Steel plate for hydropower and production method thereof
By using low-C, high-Ni chemical composition and anti-oxidation coating spraying in hydropower steel plates combined with segmented heating and high-pressure water descaling processes, the problems of difficulty in descaling and low production efficiency of hydropower steel plates are solved, and high strength, high Toughness and excellent welding performance improve production efficiency and yield rate.
Patent Information
- Application Number
- CN202411019274.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-29
AI Technical Summary
Due to the high content of Ni and other alloying elements in existing steel plates for hydropower, it is difficult to remove scales and has low production efficiency. The iron oxide scale penetrates deep into the matrix and is difficult to completely remove, resulting in waste products and environmental pollution.
Using a low-C and high-Ni chemical composition system, combined with Si, Mn, Cr, and Mo alloy elements, anti-oxidation paint is sprayed to form a coating, and through segmented heating and high-pressure water descaling processes, the steel plate achieves high strength and high Toughness and excellent welding performance, while avoiding the penetration of iron oxide scale and improving production efficiency.
It achieves high strength, high toughness and excellent welding performance of the steel plate, reduces the difficulty of descaling, improves the yield rate and production efficiency, reduces labor and costs, avoids the penetration of iron oxide scale, and improves the surface quality.
Smart Images

Figure CN118543805B_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of material preparation, and relates to a steel plate for hydropower and a production method thereof. Background Art
[0002] Hydropower steel plates are mainly used to manufacture pressure pipes in hydropower station dams, and some are used to manufacture auxiliary facilities such as ribs, bifurcated pipes, and volutes. With the large-scale development and use of large-capacity, high-head hydropower stations, the demand for water pressure steel pipes that can withstand large flows and high pressures is increasing, which puts higher requirements on hydropower steel plates, requiring them to have higher strength, better low-temperature toughness and better welding performance.
[0003] In the existing hydropower steel plates, in order to ensure that the steel plates have both high strength and good low-temperature toughness, the content of alloy elements such as Ni in the steel plates is greatly increased. However, Ni is an element that is difficult to oxidize in steel. When the steel plate is oxidized, Fe is preferentially oxidized to form iron oxide scale, and Ni is enriched in the inner layer of the iron oxide scale, forming Ni-rich metal mesh wires and particles. These metal mesh wires and particles will also develop with the increase of temperature. This Ni-rich metal mesh wire connects the iron oxide scale with the metal matrix. Since its plasticity and thermal expansion coefficient are similar to those of the metal matrix, it is still not easy to peel off even under the impact of high-pressure water. In addition, selective oxidation of grain boundaries will occur in Ni-containing steel, causing FeO, fayalite or its eutectic to be wedge-shaped and penetrate into the metal matrix along the grain boundaries, which improves the adhesion of the iron oxide scale of Ni-containing steel and makes descaling difficult.
[0004] At present, the iron oxide scale on the surface of steel plates is mainly removed by manual grinding in the later stage. However, since the iron oxide scale penetrates deep into the steel plate matrix, excessive grinding during descaling can easily cause waste. In addition, grinding requires a lot of manpower and will cause serious environmental pollution. Summary of the invention
[0005] The purpose of the present application is to provide a production method of a hydropower steel plate, and a hydropower steel plate prepared by the production method, so as to solve the problems of difficult descaling and low production efficiency caused by the high content of alloy elements such as Ni in existing high-strength hydropower steel plates.
