Protection method of solder joints in flip-chip and superconducting quantum chip
By forming a metal protective layer on the indium solder joints of the superconducting quantum chip, the problem of the impact of hydrogen fluoride treatment on the solder joints is solved, the stability and bonding strength of the flip-chip soldering chip are improved, and the reliability of the superconducting connection at low temperatures is ensured. .
Patent Information
- Application Number
- CN202411044667.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-08-01
AI Technical Summary
During the preparation process of superconducting quantum chips, hydrogen fluoride gas treatment will affect the indium solder joints in the flip-chip soldering process, resulting in a decrease in the joint strength and stability of the solder joints, and desoldering at low temperatures.
A metal protective layer is formed on the indium solder joint, and the silicon dioxide dielectric layer is removed through hydrogen fluoride treatment to improve the bonding strength and chip stability of the indium solder joint after flip-chip welding.
The use of a metal protective layer improves the stability of flip-chip soldering chips and the bonding strength of solder joints, prevents the impact of hydrogen fluoride gas on indium solder joints, and ensures the reliability of superconducting connections at low temperatures.
Smart Images

Figure CN118555905B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of chip preparation and packaging, and specifically relates to a method for protecting solder joints in a flip-chip chip and a superconducting quantum chip, and more specifically relates to a method for protecting solder joints in a superconducting quantum flip-chip chip. Background Art
[0002] The superconducting quantum chip is the core device of the superconducting quantum computer system, which is usually composed of superconducting quantum bits, couplers, reading cavities, control lines, crossover bridges, flip-chip solder joints, etc. In order to protect the performance of superconducting quantum bits, when preparing superconducting quantum chips, you can choose to design the superconducting quantum bits and couplers on a top piece (i.e., the second chip), and design the reading cavity and control lines on another bottom piece (i.e., the first chip). Then, the bottom piece and the top piece are bonded and welded together through the flip-chip welding process to form a complete superconducting quantum chip. The flip-chip welding process is increasingly used in the research and development and preparation of superconducting quantum chips. The solder joints used in superconducting quantum chips are indium solder joints, which can be superconducting at low temperatures (≤25mK) and generate less heat.
[0003] Due to the complex wiring of the film chip, the superconducting quantum chip causes a potential difference on both sides of the line, resulting in a slot line mode. In order to suppress the slot line mode, it is necessary to prepare a crossover bridge, such as an aluminum crossover bridge, on the surface of the reading cavity and the control line. The silicon dioxide dielectric layer and the aluminum crossover bridge are prepared by deposition method pattern transfer technology, which specifically includes: depositing a silicon dioxide dielectric layer at the corresponding position on the film chip, then depositing an aluminum crossover bridge, and removing the silicon dioxide dielectric layer by hydrogen fluoride treatment. Retaining the silicon dioxide dielectric layer will have a great impact on the line impedance and loss, so it is necessary to use hydrogen fluoride gas to remove the silicon dioxide dielectric layer. In the process of removing the silicon dioxide dielectric layer, hydrogen fluoride gas will change the properties of the oxide layer on the surface of the indium solder joint. The degeneration of this oxide layer will cause the bonding strength of the bottom and top sheets to decrease after the flip-chip process, the stability of the flip-chip chip will decrease, and there will be desoldering at low temperatures. Summary of the invention
[0004] In view of the above technical problems, the present invention provides a method for protecting solder joints in a flip-chip and a superconducting quantum chip, in order to at least partially solve the above technical problems. The specific technical solutions provided by the present invention are as follows.
[0005] As a first aspect of the present invention, the present invention provides a method for protecting solder joints in a flip-chip chip, comprising: providing a first chip and a second chip, wherein metal layers under solder joints are deposited on corresponding surfaces of the first chip and the second chip, respectively; preparing a silicon dioxide dielectric layer and a crossover structure on the first chip; forming indium solder joints on the metal layer under solder joints of the first chip with the crossover structure and the metal layer under solder joints of the second chip, respectively; forming a metal protective layer on the indium solder joints of the first chip; subjecting the first chip with the metal protective layer to hydrogen fluoride treatment to remove the silicon dioxide dielectric layer; aligning and bonding the upper and lower patterns of the first chip treated with hydrogen fluoride and the second chip with the indium solder joints, and performing flip-chip welding to obtain a flip-chip chip.
