A method for producing an ingot of silicon material for CZ-type single crystal

Through the DSS directional solidification method and silicon nitride spray coating technology, combined with high-temperature slow cooking melting and flotation treatment, the problem of high impurities and low yield in Czochralski N-type single crystal silicon material has been solved, and high-purity silicon material has been prepared. Excellent properties of resistivity and minority carrier lifetime are achieved, reducing production costs.

CN118563411BActive Publication Date: 2024-10-15内蒙古上航新能源有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411050609.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-10-15
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

The existing technology is difficult to meet the high purity and low impurity requirements of Czochralski N-type single crystal silicon materials, resulting in problems such as high impurity ratio, low yield, high cost, and poor quality.

Method used

The DSS directional solidification ingot casting process is combined with silicon nitride spray coating and high-temperature slow-cooking and melting processes to process the original polycrystalline powder silicon material through cleaning and flotation to remove impurities such as iron, chromium, nickel, copper and zinc, and prepare N-type single crystal. Standard silicone material is used.

Benefits of technology

It has achieved high purity of silicon material, and its resistivity and minority carrier lifetime indicators have reached excellent standards. It can replace native polycrystalline silicon material and be used as a high-quality raw material for Czochralski N-type single crystal silicon rods, reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118563411B_ABST
    Figure CN118563411B_ABST
Patent Text Reader

Abstract

The invention discloses a method for producing an ingot of silicon material for CZ-N type single crystal, comprising the following steps S11: cleaning and treating the original polycrystalline powder silicon material; S12: loading the original polycrystalline powder silicon material and granular silicon obtained in step S11 into a quartz crucible sprayed with a silicon nitride coating; S13: placing the quartz crucible in step S12 into an ingot casting furnace and purifying it by using a DSS directional solidification ingot casting process; S14: squaring to form a rough square ingot of a rectangular shape; S15: removing impurities and removing the head and tail to obtain a sub-finished product; S16: cleaning and crushing to form a block material with a specification of 3 to 50 mm, namely, the silicon material for N type single crystal. The preparation method of the invention is simple, and the resistivity of the prepared silicon material square ingot for N type single crystal is greater than 3Ω·cm at the head and greater than 20Ω·cm at the tail, and the minority carrier lifetime average is greater than or equal to 15μs, and the original polycrystalline silicon material can be replaced and used as the silicon material for CZ-N type single crystal.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of silicon materials, and in particular to a method for producing an ingot of silicon material for a CZ-type single crystal. Background Art

[0002] There are two types of Czochralski single crystal products: P-type single crystal and N-type single crystal. Since the TOPCon cell of N-type single crystal has higher photoelectric conversion efficiency and long-term stability, Czochralski N-type single crystal is the mainstream product in the current Czochralski single crystal industry. However, N-type single crystal also has higher quality requirements on technical indicators such as the acceptor impurity boron and total metal impurity content in the silicon material.

[0003] Czochralski N-type single crystal refers to N-type semiconductor single crystal material grown by Czochralski method (CZ method for short). This preparation technology is widely used in the semiconductor industry, especially in the manufacture of solar cells and electronic devices.

[0004] The main applications of CZ-type N-type single crystals are in the following areas:

[0005] 1. Solar cells: N-type monocrystalline silicon, especially N-type monocrystalline silicon using advanced doping technology and anti-reflective coating, is widely used in the production of high-efficiency solar cells due to its high efficiency and long life.

[0006] 2. Electronic devices: N-type single crystal silicon is also one of the basic materials for electronic devices such as integrated circuits, power devices, sensors, etc., especially in high-performance applications that require high electron mobility and low noise.

[0007] 3. Special semiconductor materials: In addition to silicon, the Czochralski method can also be used to grow other types of N-type single crystal materials, such as gallium arsenide (GaAs), gallium nitride (GaN) and other compound semiconductors, which have important applications in optoelectronic devices, high-frequency electronic devices and other fields.

[0008] The CZ-pull N-type single crystal technology is one of the core technologies of the modern semiconductor industry and is of great significance for promoting the development of new energy, information technology and other fields. At present, the crushed blocks of primary polycrystalline dense rod-shaped silicon produced by the Siemens method (also known as re-feeding material) are the main raw materials for CZ-pull N-type single crystals, but the by-product of the crushing, the primary polycrystalline powder silicon material, cannot be used as silicon material for CZ-pull single crystals because of its small particle size and the presence of metal impurities and non-silicon impurities.

