A cell membrane coating with a pit-shaped topological structure and its preparation method and application

Using ultrasonic spraying to construct a cell membrane coating with a pit-like topology solves the problems of large consumption of cell membrane materials and poor stability, improves biocompatibility and anticoagulant properties, and promotes cell adhesion and growth.

CN118557814BActive Publication Date: 2024-10-18SICHUAN UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411047495.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-10-18
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

The existing cell membrane coating assembly process consumes a lot of materials and has poor stability, and it is difficult to realize topological functionalization of the two-dimensional planar structure, which affects cell adhesion, proliferation and differentiation behaviors.

Method used

The ultrasonic spraying method is used to construct a cell membrane coating with a pit-like topology. Through the mixing of cell membrane vesicle suspension and cross-linking agent and ultrasonic spraying technology, ultrafine droplets are formed to impact the coating surface, generating approximately 2-20 μm The pit structure enhances the interface area and mechanical signal stimulation.

Benefits of technology

Low-cost and simple coating preparation is achieved, which retains biological functions, enhances anticoagulant properties and biocompatibility, promotes cell adhesion and growth, and affects cell morphology, differentiation, and proliferation behaviors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118557814B_ABST
    Figure CN118557814B_ABST
Patent Text Reader

Abstract

The present invention discloses a cell membrane coating with a pit-shaped topological structure, a preparation method and an application, and belongs to the technical field of biomedical materials. The present invention first prepares a cell membrane vesicle suspension, and then uses ultrasonic atomization spraying equipment to spray the surface of a substrate material to obtain a cell membrane coating with a pit-shaped topological structure. The preparation method of the cell membrane coating of the present invention is simple and versatile. It not only retains the anti-coagulant properties and good biocompatibility of the cell membrane coating, but also further gives the coating topological structure-guided cell behaviors, such as cell adhesion, proliferation, migration and differentiation. It can be used to prepare blood-contact materials / devices, such as vascular stents, heart occluders, artificial heart valves, artificial blood vessels and other cardiovascular implants and interventional devices, as well as cardiopulmonary circulation circuits and intravenous catheters for dialysis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of biomedical materials, and in particular to a cell membrane coating with a pit-shaped topological structure and a preparation method and application thereof. Background Art

[0002] The cell membrane-derived top-down modification strategy makes full use of the functional properties of the natural membrane interface, giving the material surface good anti-fouling properties, immunomodulatory functions and good biocompatibility. At present, cell membrane-derived bionic coatings have been widely used for surface coating and targeted delivery of drug-loaded nanoparticles, and have great potential in the fields of drug delivery, bioimaging, cancer immunotherapy and detoxification. In addition, studies have explored the use of cell membrane-derived bionic coatings for surface modification of macroscopic implant devices, such as vascular stents, dental implants, and decellularized extracellular matrix scaffolds. However, the current coating assembly process relying on drip coating and dip coating consumes a large amount of cell membrane materials and has poor coating stability. At the same time, the cell membrane coatings prepared on the macroscopic surface are generally two-dimensional planar structures, and it is difficult to achieve the topological structure functionalization of the coating surface by simple methods to enhance the adhesion, proliferation and differentiation of cells on the surface. Summary of the invention

[0003] In order to solve the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a cell membrane coating with a pit-like topological structure and a preparation method and application thereof, so as to solve the problems of large consumption of cell membrane materials and poor coating stability in the existing coating assembly process.

[0004] The technical solution of the present invention to solve the above technical problem is as follows: a method for preparing a cell membrane coating having a pit-shaped topological structure is provided, comprising the following steps:

[0005] (1) extracting and separating cells, resuspending them, and then breaking the cells, collecting cell membrane fragments after washing, resuspending the cell membrane fragments and performing ultrasonication to obtain a cell membrane vesicle suspension;

[0006] (2) mixing the cell membrane vesicle suspension with a cross-linking agent to obtain a cell membrane vesicle mixed solution;

[0007] (3) adding the cell membrane vesicle mixed solution into the syringe of the ultrasonic atomization spraying equipment, performing a first ultrasonic spraying on the surface of the substrate material, and then cleaning the surface of the substrate material after the spraying;

[0008] (4) performing a second ultrasonic spraying of the surface of the substrate material obtained in step (3) with an impact solution;

[0009] (5) Drying and solidifying the cell membrane coating obtained in step (4) to obtain.

