Positive electrode lithium supplement current collector and preparation method thereof, positive electrode sheet, lithium ion battery and electrical equipment
By encapsulating oxygen capture agent and lithium supplement agent in the positive electrode lithium supplement collector, the negative impact of lithium supplement residual alkali and decomposition residue on battery performance in the positive electrode lithium supplement process is solved, and the electrical performance of lithium-ion batteries is significantly improved. Safety performance.
Patent Information
- Application Number
- CN202411062256.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-05
AI Technical Summary
The existing positive electrode lithium supplementation process has problems such as high residual alkali of lithium supplementation agent, decomposition residues occupying the pole vacancies, reducing the proportion of active substances and battery power performance, and it is difficult to avoid the phenomenon of battery cell flatulence and valve opening caused by side reactions of electrolyte. .
The oxygen trapping agent and lithium supplement agent are encapsulated in their pores by vacuum impregnation method to prepare the positive electrode lithium supplement collector to reduce the direct contact between the lithium supplement agent and the positive electrode active material, and reduce the oxygen trapping agent to capture the decomposition product of lithium supplement agent. side reactions.
It improves the electrical and safety performance of the battery, reduces the risks of cell inflation and valve opening, and improves the processing performance of the pole sheet and battery stability.
Smart Images

Figure CN118572124B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a positive electrode lithium supplement current collector and a preparation method thereof, a positive electrode plate, a lithium ion battery and an electrical device. Background Art
[0002] During the charge and discharge process of lithium-ion batteries, the electrolyte solvent is easily reduced on the surface of the negative electrode to form a solid electrolyte passivation film (SEI), which prevents the solvent from further reacting and consuming active lithium. This process is called the film formation process, which is crucial to the performance and stability of lithium-ion batteries. During the film formation process, due to a series of complex chemical reactions and physical processes, the active lithium in the positive electrode material may be lost, which in turn affects the performance and cycle life of the battery. In order to compensate for the loss of active lithium in the film formation process and improve the utilization efficiency of active lithium in the positive electrode material, researchers have proposed lithium replenishment technology. Compared with negative electrode lithium replenishment technologies such as lithium powder or lithium ribbon, the positive electrode lithium replenishment process has the advantages of simple equipment, relatively mild generation environment, low risk, and good battery consistency, but it also has many defects: 1) The positive electrode lithium replenisher has a high residual alkali content, which can easily lead to chemical gelation during the batching process, affecting the processing performance of the electrode; 2) The decomposition residues of the positive electrode lithium replenisher occupy certain electrode vacancies, reduce the electrode porosity, affect the diffusion of lithium ions on the surface of the positive electrode active particles, and lead to reduced battery power performance; 3) The positive electrode lithium replenisher reduces the proportion of active substances in the electrode and reduces the battery capacity; 4) The release products of the positive electrode lithium replenisher cause side reactions in the electrolyte, resulting in problems such as battery cell bloating and valve opening hazards.
[0003] In order to solve the above problems, the existing positive electrode lithium replenishment process has been improved, such as adding a coating containing a lithium replenisher on the current collector before preparing the positive electrode active material layer; or directly mixing the lithium replenisher slurry with the positive electrode slurry to make a positive electrode plate. These methods can solve the problem of the influence of the residual alkali of the positive electrode lithium replenisher on the production of the positive electrode plate to a certain extent, but the introduction of the lithium replenisher coating will increase the thickness of the inactive current collector and reduce the volume energy density of the battery cell. At the same time, it will increase the transmission path between the active material and the current collector, increase the internal resistance of electron transmission, and reduce the power performance; while the method of directly mixing the lithium replenisher with the positive electrode slurry has the problem of difficulty in mixing evenly, which is easy to cause the lithium replenisher to aggregate, and it is impossible to completely avoid the influence of the residual alkali of the lithium replenisher on the stability of the positive electrode slurry.
[0004] Therefore, there is still a need for an improved solution that can not only help improve the electrical performance of the battery but also ensure the safety of the battery. Summary of the invention
[0005] The purpose of the present disclosure is to provide a positive electrode lithium supplement current collector and a preparation method thereof, a positive electrode plate, a lithium ion battery and an electrical device to improve the electrical performance and safety performance of the lithium ion battery.
