A surface enhanced Raman scattering substrate and its preparation method and application
By preparing a nanosheet film with gold nanospheres grown on it, using crystal face selective growth and light-induced self-nucleation growth, combined with photodegradable polymer film technology, the problem of insufficient number and intensity of 'hot spots' in the existing technology has been solved, achieving It provides a more efficient surface-enhanced Raman scattering substrate, improving the sensitivity and application prospects of trace detection.
Patent Information
- Application Number
- CN202411062654.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-08-05
AI Technical Summary
The preparation process of the existing surface-enhanced Raman scattering substrate is complex, the preparation cycle is long, the number of 'hot spots' is not enough, and the particle gaps are not small enough, resulting in insufficient intensity of the 'hot spots', which limits its application in the field of trace detection.
By preparing nanosheets with gold nanospheres grown, using crystal face selective growth and light-induced self-nucleation growth, combined with photodegradable polymer film technology, a uniform and dense nanosheet film is formed, and the nanometer amount of gold nanosphere particle gaps are achieved level control to enhance the local electric field coupling effect.
It significantly increases the number and intensity of 'hot spots', simplifies the preparation process, shortens the preparation cycle, and improves the detection sensitivity of surface-enhanced Raman scattering substrates in fields such as food safety, environmental testing, and drug testing.
Smart Images

Figure CN118566197B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of surface enhanced Raman spectroscopy detection, in particular to a surface enhanced Raman scattering substrate and a preparation method and application thereof. Background Art
[0002] Raman spectroscopy can identify substances based on the vibration of molecules, and has shown great potential in the field of substance identification. However, the traditional Raman scattering spectrum signal is very weak and easily interfered by the fluorescence background, which is not conducive to the detection of substances. Surface enhanced Raman spectroscopy (SERS) uses a rough metal structure to prepare the Raman substrate. Under the effect of the localized surface plasmon resonance enhancement of nano-scale metal materials, the Raman signal of the analyte molecule will be greatly enhanced, thereby realizing trace detection of substances. It has broad prospects in the fields of food safety, environmental testing, and drug testing.
[0003] The local electric field enhancement characteristics on the surface of metal nanomaterials are due to the interaction between the electron cloud on the surface of the material structure and the incident light, thus forming a local surface plasmon resonance effect. This electric field resonance enhancement effect is affected by the morphology of the nanomaterial itself. Research has found (Nano Lett. 2013,13: 6113−6121) that the gap between two metal particles at the nanometer level will also produce a "hot spot" to obtain local electric field enhancement. Obviously, the more gaps there are, the more "hot spots" there will be.
[0004] The multi-hotspot surface enhanced Raman scattering substrates prepared by the prior art are all prepared by a multi-step method, first preparing metal nanoparticles, and then bringing the metal nanoparticles close to each other to obtain "hotspots". For example, a Chinese patent (ZL201510177664.X) discloses a surface enhanced Raman scattering substrate and a preparation method thereof, first synthesizing gold nanostar particles, and then assembling the gold nanostar particles as array units in a micro-nano array by means of electrophoretic deposition technology to obtain "hotspots". Another Chinese patent (ZL202211482777.7) discloses a flexible surface enhanced Raman scattering substrate with adjustable gaps and a preparation method and application thereof, first laser reducing silver ions to obtain silver nanodots, and then regulating the gaps between the nanodots by the size of the pH value. The above multi-step method for preparing a multi-"hotspot" SERS substrate is not only complex in process and long in preparation cycle, but also the number of "hotspots" is not large enough, and the gaps between the particles are not small enough, so the intensity of the obtained "hotspots" is not high enough. This limits the application of surface enhanced Raman scattering substrates in many trace detection fields. Summary of the invention
[0005] To solve the above problems, the present invention proposes a surface enhanced Raman scattering substrate and a preparation method and application thereof. The surface enhanced Raman scattering substrate not only has a large number of "hot spots", but also obtains "hot spots" of greater intensity due to very small particle gaps.
[0006] The present invention provides a method for preparing a surface enhanced Raman scattering substrate, which specifically comprises the following steps:
[0007] (1) Preparation of gold nanoparticle solution
[0008] First, prepare a HAuCl4 solution, then heat the HAuCl4 solution to boiling under stirring conditions, then add a reducing agent solution and continue stirring, Au ions will react chemically with the reducing agent in the reducing agent solution to obtain Au single substance, and the continuous reaction allows the Au single substance to continuously grow to obtain smaller gold nanoparticles, and after the stirring is completed, a gold nanoparticle solution is obtained;
[0009] (2) Preparation of gold nanosheet solution
[0010] Prepare a CTAC (cetyltrimethylammonium chloride) aqueous solution, mix it with the gold nanoparticle solution obtained in step (1) and stir to obtain a mixed solution A. The halogen element Cl in the mixed solution A is - The Au ions are reduced and the Au atoms generated continue to grow on the surface of the gold nanoparticles. However, the {111} crystal surface is adsorbed by Cl. - The gold nanoparticles cannot continue to grow due to the obstruction and can only grow along the {110} crystal plane, eventually obtaining gold nanosheets. After stirring, a gold nanosheet solution is obtained.