[0010] Furthermore, in step (1), the cells are at least one of red blood cells, platelets, macrophages, neutrophils and T lymphocytes; and the protein concentration of the cell membrane vesicle suspension is 0.5-8 mg / mL.

[0011] Furthermore, in step (2), the cross-linking agent is at least one of a polyphenol compound, a carbodiimide compound, glutaraldehyde and genipin; and the mass ratio of the cell membrane vesicle suspension to the cross-linking agent is 1-20:1.

[0012] Furthermore, the polyphenol compound is pyrogallol, tannic acid or epigallocatechin gallate.

[0013] Furthermore, the carbodiimide compound is carbodiimide hydrochloride or N-cyclohexyl-N'-(2-morpholinoethyl)carbodiimide methyl p-toluenesulfonate.

[0014] Furthermore, the ultrasonic spraying in step (3) includes the following steps: controlling the distance between the nozzle and the surface of the substrate material to be 2-10 cm, and then spraying 20-100 layers on the surface of the substrate material at an ultrasonic frequency of 25-250 kHz, an ultrasonic power of 0.5-10 W, a solution propulsion rate of 0.01-0.1 mL / min and a gas pressure of 0.5-1 psi.

[0015] Furthermore, the shock solution in step (4) is deionized water, phosphate buffer or physiological saline.

[0016] Furthermore, the ultrasonic spraying in step (4) includes the following steps: controlling the distance between the nozzle and the surface of the substrate material to be 2-10 cm, and then spraying 1-100 layers on the surface of the substrate material at an ultrasonic frequency of 25-250 kHz, an ultrasonic power of 0.5-10 W, a solution propulsion rate of 0.01-0.1 mL / min and a gas pressure of 1-3 psi.

[0017] Furthermore, in step (3) and step (4), the substrate materials are metal-based biomaterials, polymer-based biomaterials or decellularized biological tissues.

[0018] Furthermore, in step (5), the drying and curing temperature is 30-60°C and the time is 10-60 min.

[0019] The present invention provides a cell membrane coating with a pit-shaped topological structure, which is prepared by adopting the above-mentioned preparation method.

[0020] The present invention also provides an application of a cell membrane coating having a pit-shaped topological structure in the preparation of cardiovascular materials / devices.

[0021] Furthermore, the blood contact material / device is a cardiopulmonary circulation circuit, a dialysis intravenous catheter, a vascular stent, a heart occluder, an artificial heart valve or an artificial blood vessel.

[0022] The present invention has the following beneficial effects:

[0023] (1) The present invention uses ultrasonic spraying to construct a cell membrane coating with a pit-shaped topological structure, which has the advantages of simple method, strong versatility and low cost. There is no need to etch the surface of the substrate in advance, avoiding harsh and expensive photoetching, plasma etching and other technologies, reducing costs and increasing the selectivity of the substrate.

[0024] (2) The present invention utilizes the difference in rigidity before and after cross-linking of the cell membrane coating, and uses ultrafine droplets generated by ultrasonic spraying to impact the coating surface to obtain a cell membrane coating with a pit-shaped topological structure. This method completely retains the biological function of the cell membrane coating and enhances the anti-coagulation performance and biocompatibility of the material.

[0025] (3) By utilizing the impact of ultrafine droplets generated by ultrasonic spraying, a pit-like structure of about 2-20 μm can be generated on the surface of the cell membrane coating, and as the number of impacts increases, the height of the pit structure changes from nanoscale (80 nm) to submicron (600 nm). The cell membrane coating with a pit-like topological structure expands the interface area and can effectively enhance the adhesion and growth of cells on the surface. At the same time, the adhered cells are stimulated by the enhanced mechanical signals on the surface of the pit-like topological structure coating, and the cytoskeleton transmits the force from the membrane to the cell nucleus, directly affecting the expression of genes and proteins through complex biological pathways, thereby affecting cell morphology, differentiation and proliferation behavior. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a schematic diagram of the preparation process of the cell membrane coating with a pit-shaped topological structure of the present invention;

[0027] Figure 2 The scanning electron microscope images are of the cell membrane coatings prepared from the naked polylactic acid substrate, the comparative example and Examples 1-2; wherein, Figure A is the naked polylactic acid substrate; Figure B is the cell membrane coating prepared from the comparative example; Figure C is the cell membrane coating prepared from Example 1; and Figure D is the cell membrane coating prepared from Example 2;