[0006] In order to achieve the above-mentioned object, the present disclosure provides a positive electrode lithium replenishing current collector in a first aspect, comprising a porous current collector, wherein pores of the porous current collector contain an oxygen capture agent and a lithium replenishing agent.
[0007] Optionally, the oxygen scavenger comprises an aromatic compound and / or a thioamino compound.
[0008] Optionally, the oxygen capture agent includes at least one of 2,2'-biphenyl butanedione, methyl cinnamate, dithioaminomethane, diphenylacetone and diphenylanthracene.
[0009] Optionally, the lithium supplement includes at least one of lithium ferrite, lithium oxalate, lithium nickelate and lithium carbonate.
[0010] Optionally, the porosity of the porous current collector is 20-70%.
[0011] Optionally, the porous current collector has first pores with a pore size of 50nm-100nm and second pores with a pore size of 10μm-100μm, the pore volume of the first pores accounts for 10-30% of the total pore volume, and the pore volume of the second pores accounts for 70-90% of the total pore volume.
[0012] Optionally, the oxygen capture agent is accommodated in the first pores, and the lithium supplement agent is accommodated in the second pores.
[0013] Optionally, based on 100 parts by weight of the positive electrode lithium replenisher, the content of the oxygen capture agent is 0.1 to 5 parts by weight, and the content of the lithium replenisher is 1 to 50 parts by weight.
[0014] Optionally, the pores of the porous current collector further contain a binder and a conductive agent, and the weight ratio of the lithium supplement agent, the binder and the conductive agent is 100: (1-20): (0.5-20).
[0015] Optionally, the conductive agent includes at least one of carbon black, carbon tube and graphene.
[0016] In a second aspect of the present disclosure, a method for preparing the positive electrode lithium supplement current collector according to the first aspect of the present disclosure is provided, the method comprising:
[0017] A porous current collector is obtained, and a mixed slurry containing an oxygen capture agent, a lithium supplement agent and a solvent is prepared;
[0018] The mixed slurry is loaded into the pores of the porous current collector, and then the solvent is removed to obtain a positive electrode lithium supplement current collector.
[0019] Optionally, based on 100 parts by weight of the lithium supplement slurry, the content of the solvent is 40 to 80 parts by weight;
[0020] And / or, the method of loading the mixed slurry into the pores of the porous current collector is a vacuum impregnation method, and the conditions of the vacuum impregnation method include: a vacuum degree of 5-50 Pa, a temperature of 20-50° C., and an impregnation time of 5-15 h.
[0021] Optionally, the porous current collector has a first pore with a pore size of 50 nm to 100 nm and a second pore with a pore size of 10 μm to 100 μm, the pore volume of the first pore accounts for 10 to 30% of the total pore volume, and the pore volume of the second pore accounts for 70 to 90% of the total pore volume; the method comprises:
[0022] The foil-shaped current collector is subjected to a first etching treatment to obtain a current collector containing the first hole; wherein the conditions of the first etching treatment include: an ion beam current of 10-30 pA, a dwell time of 100-300 μs, a laser drilling frequency of 100-200 Hz, and a drilling speed of 1-2 m / min;
[0023] Prepare a first slurry containing the oxygen capture agent, and load the first slurry into the first hole of the current collector containing the first hole by a first vacuum impregnation to obtain a current collector after the first vacuum impregnation; wherein the conditions of the first vacuum impregnation include: a vacuum degree of 5-50 Pa, a temperature of 20-50° C., and an impregnation time of 5-15 h;
[0024] The current collector after the first vacuum impregnation is subjected to a second etching treatment to obtain a current collector containing the second hole; wherein the conditions of the second etching treatment include: an ion beam current of 10-30 pA, a dwell time of 300-500 μs, a laser drilling frequency of 100-200 Hz, and a drilling speed of 0.5-1.5 m / min;
[0025] A second slurry containing the lithium replenishing agent and a solvent is prepared, and the second slurry is loaded into the second hole of the current collector containing the second hole by a second vacuum impregnation, and then the solvent is removed to obtain a positive electrode lithium replenishing current collector; wherein the conditions of the second vacuum impregnation include: a vacuum degree of 5-50 Pa, a temperature of 20-50° C., and an impregnation time of 5-15 h.