[0006] To achieve one of the above-mentioned application purposes, an embodiment of the present application provides a method for producing a steel plate for hydropower, wherein the chemical composition of the steel plate includes, by mass percentage: C 0.06-0.12%, Si≤0.1%, Mn 1.15-1.55%, Cr 0.10-0.45%, Ni 0.5-1.5%, Mo 0.15-0.55%, and the rest is Fe and unavoidable impurities; the production method includes the steps of spraying, heating and descaling, rolling, and heat treatment of continuous casting billets in sequence;
[0007] In the continuous casting billet spraying process, after the anti-oxidation coating is prepared into a solution, the surface of the continuous casting billet is sprayed to form a coating, and the chemical components of the anti-oxidation coating include, by mass percentage: SiO2 55-65%, Al2O3 8-12%, ZrO2 7-12%, Na2SiO3 14-20%, SiC 6-10%;
[0008] In the heating and descaling process, the continuous casting billet after the spraying process is heated in sequence according to the recovery section, the preheating section, the first heating section, the second heating section and the third heating section, and descaling is performed immediately after the heating is completed; the heating temperature of the recovery section is 800-950°C, and the heating time is 90-120min; the heating temperature of the preheating section is 950-1050°C, and the heating time is 50-70min; the heating temperature of the first heating section is 1050-1150°C, and the heating time is 80-100min; the heating temperature of the second heating section is 1150-1180°C, and the heating time is 80-100min; the heating temperature of the third heating section is 1140-1160°C, and the heating time is 50-70min;
[0009] In the rolling process, the slab is descaled between passes;
[0010] In the heat treatment step, the steel plate having a thickness of t obtained in the rolling step is sequentially quenched and tempered.
[0011] As a further improvement of one embodiment of the present application, in the continuous casting billet spraying process, the thermal expansion coefficient α of the anti-oxidation coating is t The thermal expansion coefficient α of the continuous casting billet p The absolute value of the difference Δα>25%×α p , Δα=α t -α p .
[0012] As a further improvement of one embodiment of the present application, the thermal expansion coefficient α of the anti-oxidation coating is t Calculated by the following formula:
[0013] α t =∑m(i)α(i) / ∑m(i),
[0014] Wherein, m(i) is the mass percentage of each chemical component in the anti-oxidation coating, α(i) is the expansion coefficient of each chemical component in the anti-oxidation coating, α(SiO2)=0.5×10 -6 / ℃,α(Al2O3)=8.8×10 -6 / ℃,α(ZrO2)=10×10 -6 / ℃,α(Na2SiO3)=6×10 -6 / ℃,α(SiC)=4.7×10 -6 / ℃.
[0015] As a further improvement of one embodiment of the present application, the thermal expansion coefficient α of the anti-oxidation coating is t 5×10 -6 / ℃~8×10 -6 / ℃, the thermal expansion coefficient of the continuous casting billet is α p 12.1×10 -6 / ℃~13.0×10 -6 / ℃.
[0016] As a further improvement of an embodiment of the present application, the particle size of the anti-oxidation coating is 0.3~0.6 microns.
[0017] As a further improvement of one embodiment of the present application, in the spraying process, the anti-oxidation coating and water are mixed into a solution in a mass ratio of 1:1 using a sprayer, and then allowed to stand for aging, and then sprayed on the surface of the continuous casting billet to form a coating, and the spray outlet pressure of the sprayer is controlled to be 7~8MPa, and the coating thickness is controlled to be 0.3~0.6mm.
[0018] As a further improvement of an embodiment of the present application, in the heating descaling process, the descaling water pressure is controlled to be ≥18MPa;
[0019] In the rolling process, the slab is descaled with high-pressure water between passes, and the descaling water pressure is controlled to be ≥15MPa.
[0020] As a further improvement of an embodiment of the present application, in the heat treatment process, the quenching temperature is 860~900°C, the quenching time T1=1.6×t+(20~45), the unit of T1 is min, and after quenching, it is quickly cooled to room temperature and then tempered. The tempering temperature is 580~620°C, the tempering time T2=3×t+(20~45), the unit of T2 is min, and the unit of t is mm.
[0021] In order to achieve one of the above-mentioned application purposes, an embodiment of the present application further provides a hydropower steel plate, which is prepared by the production method of the hydropower steel plate as described above.
[0022] As a further improvement of an embodiment of the present application, the thickness of the steel plate is 25~100 mm, the yield strength is 690~1000 MPa, the tensile strength is 780~1100 MPa, the elongation after fracture is ≥14%, and the impact energy at -40°C is ≥100 J.