[0006] As a second aspect of the present invention, the present invention provides a superconducting quantum chip, which is manufactured using the above method.
[0007] In an embodiment of the present invention, on the first chip, a silicon dioxide dielectric layer and a crossover are first prepared, and then an indium solder joint and a metal protective layer are prepared, and then the silicon dioxide dielectric layer is removed by hydrogen fluoride gas. In the process of removing the silicon dioxide dielectric layer by hydrogen fluoride gas, the metal protective layer on the surface of the indium solder joint can protect the indium solder joint from the influence of hydrogen fluoride gas, improve the bonding strength of the indium solder joint after flip-chip welding, and then improve the stability of the flip-chip chip. The method for protecting solder joints in the flip-chip chip provided by the present invention can be generally applied to the research and development and preparation of various chips that require flip-chip welding processes, such as superconducting quantum computing chips. For some processes that have an impact on indium solder joints, such as hydrogen fluoride treatment or aluminum, zinc metal covering, the metal protective layer has a good protective effect on the indium solder joints. BRIEF DESCRIPTION OF THE DRAWINGS
[0008] Figure 1 A flow chart of a method for protecting a solder joint in one embodiment of the present invention;
[0009] Figure 2 This is a flow chart of the preparation of the superconducting quantum chip in Example 1 of the present invention;
[0010] Figure 3 This is a schematic diagram of the structure of the wiring layer of the substrate before flip-chip bonding in Example 1 of the present invention;
[0011] Figure 4 This is a schematic diagram of the indium solder joint structure after flip-chip soldering in Example 1 of the present invention;
[0012] Figure 5 This is a schematic diagram of the wiring layer of the substrate in Embodiment 1 of the present invention;
[0013] Figure 6 This is a schematic diagram of the top sheet wiring layer in Example 1 of the present invention;
[0014] Figure 7This is an X-ray photoelectron spectrum of the surface of the indium solder joint in Example 1 of the present invention;
[0015] Figure 8 This is an X-ray photoelectron spectrum of the surface of the indium solder joint after hydrogen fluoride treatment in Example 1 of the present invention;
[0016] Fig. 9 This is a scanning electron microscope image of an indium solder joint covered with a metal protective layer in Example 1 of the present invention;
[0017] Fig.10 This is a scanning electron microscope image of the manually unplugged weld in Example 1 of the present invention;
[0018] Fig.11 This is a diagram showing the resistance change of the superconducting quantum chip during the cooling process in Example 1 of the present invention;
[0019] Fig.12 This is a graph showing the resistance change of the indium solder joint of the superconducting quantum chip at room temperature in Example 1 of the present invention;
[0020] Fig.13 This is a graph showing the resistance change of the indium solder joint of the superconducting quantum chip at 12mK in Example 1 of the present invention. DETAILED DESCRIPTION
[0021] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings.
[0022] At present, when preparing superconducting quantum chips, hydrogen fluoride gas treatment will affect the indium solder joints in the flip-chip process. The present invention provides a method for protecting the solder joints in a flip-chip chip and a superconducting quantum chip. By forming a metal protection layer on the indium solder joints, the indium solder joints can be protected from the influence of hydrogen fluoride gas, the bonding strength of the indium solder joints after flip-chip welding is improved, and the stability of the flip-chip chip is improved.
[0023] As a first aspect of the present invention, the present invention provides a method for protecting solder joints in a flip chip, such as Figure 1 As shown, steps S1-S6 are included.
[0024] S1: providing a first chip and a second chip, wherein corresponding surfaces of the first chip and the second chip are respectively deposited with under-brick metallization layers (UBM layers).