[0009] CN115787082A provides a method for casting a purified ingot for a single crystal, which includes a crucible charging method and a casting process control method. The single crystal purified ingot is mainly composed of block material, crushed material, fragments, and granular material. The block material is loaded in the middle and top cover of the crucible, and the crushed material, fragments, and granular material are loaded at the bottom and around the crucible; the casting process control method mainly controls the top and around the crucible to melt first and the bottom of the crucible to melt later by heating the top, side, and bottom of the crucible at the same time. Under the condition of complex material conditions, the purified ingot for single crystal can effectively increase the single furnace charging amount by more than 10% and control the risk of silicon leakage. This melting process formula heats the top / side / bottom at the same time, shortens the impact of high-temperature silicon liquid on the silicon nitride coating of the crucible, and can completely solve the risk of secondary solidification of the bottom silicon liquid. Impurities are discharged through silicon liquid convection, tumbling, argon gas circulation, etc., to solve the problems of high impurity ratio, low yield, high cost, and poor quality of purified ingot for single crystal. However, it still cannot meet the demand for N-type single crystal silicon materials. Summary of the invention

[0010] In view of the shortcomings of the prior art, the present invention provides a method for producing an ingot of silicon material for CZ-N type single crystal, comprising the following steps:

[0011] S11: After the original polycrystalline silicon powder is cleaned, the total content of five surface metal impurities of iron, chromium, nickel, copper and zinc is ≤20ppb;

[0012] S12: placing the raw polycrystalline silicon powder material and granular silicon obtained in step S11 into a quartz crucible sprayed with a silicon nitride coating;

[0013] S13: placing the quartz crucible in step S12 into an ingot casting furnace and purifying it by using a DSS directional solidification ingot casting process to cast and produce a crude silicon material for N-type single crystal;

[0014] S14: Squaring the crude N-type single crystal silicon material obtained in step S13 into a rough rectangular ingot;

[0015] S15: The rough ingot obtained in step S14 is subjected to comprehensive judgment based on the test results of minority carrier lifetime, resistivity, infrared flaw detection and carbon oxygen content, and then the unqualified parts at the head, tail and middle of the rough ingot are cut off. The remaining parts are ground and polished, and then infrared flaw detection is performed again. After the detected black spot impurities are cut off for the second time, a qualified N-type single crystal silicon material semi-finished product is obtained;

[0016] S16: The semi-finished N-type single crystal silicon material obtained in step S15 is cleaned and crushed into blocks with a size of 3-50 mm, i.e., N-type single crystal silicon material, which can be used as a raw material for CZ-pulled N-type single crystal silicon rods.

[0017] Furthermore, in the step S12, the quartz crucible sprayed with the silicon nitride coating is sprayed by a method comprising: pouring 800-1000g of silicon nitride powder, 2000-3000ml of deionized pure water, 300-400g of silica sol and 5-10g of polyvinyl alcohol binder into a measuring bucket and mixing them to prepare a silicon nitride spray solution; placing the measuring bucket with the prepared solution on a stirring table bracket, inserting an agitator and opening the pneumatic valve to start stirring, the stirring time is not less than 20 minutes, and the prepared silicon nitride solution needs to be in a stirring state all the time; lifting the qualified quartz crucible on the crucible heating table for heating, and starting the spraying operation when the temperature of the inner wall of the quartz crucible reaches 50°C-70°C. The spraying process includes spraying from a horizontal path and a longitudinal path. The sprayed crucible is pre-activated at 800°C for 2h, and then activated at 1000°C for 3h before use, which has a better effect and produces less impurities.

[0018] Furthermore, in the ingot casting process in step S13, a high-power rapid heating method is used in the heating stage, and a high-temperature slow cooking method is used in the melting stage to remove impurities efficiently. The specific process control method is as follows:

[0019] S21: Use power control mode to increase temperature in the heating stage. Maintain 98% high power and quickly increase temperature in the later stage of heating. When TC1 temperature reaches 1540℃, it will automatically jump to the first step of melting.

[0020] S22: In the first step of melting, the furnace pressure is controlled at 500 mbar. In the temperature control mode, TC1 is maintained at a high temperature of 1540°C to melt the silicon material in the crucible. When the power curve drops significantly and the temperature of the bottom TC2 rises rapidly, it is determined that all the silicon material in the crucible has been melted. Then, the process manually jumps to the last step of melting for rapid cooling, crystallization, and annealing. The crystallization temperature is 1400-1436°C, and the annealing temperature is 1370°C. Because the quartz crucible will undergo plastic deformation at 1200~1450℃ and has the high mechanical strength characteristics of structural ceramics above 1450℃, a high power of 98% is used for rapid heating during the heating stage, and the heating time from 1200~1540℃ is controlled within 3~4 hours. The temperature in the ingot casting furnace rises rapidly to accelerate the melting of the silicon material around the crucible into liquid, which can reduce the problem of black spot impurities caused by the top silicon material melting and flowing to the side wall during the heating stage and then squeezing the crucible due to secondary solidification at low temperature, the deformation of the crucible causing the silicon nitride coating to break, and the silicon nitride powder falling into the silicon liquid. Second, shorten the heating time. High temperature and slow cooking during the melting stage can reduce the agglomeration of impurities. With the convection of heat, the impurities in the silicon liquid are more easily discharged to the top of the liquid surface. Only during the directional solidification and crystallization can the impurities in the crystal be reduced, so as to meet the high standard requirement of impurity-free silicon ingots for N-type single crystal materials and improve the ingot casting yield.