[0026] In a third aspect of the present disclosure, a positive electrode plate is provided, comprising the positive electrode lithium replenishing current collector according to the first aspect of the present disclosure and a positive electrode active material layer arranged on the surface of the positive electrode lithium replenishing current collector.
[0027] A fourth aspect of the present disclosure provides a lithium-ion battery, comprising the positive electrode sheet described in the third aspect of the present disclosure.
[0028] A fifth aspect of the present disclosure provides an electrical device comprising the lithium-ion battery described in the fourth aspect of the present disclosure.
[0029] Through the above technical scheme, the present invention integrates the lithium supplement agent and the oxygen capture agent into the porous current collector, reduces or avoids direct contact between the lithium supplement agent and the positive electrode active material, thereby reducing the influence of the residual alkali substances of the lithium supplement agent on the stability of the positive electrode material and improving the processing performance of the electrode sheet; at the same time, the lithium supplement agent and its decomposition residues can be retained in the pores of the porous current collector, reducing the negative impact on the battery power performance and capacity, and effectively improving the electrical performance; in addition, the oxygen capture agent can avoid the electrolyte side reaction caused by the release product of the lithium supplement agent, thereby reducing the risk of gas production, reducing the battery cell bloating and valve opening phenomenon, and significantly improving the battery safety performance.
[0030] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:
[0032] Figure 1 It is a structural schematic diagram of a specific implementation of the positive electrode plate provided by the present invention.
[0033] Description of Reference Numerals
[0034] 1—positive electrode lithium supplement current collector, 2—positive electrode active material layer. DETAILED DESCRIPTION
[0035] The specific implementation of the present disclosure is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described herein is only used to illustrate and explain the present disclosure, and is not used to limit the present disclosure.
[0036] In a first aspect of the present disclosure, a positive electrode lithium replenishing current collector is provided, comprising a porous current collector, wherein pores of the porous current collector contain an oxygen capture agent and a lithium replenishing agent.
[0037] According to the present disclosure, since the porous current collector has a porous structure, encapsulating the oxygen capture agent and the lithium supplement agent in the pores of the porous current collector can reduce or avoid direct contact between the lithium supplement agent and the positive electrode active material, thereby reducing the influence of the residual alkali substances of the lithium supplement agent on the stability of the positive electrode material and improving the processing performance of the electrode sheet; at the same time, the lithium supplement agent and its decomposition residues can be retained in the pores of the porous current collector, and will not reduce the porosity of the active material area due to occupying the vacant space of the electrode sheet, thereby reducing the negative impact on the battery power performance and capacity, and effectively improving the electrical performance; in particular, the oxygen capture agent can be used to capture and neutralize the singlet oxygen molecules (singlet oxygen) released by the decomposition of the lithium supplement agent to inhibit the occurrence of side reactions such as electrolyte decomposition and oxidation caused by it, thereby reducing the risk of gas production, reducing the bloating and valve opening of the battery cell, and significantly improving the battery safety performance.
[0038] The oxygen capture agent is an organic compound that can react specifically with singlet oxygen. In the present disclosure, the oxygen capture agent may include aromatic compounds and / or thioamino compounds, wherein the aromatic compound may include at least one of aromatic ketones, aromatic esters, aromatic alcohols, aromatic hydrocarbons, aromatic aldehydes, aromatic phenols and halogenated aromatic hydrocarbons. For example, the aromatic ketone may include 2,2'-biphenyl butanedione, diphenylacetone, etc.; the aromatic hydrocarbon may include diphenylanthracene, etc.; the aromatic ester may include methyl cinnamate, ethyl benzoate, ethyl cinnamate, etc.; the aromatic aldehyde may include vanillin, etc.; the thioamino compound may include dithioaminomethane, etc.; the aromatic phenol may include catechol, phenol, etc.; the aromatic alcohol may include benzyl alcohol, etc.; the halogenated aromatic hydrocarbon may include brominated benzene, tetrachlorobenzene, etc.
[0039] In a preferred embodiment, the oxygen capture agent includes at least one of 2,2'-biphenyl butanedione, methyl cinnamate, dithioaminomethane, diphenylacetone and diphenylanthracene. Using the above organic compounds as oxygen capture agents is conducive to efficiently capturing singlet oxygen molecules, effectively inhibiting electrolyte side reactions, significantly reducing gas production risks, and improving battery safety performance.