[0025] S2: preparing a silicon dioxide dielectric layer and a crossover bridge structure on the first chip.
[0026] S3: forming indium bumps (In Bumps) on the UBM layer of the first chip and the UBM layer of the second chip respectively.
[0027] S4: forming a metal protective layer (capping layer) on the indium solder joints of the first chip.
[0028] S5: performing hydrogen fluoride treatment on the first chip formed with the metal protection layer to remove the silicon dioxide dielectric layer.
[0029] S6: Align and bond the upper and lower patterns of the first chip treated with hydrogen fluoride and the second chip with indium solder joints, and perform flip-chip bonding to obtain a flip-chip chip.
[0030] In an embodiment of the present invention, on the first chip, a silicon dioxide dielectric layer and a crossover are first prepared, and then an indium solder joint and a metal protective layer are prepared, and then the silicon dioxide dielectric layer is removed by hydrogen fluoride gas. In the process of removing the silicon dioxide dielectric layer by hydrogen fluoride gas, the metal protective layer on the surface of the indium solder joint can protect the indium solder joint from the influence of hydrogen fluoride gas, improve the bonding strength of the indium solder joint after flip-chip welding, and then improve the stability of the flip-chip chip. The method for protecting solder joints in the flip-chip chip provided by the present invention can be generally applied to the research and development and preparation of various chips that require flip-chip welding processes, such as superconducting quantum computing chips. For some processes that have an impact on indium solder joints, such as hydrogen fluoride treatment or aluminum, zinc metal covering, the metal protective layer has a good protective effect on the indium solder joints.
[0031] According to an embodiment of the present invention, the method for protecting solder joints in the flip-chip chip may further include: forming a metal protection layer on the indium solder joints of the second chip. Figure 1 The method shown forms a metal protective layer only on the indium solder joints of the first chip. When the subsequent processing damages the indium solder joints on the second chip, a metal protective layer can also be formed on the second chip to protect the indium solder joints. For example: when the flip-chip chip is a semiconductor chip, a layer of electroplating is usually formed on the surface of the first chip and the second chip to protect the semiconductor chip from corrosion. Among them, the material of the electroplating layer includes one or more of aluminum and zinc. At this time, if the electroplating layer is directly formed on the surface of the indium solder joint, it will cause the indium solder joint and metals such as aluminum and zinc to undergo co-metal corrosion. Therefore, it is necessary to form a metal protective layer on the surface of the indium solder joints of the first chip and the second chip, and then form an electroplating layer. At this time, the metal protective layer formed on the indium solder joints of the first chip and the second chip can protect the indium solder joints and prevent the indium solder joints from undergoing co-metal corrosion with metals such as aluminum and zinc.
[0032] According to an embodiment of the present invention, the method for protecting solder joints in the flip-chip chip further includes: after the first chip and the second chip are aligned and bonded for flip-chip bonding, the flip-chip chip is packaged. The chip is fanned out through a sample box by packaging, and then interconnected with a measurement system by a signal line to achieve microwave signal transmission. The packaging can also provide mechanical support and protection for the flip-chip chip to prevent the external environment from damaging the chip.
[0033] According to an embodiment of the present invention, the method for protecting solder joints in the above flip-chip chip further includes: after packaging, performing a stability test on the flip-chip chip. In order to detect the stability of the flip-chip chip during operation, the flip-chip chip is packaged and then subjected to a stability test. The stability test includes multiple temperature rise and fall cycles; the temperature rise and fall cycle includes: cooling from 295K to 12mK, and then heating to 295K. The temperature rise and fall cycle is used to test whether the indium solder joint is disconnected or not connected after flip-chip welding.