[0021] Furthermore, the cleaning process in step S11 includes the following steps:

[0022] S31: Use a rotary sintering furnace to burn and remove organic matter such as wood chips, plastics and epoxy resin in the original polycrystalline powder silicon material. The temperature of the sintering furnace is controlled at about 700-800°C, and the silicon material is collected by rotating out from the discharge port;

[0023] S32: The silicon material obtained in step S31 is passed through a three-stage concentrator equipped with magnetic rollers to remove magnetic metal objects in the powdered material;

[0024] S33: Put the silicon material demagnetized in step S32 into a basket, and soak it in a mixed solution tank containing hydrofluoric acid, hydrochloric acid, an oxidant and a flotation agent for 40 to 60 minutes to remove the oxide film on the surface of the silicon material and make the silicon material float on the surface with strong hydrophobicity;

[0025] S34: Lift the flower basket and leave it empty for 2-3 minutes. After draining the soaking solution, pour the silicon material into the flotation tank. The powdered material will float on the water surface and flow downstream, while the impurities will sink to the bottom of the tank. Clean silicon material can be collected at the end of the flotation tank. The flotation recovery rate is >98%;

[0026] S35: The silicon material obtained in step S34 is rinsed with a slide shower device to remove the residual acid in the silicon material to make it neutral;

[0027] S36: putting the neutral silicon material obtained in step S35 into a spin dryer for drying, and then drying it in a constant temperature rotary drying furnace at a temperature of 400-500° C.;

[0028] S37: The silicon material dried in step S36 is passed through a three-stage concentrator equipped with magnetic rollers to remove magnetic metal objects in the powder and crushed materials again, so that the total content of five surface metal impurities (iron, chromium, nickel, copper and zinc) is ≤20ppb.

[0029] Furthermore, in step S33, the flotation agent is a mixture of sodium dodecyl sulfate and oleic acid, and the mass ratio thereof is 1:1.

[0030] Furthermore, in the step S33, the contents of hydrofluoric acid, hydrochloric acid, oxidant and flotation agent in the mixed solution are 0.5wt%, 0.2wt%, 0.3wt% and 0.1wt% respectively.

[0031] Furthermore, in the combustion process of step S31, pure oxygen is introduced for combustion. The use of pure oxygen for combustion can make the combustion more intense and the combustibles be removed more thoroughly.

[0032] Furthermore, in step S33, the oxidant is 27.5 wt % of one of hydrogen peroxide, percarbonic acid amide, and tert-butyl hydroperoxide.

[0033] Furthermore, the flower basket in step S33 is an acid corrosion resistant flower basket.

[0034] The preparation method of the present invention is simple, the process parameters are safe and feasible, the cost is low, the resistivity of the prepared N-type single crystal silicon material ingot is greater than 3Ω·cm at the head, greater than 20Ω·cm at the tail, the minority carrier lifetime average is ≥15μs, the performance is excellent, the original polycrystalline silicon material can be replaced, and it can be used as the silicon material for CZ-pull N-type single crystal. The prepared single crystal silicon rod can meet the quality standards in various indicators such as the minority carrier lifetime. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 The silicon material for N-type single crystal prepared in Example 2 of the present invention replaces the native polycrystalline silicon material and is used 100% as the silicon material for CZ-pulled N-type single crystal. The minority carrier lifetime mean data of the CZ-pulled N-type single crystal silicon rod are shown. DETAILED DESCRIPTION

[0036] The following is a clear and complete description of the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention.

[0037] It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention.