[0023] Compared with the prior art, the beneficial effects of this application include:
[0024] (1) Based on the optimized design of chemical composition and combined with the production process control plan, an anti-oxidation coating is sprayed on the surface of the continuous casting billet after continuous casting to form an anti-oxidation coating. Combined with the segmented controlled heating in the heating process, descaling is performed immediately after heating and between passes in the rolling process. This achieves comprehensive optimization of the steel plate in terms of strength, toughness, welding performance and production efficiency. In addition, the surface of the steel plate obtained after rolling is free of iron oxide scale, and no manual descaling is required, which greatly improves the yield rate and production efficiency, saving manpower and costs.
[0025] (2) The steel plate adopts a chemical composition system of low C and high Ni, combined with the control of the content of Si, Mn, Cr, and Mo alloy elements, which lays the foundation for the steel plate to have high strength, high toughness and excellent welding performance; combined with the chemical composition design scheme of the anti-oxidation coating, the coating formed by it can be reasonably matched with the chemical composition of the substrate formed by the continuous casting billet, which can not only reduce the oxidation of the substrate, but also the coating can be self-stripped during the subsequent heating and descaling. On the one hand, the difficulty of descaling is reduced, and the problem of iron oxide scale being pressed into the substrate due to unclean descaling is avoided, which saves labor and improves production efficiency. On the other hand, it effectively avoids the surface defect problem caused by descaling and improves the yield rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 is a surface photograph of the steel plate in Example 1;
[0027] Figure 2 is a surface photograph of the steel plate in Example 2;
[0028] Figure 3 This is a surface photograph of the steel plate in Example 3. DETAILED DESCRIPTION
[0029] The technical solution of the present application is further introduced below in conjunction with specific implementation methods, but the scope of protection required is not limited to the description.
[0030] One embodiment of the present application provides a method for producing a hydropower steel plate, and a hydropower steel plate prepared by the production method. The steel plate is suitable for manufacturing pressure pipes in hydropower station dams, or auxiliary facilities such as ribs, bifurcated pipes, and volutes.
[0031] In this application, on the basis of chemical composition optimization design, combined with the production process control plan, an anti-oxidation coating is sprayed on the surface of the slab before heating to form an anti-oxidation coating, combined with the segmented controlled heating of the heating process, and descaling is performed immediately after heating, as well as descaling between passes in the rolling process, thereby achieving comprehensive optimization of the steel plate in terms of strength, toughness, welding performance, production efficiency, etc., and the surface of the steel plate obtained after rolling is free of iron oxide scale, and no manual descaling is required, which greatly improves the yield rate and production efficiency, and saves manpower and costs.
[0032] Specifically, in terms of chemical composition, in the present application, the chemical composition of the steel plate includes, by mass percentage: C 0.06~0.12%, Si≤0.1%, Mn 1.15~1.55%, Cr 0.10~0.45%, Ni 0.5~1.5%, Mo 0.15~0.55%, and the rest is Fe and unavoidable impurities.
[0033] In this way, by adopting a chemical composition system of low C and high Ni, combined with the control of the content of Si, Mn, Cr, and Mo alloy elements, the foundation is laid for the steel plate to have high strength, high toughness and excellent welding performance.
[0034] The effects of the chemical components and the content control in one embodiment of the present application have the following effects:
[0035] C, Mn: can effectively improve the hardenability and strength of the steel plate, but too much C and Mn will lead to an increase in carbon equivalent and cold crack sensitivity coefficient, resulting in poor low-temperature toughness and welding performance. In this application, the C content is controlled to 0.06~0.12%, and the Mn content is controlled to 1.15~1.55%, so that the strength and welding performance of the steel plate can be taken into account.
[0036] Si: It is the main deoxidizing element, but too high Si will make it difficult to descale the slab. In this application, the Si content is controlled to Si≤0.1%.
[0037] Cr, Mo: can effectively improve the hardenability of the material, increase tempering stability, and compensate for the loss of hardenability and strength caused by low C and Mn content, but too much Cr and Mo will also lead to poor welding performance. In this application, the Cr content is controlled to 0.10~0.45%, and the Mo content is controlled to 0.15~0.55%;
[0038] Ni: It has a significant effect of reducing the cold brittle transition temperature. It is an important alloying element in high-strength hydroelectric steel. It can improve the strength and toughness of the steel plate, but it easily makes it difficult to descale the high-strength hydroelectric steel. In this application, the Ni content is controlled to be 0.5~1.5%.