[0034] According to an embodiment of the present invention, the material of the metal protective layer includes any one of Ti / Au, Pt / Au, and TiN, and the material of the metal layer under the solder joint includes any one of Ti / Au, Pt / Au, and TiN, wherein Ti / Au refers to an Au layer superimposed on a Ti layer, and Pt / Au refers to an Au layer superimposed on a Pt layer. When the first chip and the second chip are flip-chip soldered, a structure of metal layer under the solder joint-indium solder joint-metal protective layer-indium solder joint-metal layer under the solder joint is formed. For superconducting quantum chips, the resistance of the metal protective layer and the metal layer under the solder joint must be small enough. Therefore, the metal layer under the solder joint and the metal protective layer generally select materials such as Ti / Au, Pt / Au, and TiN, because the resistance of these materials is small at low temperatures. When the metal materials on both sides are superconductors, electrons can pass through the metal protective layer and the metal layer under the solder joint without loss, further reducing the chip resistance. The material of the metal protective layer and the material of the metal layer under the solder joint can be the same or different, for example, the metal protective layer is Ti / Au, the metal layer under the solder joint is TiN, or both the metal protective layer and the metal layer under the solder joint are TiN. When the material of the metal protective layer or the metal layer under the solder joint is Pt / Au or Ti / Au, since the resistance of Ti and Pt is relatively large, the thickness of the Ti layer and the Pt layer is set to be at most 10nm. At this time, Ti and Pt are added only to increase the adhesion between the indium solder joint or the chip, and the metal protective layer or the metal layer under the solder joint is still mainly Au.
[0035] According to an embodiment of the present invention, the metal protective layer has the same lateral size as the indium solder joint. For example, when the indium solder joint is a square structure, the metal protective layer is a square structure with the same side length as the indium solder joint. When the indium solder joint is a circular structure, the metal protective layer is a circular structure with the same diameter as the indium solder joint. The thickness of the metal protective layer is 30-300nm, for example, it can be 30nm, 50nm, 100nm, 150nm, 200nm, 250nm, 300nm, etc. The metal protective layer is used to protect the indium solder joint to prevent the oxide layer structure of the indium solder joint from being affected. Since the flatness of the indium solder joint itself is not good (in order to ensure the firmness of the solder joint after flip-chip welding, it is generally not prepared very flat), if the metal protective layer is too thin, it cannot cover the indium solder joint well and cannot provide good protection for the indium solder joint. If the metal protective layer is too thick, it may affect the firmness of the indium solder joint and reduce the stability of the flip-chip chip.
[0036] According to an embodiment of the present invention, indium is a superconducting welding material, which is a superconductor at low temperature (≤25mK). After flip-chip welding, superconducting connection between flip-chip chips can be achieved, and the thickness of the indium solder joint is generally in the micron level. In the field of superconducting quantum chips, the thickness of the indium solder joint is preferably 5-20μm, for example, 5μm, 10μm, 15μm, 20μm, etc.; more preferably 7-12μm, for example, 7μm, 10μm, 12μm, etc. When the deformation of the indium solder joint before and after flip-chip welding is generally about 50%, the chip stability after welding is better. If the deformation is too small, the bonding firmness between the indium solder joints is not enough, and the solder joint connection is easily affected by external stress and broken at low temperature, especially during the heating and cooling cycle. If the deformation is too large, a thicker indium solder joint is required, which has high requirements on the process, and also occupies more space, which limits the arrangement and design of other components. Generally, the appropriate thickness of the indium solder joint can be selected according to the spacing after flip-chip welding.
[0037] According to an embodiment of the present invention, the side length ratio of the metal layer under the solder joint to the indium solder joint is 1.5-3:1, for example, it can be 1.5:1, 2:1, 2.5:1, 3:1, etc.; the thickness of the metal layer under the solder joint is 100-300nm, for example, it can be 100nm, 150nm, 200nm, 250nm, 300nm, etc. The metal layer under the solder joint can avoid the co-metal between the indium solder joint and the wiring layer or other metal in contact with the first chip and the second chip, which causes the metal in the contact part to be etched and lost, causing the problem of circuit breaking or performance degradation in the flip-chip chip. Therefore, the size of the metal layer under the solder joint needs to be larger than the size of the indium solder joint. There is no specific requirement for the shape of the indium solder joint, which can be determined by the user according to actual process requirements. For example, the indium solder joint is 14×14-18×18 μm 2 Square pillars, the metal layer under the solder joint is 28×28-36×36 μm 2 At the same time, the thickness of the metal layer under the solder joint also needs to be controlled. If it is too thin, the indium solder joint will be etched together with the metal of the wiring layer on the first chip and the second chip, and the separation effect will not be achieved; if it is too thick, the chip resistance will increase.