[0028] Figure 3 Fluorescence staining images of platelet adhesion of naked polylactic acid substrates, comparative examples, and polylactic acid substrates modified with cell membrane coatings prepared in Examples 1-2; wherein, Figure A is a naked polylactic acid substrate; Figure B is a polylactic acid substrate modified with cell membrane coatings prepared in the comparative example; Figure C is a polylactic acid substrate modified with cell membrane coatings prepared in Example 1; and Figure D is a polylactic acid substrate modified with cell membrane coatings prepared in Example 2;

[0029] Figure 4 These are fluorescence staining images of endothelial cells of naked polylactic acid substrate, comparative example and polylactic acid substrate modified with cell membrane coating prepared in Examples 1-2; wherein, Figure A is a naked polylactic acid substrate; Figure B is a polylactic acid substrate modified with cell membrane coating prepared in the comparative example; Figure C is a polylactic acid substrate modified with cell membrane coating prepared in Example 1; and Figure D is a polylactic acid substrate modified with cell membrane coating prepared in Example 2. DETAILED DESCRIPTION

[0030] The principles and features of the present invention are described below in conjunction with the examples, which are only used to explain the present invention and are not intended to limit the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.

[0031] The preparation method of the cell membrane coating with topological structure of Examples 1-4 is as follows Figure 1 shown.

[0032] Example 1

[0033] A method for preparing a cell membrane coating having a pit-shaped topological structure comprises the following steps:

[0034] (1) Whole blood was centrifuged to obtain red blood cells, which were washed three times with PBS solution and resuspended in pre-cooled 0.25× PBS solution (containing 0.5 mM EDTA, 0.1 mM PMSF) and placed in a 4°C refrigerator for 2 h. The solution was centrifuged at 10,000 g for 20 min, the supernatant was discarded and washed three times with PBS solution, and finally resuspended and sonicated to obtain a milky white red blood cell membrane vesicle suspension, where the protein concentration of the cell membrane vesicle suspension was 4 mg / mL;

[0035] (2) mixing the cell membrane vesicle suspension obtained in step (1) with an aqueous solution of 2 mg / mL EGCG in equal volumes to prepare a cell membrane vesicle mixed solution;

[0036] (3) Add the cell membrane vesicle mixed solution obtained in step (2) into a gas-tight syringe, adjust the nozzle to 5 cm away from the surface of the polylactic acid substrate, and spray it layer by layer on the surface of the cleaned substrate material at an ultrasonic frequency of 120 kHz, an ultrasonic power of 1 W, and a gas pressure of 1 psi, wherein the propulsion rate of the cell membrane vesicle mixed solution is 0.03 mL / min, spray 40 layers, and rinse with deionized water 3 times;

[0037] (4) Replace the cell membrane vesicle mixed solution with deionized water and add it to the airtight syringe of the ultrasonic atomization spraying equipment. Adjust the nozzle to 5 cm away from the material surface and spray it layer by layer on the material surface at an ultrasonic frequency of 120 kHz, an ultrasonic power of 1 W, and a gas pressure of 3 psi. The propulsion rate of the deionized water solution is 0.01 mL / min, and 3 layers are sprayed.

[0038] (5) The cell membrane coating obtained in step (4) was dried and cured at 40°C for 30 min to obtain a cell membrane coating with a pit-like topological structure, the electron microscopy image of which is shown in FIG. Figure 2 As shown in Figure C. Figure 2 As shown in Figure C, randomly distributed pit-like structures are formed on the surface of the cell membrane coating prepared in this example, with a diameter of 2-20 μm and a pit depth of 80 nm.

[0039] Example 2

[0040] A method for preparing a cell membrane coating having a pit-shaped topological structure comprises the following steps:

[0041] (1) Whole blood was centrifuged to obtain red blood cells, which were washed three times with PBS solution and resuspended in pre-cooled 0.25× PBS solution (containing 0.5 mM EDTA and 0.1 mM PMSF protease inhibitor), placed in a 4°C refrigerator for 2 hours, and then centrifuged at 10,000 g for 20 min. The supernatant was discarded and washed three times with PBS solution. Finally, a milky white red blood cell membrane vesicle suspension was obtained after resuspending and sonication. The protein concentration of the red blood cell membrane vesicle suspension was 4 mg / mL.