[0011] (3) Preparation of nanosheet solution with gold nanospheres
[0012] Prepare a silver nitrate aqueous solution, add the AgNO3 aqueous solution to the gold nanosheet solution obtained in step (2), + will react with the Cl - The ions combine to form a precipitate AgCl, which is stirred at a speed of 800 rpm. AgCl will randomly precipitate on various surfaces of the gold nanosheets. After the stirring is completed, a mixed solution B is obtained. Then, under the condition of irradiating the mixed solution B with light of a wavelength of 520±5 nm, HAuCl4 solution and a reducing agent solution are added to the mixed solution B and stirred. At the surface position of the gold nanosheet where no AgCl is precipitated, Au atoms generated after the Au ions are reduced self-nucleate and grow at the above-mentioned position under the induction of light. As they continue to grow, gold nanosphere particles are obtained. The gold nanosphere particles grow on the aforementioned gold nanosheets, that is, a nanosheet solution with gold nanospheres grown therein is finally obtained.
[0013] (4) Preparation of surface-enhanced Raman scattering substrate
[0014] a. After the nanosheet solution with gold nanospheres grown thereon prepared in step (3) is allowed to stand, the supernatant is removed, and then ultrapure water is added for washing to remove the unreacted excess reagent to obtain nanosheets with gold nanospheres grown thereon, and then 50 mL of ethanol is added and stirred to disperse the nanosheets with gold nanospheres grown thereon in the ethanol, and then 5 g of PMMA polymer material and 1 g of photosensitizer material are added and stirred to obtain a mixed solution C, and finally the mixed solution C is spin-coated on the surface of the substrate, and then the substrate is heated at a constant temperature for 10 min.
[0015] b. After the constant temperature heating is completed, continue to spin-coat the mixed solution C on the surface of the above-mentioned substrate, and then heat it at a constant temperature for 10 minutes. This cycle is repeated 5-10 times (one cycle here means spin-coating the mixed solution C first, and then heating it at a constant temperature for 10 minutes). Finally, a substrate with multiple thin film layers deposited is obtained, and each thin film layer contains nanosheets grown with gold nanospheres, PMMA and photosensitizer materials.
[0016] c. Place the substrate with the multi-layer thin film layer under a 300nm wavelength ultraviolet lamp for 10 minutes, then stop irradiating for 5 minutes, and then continue irradiating for 10 minutes, and repeat this cycle 3-10 times (one cycle here means irradiating under a 300nm wavelength ultraviolet lamp for 10 minutes, and then stop irradiating for 5 minutes), where stopping irradiation is to prevent the morphology of the nanosheets with gold nanospheres from degrading under the high temperature conditions generated by the ultraviolet lamp. Under the irradiation of ultraviolet light, the photosensitizer material undergoes a dehydrogenation reaction between adjacent molecules, transfers energy to PMMA molecules, triggers the photodegradation reaction of PMMA molecules, and generates carbon dioxide, water and small molecules. After the photosensitizer material and PMMA decompose, the nanosheets with gold nanospheres will slowly fall to the surface of the substrate, thereby obtaining a uniform and dense nanosheet film with gold nanospheres, that is, a surface enhanced Raman scattering substrate of nanosheets with gold nanospheres.
[0017] Furthermore, in step (1), the HAuCl4 solution is prepared by dissolving solid HAuCl4 in ultrapure water, stirring it at a speed of 700 rpm for 5-8 minutes at room temperature to obtain a HAuCl4 solution, which is golden yellow.
[0018] Furthermore, the specific conditions for stirring after adding the reducing agent solution in step (1) are a stirring speed of 700 rpm and a stirring time of 15 min.
[0019] Furthermore, in step (2), the mass fraction of the CTAC aqueous solution is 0.5-20%, and the volume is 1 mL-50 mL.
[0020] Furthermore, in step (3), the concentration of the AgNO3 aqueous solution is 0.01-20 mmol / L, and the volume is 1 mL-100 mL.
[0021] Furthermore, the concentration of the HAuCl4 solution in steps (1), (2) and (3) is 0.1-50 mmol / L, and the volume is 1 mL-100 mL.
[0022] Furthermore, in steps (1), (2) and (3), the reducing agent in the reducing agent solution includes at least one of C6H5O7Na3, C6H8O6, NaBH4 and N2H4·H2O; the solvent in the reducing agent solution is water, and the mass fraction of the reducing agent solution is 0.01-10% and the volume is 1 mL-150 mL.
[0023] Furthermore, in step (4), the nanosheets grown with gold nanospheres obtained in step a have a size of 5-50 μm and a thickness of 50-120 nm.
[0024] Furthermore, the photosensitizer material in step (4) includes at least one of benzophenone and p-benzoquinone.
[0025] Furthermore, the temperature of the constant temperature heating in step (4) is 40-60°C.
[0026] Furthermore, in step (4), the substrate is one of a glass sheet, a silicon sheet, and a copper sheet.
[0027] Furthermore, in step (4), the spin coating speed is 1000-3000 rpm, and the spin coating time is 10-45 s.