[0038] According to an embodiment of the present invention, a metal protective layer is deposited on an indium solder joint by a deposition method pattern transfer technique, an indium solder joint is deposited on a metal layer under the solder joint by a deposition method pattern transfer technique, and a metal layer under the solder joint is deposited on a first chip and a second chip by a deposition method pattern transfer technique. The deposition method pattern transfer technique includes: pattern formation, deposition process, and pattern transfer; wherein, the deposition method in the deposition process includes any one of electron beam evaporation coating, thermal evaporation coating, and magnetron sputtering, and the deposition methods commonly used in semiconductor circuit processing technology can also be used. For example, a metal layer under the solder joint can be formed by electron beam evaporation coating of Ti / Au, an indium solder joint can be prepared by thermal evaporation coating of indium, and a metal protective layer can be formed by electron beam evaporation coating of Ti / Au. The specific process can be determined by the user.
[0039] In an embodiment of the present invention, based on a relatively high-quality superconducting film, a superconducting wiring layer is prepared by etching pattern transfer technology to obtain a first chip and a second chip. The etching pattern transfer technology includes: pattern formation, etching process and pattern transfer; wherein, the etching process in the etching process includes any one of inductively coupled plasma dry etching (ICP), reactive ion dry etching (RIE), and chemical solution wet etching, and the etching process commonly used in semiconductor circuit processing technology can also be used. The material of the first chip and the second chip includes any one of aluminum, niobium, tantalum, and titanium nitride. The thickness of the first chip and the second chip is generally 100-300nm, for example, it can be 100nm, 150nm, 200nm, 250nm, 300nm, etc. There is generally no special restriction here, and it can be adjusted according to your needs.
[0040] In the embodiment of the present invention, the superconducting quantum chip is sensitive to temperature. The temperature of the flip-chip welding process is generally 25-100°C, for example, 25°C, 50°C, 75°C, 100°C, etc. Too high a temperature may cause loss of the Josephson junction, so high-temperature reflow soldering is generally not used in the flip-chip welding process.
[0041] As a second aspect of the present invention, the present invention provides a superconducting quantum chip, which is manufactured using the above method.
[0042] The present invention is further described below by examples and related test experiments. In the detailed description below, for ease of explanation, many specific details are set forth to provide a comprehensive understanding of the embodiments of the present invention. However, it is obvious that one or more embodiments may also be implemented without these specific details. And, in the absence of conflict, the details in the following embodiments may be combined into other feasible embodiments at will. All instruments, consumables and reagents in the following examples, if not otherwise specified, may be obtained from commercial sources.
[0043] Example 1
[0044] In this embodiment 1, a superconducting quantum chip is prepared by using the method for protecting solder joints in a flip-chip provided by the present invention.
[0045] Figure 2 This is a flow chart of the preparation of the superconducting quantum chip in Example 1 of the present invention. Figure 3 This is a schematic diagram of the structure of the substrate wiring layer before flip-chip bonding in Example 1 of the present invention. Figure 4 Schematic diagram of the solder joint structure after flip-chip welding in Example 1 of the present invention.
[0046] like Figure 2 As shown, the specific preparation steps are as follows, including S201-S208.
[0047] S201: preparing a superconducting aluminum film for preparing a bottom wiring layer (ie, a first chip) and a top wiring layer (ie, a second chip).