[0038] Example 1

[0039] A method for producing an ingot of silicon material for a CZ-type single crystal comprises the following steps:

[0040] S11: After the original polycrystalline silicon powder is cleaned, the total content of five surface metal impurities of iron, chromium, nickel, copper and zinc is ≤20ppb;

[0041] S12: placing the raw polycrystalline silicon powder material and granular silicon obtained in step S11 into a quartz crucible sprayed with a silicon nitride coating;

[0042] S13: placing the quartz crucible in step S12 into an ingot casting furnace and purifying it by using a DSS directional solidification ingot casting process to cast and produce a crude silicon material for N-type single crystal;

[0043] S14: Squaring the crude N-type single crystal silicon material obtained in step S13 into a rough rectangular ingot;

[0044] S15: The rough ingot obtained in step S14 is subjected to comprehensive judgment based on the test results of minority carrier lifetime, resistivity, infrared flaw detection and carbon oxygen content, and then the unqualified parts at the head, tail and middle of the rough ingot are cut off. The remaining parts are ground and polished, and then infrared flaw detection is performed again. After the detected black spot impurities are cut off for the second time, a qualified N-type single crystal silicon material semi-finished product is obtained;

[0045] S16: The semi-finished N-type single crystal silicon material obtained in step S15 is cleaned and crushed into blocks with a size of 5-25 mm, namely the N-type single crystal silicon material, which can be used as a raw material for CZ-pulled N-type single crystal silicon rods.

[0046] The quartz crucible sprayed with silicon nitride coating in step S12 is sprayed by pouring 800-1000g of silicon nitride powder, 2000-3000ml of deionized pure water, 300-400g of silica sol and 5-10g of polyvinyl alcohol binder into a measuring bucket and mixing them to prepare a silicon nitride spray solution; placing the measuring bucket with the prepared solution on a stirring table bracket, inserting a stirrer and opening the pneumatic valve to start stirring for no less than 20 minutes, and stirring the prepared nitride powder. The silicon solution needs to be kept in a stirring state; the qualified quartz crucible is lifted and placed on the crucible heating table for heating. When the temperature of the inner wall of the quartz crucible reaches 50°C to 70°C, the spraying operation is started. The spraying process includes spraying from a horizontal path and a longitudinal path. The crucible after spraying is pre-activated at 800°C for 2h, and then activated at 1000°C for 3h before use. The above-mentioned spraying method adopts application number CN117654840A "A spraying method for reducing the sticking rate of polycrystalline silicon ingots" for spraying.

[0047] In the ingot casting process in step S13, a high-power rapid heating is adopted in the heating stage, and a high-temperature slow cooking and efficient impurity removal method is adopted in the melting stage. The specific process control method is as follows:

[0048] S21: Use power control mode to increase temperature in the heating stage. Maintain 98% high power to quickly increase temperature in the later stage of heating. When TC1 temperature reaches 1540℃, it automatically jumps to the first step of melting.

[0049] S22: In the first step of melting, the furnace pressure is controlled at 500 mbar. In the temperature control mode, TC1 is maintained at a high temperature of 1540°C to melt the silicon material in the crucible. When the power curve drops significantly and the temperature of the bottom TC2 rises rapidly, it is determined that all the silicon material in the crucible has been melted. Then, the process manually jumps to the last step of melting for rapid cooling, crystallization, and annealing. The crystallization temperature is 1400-1436°C, and the annealing temperature is 1370°C.

[0050] The cleaning process in step S11 above includes the following steps:

[0051] S31: Use a rotary sintering furnace to burn and remove organic matter such as wood chips, plastics and epoxy resin in the original polycrystalline powder silicon material. The temperature of the sintering furnace is controlled at about 700-800°C. The silicon material is collected by rotating out from the discharge port. Pure oxygen is introduced during the combustion process for combustion.

[0052] S32: The silicon material obtained in step S31 is passed through a three-stage concentrator equipped with magnetic rollers to remove magnetic metal objects in the powdered material;

[0053] S33: putting the silicon material demagnetized in step S32 into a basket, and soaking it in a mixed solution tank containing hydrofluoric acid, hydrochloric acid, 27.5wt% hydrogen peroxide and a flotation agent for 40-60 minutes to remove the oxide film on the surface of the silicon material, and make the silicon material float on the surface with strong hydrophobicity, the flotation agent is a mixture of sodium dodecyl sulfate and oleic acid, the mass ratio of which is 1:1, the contents of hydrofluoric acid, hydrochloric acid, oxidant and flotation agent in the mixed solution are 0.5wt%, 0.2wt%, 0.3wt% and 0.1wt% respectively, and the basket is an acid corrosion resistant basket;

[0054] S34: Lift the flower basket and leave it empty for 2-3 minutes. After draining the soaking solution, pour the silicon material into the flotation tank. The powdered material will float on the water surface and flow downstream, while the impurities will sink to the bottom of the tank. Clean silicon material can be collected at the end of the flotation tank. The flotation recovery rate is >98%;

[0055] S35: The silicon material obtained in step S34 is rinsed with a slide shower device to remove the residual acid in the silicon material to make it neutral;

[0056] S36: putting the neutral silicon material obtained in step S35 into a spin dryer for drying, and then drying it in a constant temperature rotary drying furnace at a temperature of 400-500° C.;

[0057] S37: The silicon material dried in step S36 is passed through a three-stage concentrator equipped with magnetic rollers to remove magnetic metal objects in the powder and crushed materials again, so that the total content of five surface metal impurities (iron, chromium, nickel, copper and zinc) is ≤20ppb.