[0040] According to the present disclosure, the lithium supplement agent is a lithium-containing compound, specifically, the lithium supplement agent may include at least one of lithium ferrite, lithium oxalate, lithium nickelate and lithium carbonate, preferably at least one selected from lithium ferrite and lithium nickelate. The lithium supplement agent may be in the form of particles, and may have a particle size matching the pore size of the porous current collector. For example, the particle size of the lithium supplement agent may be 1 μm to 100 μm.
[0041] According to the present disclosure, the porous current collector has a porous structure. In order to have a better lithium supplementation effect, the porosity of the porous current collector can be 20-70%, preferably 30-50%. The porosity refers to the percentage of the pore volume in the porous current collector to the total volume (i.e., apparent volume) of the porous current collector in the natural state.
[0042] The holes in the porous current collector are evenly distributed and can be through holes or blind holes; preferably, the holes in the porous current collector are through holes (i.e. holes that penetrate the current collector) to improve the lithium replenishment effect. The holes in the porous current collector can have a certain pore size range, so that a certain amount of lithium replenishment agent and oxygen capture agent can be accommodated. The specific pore size can be adjusted according to actual needs. For example, the pore size of the pores of the porous current collector can be 50 nm~100μm.
[0043] In a preferred embodiment, the porous current collector may have a first pore with a pore size of 50nm~100nm and a second pore with a pore size of 10μm~100μm, the pore volume of the first pore accounts for 10~30% of the total pore volume, and the pore volume of the second pore accounts for 70~90% of the total pore volume. Further, the oxygen capture agent can be accommodated in the first pore, and the lithium supplement agent can be accommodated in the second pore. At this time, the lithium supplement agent has a particle size that matches the pore size of the second pore. By setting the oxygen capture agent in a smaller pore and the lithium supplement agent in a larger pore, it is beneficial to further optimize the lithium supplement effect and reduce the risk of gas production, so that the battery has significantly improved electrical performance and safety performance.
[0044] The porous current collector may be made of a material commonly used in the art, such as aluminum foil. The thickness of the porous current collector may be adjusted within a certain range, and specifically, the thickness of the porous current collector may be 10 μm to 70 μm.
[0045] According to the present disclosure, the amount of the oxygen capture agent and the lithium supplement agent can be adjusted within a certain range. In a specific embodiment, based on 100 parts by weight of the positive electrode lithium supplement current collector, the content of the oxygen capture agent can be 0.1 to 5 parts by weight, preferably 0.5 to 2 parts by weight; the content of the lithium supplement agent can be 1 to 50 parts by weight, preferably 5 to 20 parts by weight. By controlling the amount of the oxygen capture agent and the lithium supplement agent, favorable battery electrical performance and safety performance can be achieved.
[0046] Furthermore, the pores of the porous current collector also contain a binder and a conductive agent. At this time, the pores of the porous current collector also contain a binder and a conductive agent. The weight ratio of the lithium supplement, the binder and the conductive agent can be 100: (1-20): (0.5-20); under the above content ratio, it is beneficial to reduce the resistivity of the electrode sheet and improve the electrical performance of the battery. Among them, the types of the binder and the conductive agent can be common in the art, specifically, the binder can be polyvinylidene fluoride (PVDF); the conductive agent can include at least one of carbon black, carbon tubes, and graphene.
[0047] In a second aspect of the present disclosure, a method for preparing the positive electrode lithium supplement current collector according to the first aspect of the present disclosure is provided, the method comprising the following steps S1-S2:
[0048] S1. Obtain a porous current collector and prepare a mixed slurry containing an oxygen capture agent, a lithium supplement agent and a solvent;
[0049] S2, loading the mixed slurry into the pores of the porous current collector, and then removing the solvent to obtain a positive electrode lithium supplement current collector.
[0050] In step S1, the porous current collector may be a commercially available product having the characteristics described above, or may be prepared using existing technology. In one embodiment, the method for preparing the porous current collector includes: etching the foil-like current collector to obtain the porous current collector. The etching conditions may include: focused ion beam etching using an ion beam current of 1 to 50 pA, a dwell time of 50 to 1000 μs, laser drilling using a laser frequency of 100 to 500 Hz, and a drilling speed of 0.5 to 5 m / min.