[0048] S202: Prepare the bottom wiring layer C01a and the top wiring layer C01b (CPW layer), that is, Figure 3 and Figure 4 As shown in . Specifically, the bottom film wiring layer and the top film wiring layer are prepared by etching pattern transfer technology, wherein the etching process adopts chemical solution wet etching. In order to test whether the solder joint protection method is effective, the bottom film wiring layer and the top film wiring layer are prepared into the same coplanar waveguide superconducting wiring layer to provide a wiring layer and a ground plane layer, which can be adjusted according to actual needs, and there are no special requirements here.
[0049] Figure 5 is a schematic diagram of the wiring layer of the substrate in Embodiment 1 of the present invention, Figure 6 Schematic diagram of the top wiring layer in Example 1 of the present invention. Specifically, the bottom wiring layer is 9.3×9.3 mm 2 Square structure, top wiring layer is 6.3×6.3 mm 2 Square structure, the thickness of the bottom wiring layer and the top wiring layer are both 100nm.
[0050] S203: Prepare the metal layer under the solder joint (UBM layer), that is, Figure 3 and Figure 4 The UBM layer U01a on the bottom wiring layer and the UBM layer U01b on the top wiring layer in the figure. Specifically, the metal layer under the solder joint is prepared at the corresponding positions on the bottom wiring layer and the top wiring layer by the deposition method pattern transfer technology, wherein the deposition method adopts electron beam evaporation coating. The metal layer under the solder joint is 30×30 μm 2 Square structure, thickness is 200nm, material is Ti / Au, and the thickness of Ti layer is 10nm.
[0051] S204: Preparation of In Bump Figure 3 and Figure 4 Indium solder joints B01a on the bottom film wiring layer and indium solder joints B01b on the top film wiring layer. Before forming the indium solder joints, a silicon dioxide dielectric layer and a cross-bridge structure need to be prepared. Hydrogen fluoride treatment is introduced to remove the silicon dioxide dielectric layer. Since the operation that affects the indium solder joints is the hydrogen fluoride treatment, in order to investigate the stability and simple operation of the indium solder joints, this embodiment omits the preparation of the silicon dioxide dielectric layer and the cross-bridge structure, and only retains the hydrogen fluoride treatment process. The indium solder joints are directly prepared after the metal layer under the solder joints is prepared. Specifically, the indium solder joints are prepared on the metal layer under the solder joints by deposition method pattern transfer technology, wherein the deposition method adopts thermal evaporation coating. The indium solder joints are 16×16 μm 2 The thickness of the tetragonal column is 10 μm.
[0052] S205: Prepare a metal protective layer (capping layer), that is, Figure 3 and Figure 4 The metal protective layer U02a on the bottom wiring layer and the metal protective layer U02b on the top wiring layer in the embodiment of the present invention are shown in FIG. Specifically, the metal protective layer is prepared on the indium solder joint by a deposition method pattern transfer technology, wherein the deposition method adopts electron beam evaporation coating. The same metal as the UBM layer is used as the metal protective layer, and the thickness of the metal protective layer is 30nm, wherein the thickness of the Ti layer is 10nm.
[0053] S206: Hydrogen fluoride treatment, verify the protective effect of the metal protective layer on the indium solder joints through hydrogen fluoride treatment. Specifically, the bottom film wiring layer and the top film wiring layer formed with the metal protective layer are placed in hydrogen fluoride gas, the gas pressure can be selected to be 50-600mTorr, and the treatment time can be selected to be 5-60min. The specific parameters are adjusted according to your own needs. In this embodiment, the hydrogen fluoride gas pressure is selected to be 600mTorr, and the treatment time is 60min.
[0054] S207: Flip-chip welding: Use a placement machine to align and bond the metal protective layer on the bottom wiring layer and the metal protective layer on the top wiring layer, and perform welding. The welding temperature is 100°C.
[0055] S208: Packaging: packaging the soldered chip into a printed circuit board (PCB) sample box by wire bonding.
[0056] Testing and Characterization:
[0057] The superconducting quantum chip obtained in the above embodiment is subjected to relevant tests and characterizations.