[0042] (2) mixing the cell membrane vesicle suspension obtained in step (1) with a 2 mg / mL EGCG-containing Tris-HCl buffer solution (50 mM, pH = 8.5) in equal volumes to prepare a cell membrane vesicle mixed solution;

[0043] (3) Add the cell membrane vesicle mixed solution obtained in step (2) into a gas-tight syringe, adjust the nozzle to 5 cm away from the surface of the polylactic acid substrate, and spray it layer by layer on the surface of the cleaned substrate material at an ultrasonic frequency of 120 kHz, an ultrasonic power of 1 W, and a gas pressure of 1 psi, wherein the propulsion rate of the cell membrane vesicle mixed solution is 0.03 mL / min, spray 100 layers, and rinse with deionized water 3 times;

[0044] (4) Replace the cell membrane vesicle mixed solution with deionized water and add it to the gas-tight syringe. Adjust the nozzle to 5 cm away from the material surface and spray it layer by layer on the material surface at an ultrasonic frequency of 120 kHz, an ultrasonic power of 1 W, and a gas pressure of 3 psi. The propulsion rate of the deionized water solution is 0.01 mL / min, and 50 layers are sprayed.

[0045] (5) The cell membrane coating obtained in step (4) was dried and cured at 40°C for 30 min to obtain a cell membrane coating with a pit-like topological structure, the electron microscope scanning image of which is shown in FIG. Figure 2 As shown in Figure D. Figure 2 As can be seen from Figure D, the depth of the pit-like structure further increases to the submicron level (600 nm), and the diameter of the pit-like structure is 5-10 μm.

[0046] Example 3

[0047] A method for preparing a cell membrane coating having a pit-shaped topological structure comprises the following steps:

[0048] (1) Whole blood was centrifuged to obtain platelets, which were then resuspended in a PBS solution containing 1 mM EDTA. Protease inhibitors were then added and the platelets were repeatedly frozen and thawed three times. The platelet membrane vesicle suspension was obtained by washing, resuspending and sonicating three times in sequence. The protein concentration of the platelet membrane vesicle suspension was 2 mg / ml.

[0049] (2) mixing the cell membrane vesicle suspension obtained in step (1) with a 0.5 mg / ml EGCG-containing Tris-HCl buffer solution (50 mM, pH = 8.5) in equal volumes to prepare a cell membrane vesicle mixed solution;

[0050] (3) Add the cell membrane vesicle mixed solution obtained in step (2) into a gas-tight syringe, adjust the nozzle to 5 cm away from the surface of the titanium foil material, and spray it layer by layer on the surface of the cleaned substrate material at an ultrasonic frequency of 120 kHz, an ultrasonic power of 1.5 W, and a gas pressure of 1 psi. The propulsion rate of the cell membrane vesicle mixed solution is 0.02 mL / min. Spray 50 layers and rinse with deionized water 3 times.

[0051] (4) Replace the cell membrane vesicle mixed solution with deionized water and add it to the gas-tight syringe. Adjust the nozzle to 5 cm away from the surface of the titanium foil material, and spray it layer by layer on the surface of the material at an ultrasonic frequency of 120 kHz, an ultrasonic power of 1 W, and a gas pressure of 3 psi. The propulsion rate of the deionized water solution is 0.01 mL / min, and 3 layers are sprayed.

[0052] (5) The cell membrane coating obtained in step (4) is dried and cured at 40°C for 30 min to obtain a cell membrane coating with a pit-like topological structure. Randomly distributed pit-like structures are formed on the surface of the coating, with a diameter of 2-20 μm and a pit depth of 80 nm.

[0053] Example 4

[0054] A method for preparing a cell membrane coating having a pit-shaped topological structure comprises the following steps:

[0055] (1) The collected neutrophils were resuspended in 0.25× PBS buffer solution (containing 0.5 mM EDTA and 0.1 mM PMSF) and homogenized 30 times using a glass homogenizer. The subcellular organelles were removed by multiple gradient centrifugation. The precipitate was resuspended in PBS solution and then ultrasonicated to obtain a neutrophil vesicle suspension, wherein the protein concentration of the neutrophil membrane vesicle suspension was 1.5 mg / mL;

[0056] (2) mixing the cell membrane vesicle suspension obtained in step (1) with an aqueous solution of 1 mg / mL EGCG in equal volumes to prepare a cell membrane vesicle mixed solution;

[0057] (3) Add the cell membrane vesicle mixed solution obtained in step (2) into a gas-tight syringe, adjust the nozzle to 3.5 cm away from the surface of the decellularized bovine pericardium material, and spray it layer by layer on the surface of the cleaned substrate material at an ultrasonic frequency of 120 kHz, an ultrasonic power of 1.4 W, and a gas pressure of 1 psi. The propulsion rate of the cell membrane vesicle mixed solution is 0.02 mL / min, and 100 layers are sprayed. Rinse with deionized water three times;