[0058] Example 2

[0059] A method for producing an ingot of silicon material for a CZ-type single crystal comprises the following steps:

[0060] S11: After the original polycrystalline silicon powder is cleaned, the total content of five surface metal impurities of iron, chromium, nickel, copper and zinc is ≤20ppb;

[0061] S12: placing the raw polycrystalline silicon powder material and granular silicon obtained in step S11 into a quartz crucible sprayed with a silicon nitride coating;

[0062] S13: placing the quartz crucible in step S12 into an ingot casting furnace and purifying it by using a DSS directional solidification ingot casting process to cast and produce a crude silicon material for N-type single crystal;

[0063] S14: Squaring the crude N-type single crystal silicon material obtained in step S13 into a rough rectangular ingot;

[0064] S15: The rough ingot obtained in step S14 is subjected to comprehensive judgment based on the test results of minority carrier lifetime, resistivity, infrared flaw detection and carbon oxygen content, and then the unqualified parts at the head, tail and middle of the rough ingot are cut off. The remaining parts are ground and polished, and then infrared flaw detection is performed again. After the detected black spot impurities are cut off for the second time, a qualified N-type single crystal silicon material semi-finished product is obtained;

[0065] S16: The semi-finished N-type single crystal silicon material obtained in step S15 is cleaned and crushed into blocks with a size of 10-30 mm, i.e., N-type single crystal silicon material, which can be used as a raw material for CZ-pulled N-type single crystal silicon rods.

[0066] The quartz crucible sprayed with silicon nitride coating in step S12 is sprayed by a method comprising: pouring 800-1000g of silicon nitride powder, 2000-3000ml of deionized pure water, 300-400g of silica sol and 5-10g of polyvinyl alcohol binder into a measuring bucket and mixing them to prepare a silicon nitride spray solution; placing the measuring bucket with the prepared solution on a stirring table bracket, inserting a stirrer and opening a pneumatic valve to start stirring, the stirring time is not less than 20 minutes, and the prepared silicon nitride solution needs to be in a stirring state all the time; lifting the qualified quartz crucible and placing it on a crucible heating table for heating, and starting the spraying operation when the temperature of the inner wall of the quartz crucible reaches 50°C-70°C, the spraying process includes spraying from a horizontal path and spraying from a vertical path, and the sprayed crucible is pre-activated at 800°C for 2h, and then activated at 1000°C for 3h before use.

[0067] In the ingot casting process in step S13, a high-power rapid heating is adopted in the heating stage, and a high-temperature slow cooking and efficient impurity removal method is adopted in the melting stage. The specific process control method is as follows:

[0068] S21: Use power control mode to increase temperature in the heating stage. Maintain 98% high power and quickly increase temperature in the later stage of heating. When TC1 temperature reaches 1540℃, it will automatically jump to the first step of melting.

[0069] S22: In the first step of melting, the furnace pressure is controlled at 500 mbar. In the temperature control mode, TC1 is maintained at a high temperature of 1540°C to melt the silicon material in the crucible. When the power curve drops significantly and the temperature of the bottom TC2 rises rapidly, it is determined that all the silicon material in the crucible has been melted. Then, the process manually jumps to the last step of melting for rapid cooling, crystallization, and annealing. The crystallization temperature is 1400-1436°C, and the annealing temperature is 1370°C.

[0070] The cleaning process in step S11 above includes the following steps:

[0071] S31: Use a rotary sintering furnace to burn and remove organic matter such as wood chips, plastics and epoxy resin in the original polycrystalline powder silicon material. The temperature of the sintering furnace is controlled at about 700-800°C. The silicon material is collected by rotating out from the discharge port. Pure oxygen is introduced during the combustion process for combustion.

[0072] S32: The silicon material obtained in step S31 is passed through a three-stage concentrator equipped with magnetic rollers to remove magnetic metal objects in the powdered material;

[0073] S33: putting the silicon material demagnetized in step S32 into a basket, and soaking it in a mixed solution tank containing hydrofluoric acid, hydrochloric acid, percarbonic acid amide and a flotation agent for 40 to 60 minutes to remove the oxide film on the surface of the silicon material, and make the silicon material float on the surface with strong hydrophobicity, wherein the flotation agent is a mixture of sodium dodecyl sulfate and oleic acid in a mass ratio of 1:1, and the contents of hydrofluoric acid, hydrochloric acid, oxidant and flotation agent in the mixed solution are 0.5wt%, 0.2wt%, 0.3wt% and 0.1wt% respectively, and the basket is an acid corrosion resistant basket;