[0058] In order to detect the effect of hydrogen fluoride treatment on indium solder joints, the substrate wiring layer prepared with indium solder joints was treated with hydrogen fluoride, and the elements on the surface of the indium solder joints were analyzed by X-ray photoelectron spectroscopy (XPS).
[0059] Figure 7 is the X-ray photoelectron spectrum of the surface of the indium solder joint in Example 1 of the present invention, Figure 8 This is an X-ray photoelectron spectrum of the surface of the indium solder joint after hydrogen fluoride treatment in Example 1 of the present invention.
[0060] like Figure 7 and Figure 8 As shown in the figure, after hydrogen fluoride treatment, O1s (OH) on the surface of the indium solder joint increased significantly, while O1s (O-In) decreased relatively. O1s represents the 1s electron orbit of the oxygen atom, (OH) represents the chemical bond between the oxygen atom and the hydrogen atom, and (O-In) represents the chemical bond between the oxygen atom and the indium atom. The characterization results show that the chemical bonds between the oxygen atoms and the hydrogen atoms on the surface of the indium solder joint increased, while the chemical bonds between the oxygen atoms and the indium atoms decreased, which means that the composition of the oxide layer on the surface of the indium solder joint has changed.
[0061] The indium solder joints covered with the metal protection layer in the above embodiment were scanned using a scanning electron microscope (SEM).
[0062] Fig. 9 This is a scanning electron microscope image of an indium solder joint covered with a metal protective layer in Example 1 of the present invention.
[0063] like Fig. 9 As shown in the figure, the indium solder joint is covered with a 30nm thick Ti / Au metal protective layer, which can cover the entire upper surface of the indium solder joint. There is leakage in a small local area, but the impact is not serious. If the metal protective layer is too thin, it will not be able to form a good protection for the upper surface of the indium solder joint, and it will not be able to suppress the change of the oxide layer on the surface of the indium solder joint. At the same time, due to the large surface roughness of the indium solder joint, if the metal protective layer is too thin, some areas of the indium solder joint will be exposed. In the figure above, the thickness of the metal protective layer is relatively extreme, and a small part of the indium solder joint area has been exposed.
[0064] Furthermore, in order to detect the firmness of the indium solder joints after flip-chip bonding, the solder joints were manually pulled apart after flip-chip bonding and scanned using a scanning electron microscope (SEM).
[0065] Fig.10 This is a scanning electron microscope image of the manually unplugged weld in Example 1 of the present invention.
[0066] like Fig.10 As shown in the figure, after flip-chip welding, the welding joint is manually pulled apart, and it can be seen that there is obvious "wire pulling" phenomenon at the welding joint, indicating that the flip-chip welding is relatively firm.
[0067] Furthermore, in order to detect the protective effect of the metal protective layer on the indium solder joints, the stability test of the superconducting quantum chip was carried out. The specific test process is: connect all ports of the superconducting quantum chip to the DC current signal, test the on-off in the dilution refrigerator, and perform three temperature rise and fall cycles, that is, cool down from 295K to 12mK, and then heat up to 295K, and cycle three times. No circuit breakage was found. Since the indium solder joints are superconducting at low temperatures, the total resistance of the indium solder joints in the superconducting quantum chip is much smaller than the resistance in the measurement circuit. The resistance can no longer be measured using the 4-terminal method. Therefore, the resistance change of the superconducting quantum chip during the low-temperature cycle is tested using the 2-terminal method, that is, two wires are used to connect the two ends of the superconducting quantum chip, and the resistance value is calculated by measuring the voltage and current between the two ends.
[0068] Fig.11 This is a diagram showing the resistance change of the superconducting quantum chip during the cooling process in Example 1 of the present invention.
[0069] like Fig.11 As shown in the figure, the solid line in the figure is the resistance of the measurement circuit itself, and the dotted line in the figure is the resistance change caused by the superconducting quantum chip due to cooling during the test. From the figure, the superconducting transformation process of the superconducting quantum chip during the cooling process can be clearly observed.