[0028] The present invention also provides a surface enhanced Raman scattering substrate obtained according to the above preparation method and application of the surface enhanced Raman scattering substrate in surface enhanced Raman scattering spectrum detection technology.
[0029] The present invention first prepares a nanosheet with gold nanospheres grown thereon by crystal face selective growth and light-induced self-nucleation growth. The gold nanospheres on the nanosheet grow randomly and a large number of "hot spots" are formed between the gold nanospheres themselves and the adjacent particles, and the gaps between adjacent gold nanosphere particles are very small. In the synthesis process, the crystal face selective adsorption characteristics of the halogen elements and the self-nucleation characteristics of the gold atoms induced by light are fully utilized to promote the growth of gold nanosphere particles (the amount of AgCl precipitates is small) at the position without AgCl precipitates on the nanosheet. On this basis, a photodegradable multilayer polymer film technology is proposed. After the polymer film is decomposed, the nanosheet with gold nanospheres grown on the upper layer slowly falls to the surface of the substrate, thereby preparing a uniform and dense nanosheet surface enhanced Raman scattering substrate with gold nanospheres grown thereon. The distance between the gold nanospheres can also be regulated at the nanometer level, thereby forming a strong "hot spot" under the action of the coupling effect. Since the local electric field strength formed by the coupling effect between metal nanoparticles is much greater than the local electric field strength on the surface of a single particle, the prepared surface-enhanced Raman scattering substrate has broad prospects in the fields of food safety, environmental testing, and drug testing.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] (1) The surface enhanced Raman scattering substrate prepared by the present invention is composed of a nanosheet with a large number of gold nanospheres, in which each gold nanosphere particle forms a "hot spot" with other gold nanosphere particles, so the number of "hot spots" in this structure is greater. More importantly, the gold nanosphere particles on the nanosheet grow naturally. Compared with the traditional surface enhanced Raman scattering substrate, in addition to obtaining a larger number of "hot spots", the core lies in that the gaps between adjacent gold nanosphere particles can be nanometer-level, so the intensity of the obtained "hot spots" is also stronger;
[0032] (2) The method for preparing the surface enhanced Raman scattering substrate proposed in the present invention utilizes the photodegradable polymer film technology. After the polymer film is decomposed, the nanosheets grown with gold nanospheres will slowly fall to the surface of the substrate, thereby achieving a more dense nanosheet film grown with gold nanospheres. This highly dense film cannot be achieved by the traditional single-layer spin coating method. By controlling the number of spin-coated film layers, the gap between the gold nanosphere particles can be regulated at the nanometer level, thereby obtaining a stronger "hot spot" intensity.
[0033] (3) The thin film preparation process of the present invention only requires a spin coater for simple spin coating. Compared with the expensive evaporation equipment relied on by the physical method, the process is simpler and the entire spin coating process only takes a dozen minutes. The preparation cycle is also shorter than that of the physical method or chemical self-assembly technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 The local electric field resonance spectra when the gaps between particles are 3 nm, 1.5 nm, 0.8 nm, 0.5 nm, and 0.2 nm, respectively. The particles refer to the gold nanosphere particles on the Raman scattering substrate. Figure 1 The upper right corner shows the coupling electric field distribution between two gold nanosphere particles;
[0035] Figure 2 This is a SEM image of the nanosheets grown with gold nanospheres in step (4) of Example 1.
[0036] Figure 3 It is a schematic flow chart of a method for preparing a surface enhanced Raman scattering substrate according to an embodiment of the present invention, wherein 1 is a substrate, 2 is a thin film layer, and 3 is a nanosheet on which gold nanospheres are grown.
[0037] Figure 4 This is a surface SEM image of the surface enhanced Raman scattering substrate prepared in Example 1.
[0038] Figure 5 Comparative spectra of the Raman signals of adenine molecules of the surface-enhanced Raman scattering substrate prepared in Example 1 and the surface-enhanced Raman scattering substrate obtained by photodegrading one layer prepared in Comparative Example 1. DETAILED DESCRIPTION
[0039] In order to better understand the content of the present invention, the present invention will be further described below in conjunction with specific embodiments and drawings. The following embodiments are implemented based on the technology of the present invention, and detailed implementation methods and operating steps are given, but the protection scope of the present invention is not limited to the following embodiments.
[0040] The ethanol used in the examples and comparative examples was analytical pure ethanol with a purity of 99%.
[0041] Embodiment 1:
[0042] (1) Preparation of gold nanoparticle solution
[0043] First, solid HAuCl4 was dissolved in ultrapure water and stirred at 700 rpm for 5 min at room temperature to obtain a golden HAuCl4 solution with a volume of 50 mL and a concentration of 0.1 mmol / L. The HAuCl4 solution was heated under stirring until boiling, and then 15 mL of a 0.05% C6H5O7Na3 aqueous solution was added, and then the solution was stirred at 700 rpm for 15 min. After the stirring was completed, wine-red smaller gold nanoparticles were generated in the solution, and a gold nanoparticle solution was obtained.