[0051] The mixed slurry may also contain a binder and a conductive agent, and the proportion of each component meets the range described above. The specific material types of the oxygen capture agent, lithium supplement agent, binder and conductive agent are as described above. The solvent may be N-methylpyrrolidone (NMP), and the content of the solvent may be 40 to 80 parts by weight based on 100 parts by weight of the mixed slurry. The mixed slurry can be obtained by mixing the above components.
[0052] In step S2, the method for loading the mixed slurry into the pores of the porous current collector may be a vacuum impregnation method, and the conditions of the vacuum impregnation method may include: a vacuum degree of 5 to 50 Pa, a temperature of 20 to 50° C., and an impregnation time of 5 to 15 hours. The method for removing the solvent is well known to those skilled in the art, for example, the porous current collector may be dried to remove the solvent, and the drying conditions may be conventional in the art, for example: a temperature of 50° C. to 100° C. and a time of 5 min to 10 min.
[0053] In the above-mentioned porous current collector having a first hole with a pore size of 50nm-100nm and a second hole with a pore size of 10μm-100μm, the oxygen capture agent is contained in the first hole, and the lithium replenishing agent is contained in the second hole. In a preferred embodiment, the method for preparing the positive electrode lithium replenishing current collector comprises the following steps:
[0054] The foil-shaped current collector is subjected to a first etching treatment to obtain a current collector containing a first hole; wherein the conditions of the first etching treatment may include: an ion beam current of 10-30 pA, a dwell time of 100-300 μs, a laser drilling frequency of 100-200 Hz, and a drilling speed of 1-2 m / min;
[0055] Prepare a first slurry containing an oxygen capture agent, and load the first slurry into the first hole of the current collector containing the first hole by a first vacuum impregnation to obtain a current collector after the first vacuum impregnation; wherein the conditions of the first vacuum impregnation may include: a vacuum degree of 5-50 Pa, a temperature of 20-50° C., and an impregnation time of 5-15 h;
[0056] The current collector after the first vacuum impregnation is subjected to a second etching treatment to obtain a current collector containing a second hole; wherein the conditions of the second etching treatment may include: an ion beam current of 10-30 pA, a dwell time of 300-500 μs, a laser drilling frequency of 100-200 Hz, and a drilling speed of 0.5-1.5 m / min;
[0057] A second slurry containing a lithium replenishing agent and a solvent is prepared, and the second slurry is loaded into the second pores of the current collector containing the second pores by a second vacuum impregnation, and then the solvent is removed to obtain a positive electrode lithium replenishing current collector; wherein the conditions of the second vacuum impregnation may include: a vacuum degree of 5 to 50 Pa, a temperature of 20 to 50° C., and an impregnation time of 5 to 15 hours. The second slurry may also contain the above-mentioned binder and conductive agent.
[0058] In a third aspect of the present disclosure, a positive electrode sheet is provided, referring to Figure 1 As shown, it includes the positive electrode lithium replenishing current collector 1 described in the first aspect of the present disclosure and a positive electrode active material layer 2 arranged on the surface of the positive electrode lithium replenishing current collector 1.
[0059] The positive electrode active material layer 2 is formed of a positive electrode active material, and the positive electrode active material may be lithium iron phosphate, lithium manganese iron phosphate, etc. The amount of the positive electrode active material may be adjusted within a certain range. For example, the weight ratio of the positive electrode active material to the lithium supplement may be (100-105):1. The surface density of the positive electrode active material may be 360-500 g / m 2 , compacted density can be 2~2.6 g / m3 .
[0060] The present disclosure has no special limitation on the preparation method of the positive electrode sheet. The positive electrode active material can be coated on the surface of the positive electrode lithium supplement current collector 1 by using processes and equipment well known in the art, and the positive electrode sheet can be obtained by drying.
[0061] The positive electrode sheet disclosed in the present invention not only has an excellent lithium supplementation effect, which is beneficial to slowing down the loss of active lithium in the positive electrode material, but also can effectively inhibit electrolyte side reactions and reduce the risk of gas production. In addition, it has good processability and is suitable for large-scale industrial production. The use of the positive electrode sheet in lithium-ion batteries is conducive to improving the capacity and power performance of the battery, avoiding the hidden dangers of battery cell bloating and valve opening, and significantly improving the safety performance and stability of the battery.