[0074] S34: Lift the flower basket and leave it empty for 2-3 minutes. After draining the soaking solution, pour the silicon material into the flotation tank. The powdered material will float on the water surface and flow downstream, while the impurities will sink to the bottom of the tank. Clean silicon material can be collected at the end of the flotation tank. The flotation recovery rate is >98%;

[0075] S35: The silicon material obtained in step S34 is rinsed with a slide shower device to remove the residual acid in the silicon material to make it neutral;

[0076] S36: putting the neutral silicon material obtained in step S35 into a spin dryer for drying, and then drying it in a constant temperature rotary drying furnace at a temperature of 400-500° C.;

[0077] S37: The silicon material dried in step S36 is passed through a three-stage concentrator equipped with magnetic rollers to remove magnetic metal objects in the powder and crushed materials again, so that the total content of five surface metal impurities (iron, chromium, nickel, copper and zinc) is ≤20ppb.

[0078] Example 3

[0079] A method for producing an ingot of silicon material for a CZ-type single crystal comprises the following steps:

[0080] S11: After the original polycrystalline silicon powder is cleaned, the total content of five surface metal impurities of iron, chromium, nickel, copper and zinc is ≤20ppb;

[0081] S12: placing the raw polycrystalline silicon powder material and granular silicon obtained in step S11 into a quartz crucible sprayed with a silicon nitride coating;

[0082] S13: placing the quartz crucible in step S12 into an ingot casting furnace and purifying it by using a DSS directional solidification ingot casting process to cast and produce a crude silicon material for N-type single crystal;

[0083] S14: Squaring the crude N-type single crystal silicon material obtained in step S13 into a rough rectangular ingot;

[0084] S15: The rough ingot obtained in step S14 is subjected to comprehensive judgment based on the test results of minority carrier lifetime, resistivity, infrared flaw detection and carbon oxygen content, and then the unqualified parts at the head, tail and middle of the rough ingot are cut off. The remaining parts are ground and polished, and then infrared flaw detection is performed again. After the detected black spot impurities are cut off for the second time, a qualified N-type single crystal silicon material semi-finished product is obtained;

[0085] S16: The semi-finished N-type single crystal silicon material obtained in step S15 is cleaned and crushed into blocks with a size of 20-40 mm, i.e., N-type single crystal silicon material, which can be used as a raw material for CZ-pulled N-type single crystal silicon rods.

[0086] The quartz crucible sprayed with silicon nitride coating in step S12 is sprayed by a method comprising: pouring 800-1000g of silicon nitride powder, 2000-3000ml of deionized pure water, 300-400g of silica sol and 5-10g of polyvinyl alcohol binder into a measuring bucket and mixing them to prepare a silicon nitride spray solution; placing the measuring bucket with the prepared solution on a stirring table bracket, inserting a stirrer and opening a pneumatic valve to start stirring, the stirring time is not less than 20 minutes, and the prepared silicon nitride solution needs to be in a stirring state all the time; lifting the qualified quartz crucible and placing it on a crucible heating table for heating, and starting the spraying operation when the temperature of the inner wall of the quartz crucible reaches 50°C-70°C, the spraying process includes spraying from a horizontal path and spraying from a vertical path, and the sprayed crucible is pre-activated at 800°C for 2h, and then activated at 1000°C for 3h before use.

[0087] In the ingot casting process in step S13, a high-power rapid heating is adopted in the heating stage, and a high-temperature slow cooking and efficient impurity removal method is adopted in the melting stage. The specific process control method is as follows:

[0088] S21: Use power control mode to increase temperature in the heating stage. Maintain 98% high power and quickly increase temperature in the later stage of heating. When TC1 temperature reaches 1540℃, it will automatically jump to the first step of melting.

[0089] S22: In the first step of melting, the furnace pressure is controlled at 500 mbar. In the temperature control mode, TC1 is maintained at a high temperature of 1540°C to melt the silicon material in the crucible. When the power curve drops significantly and the temperature of the bottom TC2 rises rapidly, it is determined that all the silicon material in the crucible has been melted. Then, the process manually jumps to the last step of melting for rapid cooling, crystallization, and annealing. The crystallization temperature is 1400-1436°C, and the annealing temperature is 1370°C.

[0090] The cleaning process in step S11 above includes the following steps:

[0091] S31: Use a rotary sintering furnace to burn and remove organic matter such as wood chips, plastics and epoxy resin in the original polycrystalline powder silicon material. The temperature of the sintering furnace is controlled at about 700-800°C. The silicon material is collected by rotating out from the discharge port. Pure oxygen is introduced during the combustion process for combustion.