[0044] (2) Preparation of gold nanosheet solution
[0045] Prepare 2 mL of 0.5% CTAC aqueous solution and mix it with the gold nanoparticle solution obtained in step (1) to obtain a mixed solution A. Then, add 20 mL of 0.1 mmol / L HAuCl4 solution and 6 mL of 0.05% C6H5O7Na3 aqueous solution to the mixed solution A to finally obtain a gold nanosheet solution.
[0046] (3) Preparation of nanosheet solution with gold nanospheres
[0047] A 0.05 mmol / L AgNO3 aqueous solution was prepared, 2 mL of the AgNO3 aqueous solution was added to the gold nanosheet solution obtained in step (2), and the mixture was stirred at 800 rpm to obtain a mixed solution B. Then, under the condition of irradiating the mixed solution B with light of 520±5 nm wavelength, 10 mL of 0.1 mmol / L HAuCl4 solution and 3 mL of 0.05% C6H5O7Na3 aqueous solution were added to the mixed solution B, and finally a nanosheet solution with gold nanospheres grown thereon was obtained.
[0048] (4) Preparation of surface-enhanced Raman scattering substrate
[0049] a. After the nanosheet solution with gold nanospheres grown thereon prepared in step (3) is allowed to stand, the supernatant is removed, and the solution is washed three times with ultrapure water to obtain nanosheets with gold nanospheres grown thereon, and then 50 mL of ethanol is added for stirring, followed by adding 5 g of PMMA polymer material and 1 g of benzophenone for thorough stirring and mixing to obtain a mixed solution C, and finally the mixed solution C is spin-coated on a flat substrate surface with the aid of a spin coater, wherein the substrate is a glass sheet, the spin coater has a rotation speed of 1500 rpm, and the spin coating time is 20 s, and then the substrate is placed on a 50° C. constant temperature heating table for 10 min.
[0050] b. After the constant temperature heating is completed, the mixed solution C is continued to be spin-coated on the above substrate using a spin coater, and then the mixed solution C is subjected to constant temperature heating at 50°C for 10 minutes. This cycle is repeated 6 times to obtain a substrate with 6 thin film layers deposited thereon, each of which contains nanosheets with gold nanospheres grown thereon, PMMA, and photosensitizer materials.
[0051] c. Place the substrate with 6 thin film layers deposited under a UV lamp with a power of 400 W and a wavelength of 300 nm for 10 minutes, then stop irradiating for 5 minutes, and then continue irradiating, and repeat this cycle 5 times to obtain a uniform and dense nanosheet film with gold nanospheres grown on it, that is, a nanosheet surface enhanced Raman scattering substrate with gold nanospheres grown on it.
[0052] Embodiment 2:
[0053] (1) Preparation of gold nanoparticle solution
[0054] First, solid HAuCl4 was dissolved in ultrapure water and stirred at 700 rpm for 5 min at room temperature to obtain a golden HAuCl4 solution with a volume of 50 mL and a concentration of 1 mmol / L. The HAuCl4 solution was heated under stirring until boiling, and then 15 mL of a 0.5% C6H5O7Na3 aqueous solution was added, and then the solution was stirred at 700 rpm for 15 min. After the stirring was completed, wine-red smaller gold nanoparticles were generated in the solution, and a gold nanoparticle solution was obtained.
[0055] (2) Preparation of gold nanosheet solution
[0056] Prepare 10 mL of 1% CTAC aqueous solution, mix it with the gold nanoparticle solution obtained in step (1) to obtain a mixed solution A, then add 20 mL of 1 mmol / L HAuCl4 solution and 6 mL of 0.5% C6H5O7Na3 aqueous solution to the mixed solution A, and finally obtain a gold nanosheet solution.
[0057] (3) Preparation of nanosheet solution with gold nanospheres
[0058] A 0.5 mmol / L AgNO3 aqueous solution was prepared, 2 mL of the AgNO3 aqueous solution was added to the gold nanosheet solution obtained in step (2), and the mixture was stirred at 800 rpm to obtain a mixed solution B. Then, under the condition of irradiating the mixed solution B with light of 520±5 nm wavelength, 10 mL of 1 mmol / L HAuCl4 solution and 3 mL of 0.5% C6H5O7Na3 aqueous solution were added to the mixed solution B, and finally a nanosheet solution with gold nanospheres grown thereon was obtained.
[0059] (4) Preparation of surface-enhanced Raman scattering substrate
[0060] a. After the nanosheet solution with gold nanospheres grown thereon prepared in step (3) is allowed to stand, the supernatant is removed, and the solution is washed three times with ultrapure water to obtain nanosheets with gold nanospheres grown thereon, and then 50 mL of ethanol is added for stirring, followed by adding 5 g of PMMA polymer material and 1 g of benzophenone for thorough stirring and mixing to obtain a mixed solution C, and finally the mixed solution C is spin-coated on a flat substrate surface with the aid of a spin coater, wherein the substrate is a glass sheet, the spin coater has a rotation speed of 1500 rpm, and the spin coating time is 20 s, and then the substrate is placed on a 50° C. constant temperature heating table for 10 min.
[0061] b. After the constant temperature heating is completed, the mixed solution C is continued to be spin-coated on the above substrate using a spin coater, and then the mixed solution C is subjected to constant temperature heating at 50°C for 10 minutes. This cycle is repeated 6 times to obtain a substrate with 6 thin film layers deposited thereon, each of which contains nanosheets with gold nanospheres grown thereon, PMMA, and photosensitizer materials.