[0058] (4) Replace the cell membrane vesicle mixed solution with deionized water and add it to the airtight syringe of the ultrasonic atomization spraying equipment. Adjust the nozzle to 5 cm away from the surface of the bovine pericardium material. Spray it layer by layer on the surface of the material at an ultrasonic frequency of 120 kHz, an ultrasonic power of 1.4 W, and a gas pressure of 3 psi. The propulsion rate of the deionized water solution is 0.01 mL / min, and 50 layers are sprayed.

[0059] (5) The cell membrane coating obtained in step (4) is dried and cured at 40°C for 30 min to obtain a cell membrane coating having a pit-like topological structure. The depth of the pit-like structure is further increased to the submicron level (600 nm), and the size of the pit-like structure is 5-10 μm.

[0060] Comparative Example

[0061] A method for preparing a polyphenol cross-linked cell membrane coating comprises the following steps:

[0062] (1) Whole blood was centrifuged to obtain red blood cells, which were washed three times with PBS solution and resuspended in pre-cooled 0.25× PBS solution (containing 0.5 mM EDTA and 0.1 mM PMSF) and placed in a 4°C refrigerator for 2 h. The solution was centrifuged at 10,000 g for 20 min, the supernatant was discarded and washed three times with PBS solution, and finally resuspended and sonicated to obtain a milky white red blood cell membrane vesicle suspension, where the protein concentration of the red blood cell membrane vesicle suspension was 4 mg / mL;

[0063] (2) mixing the cell membrane vesicle suspension obtained in step (1) with an aqueous solution of 2 mg / mL EGCG in equal volumes to prepare a cell membrane vesicle mixed solution;

[0064] (3) The cell membrane vesicle mixed solution obtained in step (2) was added to a gas-tight syringe, and the nozzle was adjusted to 5 cm away from the surface of the polylactic acid substrate. The mixed solution was sprayed layer by layer on the surface of the cleaned substrate material at an ultrasonic frequency of 120 kHz, an ultrasonic power of 1 W, and a gas pressure of 1 psi. The propulsion rate of the mixed solution of cell membrane vesicles was 0.03 mL / min. 40 layers were sprayed and washed with deionized water for 3 times to obtain a polyphenol cross-linked red blood cell membrane coating. The electron microscope scanning image is shown in FIG. Figure 2 As shown in Figure B, the coating surface is smooth and no excess cell membrane vesicles are adsorbed on the surface.

[0065] Test Example 1 Platelet Adhesion Test

[0066] The bare polylactic acid substrate, the polylactic acid substrate modified with the erythrocyte membrane coating of the pit-shaped topology obtained in Example 1-2, and the polylactic acid substrate modified with the polyphenol cross-linked erythrocyte membrane coating obtained in the comparative example were mixed with platelet-rich plasma, respectively, and incubated at 37°C for 1 h. After the incubation, the incubated polylactic acid substrate was washed 3 times with PBS solution, and the adhesion of platelets was observed under a fluorescence microscope by fluorescence staining. The results are as follows: Figure 3 shown.

[0067] Depend on Figure 3 It can be seen that compared with the naked polylactic acid substrate and the polyphenol cross-linked erythrocyte membrane coating modified polylactic acid substrate obtained in the comparative example (see Figure 3 Figures A and B in the figure), the platelets adhered to the surface of the polylactic acid substrate modified with the red blood cell membrane coating with the pit-like topological structure obtained in Example 1-2 were significantly reduced (see Figure 3 C and D in the figure). The erythrocyte membrane coating with the pit-like topological structure obtained in Example 1-2 inherits the natural anticoagulant property of the erythrocyte membrane coating cross-linked with polyphenol in the comparative example, indicating that the introduction of the pit-like topological structure does not change the good biocompatibility of the coating.

[0068] Experimental Example 2 Endothelial cell adhesion assay

[0069] The bare polylactic acid substrate, the polylactic acid substrate modified with the erythrocyte membrane coating of the pit-shaped topology obtained in Example 1-2, and the polylactic acid substrate modified with the polyphenol cross-linked erythrocyte membrane coating obtained in the comparative example were co-cultured with endothelial cells in a 37°C, 5% CO2 incubator for 1 day, and the adhesion of the endothelial cells and the differences in cell morphology were observed and compared by fluorescent staining. The results are as follows: Figure 4 shown.

