiment and embodiment 1 is that the mass ratio of the alkaline emulsion and terephthaloylboric acid in step (2) is adjusted so that the doping amount of the boron element is 20 wt %.

[0157] The rest of the preparation methods and parameters were the same as those in Example 1.

[0158] Example 9

[0159] The difference between this embodiment and embodiment 1 is that spray drying is not performed in step (3).

[0160] The rest of the preparation methods and parameters were the same as those in Example 1.

[0161] Example 10

[0162] The difference between this embodiment and embodiment 1 is that the temperature of the reduction reaction in step (4) is 150°C.

[0163] The rest of the preparation methods and parameters were the same as those in Example 1.

[0164] Embodiment 11

[0165] The difference between this embodiment and embodiment 1 is that the temperature of the reduction reaction in step (4) is 650°C.

[0166] The rest of the preparation methods and parameters were the same as those in Example 1.

[0167] Example 12

[0168] The difference between this embodiment and embodiment 1 is that the temperature of the carbonization treatment in step (5) is 800°C.

[0169] The rest of the preparation methods and parameters were the same as those in Example 1.

[0170] Example 13

[0171] The difference between this embodiment and embodiment 1 is that the temperature of the carbonization treatment in step (5) is 1700°C.

[0172] The rest of the preparation methods and parameters were the same as those in Example 1.

[0173] Comparative Example 1

[0174] The difference between this comparative example and Example 1 is that there is no embedding of carbon dots and boron doping in the disordered carbon matrix, that is, starch is dispersed in deionized water, stirred evenly to form starch emulsion, and directly spray-dried to prepare starch microspheres.

[0175] The rest of the preparation methods and parameters were the same as those in Example 1.

[0176] Performance Testing

[0177] The hard carbon microsphere negative electrode material prepared in the above embodiment and comparative example is used to prepare a CR2032 button battery, and the specific steps include:

[0178] The hard carbon microsphere negative electrode material, carbon black and polyvinylidene fluoride were mixed in a mass ratio of 80:10:10 to form a slurry, which was then evenly scraped onto the current collector aluminum foil. After drying, the electrode pieces were cut. The battery was assembled in a glove box with Ar atmosphere, using metallic sodium as the counter electrode and 1M NaClO4 (the solvent included ethylene carbonate and diethyl carbonate in a volume ratio of 1:1) solution as the electrolyte to form a CR2032 button battery.

[0179] The above CR2032 button battery was charged and discharged under the following conditions:

[0180] The current density was 20 mA / g and the voltage was 0.001–2 V.

[0181] The test results are shown in Table 1.

[0182] Table 1

[0183]

[0184] analyze:

[0185] As can be seen from the above table, the present invention uniformly embeds carbon dots in the disordered carbon structure and simultaneously performs boron doping, which not only forms a stable carbon skeleton and solves the problems of poor thermal stability of starch and structural melting and foaming, but also effectively reduces the activation energy of the transformation of amorphous carbon to crystalline carbon, enhances the interconnection of carbon dots with fewer defects and higher degree of graphitization in the matrix, forms a continuous conductive path in the disordered matrix, and boron doping effectively improves the ion adsorption and diffusion rate, which helps the hard carbon microsphere negative electrode material to maintain high Coulomb efficiency and cycle stability while taking into account its capacity performance.

[0186] It can be seen from Examples 1 and 6 that if the alkaline emulsion is not prepared, the degree of reaction between the boron source and starch will be low, the dispersion effect of the boron source will be poor, and the internal pore structure of the starch-based hard carbon cannot be effectively regulated.

[0187] It can be seen from Example 1 and Examples 7-8 that if the doping amount of the boron element is too low, the active hydroxyl groups in the starch molecules cannot be fully consumed, resulting in the inability to effectively fix the carbon skeleton and a low carbon yield; if the doping amount of the boron element is too much, the boron source cannot be dispersed at the molecular level in the starch, and in the subsequent carbonization process, B2O3 crystals are prone to aggregate and grow to form a larger pore structure, which will consume a large amount of sodium ions, increase the irreversible capacity, and reduce the initial coulombic efficiency.