[0062] c. Place the substrate with 6 thin film layers deposited under a UV lamp with a power of 400 W and a wavelength of 300 nm for 10 minutes, then stop irradiating for 5 minutes, and then continue irradiating, and repeat this cycle 5 times to obtain a uniform and dense nanosheet film with gold nanospheres grown on it, that is, a nanosheet surface enhanced Raman scattering substrate with gold nanospheres grown on it.
[0063] Embodiment 3:
[0064] (1) Preparation of gold nanoparticle solution
[0065] First, solid HAuCl4 was dissolved in ultrapure water and stirred at 700 rpm for 5 min at room temperature to obtain a golden HAuCl4 solution with a volume of 50 mL and a concentration of 50 mmol / L. The HAuCl4 solution was heated under stirring until boiling, and then 45 mL of a C6H5O7Na3 aqueous solution with a mass fraction of 8.5% was added, and then the solution was stirred at 700 rpm for 15 min. After the stirring was completed, wine-red smaller gold nanoparticles were generated in the solution, and a gold nanoparticle solution was obtained.
[0066] (2) Preparation of gold nanosheet solution
[0067] Prepare 10 mL of 5% CTAC aqueous solution, mix it with the gold nanoparticle solution obtained in step (1) to obtain a mixed solution A, then add 5 mL of 0.5 mmol / L HAuCl4 solution and 1 mL of 0.5% C6H5O7Na3 aqueous solution to the mixed solution A, and finally obtain a gold nanosheet solution.
[0068] (3) Preparation of nanosheet solution with gold nanospheres
[0069] A 5 mmol / L AgNO3 aqueous solution was prepared, 2 mL of the AgNO3 aqueous solution was added to the gold nanosheet solution obtained in step (2), and the mixture was stirred at 800 rpm to obtain a mixed solution B. Then, under the condition of irradiating the mixed solution B with light of 520±5 nm wavelength, 3 mL of 0.3 mmol / L HAuCl4 solution and 1 mL of 0.25% C6H5O7Na3 aqueous solution were added to the mixed solution B, and finally a nanosheet solution with gold nanospheres grown thereon was obtained.
[0070] (4) Preparation of surface-enhanced Raman scattering substrate
[0071] a. After the nanosheet solution with gold nanospheres grown thereon prepared in step (3) is allowed to stand, the supernatant is removed, and the solution is washed three times with ultrapure water to obtain nanosheets with gold nanospheres grown thereon, and then 50 mL of ethanol is added for stirring, followed by adding 5 g of PMMA polymer material and 1 g of benzophenone for thorough stirring and mixing to obtain a mixed solution C, and finally the mixed solution C is spin-coated on a flat substrate surface with the aid of a spin coater, wherein the substrate is a glass sheet, the spin coater has a rotation speed of 1500 rpm, and the spin coating time is 20 s, and then the substrate is placed on a 50° C. constant temperature heating table for 10 min.
[0072] b. After the constant temperature heating is completed, the mixed solution C is continued to be spin-coated on the above substrate using a spin coater, and then the mixed solution C is subjected to constant temperature heating at 50°C for 10 minutes. This cycle is repeated 6 times to obtain a substrate with 6 thin film layers deposited thereon, each of which contains nanosheets with gold nanospheres grown thereon, PMMA, and photosensitizer materials.
[0073] c. Place the substrate with 6 thin film layers deposited under a UV lamp with a power of 400 W and a wavelength of 300 nm for 10 minutes, then stop irradiating for 5 minutes, and then continue irradiating, and repeat this cycle 5 times to obtain a uniform and dense nanosheet film with gold nanospheres grown on it, that is, a nanosheet surface enhanced Raman scattering substrate with gold nanospheres grown on it.
[0074] Embodiment 4:
[0075] (1) Preparation of gold nanoparticle solution
[0076] First, solid HAuCl4 was dissolved in ultrapure water and stirred at 700 rpm for 8 min at room temperature to obtain a golden HAuCl4 solution with a volume of 100 mL and a concentration of 0.1 mmol / L. The HAuCl4 solution was heated under stirring until boiling, and then 1 mL of 10% NaBH4 aqueous solution was added. The solution was stirred at 700 rpm for 15 min. After the stirring, smaller wine-red gold nanoparticles were generated in the solution, and a gold nanoparticle solution was obtained.
[0077] (2) Preparation of gold nanosheet solution
[0078] 1 mL of 20% CTAC aqueous solution was prepared and mixed with the gold nanoparticle solution obtained in step (1) to obtain a mixed solution A. Subsequently, 100 mL of 0.1 mmol / L HAuCl4 solution and 100 mL of 10% NaBH4 aqueous solution were added to the mixed solution A to finally obtain a gold nanosheet solution.