[0092] S32: The silicon material obtained in step S31 is passed through a three-stage concentrator equipped with magnetic rollers to remove magnetic metal objects in the powdered material;

[0093] S33: putting the silicon material demagnetized in step S32 into a basket, and soaking it in a mixed solution tank containing hydrofluoric acid, hydrochloric acid, tert-butyl hydroperoxide and a flotation agent for 40 to 60 minutes to remove the oxide film on the surface of the silicon material, and make the silicon material float on the surface with strong hydrophobicity, the flotation agent is a mixture of sodium dodecyl sulfate and oleic acid, the mass ratio of which is 1:1, the contents of hydrofluoric acid, hydrochloric acid, oxidant and flotation agent in the mixed solution are 0.5wt%, 0.2wt%, 0.3wt% and 0.1wt% respectively, and the basket is an acid corrosion resistant basket;

[0094] S34: Lift the flower basket and leave it empty for 2-3 minutes. After draining the soaking solution, pour the silicon material into the flotation tank. The powdered material will float on the water surface and flow downstream, while the impurities will sink to the bottom of the tank. Clean silicon material can be collected at the end of the flotation tank. The flotation recovery rate is >98%;

[0095] S35: The silicon material obtained in step S34 is rinsed with a slide shower device to remove the residual acid in the silicon material to make it neutral;

[0096] S36: putting the neutral silicon material obtained in step S35 into a spin dryer for drying, and then drying it in a constant temperature rotary drying furnace at a temperature of 400-500° C.;

[0097] S37: The silicon material dried in step S36 is passed through a three-stage concentrator equipped with magnetic rollers to remove magnetic metal objects in the powder and crushed materials again, so that the total content of five surface metal impurities (iron, chromium, nickel, copper and zinc) is ≤20ppb.

[0098] The silicon material ingots for CZ-type single crystals prepared by the present invention meet the following technical requirements:

[0099]

[0100] The minority carrier lifetime and resistivity data of the N-type single crystal material ingot prepared in Example 2 of the present invention are as follows:

[0101] Serial number level Silicon ingot number Conductive type Head resistance, Ω·cm Tail resistance Ω·cm Minimum minority carrier lifetime, μs Mean minority carrier lifetime, μs 1 N-level DJ434406JA PN 57.24 65.14 15 37.26-41.29 2 N-level DJ422406JA PN 13.09 306 14 25.26-34.77 3 N-level DJ417501JA PN 9.14 255 16 33.28-48.5 4 N-level DJ401501JA N 5.79 214 14 34.63-35.59 5 N-level DJ452501JA N 4.65 64.5 16 35.25-38.85 6 N-level DJ411501JA N 7.23 66.73 16 29.14-31.52 7 N-level DJ423502JA N 5.12 154 32 61.38-73.65 8 N-level DJ407501JA N 7.51 94.52 19 42.49-67.59 9 N-level DJ459501JA N 5.04 81.74 38 67.41-72.65 10 N-level DJ416501JA N 45.01 227 13 21.47-23.6

[0102] The silicon material for N-type single crystal prepared in Example 2 of the present invention replaces the native polycrystalline silicon material and is used 100% as the silicon material for CZ-pulled N-type single crystal. The average minority carrier lifetime data of the CZ-pulled N-type single crystal silicon rod is shown in Figure 1 .

[0103] It can be seen from the above data that the resistivity of the N-type single crystal material ingot prepared by the present invention is >3Ω·cm at the head and >20Ω·cm at the tail, and the average minority carrier lifetime is ≥15μs. It has excellent performance and can replace native polycrystalline silicon material and be used as silicon material for CZ-pulled N-type single crystals. The prepared single crystal silicon rods and various indicators such as minority carrier lifetime can meet the quality standards.