[0062] In a fourth aspect of the present disclosure, a lithium-ion battery is provided, comprising the positive electrode sheet described in the third aspect of the present disclosure. The present disclosure has no particular restrictions on the specific structure of the lithium-ion battery, which may include other structures commonly found in the art, such as a negative electrode, a separator, and an electrolyte, etc. The specific types of materials may be those known to those skilled in the art, and will not be described in detail in the present disclosure.
[0063] A fifth aspect of the present disclosure provides an electrical device comprising the lithium-ion battery described in the fourth aspect of the present disclosure.
[0064] The present disclosure is further illustrated by the following examples, but is not intended to limit the present disclosure.
[0065] The raw materials and reagents used in the examples and comparative examples are all commercially available products.
[0066] Among them, the test method for the porosity of the current collector is the mercury injection porosity test, and the test method for the pore distribution is the BET pore size distribution test.
[0067] Example 1
[0068] A lithium supplement (lithium ferrite), an oxygen capture agent (methyl cinnamate), a binder (PVDF), a conductive agent (carbon black), and a solvent (N-methylpyrrolidone) are mixed in a weight ratio of 10:1:0.2:0.1:10 to obtain a mixed slurry.
[0069] The aluminum foil current collector with a thickness of 20 μm was etched under the conditions of a focused ion beam current of 10pA, a dwell time of 200 μs, a laser frequency of 200 Hz, and a drilling speed of 1 m / min to obtain a porous aluminum foil current collector with a porosity of 50%. The mixed slurry was loaded into the pores of the aluminum foil porous current collector by vacuum impregnation (conditions: vacuum degree 5Pa, temperature 20°C, time 5h), and the positive electrode lithium replenishment current collector was obtained after drying. Based on 100 parts by weight of the positive electrode lithium replenishment current collector, the content of the oxygen capture agent was 0.5 parts by weight, and the content of the lithium replenishment agent was 5 parts by weight.
[0070] Lithium iron phosphate (surface density 400 g / m 2 , compacted density is 2.6 g / m 3 ) slurry is coated on the surface of the above-mentioned positive electrode lithium replenishing current collector (the weight ratio of lithium iron phosphate slurry to lithium replenishing agent is 100:1). During the coating process, it can be seen that the active material slurry always has good fluidity, and then it is dried to obtain the positive electrode sheet.
[0071] Example 2
[0072] The positive electrode sheet was prepared according to the method of Example 1, except that the mixed slurry was loaded into the pores of the aluminum foil porous current collector by vacuum impregnation (conditions: vacuum degree 5Pa, temperature 20°C, time 10h), and the positive electrode lithium supplement current collector was obtained after drying. The same lithium supplement slurry as in Example 1 was loaded into the pores of the aluminum foil porous current collector by vacuum impregnation under the same conditions, with 100 parts by weight of the positive electrode lithium supplement current collector as the reference, wherein the content of the oxygen capture agent was 1 part by weight, and the content of the lithium supplement agent was 10 parts by weight.
[0073] Example 3
[0074] The positive electrode sheet was prepared according to the method of Example 1, except that the mixed slurry was loaded into the pores of the aluminum foil porous current collector by vacuum impregnation (conditions: vacuum degree 5Pa, temperature 40°C, time 15h), and the positive electrode lithium supplement current collector was obtained after drying. The same lithium supplement slurry as in Example 1 was loaded into the pores of the aluminum foil porous current collector by vacuum impregnation under the same conditions, with 100 parts by weight of the positive electrode lithium supplement current collector as the basis, wherein the content of the oxygen capture agent was 2 parts by weight, and the content of the lithium supplement agent was 20 parts by weight.
[0075] Example 4
[0076] An oxygen capture agent (methyl cinnamate) is used as the first slurry; a lithium supplement agent (lithium ferrite), a binder (PVDF), a conductive agent (carbon black), and a solvent (N-methylpyrrolidone) are mixed to obtain a second slurry, and the weight ratio of the lithium supplement agent, the binder, the conductive agent, and the solvent is 20:1.5:0.2:0.1:20.