[0079] (3) Preparation of nanosheet solution with gold nanospheres
[0080] A 0.01 mmol / L AgNO3 aqueous solution was prepared, 100 mL of the AgNO3 aqueous solution was added to the gold nanosheet solution obtained in step (2), and the mixture was stirred at 800 rpm to obtain a mixed solution B. Then, under the condition of irradiating the mixed solution B with light of 520±5 nm wavelength, 100 mL of a 0.1 mmol / L HAuCl4 solution and 100 mL of a 10% by mass NaBH4 aqueous solution were added to the mixed solution B, and finally a nanosheet solution with gold nanospheres grown thereon was obtained.
[0081] (4) Preparation of surface-enhanced Raman scattering substrate
[0082] a. After the nanosheet solution with gold nanospheres grown thereon prepared in step (3) is allowed to stand, the supernatant is removed, and the solution is washed three times with ultrapure water to obtain nanosheets with gold nanospheres grown thereon, and then 50 mL of ethanol is added for stirring, followed by adding 5 g of PMMA polymer material and 1 g of p-benzoquinone for thorough stirring and mixing to obtain a mixed solution C, and finally the mixed solution C is spin-coated on a flat substrate surface with the aid of a spin coater, wherein the substrate is a silicon wafer, the spin coater has a rotation speed of 1000 rpm, and the spin coating time is 45 s, and then the substrate is placed on a 60° C. constant temperature heating table for 10 min.
[0083] b. After the constant temperature heating is completed, the mixed solution C is continued to be spin-coated on the above substrate using a spin coater, and then the mixed solution C is subjected to constant temperature heating at 60°C for 10 minutes. This cycle is repeated 6 times to obtain a substrate with 6 thin film layers deposited thereon, each of which contains nanosheets with gold nanospheres grown thereon, PMMA, and photosensitizer materials.
[0084] c. Place the substrate with 6 thin film layers deposited under a UV lamp with a power of 400 W and a wavelength of 300 nm for 10 minutes, then stop irradiating for 5 minutes, and then continue irradiating, and repeat this cycle 5 times to obtain a uniform and dense nanosheet film with gold nanospheres grown on it, that is, a nanosheet surface enhanced Raman scattering substrate with gold nanospheres grown on it.
[0085] Embodiment 5:
[0086] (1) Preparation of gold nanoparticle solution
[0087] First, solid HAuCl4 was dissolved in ultrapure water and stirred at 700 rpm for 7 minutes at room temperature to obtain a golden HAuCl4 solution with a volume of 1 mL and a concentration of 50 mmol / L. The HAuCl4 solution was heated under stirring until boiling, and then 150 mL of a C6H8O6 aqueous solution with a mass fraction of 0.01% was added, and then the stirring was continued at 700 rpm for 15 minutes. After the stirring was completed, wine-red smaller gold nanoparticles were generated in the solution, and a gold nanoparticle solution was obtained.
[0088] (2) Preparation of gold nanosheet solution
[0089] Prepare 50 mL of 0.5% CTAC aqueous solution, mix it with the gold nanoparticle solution obtained in step (1) to obtain a mixed solution A, then add 1 mL of 50 mmol / L HAuCl4 solution and 150 mL of 0.01% C6H8O6 aqueous solution to the mixed solution A, and finally obtain a gold nanosheet solution.
[0090] (3) Preparation of nanosheet solution with gold nanospheres
[0091] A 20 mmol / L AgNO3 aqueous solution was prepared, 1 mL of the AgNO3 aqueous solution was added to the gold nanosheet solution obtained in step (2), and the mixture was stirred at 800 rpm to obtain a mixed solution B. Then, under the condition of irradiating the mixed solution B with light of 520±5 nm wavelength, 1 mL of 50 mmol / L HAuCl4 solution and 150 mL of 0.01% C6H8O6 aqueous solution were added to the mixed solution B respectively, and finally a nanosheet solution with gold nanospheres grown thereon was obtained.
[0092] (4) Preparation of surface-enhanced Raman scattering substrate
[0093] a. After the nanosheet solution with gold nanospheres grown thereon prepared in step (3) is allowed to stand, the supernatant is removed, and the solution is washed three times with ultrapure water to obtain nanosheets with gold nanospheres grown thereon, and then 50 mL of ethanol is added for stirring, followed by adding 5 g of PMMA polymer material and 1 g of p-benzoquinone for thorough stirring and mixing to obtain a mixed solution C, and finally the mixed solution C is spin-coated on a flat substrate surface with the aid of a spin coater, wherein the substrate is a copper sheet, the spin coater has a rotation speed of 3000 rpm, and the spin coating time is 10 s, and then the substrate is placed on a 40° C. constant temperature heating table for 10 min.
[0094] b. After the constant temperature heating is completed, the mixed solution C is continued to be spin-coated on the above substrate using a spin coater, and then the substrate is subjected to constant temperature heating treatment at 40°C for 10 minutes. This cycle is repeated 6 times to finally obtain a substrate with 6 thin film layers deposited thereon, each of which contains nanosheets with gold nanospheres grown thereon, PMMA, and photosensitizer materials.
[0095] c. Place the substrate with 6 thin film layers deposited under a UV lamp with a power of 400 W and a wavelength of 300 nm for 10 minutes, then stop irradiating for 5 minutes, and then continue irradiating, and repeat this cycle 5 times to obtain a uniform and dense nanosheet film with gold nanospheres grown on it, that is, a nanosheet surface enhanced Raman scattering substrate with gold nanospheres grown on it.