[0039] In this embodiment, based on the above chemical composition, the production technology is improved to achieve comprehensive optimization of the strength, toughness, welding performance, surface quality, production efficiency and other aspects of the obtained steel plate.
[0040] Specifically, in the production method of the hydropower steel plate, the steps of molten steel smelting, continuous casting, continuous casting billet spraying, heating and descaling, rolling and heat treatment are carried out in sequence to obtain the finished steel plate.
[0041] The production method of the hydropower steel plate is introduced in detail below.
[0042] (1) Molten steel smelting
[0043] The raw materials are smelted to obtain molten steel, wherein the chemical composition of the molten steel includes, by mass percentage, C 0.06-0.12%, Si≤0.1%, Mn 1.15-1.55%, Cr 0.10-0.45%, Ni 0.5-1.5%, Mo 0.15-0.55%, and the rest is Fe and unavoidable impurities.
[0044] It can be understood that the chemical composition of the molten steel obtained in the molten steel smelting process and the chemical composition of the continuous casting billet obtained in the continuous casting process are the same as the chemical composition of the steel plate, and are consistent with the chemical composition described above, and will not be repeated here.
[0045] (2) Continuous casting process
[0046] A continuous casting machine is used to perform full-protection casting on the molten steel obtained in the molten steel smelting process to obtain a continuously cast billet.
[0047] (3) Continuous casting slab spraying process
[0048] After the anti-oxidation coating is configured into a solution, it is sprayed on the surface of the continuous casting billet to form a coating, and then dried. The chemical components of the anti-oxidation coating include, by mass percentage, SiO2 55-65%, Al2O3 8-12%, ZrO2 7-12%, Na2SiO3 14-20%, and SiC 6-10%.
[0049] By adopting the above-mentioned anti-oxidation coating chemical composition system, the coating formed by it can be reasonably matched with the chemical composition of the substrate formed by the continuous casting billet, which can not only reduce the oxidation of the substrate, but also the coating can be self-peeled during the subsequent heating and descaling. On the one hand, the difficulty of descaling is reduced, and the problem of iron oxide being pressed into the substrate due to unclean descaling is avoided, which saves labor and improves production efficiency. On the other hand, it effectively avoids the problem of surface defects caused by descaling and improves the yield rate.
[0050] Specifically, the control of the chemical components and their contents in the anti-oxidation coating has the following effects:
[0051] SiO2 is the main substance that makes up the anti-oxidation coating, and is also the main reason why the coating forms a dense viscous glass film at high temperature. Its content determines the melting point and density of the coating. In this application, the content of SiO2 is controlled to be 55-65%.
[0052] Al2O3 can increase the viscosity of the coating at high temperature, increase the softening temperature of the coating, and adjust the thermal expansion coefficient of the coating; Al2O3 can capture the free oxygen diffused into the coating during heating to form a four-coordinate substance (Al 3+ The tetrahedral structure formed by the ions and four oxygen atoms is filled into the silicon-oxygen structure of the coating to fill the cracks and holes formed in the coating under high temperature. In this application, the content of Al2O3 is controlled to be 8-12%.
[0053] ZrO2 has a high melting point and is a high temperature resistant filler. During the heating process, when the heating temperature reaches 1000°C, ZrO2 undergoes a crystal transformation from a monoclinic phase to a tetragonal phase. This process is accompanied by a change in volume, which causes the coating volume to expand and makes it easy for the coating to peel off from the substrate surface. In this application, the content of ZrO2 is controlled to be 7-12%.
[0054] As a binder, Na2SiO3 is beneficial to improve the coating performance and suspension performance of the coating material, and affects the strength and density of the coating. If its content is too low, it will lead to problems such as loose coating structure, bubbles, pores, and failure to completely wrap the substrate surface. If its content is too high, it will increase the bonding force between the coating and the substrate, and it is not easy to fall off during the cooling process of the coating. In this application, the content of Na2SiO3 is controlled to be 14~20%.