[0070] Fig.12 This is a diagram showing the resistance change of the indium solder joint of the superconducting quantum chip at room temperature in Example 1 of the present invention.
[0071] like Fig.12 As shown, as the number of indium solder joints increases, the resistance changes linearly, which means that after flip-chip bonding, all 800 indium solder joints on the bottom wiring layer and the top wiring layer are connected.
[0072] Fig.13 This is a graph showing the resistance change of the indium solder joint of the superconducting quantum chip at 12mK in Example 1 of the present invention.
[0073] like Fig.13 As shown in the figure, as the number of indium solder joints increases, the resistance changes irregularly. This is because the resistance of the indium solder joint itself is small at 12mK, and the overall resistance of the superconducting quantum chip is also small. Therefore, as the number of indium solder joints increases, the resistance of the superconducting quantum chip changes less, and the measured resistance at this time is the resistance of the measurement circuit.
[0074] In summary, the indium solder joints were protected by a metal protective layer and flip-chip soldered after hydrogen fluoride treatment. The superconducting quantum chip after soldering did not show any disconnection of the solder joints after multiple low-temperature cycles. At the same time, the chip spacing after flip-chip soldering did not change after multiple temperature rise and fall cycles, which confirmed the result that all the indium solder joints were connected.
[0075] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for protecting solder joints in a superconducting quantum flip-chip, characterized in that: include: Providing a first chip and a second chip, wherein corresponding surfaces of the first chip and the second chip are respectively deposited with under solder joint metal layers; Preparing a silicon dioxide dielectric layer and a crossover structure on the first chip; Forming indium solder joints respectively on the under-solder joint metal layer of the first chip having the crossover structure and the under-solder joint metal layer of the second chip; forming a metal protection layer on the indium solder joints of the first chip; Performing hydrogen fluoride treatment on the first chip formed with the metal protection layer to remove the silicon dioxide dielectric layer; Aligning and bonding the upper and lower patterns of the first chip treated with hydrogen fluoride and the second chip with indium solder joints, and performing flip-chip welding to obtain a superconducting quantum flip-chip welding chip; Wherein, the material of the metal protective layer includes any one of Ti / Au, Pt / Au, and TiN, and the thickness of the metal protective layer is 30-300nm.
2. The method according to claim 1, characterized in that The method further includes: forming a metal protection layer on the indium solder joints of the second chip.
3. The method according to claim 1 or 2, characterized in that: The material of the metal layer under the solder joint includes any one of Ti / Au, Pt / Au and TiN.
4. The method according to claim 3, characterized in that The metal protection layer has the same lateral dimension as the indium solder joint, and the thickness of the indium solder joint is 5-20 μm.
5. The method according to claim 4, characterized in that The side length ratio of the metal layer under the solder joint to the indium solder joint is 1.5-3:1, and the thickness of the metal layer under the solder joint is 100-300nm.
6. The method according to claim 1 or 2, characterized in that: The metal protection layer is deposited on the indium solder joint by a deposition method pattern transfer technology; Wherein, the deposition method in the deposition pattern transfer technology includes any one of electron beam evaporation coating, thermal evaporation coating, and magnetron sputtering.
7. The method according to claim 1 or 2, characterized in that: After the first chip and the second chip are aligned and bonded to each other for flip-chip welding, the method further includes: packaging the superconducting quantum flip-chip welding chip.
8. The method according to claim 7, characterized in that After the packaging, the method further comprises: performing a stability test on the superconducting quantum flip-chip; Wherein, the stability test includes multiple temperature rise and fall cycles; The temperature rise and fall cycle includes: cooling from 295K to 12mK, and then heating to 295K.
9. A superconducting quantum chip, characterized in that: Prepared by the method described in any one of claims 1 to 8.
Citation Information
Patent Citations
Chip packaging structure and packaging method
CN116936488A