[0096] Comparative Example 1:
[0097] The preparation methods of steps (1), (2) and (3) in this comparative example are the same as those in Example 1, and step (4) is as follows:
[0098] (4) Preparation of surface-enhanced Raman scattering substrate
[0099] The nanosheet solution with gold nanospheres grown thereon prepared in step (3) was allowed to stand, and the supernatant was removed. The solution was washed three times with ultrapure water to obtain nanosheets with gold nanospheres grown thereon. 50 mL of ethanol solution was then added for stirring. Subsequently, 5 g of PMMA polymer material and 1 g of benzophenone were added for thorough stirring and mixing to obtain a mixed solution C. Finally, the mixed solution C was spin-coated on a flat substrate surface with the aid of a spin coater. The substrate was a glass sheet. The spin coater speed was 1500 rpm. The spin coating time was 20 s. The substrate was then placed on a 50° C. constant temperature heating table for 10 min. After the constant temperature heating was completed, a substrate with one thin film layer deposited thereon was obtained. The substrate with one thin film layer deposited thereon was placed under an ultraviolet lamp with a power of 400 W and a wavelength of 300 nm for irradiation for 10 min. The irradiation was then stopped for 5 min, and then continued for irradiation. This cycle was repeated 5 times to obtain a surface enhanced Raman scattering substrate.
[0100] Finite element algorithm is used for modeling simulation calculation, gold spherical nanoparticles are set, and the gaps between the particles are set to 3nm, 1.5nm, 0.8nm, 0.5nm, and 0.2nm, respectively, to simulate and obtain the local electric field resonance spectrum. The simulation of the local electric field in the present invention uses the software COMSOL, and the reference for the method of use is: ACS Nano, 2016, 10, 581-587; Appl. Phys. Lett.2013, 102, 153108. The specific process of the simulation of the present invention is: first, two spherical geometric structure models are constructed; second, the material parameters of the spherical geometric structure, that is, the dielectric constant of gold, are set; then the structural model is meshed, and the wavelength range of the calculation is set to 350-850nm, where the step size is 5nm; finally, the calculation is started, and the local electric field intensity corresponding to each wavelength is calculated using the post-processing function of the software, and the local electric field resonance spectrum is obtained by fitting with the help of the Origin drawing tool.
[0101] The local electric field resonance spectra when the gaps between particles are 3nm, 1.5nm, 0.8nm, 0.5nm, and 0.2nm are shown in the figure below. Figure 1 As shown, the particles refer to the gold nanosphere particles on the Raman scattering substrate. Figure 1 The upper right corner shows the coupling electric field distribution between two gold nanosphere particles. Figure 1 It can be seen that the smaller the gap, the greater the intensity of the electric field resonance peak, which further illustrates that the coupling effect between particles is stronger.
[0102] Figure 2 This is a SEM image of the nanosheet with gold nanospheres grown in step (4) of Example 1. Figure 2 The arrow in the middle points to the gap between two gold nanosphere particles close to each other. Figure 2 It can be seen that the size of the nanosheets is 5-50 μm and the thickness is 50-120 nm.
[0103] Figure 3 The figure is a schematic flow chart of a method for preparing a surface enhanced Raman scattering substrate according to an embodiment of the present invention.
[0104] Figure 4 The surface SEM image of the surface enhanced Raman scattering substrate prepared in Example 1. Figure 4 It can be seen that the nanosheet particle film with gold nanospheres grown on the surface of the surface enhanced Raman scattering substrate not only has good density but also has good uniformity.
[0105] In order to further verify the enhancement effect of the surface enhanced Raman scattering substrate prepared by the present invention, the surface enhanced Raman scattering substrate prepared in Example 1 was compared with the surface enhanced Raman scattering substrate prepared in Comparative Example 1, i.e., one layer of photodegradation treated surface enhanced Raman scattering substrate. First, an adenine ethanol solution was prepared, i.e., adenine was dispersed in anhydrous ethanol, and the concentration of adenine was 1×10 -8 mol / L, the surface enhanced Raman scattering substrate prepared in Example 1 is recorded as sample A, and the surface enhanced Raman scattering substrate prepared in Comparative Example 1 is recorded as sample B. A piece of sample A and sample B are respectively taken and vertically immersed in the above-prepared adenine solution for 2.5 hours, and then sample A and sample B are taken out and dried, and finally Raman spectra are tested respectively with a Raman spectrometer. The test results are shown in Figure 5 As shown, from Figure 5 It can be seen that the characteristic peak of sample A (same Raman shift) is much higher than that of sample B. This is mainly because the surface-enhanced Raman scattering substrate prepared in comparative example 1 by photodegradation treatment has a large distance between the nanosheets on its surface, and cannot utilize the "hot spot" formed by the coupling effect between the gold nanosphere particles for enhancement. Therefore, the surface-enhanced Raman scattering substrate prepared in Example 1 of the present invention has higher sensitivity.