[0055] SiC: During the heating process, SiC reacts with O2, thereby consuming oxygen diffused into the coating, causing the substrate surface to be oxygen-deficient or oxygen-free, and reducing the oxidation of the substrate. In this application, the content of SiC is controlled to be 6-10%.
[0056] Preferably, the thermal expansion coefficient of the anti-oxidation coating is t The thermal expansion coefficient α of the continuous casting billet p The absolute value of the difference Δα>25%×α p , Δα=α t -α p By controlling the thermal expansion coefficient α of the anti-oxidation coating t The thermal expansion coefficient α of the continuous casting billet pThe relationship between the thermal expansion coefficients of the coating formed by the anti-oxidation coating and the substrate formed by the continuous casting billet is reasonably matched. On the one hand, it is beneficial for the coating to self-strip during descaling after subsequent heating. On the other hand, it can avoid excessive stress in the coating during the heating process, which may cause the coating to crack or peel off, thereby reducing the protective effect.
[0057] Wherein, the thermal expansion coefficient α of the anti-oxidation coating is t Calculated by the following formula:
[0058] α t =∑m(i)α(i) / ∑m(i),
[0059] Wherein, m(i) is the mass percentage of each chemical component in the anti-oxidation coating, for example, if the mass percentage of SiO2 is 55%, then m(i)=55%;
[0060] α(i) is the expansion coefficient of each chemical component in the anti-oxidation coating, α(SiO2)=0.5×10 -6 / ℃,α(Al2O3)=8.8×10 -6 / ℃,α(ZrO2)=10×10 -6 / ℃,α(Na2SiO3)=6×10 -6 / ℃,α(SiC)=4.7×10 -6 / ℃.
[0061] Preferably, in this embodiment, the thermal expansion coefficient α of the anti-oxidation coating is t 5×10 -6 / ℃~8×10 -6 / ℃, the thermal expansion coefficient of the continuous casting billet is α p 12.1×10 -6 / ℃~13.0×10 -6 / ℃.
[0062] The thermal expansion coefficient of the continuous casting billet can be obtained by using a German NETZSCH DIL 402C thermal expansion instrument, and argon protection is adopted during the entire experimental process.
[0063] α p Calculated by the following formula:
[0064] ,
[0065] Wherein, L0 is the original length of the sample at room temperature T0, in mm; Li is the length of the sample at temperature Ti, in mm.
[0066] Preferably, the particle size of the anti-oxidation coating is 0.3-0.6 microns.
[0067] The smaller the particle size of the anti-oxidation coating, the more conducive it is to subsequent spraying and the protective effect of the coating, but too small a particle size will increase the production cost of the coating. In this application, the particle size of the anti-oxidation coating is controlled to be 0.3~0.6 microns.
[0068] The anti-oxidation coating is prepared by the following method:
[0069] The chemical components in the above-mentioned anti-oxidation coating are mixed according to the above-mentioned mass percentages, then poured into a stainless steel grinding jar, grinding media are added, and then a certain amount of deionized water is added. A planetary ball mill is used to complete ball milling dispersion under different ball milling parameters to make the chemical components mixed, uniform, and sieved to obtain the anti-oxidation coating.
[0070] Specifically, the anti-oxidation coating and water are prepared into a solution in a mass ratio of 1:1 by a sprayer, and the solution is allowed to stand for aging, and then sprayed onto the surface of the continuous casting billet to form a coating.
[0071] Preferably, the spray outlet pressure of the sprayer is controlled to be 7-8 MPa, and the coating thickness is controlled to be 0.3-0.6 mm.
[0072] The spray flow and coating thickness can be controlled by controlling the spray outlet pressure of the spray machine. If the coating is too thin, its anti-oxidation effect is poor. If the coating is too thick, the coating is prone to cracks during the drying process after spraying, and the thermal conductivity of the coating will be reduced, thereby prolonging the heating time under the same heating temperature.
[0073] (4) Heating and descaling process
[0074] The continuous casting billet after the spraying process is heated in sequence according to the recovery section, the preheating section, the first heating section, the second heating section and the third heating section, and descaling is performed immediately after the heating is completed.