[0188] It can be seen from Examples 1 and 9 that if spray drying is not performed in step (3), the obtained sample will form irregular particle morphology, which is not conducive to the controllable preparation of regular spherical particles with narrow particle size distribution.

[0189] It can be seen from Example 1 and Examples 10-11 that if the temperature of the reduction reaction is too low, the excess oxygen in the precursor cannot be effectively removed, which is not conducive to the closure of open pores during high-temperature carbonization, and is not conducive to the directional arrangement of the derived hard carbon layer, forming a local ordered microcrystalline structure, reducing the defect concentration, and resulting in a lower initial efficiency; if the temperature of the reduction reaction is too high, excessive deoxidation will introduce new defects such as vacancies, hindering the improvement of order, which is also not conducive to the improvement of its initial efficiency.

[0190] It can be seen from Example 1 and Examples 12-13 that if the temperature of the carbonization treatment is too low, the open pores cannot be effectively closed, and sufficient closed pores cannot be formed, which is not conducive to the improvement of the platform capacity; if the carbonization temperature is too high, although it is conducive to the formation of new closed pores, the migration, accumulation and growth of the graphite layer will cause the closed pores to shrink and the spacing to decrease, hindering the diffusion of sodium ions into the closed pores, thereby reducing the platform capacity.

[0191] It can be seen from Example 1 and Comparative Example 1 that if there is no embedding of carbon dots in the disordered carbon matrix, it will cause problems such as structural melting and foaming of starch during direct heat treatment, thereby reducing its carbon yield; at the same time, a continuous conductive path cannot be formed in the disordered matrix, which is not conducive to the hard carbon microsphere negative electrode material maintaining high Coulomb efficiency and cycle stability while taking into account its capacity performance.

[0192] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a hard carbon microsphere negative electrode material, characterized in that: The preparation method comprises the following steps: (1) Pre-treating the starch raw material, and then adding a boron source and mixing to obtain a mixture; (2) drying the mixture to obtain composite precursor microspheres, and then performing a reduction reaction to obtain composite microsphere intermediates; (3) carbonizing the composite microsphere intermediate to obtain the hard carbon microsphere negative electrode material; The hard carbon microsphere negative electrode material comprises a disordered carbon matrix and carbon dots embedded in the disordered carbon matrix; The hard carbon microsphere negative electrode material is doped with boron; The doping amount of the boron element is 1-15wt%; The interlayer spacing of the hard carbon microsphere negative electrode material is 0.37-0.4nm; The diameter of the hard carbon microsphere negative electrode material is 5-30 μm; The specific surface area of ​​the hard carbon microsphere negative electrode material is 1-20 m 2 / g; The carbon yield of the hard carbon microsphere negative electrode material is 28-50wt%; The hard carbon microsphere negative electrode material has a porous structure, and the pore size of the hard carbon microsphere negative electrode material is 0.4-1.5 nm.

2. The preparation method according to claim 1, characterized in that: The specific steps of the pre-treatment in step (1) include: The starch raw material is dispersed in water to obtain starch emulsion, and then an alkali solution is added to adjust the pH value to obtain an alkaline emulsion; The starch raw material includes at least one of wheat starch, sorghum starch, corn starch, mung bean starch, potato starch, sweet potato starch, water chestnut starch, lotus root starch, water chestnut starch, arrowroot starch, cassava starch and crystal flour; The alkali solution includes at least one of sodium hydroxide solution, potassium hydroxide solution and ammonia water; The pH value is 9-11.

3. The preparation method according to claim 2, characterized in that: The boron source in step (1) includes boric acid and / or terephthalic acid; The mass ratio of the alkaline emulsion to the boron source is (1-10):(10-1); The mixing method in step (1) includes ultrasonic dispersion; The ultrasonic dispersion time is 10-120 min, and the ultrasonic dispersion power is 100-800 W.