[0106] The above is only an embodiment of the present invention, and does not limit the present invention in any form. The present invention can also have other forms of embodiments according to the above structures and functions, which are not listed one by one. Therefore, any simple modification, equivalent change and modification made by any technician familiar with the profession to the above embodiment according to the technical essence of the present invention without departing from the scope of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.
Claims
1. A method for preparing a surface enhanced Raman scattering substrate, characterized in that: The specific steps include: (1) Preparation of gold nanoparticle solution First, a HAuCl4 solution is prepared, and then the HAuCl4 solution is heated to boiling under stirring conditions, and then a reducing agent solution is added and continued to be stirred. After the stirring is completed, a gold nanoparticle solution is obtained; (2) Preparation of gold nanosheet solution The CTAC aqueous solution is mixed with the gold nanoparticle solution obtained in step (1) and stirred to obtain a mixed solution A, and then the HAuCl4 solution and the reducing agent solution are added to the mixed solution A respectively and stirred to obtain a gold nanosheet solution after the stirring is completed; wherein the mass fraction of the CTAC aqueous solution is 0.5-20%, and the volume is 1mL-50mL; (3) Preparation of nanosheet solution with gold nanospheres The AgNO3 aqueous solution is added to the gold nanosheet solution obtained in step (2) and stirred at a speed of 800 rpm. After the stirring is completed, a mixed solution B is obtained. Then, under the condition of light irradiation with a wavelength of 520±5 nm, a HAuCl4 solution and a reducing agent solution are added to the mixed solution B respectively and stirred, and finally a nanosheet solution with gold nanospheres grown thereon is obtained; wherein the concentration of the AgNO3 aqueous solution is 0.01-20 mmol / L and the volume is 1 mL-100 mL; (4) Preparation of surface-enhanced Raman scattering substrate a. After the nanosheet solution with gold nanospheres grown thereon prepared in step (3) is allowed to stand, the supernatant is removed, and then ultrapure water is added for washing to obtain nanosheets with gold nanospheres grown thereon, which are then dispersed in 50 mL of ethanol, and then 5 g of PMMA and 1 g of photosensitizer material are added and stirred to obtain a mixed solution C, and finally the mixed solution C is spin-coated on the surface of the substrate, and then the substrate is heated at a constant temperature for 10 min; the nanosheets with gold nanospheres grown thereon obtained in this step have a size of 5-50 μm and a thickness of 50-120 nm; b. After the constant temperature heating is completed, continue to spin-coat the mixed solution C on the surface of the substrate, and then heat it at a constant temperature for 10 minutes, and repeat this cycle 5-10 times to finally obtain a substrate with a multi-layer thin film layer deposited thereon; c. Place the substrate with the multi-layer thin film layer deposited under a 300nm wavelength ultraviolet lamp for 10 minutes, then stop irradiating for 5 minutes, and then continue irradiating for 10 minutes, and repeat this cycle 3-10 times to obtain a nanosheet surface enhanced Raman scattering substrate with gold nanospheres grown on it; In steps (1), (2) and (3), the concentration of HAuCl4 solution is 0.1-50 mmol / L, and the volume is 1 mL-100 mL; the reducing agent in the reducing agent solution includes at least one of C6H5O7Na3, C6H8O6, NaBH4, and N2H4·H2O; the solvent in the reducing agent solution is water, and the mass fraction of the reducing agent solution is 0.01-10%, and the volume is 1 mL-150 mL.
2. The method for preparing a surface enhanced Raman scattering substrate according to claim 1, characterized in that: In step (1), the HAuCl4 solution is prepared by dissolving solid HAuCl4 in ultrapure water and stirring it at a speed of 700 rpm for 5-8 minutes at room temperature to obtain a HAuCl4 solution, which is golden yellow. The specific conditions for stirring after adding the reducing agent solution are a stirring speed of 700 rpm and a stirring time of 15 minutes.
3. The method for preparing a surface enhanced Raman scattering substrate according to claim 1, characterized in that: In step (4), the photosensitizer material includes at least one of benzophenone and p-benzoquinone, and the substrate is one of a glass sheet, a silicon sheet, and a copper sheet.
4. The method for preparing a surface enhanced Raman scattering substrate according to claim 1, characterized in that: In step (4), the temperature of the constant temperature heating is 40-60° C., the spin coating speed is 1000-3000 rpm, and the spin coating time is 10-45 s.
5. A surface enhanced Raman scattering substrate prepared by the preparation method according to any one of claims 1 to 4.
6. Use of the surface enhanced Raman scattering substrate as claimed in claim 5 in surface enhanced Raman scattering spectrum detection technology.
Citation Information
Patent Citations
Surface-enhanced Raman spectroscopy substrate and preparation method thereof
CN104792766A
Gap-adjustable flexible surface enhanced Raman scattering substrate and preparation method and application thereof
CN115746360A
Preparation method of recyclable surface-enhanced Raman-spectrum active substrate
CN103048304A
Preparation method of flower-like gold nanoparticles and application of flower-like gold nanoparticles serving as SERS (surface enhanced Raman scattering) enhanced substrates
CN104690288A
Core-shell-structure silver-gold nanosheet based on epitaxial growth and preparation method and application thereof
CN105014094A