Claims

1. A method for producing an ingot of silicon material for CZ-type single crystal, characterized in that: The following steps are included S11: After the original polycrystalline silicon powder is cleaned, the total content of five surface metal impurities of iron, chromium, nickel, copper and zinc is ≤20ppb; S12: placing the raw polycrystalline silicon powder material and granular silicon obtained in step S11 into a quartz crucible sprayed with a silicon nitride coating; S13: placing the quartz crucible in step S12 into an ingot casting furnace and purifying it by using a DSS directional solidification ingot casting process to cast and produce a crude silicon material for N-type single crystal; S14: Squaring the crude N-type single crystal silicon material obtained in step S13 into a rough rectangular ingot; S15: The rough ingot obtained in step S14 is subjected to comprehensive judgment based on the test results of minority carrier lifetime, resistivity, infrared flaw detection and carbon oxygen content, and then the unqualified parts at the head, tail and middle of the rough ingot are cut off. The remaining parts are ground and polished, and then infrared flaw detection is performed again. After the detected black spot impurities are cut off for the second time, a qualified N-type single crystal silicon material semi-finished product is obtained; S16: The semi-finished N-type single crystal silicon material obtained in step S15 is cleaned and crushed into blocks with a size of 3-50 mm, i.e., N-type single crystal silicon material, which can be used as a raw material for CZ-pulled N-type single crystal silicon rods; The cleaning process in step S11 includes the following steps: S31: Use a rotary sintering furnace to burn and remove wood chips, plastics and epoxy resins in the original polycrystalline powder silicon material. The temperature of the sintering furnace is controlled at about 700-800°C, and the silicon material is collected by rotating out from the discharge port; S32: The silicon material obtained in step S31 is passed through a three-stage concentrator equipped with magnetic rollers to remove magnetic metal objects in the powdered material; S33: putting the silicon material demagnetized in step S32 into a basket, and soaking it in a mixed solution tank containing hydrofluoric acid, hydrochloric acid, an oxidant and a flotation agent for 40 to 60 minutes to remove the oxide film on the surface of the silicon material, and make the silicon material float on the surface with strong hydrophobicity, wherein the oxidant is one of 27.5wt% hydrogen peroxide, percarbonic acid amide and tert-butyl hydroperoxide, and the flotation agent is a mixture of sodium dodecyl sulfate and oleic acid, and the mass ratio thereof is 1:1; S34: Lift the flower basket and leave it empty for 2-3 minutes. After draining the soaking solution, pour the silicon material into the flotation tank. The powdered material will float on the water surface and flow downstream, while the impurities will sink to the bottom of the tank. Clean silicon material can be collected at the end of the flotation tank. The flotation recovery rate is >98%; S35: The silicon material obtained in step S34 is rinsed with a slide shower device to remove the residual acid in the silicon material to make it neutral; S36: putting the neutral silicon material obtained in step S35 into a spin dryer for drying, and then drying it in a constant temperature rotary drying furnace at a temperature of 400-500° C.; S37: The silicon material dried in step S36 is passed through a three-stage concentrator equipped with magnetic rollers to remove magnetic metal objects in the powder and crushed materials again, so that the total content of five surface metal impurities (iron, chromium, nickel, copper and zinc) is ≤20ppb; The quartz crucible sprayed with silicon nitride coating in step S12 is sprayed by a method comprising: pouring 800-1000g of silicon nitride powder, 2000-3000ml of deionized pure water, 300-400g of silica sol and 5-10g of polyvinyl alcohol binder into a measuring barrel and mixing them to prepare a silicon nitride spray solution; placing the measuring barrel with the prepared solution on a stirring table bracket, inserting a stirrer and opening a pneumatic valve to start stirring, the stirring time is not less than 20 minutes, and the prepared silicon nitride solution needs to be in a stirring state all the time; lifting the qualified quartz crucible on a crucible heating table for heating, and starting the spraying operation when the temperature of the inner wall of the quartz crucible reaches 50°C-70°C, the spraying process includes spraying from a horizontal path and spraying from a vertical path, and the sprayed crucible is pre-activated at 800°C for 2h, and then activated at 1000°C for 3h before use, which has a better effect and produces less impurities; In the ingot casting process in step S13, a high-power rapid heating is adopted in the heating stage, and a high-temperature slow cooking and efficient impurity removal method is adopted in the melting stage. The specific process control method is as follows: S21: Use power control mode to increase temperature in the heating stage. Maintain 98% high power to quickly increase temperature in the later stage of heating. When TC1 temperature reaches 1540℃, it automatically jumps to the first step of melting. S22: In the first step of melting, the furnace pressure is controlled at 500 mbar. In the temperature control mode, TC1 is maintained at a high temperature of 1540°C to melt the silicon material in the crucible. When the power curve drops significantly and the temperature of the bottom TC2 rises rapidly, it is determined that all the silicon material in the crucible has been melted. Then, the process manually jumps to the last step of melting for rapid cooling, crystallization, and annealing. The crystallization temperature is 1400-1436°C, and the annealing temperature is 1370°C.

2. The method for producing an ingot of silicon material for CZ-type single crystal according to claim 1, characterized in that: In the step S33, the contents of hydrofluoric acid, hydrochloric acid, oxidant and flotation agent in the mixed solution are 0.5wt%, 0.2wt%, 0.3wt% and 0.1wt% respectively.

3. The method for producing an ingot of silicon material for CZ-type single crystal according to claim 1, characterized in that: In the step S31, pure oxygen is introduced into the combustion process for combustion.

4. The method for producing an ingot of silicon material for CZ-type single crystal according to claim 1, characterized in that: In step S33, the flower basket is an acid corrosion resistant flower basket.