[0075] Among them, the heating temperature of the recovery section is 800~950℃, and the heating time is 90~120min; the heating temperature of the preheating section is 950~1050℃, and the heating time is 50~70min; the heating temperature of the first heating section is 1050~1150℃, and the heating time is 80~100min; the heating temperature of the second heating section is 1150~1180℃, and the heating time is 80~100min; the heating temperature of the third heating section is 1140~1160℃, and the heating time is 50~70min.
[0076] Through multi-stage segmented heating, it can be ensured that the continuous casting billet can be heated through to avoid excessive grain growth. The recovery section and the preheating section are controlled at a lower heating temperature, so as to ensure sufficient heating time, which is conducive to improving the uniformity of the temperature of the surface and core of the continuous casting billet, and the protective effect of the anti-oxidation coating; the first heating section, the second heating section, and the third heating section are controlled at a higher heating temperature, which can shorten the heating time as much as possible while ensuring that the alloy is completely dissolved, so as to avoid the failure of the anti-oxidation coating due to long-term heating.
[0077] Preferably, descaling is performed immediately after heating is completed, and the descaling water pressure is controlled to be ≥18 MPa, so as to facilitate the removal of the anti-oxidation coating and iron oxide scale on the surface of the continuous casting billet.
[0078] (5) Rolling process
[0079] The continuous casting slab after the heating and descaling process is successively subjected to two-stage rolling of rough rolling and finish rolling to obtain a steel plate with a thickness of 25 to 100 mm, and the slab is descaled between passes to prevent the iron oxide scale generated by high temperature from affecting the surface quality of the steel plate.
[0080] Preferably, the slab is descaled with high-pressure water between passes, and the descaling water pressure is controlled to be ≥15 MPa to achieve the effect of removing iron oxide scale on the surface of the continuous casting slab.
[0081] (6) Heat treatment process
[0082] The steel plate obtained in the rolling process is sequentially quenched and tempered to obtain a finished steel plate with a thickness of t, where t is in mm.
[0083] Preferably, the quenching temperature is 860-900°C, the quenching time T1=1.6×t+(20-45), the unit of T1 is min, and after quenching, it is quickly cooled to room temperature, and then tempered, the tempering temperature is 580-620°C, the tempering time T2=3×t+(20-45), the unit of T2 is min. In this way, by sufficient tempering, the steel plate can obtain a stable tempered martensite structure.
[0084] In this way, the present application, under the chemical composition system of low C and high Ni of the aforementioned steel plate, combines the control of the content of Si, Mn, Cr, and Mo alloy elements, laying the foundation for the steel plate to have high strength, high toughness and excellent welding performance; combined with the chemical composition design scheme of the anti-oxidation coating, the coating formed by it can be reasonably matched with the chemical composition of the substrate formed by the continuous casting billet, which can not only reduce the oxidation of the substrate, but also the coating can be self-peeled during the subsequent heating and descaling, on the one hand, reducing the difficulty of descaling, avoiding the problem of iron oxide being pressed into the substrate due to unclean descaling, saving labor and improving production efficiency, on the other hand, effectively avoiding the problem of surface defects caused by descaling, and improving the yield rate; further combined with the segmented controlled heating of the heating process, and descaling immediately after heating, as well as descaling between passes in the rolling process, the comprehensive optimization of the steel plate in terms of strength, toughness, welding performance and production efficiency is achieved, and the surface of the steel plate obtained after rolling is free of iron oxide scale, and no manual descaling is required, which greatly improves the yield rate and production efficiency, saving manpower and cost.
[0085] Specifically, in the present application, after the heat treatment process, the thickness of the steel plate is 25~100mm, the yield strength is 690~1000MPa, the tensile strength is 780~1100MPa, the elongation after fracture is ≥14%, and the impact energy at -40℃ is ≥100J.
[0086] The following three specific embodiments are provided to further illustrate the technical solution of the present application. Of course, these three embodiments are only a part of the many variations of the present implementation mode, but not all of them.