4. The preparation method according to claim 1, characterized in that: The specific steps of drying in step (2) include: sucking the mixture into a spray dryer using a peristaltic pump and atomizing it into droplets; The drying temperature in step (2) is 150-250°C; The reduction reaction in step (2) is carried out in a working atmosphere, wherein the gas in the working atmosphere includes a reducing gas and an inert gas; The reducing gas comprises at least one of hydrogen, methane, ammonia, ethylene and acetylene; The inert gas includes argon; The volume flow ratio of the reducing gas to the inert gas is (1-5):5; The temperature of the reduction reaction in step (2) is 200-600°C, and the time of the reduction reaction is 0.5-6h; The heating rate of the reduction reaction in step (2) is 1-5°C / min.

5. The preparation method according to claim 1, characterized in that: The carbonization treatment in step (3) is carried out in an inert atmosphere; The temperature of the carbonization treatment in step (3) is 900-1600°C, and the time of the carbonization treatment is 0.5-8h; The heating rate of the carbonization treatment in step (3) is 1-10°C / min.

6. The preparation method according to claim 1, characterized in that: The preparation method comprises the following steps: (1) Dispersing the starch raw material in deionized water, stirring evenly to obtain starch emulsion, and then adding alkali solution to adjust the pH value to 9-11 to obtain alkaline emulsion; (2) placing the alkaline emulsion and the boron source in a cell crusher at a mass ratio of (1-10):(10-1), and performing ultrasonic dispersion to obtain a mixed solution; The ultrasonic dispersion time is 10-120 min, and the ultrasonic power of the ultrasonic dispersion is 100-800 W; (3) The mixed liquid is sucked into a spray dryer through a peristaltic pump with a feeding frequency of 30-100 mL / min, atomized into droplets, and then heat exchanged with hot air to obtain composite precursor microspheres; (4) placing the composite precursor microsphere in a tube furnace under working atmosphere conditions, and heating the temperature to 200-600°C at a heating rate of 1-5°C / min, and performing a reduction reaction at a constant temperature for 0.5-6h. After the reaction is completed, cooling to room temperature to obtain a cooling product, and then washing the cooling product with an alkali solution with a concentration of 0.5-3mol / L, an organic solvent and water for 1-10h, filtering and freeze-drying to obtain a composite microsphere intermediate; The gas in the working atmosphere includes a reducing gas and an inert gas at a volume flow ratio of (1-5):5, the reducing gas includes at least one of hydrogen, methane, ammonia, ethylene and acetylene, and the inert gas includes argon; (5) placing the composite microsphere intermediate in a carbonization furnace under an inert atmosphere, heating the temperature to 900-1600°C at a heating rate of 1-10°C / min, and carbonizing the composite microsphere intermediate at a constant temperature for 0.5-8h. After the carbonization treatment, washing the composite microsphere intermediate with an acid solution with a concentration of 0.5-3mol / L, anhydrous ethanol and water at 40-95°C for 1-10h in sequence, and drying to obtain the hard carbon microsphere negative electrode material.

7. A sodium ion battery, characterized in that: The negative electrode of the sodium ion battery includes a hard carbon microsphere negative electrode material prepared by the preparation method according to any one of claims 1 to 6.

8. Use of the hard carbon microsphere negative electrode material prepared by the preparation method according to any one of claims 1 to 6 in lithium ion batteries and / or potassium ion batteries.

Citation Information

Patent Citations

  • Preparation method of lithium ion secondary battery hard-carbon microsphere negative electrode material

    CN103647082A

  • Preparation method of hard carbon microsphere anode material for lithium ion batteries

    CN106006603A

  • Preparation method of hard carbon negative electrode material of sodium ion battery

    CN111204731A

  • Carbon dot modified amorphous carbon material and preparation method and application thereof

    CN115092905A