[0070] Depend on Figure 4 It can be seen that compared with the naked polylactic acid substrate and the polyphenol cross-linked erythrocyte membrane coating modified polylactic acid substrate obtained in the comparative example (see Figure 4 A and B in the figure), the surface of the polylactic acid substrate modified with the erythrocyte membrane coating with the pit-like topological structure obtained in Example 1-2 has good biological activity, promoting the adhesion and growth of more endothelial cells on the surface (see Figure 4 C and D in the middle). The number of endothelial cells adhering to the erythrocyte membrane coating with the pit-shaped topology structure obtained in Example 1-2 increased significantly, and the cells on the coating surface had a significantly expanded morphology, indicating that the pit-shaped topology structure affected the adhesion state of the cells on the surface, which may promote the diffusion and migration of cells on the surface of the cell membrane coating with the pit-shaped topology structure.

[0071] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a cell membrane coating having a pit-like topological structure, characterized in that: The following steps are involved: (1) extracting and separating cells, resuspending them, and then breaking the cells, collecting cell membrane fragments after washing, resuspending the cell membrane fragments and performing ultrasonication to obtain a cell membrane vesicle suspension; (2) mixing the cell membrane vesicle suspension with a cross-linking agent to obtain a cell membrane vesicle mixed solution; (3) adding the cell membrane vesicle mixed solution into the syringe of the ultrasonic atomization spraying equipment, performing a first ultrasonic spraying on the surface of the substrate material, and then cleaning the surface of the substrate material after the spraying; (4) performing a second ultrasonic spraying of the surface of the substrate material obtained in step (3) with an impact solution; (5) Drying and solidifying the cell membrane coating obtained in step (4) to obtain.

2. The method for preparing a cell membrane coating having a pit-like topological structure according to claim 1, characterized in that: The cells in step (1) are at least one of red blood cells, platelets, macrophages, neutrophils and T lymphocytes; and the protein concentration of the cell membrane vesicle suspension is 0.5-8 mg / mL.

3. The method for preparing a cell membrane coating having a pit-like topological structure according to claim 1, characterized in that: In step (2), the cross-linking agent is at least one of a polyphenol compound, a carbodiimide compound, glutaraldehyde and genipin; and the mass ratio of the cell membrane vesicle suspension to the cross-linking agent is 1-20:

1.

4. The method for preparing a cell membrane coating having a pit-shaped topological structure according to claim 1, characterized in that: Ultrasonic spraying in step (3) The method comprises the following steps: controlling the distance between the nozzle and the surface of the substrate material to be 2-10 cm, and then spraying 20-100 layers on the surface of the substrate material at an ultrasonic frequency of 25-250 kHz, an ultrasonic power of 0.5-10 W, a solution advancing rate of 0.01-0.1 mL / min, and a gas pressure of 0.5-1 psi.

5. The method for preparing a cell membrane coating having a pit-shaped topological structure according to claim 1, characterized in that: The shock solution in step (4) is deionized water, phosphate buffer or physiological saline.

6. The method for preparing a cell membrane coating having a pit-shaped topological structure according to claim 1, characterized in that: Ultrasonic spraying in step (4) The method comprises the following steps: controlling the distance between the nozzle and the surface of the substrate material to be 2-10 cm, and then spraying 1-100 layers on the surface of the substrate material at an ultrasonic frequency of 25-250 kHz, an ultrasonic power of 0.5-10 W, a solution advancing rate of 0.01-0.1 mL / min and a gas pressure of 1-3 psi.

7. The method for preparing a cell membrane coating having a pit-shaped topological structure according to claim 1, characterized in that: The substrate materials in step (3) and step (4) are metal-based biomaterials, polymer-based biomaterials or decellularized biological tissues.

8. The method for preparing a cell membrane coating having a pit-like topological structure according to claim 1, characterized in that: The drying and curing temperature in step (5) is 30-60°C and the time is 10-60 min.

9. A cell membrane coating having a pit-like topological structure, characterized in that: The method is prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the cell membrane coating with a pit-like topological structure as claimed in claim 9 in the preparation of cardiovascular materials / devices.

Citation Information

Patent Citations

  • Medical device coated with a bioactive agent

    CA2484383A1

  • Transgenic cell overlapped vascular inner rack and manufacture method thereof