[0087] The three embodiments provide a steel plate respectively. The chemical compositions of the steel plates of the three embodiments are shown in Table 1 in terms of mass percentage, with the remainder being iron and unavoidable impurities.
[0088] Table 1
[0089]
[0090] The method for producing a steel plate includes the following steps.
[0091] (1) Molten steel smelting
[0092] The raw materials are smelted to obtain molten steel, the chemical composition of the molten steel is shown in Table 1 in terms of mass percentage, and the rest is iron and inevitable impurities.
[0093] (2) Continuous casting process
[0094] The molten steel obtained in the molten steel smelting process is fully casted by a continuous casting machine to obtain a continuous casting billet. The chemical composition of the continuous casting billet is shown in Table 1 in terms of mass percentage, and the rest is iron and unavoidable impurities.
[0095] (3) Continuous casting slab spraying process
[0096] First, an anti-oxidation coating is prepared. The chemical components of the anti-oxidation coating are shown in Table 2 in terms of mass percentage.
[0097] The chemical components were weighed and mixed according to the mass percentage shown in Table 2, and then poured into a stainless steel grinding jar, and grinding media was added. A certain amount of deionized water was added, and a planetary ball mill was used to complete ball milling dispersion under different ball milling parameters to mix, evenly distribute and sieve the chemical components to obtain an anti-oxidation coating with a particle size of 0.3-0.6 μm.
[0098] Table 2
[0099]
[0100] Next, the anti-oxidation coating is formulated into a solution.
[0101] The anti-oxidation coating and water are mixed into a solution in a mass ratio of 1:1 using a sprayer, and then allowed to stand for aging.
[0102] Thirdly, the surface of the continuous casting billet is sprayed to form a coating.
[0103] The spray outlet pressure of the spray machine was controlled to be 7-8 MPa, and the coating thicknesses of Examples 1 to 3 were 0.3 mm, 0.4 mm, and 0.5 mm, respectively.
[0104] Finally, dry.
[0105] (4) Heating and descaling process
[0106] The continuous casting billet after the spraying process is heated in sequence according to the recovery section, the preheating section, the first heating section, the second heating section and the third heating section. After the heating is completed, descaling is immediately performed, and the descaling water pressure is ≥18MPa.
[0107] The heating temperatures and heating times of the recovery section, preheating section, first heating section, second heating section and third heating section are shown in Table 3, respectively.
[0108] Table 3
[0109]
[0110] (5) Rolling process
[0111] The continuous casting slab after the heating and descaling process is subjected to two-stage rolling of rough rolling and finish rolling to obtain a steel plate, and the slab is descaled by high-pressure water between passes, and the descaling water pressure is controlled to be ≥15 MPa. The thickness of the steel plates of Examples 1 to 3 is shown in Table 4.
[0112] (6) Heat treatment process
[0113] The steel plate obtained in the rolling process is sequentially quenched and tempered to obtain a finished steel plate with a thickness of t.
[0114] The quenching temperatures of Examples 1 to 3 are 900°C, 890°C and 910°C, respectively; the quenching times of Examples 1 to 3 are 84min, 65min and 84min, respectively; after quenching, the steel is rapidly cooled to room temperature and then tempered; the tempering temperatures of Examples 1 to 3 are 610°C, 620°C and 590°C, respectively; and the tempering times are 140min, 104min and 140min, respectively.
[0115] The tensile properties of the steel plates of the above three embodiments were tested with reference to GB / T228.1-2021 standard, as follows:
[0116] The tensile strength and elongation of the steel plate were tested using a tensile testing machine. The test results are shown in Table 4.
[0117] The impact properties of the steel plates of the above three embodiments were tested with reference to GB / T229-2020 standard, as follows:
[0118] The -40°C impact energy of the steel plate was tested using an impact testing machine. The test results are shown in Table 4.
[0119] Table 4
[0120]
[0121] It can be seen from Table 4 that the mechanical properties of the steel plates of Examples 1 to 3 meet the use requirements of high-strength steel plates for hydropower at corresponding strength levels.
[0122] The photos of the steel plates after painting of Examples 1 to 3 are shown in FIG. Figures 1 to 3 As shown in the figure, it can be seen that the surface quality of the obtained steel plate is excellent.
[0123] It should be understood that although this specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each implementation mode may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
[0124] The detailed descriptions listed above are merely specific descriptions of feasible implementation methods of the present application. They are not intended to limit the scope of protection of the present application. Any equivalent implementation methods or changes that do not deviate from the technical spirit of the present application should be included in the scope of protection of the present application.
Claims
1. A method for producing a steel plate for hydropower, characterized in that: The chemical composition of the steel plate includes, by mass percentage, C 0.06-0.12%, Si≤0.1%, Mn 1.15-1.55%, Cr 0.10-0.45%, Ni 0.5-1.5%, Mo 0.15-0.55%, and the remainder is Fe and unavoidable impurities; the production method includes the steps of continuous casting slab spraying, heating and descaling, rolling, and heat treatment in sequence; In the continuous casting billet spraying process, after the anti-oxidation coating is prepared into a solution, the surface of the continuous casting billet is sprayed to form a coating, and the chemical components of the anti-oxidation coating include, by mass percentage: SiO2 55-65%, Al2O3 8-12%, ZrO2 7-12%, Na2SiO3 14-20%, SiC 6-10%; In the heating and descaling process, the continuous casting billet after the spraying process is heated in sequence according to the recovery section, the preheating section, the first heating section, the second heating section and the third heating section, and descaling is performed immediately after the heating is completed; the heating temperature of the recovery section is 800-950°C, and the heating time is 90-120min; the heating temperature of the preheating section is 950-1050°C, and the heating time is 50-70min; the heating temperature of the first heating section is 1050-1150°C, and the heating time is 80-100min; the heating temperature of the second heating section is 1150-1180°C, and the heating time is 80-100min; the heating temperature of the third heating section is 1140-1160°C, and the heating time is 50-70min; In the rolling process, the slab is descaled between passes; In the heat treatment step, the steel plate having a thickness of t obtained in the rolling step is sequentially quenched and tempered.
2. The method for producing a steel plate for hydropower according to claim 1, characterized in that: In the continuous casting billet spraying process, the thermal expansion coefficient of the anti-oxidation coating is α t The thermal expansion coefficient α of the continuous casting billet p The absolute value of the difference Δα>25%×α p , Δα=α t -α p .
3. The method for producing a steel plate for hydropower according to claim 1, characterized in that: The particle size of the anti-oxidation coating is 0.3-0.6 microns.
4. The method for producing a steel plate for hydropower according to claim 1, characterized in that: In the spraying process, the anti-oxidation coating and water are mixed into a solution in a mass ratio of 1:1 by a sprayer, and then allowed to stand for aging, and then sprayed on the surface of the continuous casting billet to form a coating. The spray outlet pressure of the sprayer is controlled to be 7-8 MPa, and the coating thickness is controlled to be 0.3-0.6 mm.
5. The method for producing a steel plate for hydropower according to claim 1, characterized in that: In the heating and descaling process, the descaling water pressure is controlled to be ≥18MPa; In the rolling process, the slab is descaled with high-pressure water between passes, and the descaling water pressure is controlled to be ≥15MPa.
6. The method for producing a steel plate for hydropower according to claim 1, characterized in that: In the heat treatment process, the quenching temperature is 860~900℃, the quenching time T1=1.6×t+(20~45), the unit of T1 is min, and after quenching, it is quickly cooled to room temperature and then tempered. The tempering temperature is 580~620℃, the tempering time T2=3×t+(20~45), the unit of T2 is min, and the unit of t is mm.
7. A steel plate for hydropower, characterized in that: The steel plate is prepared by the production method of the hydropower steel plate as described in any one of claims 1 to 6.
8. The hydropower steel plate according to claim 7, characterized in that: The steel plate has a thickness of 25-100 mm, a yield strength of 690-1000 MPa, a tensile strength of 780-1100 MPa, an elongation after fracture of ≥14%, and an impact energy of ≥100 J at -40°C.
Citation Information
Cited By
Hydropower steel plate and production method therefor
WO2026025779A1