[0077] A foil-shaped current collector with a thickness of 40 μm was subjected to a first etching treatment under the conditions of a current of 20 pA, a dwell time of 200 μs, a laser frequency of 200 Hz, and a drilling speed of 2 m / min to obtain a current collector containing first pores with a pore size of 50 nm to 100 nm accounting for 30% of the total pore volume; the above-mentioned first slurry was loaded into the first pores of the above-mentioned current collector by a first vacuum impregnation under the conditions of a vacuum degree of 30 Pa, a temperature of 20°C, and a time of 5 h; the obtained current collector was subjected to a second etching treatment under the conditions of a current of 30 pA, a dwell time of 300 μs, a laser frequency of 200 Hz, and a drilling speed of 1 m / min to obtain a current collector containing second pores with a pore size of 10 μm to 100 μm accounting for 70% of the total pore volume; the above-mentioned second slurry was loaded into the second pores of the above-mentioned current collector by a second vacuum impregnation under the conditions of a vacuum degree of 50 Pa, a temperature of 20°C, and a time of 10 h, and then the solvent was removed to obtain a positive electrode lithium replenishment current collector. The porosity of the positive electrode lithium replenishing current collector is 50%. Based on 100 parts by weight of the positive electrode lithium replenishing current collector, the oxygen capture agent is contained in the first hole and the content is 1.5 parts by weight, and the lithium replenishing agent is contained in the second hole and the content is 20 parts by weight.
[0078] According to the method of Example 1, the lithium iron phosphate slurry is coated on the surface of the positive electrode lithium supplement current collector. During the coating process, it can be seen that the active material slurry always has good fluidity, and then it is dried to obtain a positive electrode sheet.
[0079] Example 5
[0080] A positive electrode sheet was prepared according to the method of Example 1, except that the porosity of the porous current collector was 70%; the weight ratio of the lithium replenisher, the oxygen capture agent, the binder, the conductive agent and the solvent was 40:3:2:1:40. Based on 100 parts by weight of the positive lithium replenisher current collector, the content of the oxygen capture agent was 3 parts by weight, and the content of the lithium replenisher was 40 parts by weight.
[0081] Example 6
[0082] A positive electrode plate was prepared according to the method of Example 1, except that ethyl benzoate, an oxygen capture agent, was used to replace methyl cinnamate in Example 1.
[0083] Comparative Example 1
[0084] The lithium iron phosphate slurry is mixed with the lithium supplement agent (lithium ferrite) in a weight ratio of 100:1, and the resulting mixed slurry is coated on the surface of the aluminum foil current collector. During the coating process, it can be seen that the active material slurry has serious gelation phenomenon and cannot maintain good fluidity. Then it is dried to obtain the positive electrode sheet.
[0085] Comparative Example 2
[0086] The positive electrode lithium supplement current collector is prepared according to the method of Example 1, except that the mixed slurry does not contain an oxygen capture agent.
[0087] Test Case
[0088] The positive electrode plates of the embodiment and the comparative example were subjected to capacity test, high temperature cycle test, high temperature storage gas production test and low temperature power test. The test methods are as follows and the results are listed in Table 1.
[0089] Capacity test: The positive electrode sheets of the embodiment and the comparative example were matched with the graphite negative electrode respectively, and the soft-pack battery with a nominal capacity of about 2 Ah was prepared by the lamination method. At room temperature 25±3℃, it was charged to 3.8V at 1 / 3C constant current, left for 5min, charged to 3.8V at 0.1C, and left for 30min; discharge: at room temperature 25±3℃, it was discharged to 2.0V at 1 / 3C constant current, and left for 30min. The above steps were cycled three times, and the capacity of the last cycle was recorded as C0.
[0090] High temperature cycle test: At 60±3℃, the battery environment is adapted for 7 hours before the start of the cycle, and the test is started. The battery is charged at a constant current of 0.5C to 3.75V (the current is calculated according to the RPTs capacity test results), and the battery is left for 30 minutes. Discharge, at 60±3℃, the battery is discharged at a constant current of 0.5C to 2.0V (the current is calculated according to the RPTs capacity test results), and the battery is left for 30 minutes. Record the charge and discharge capacity / energy / voltage data. Take the discharge capacity C1 of the first cycle as a reference to calculate the capacity retention rate after 200 cycles.
[0091] High-temperature storage gas production test: At room temperature 25±3℃, charge to 3.8V at 1 / 3C constant current, let it sit for 5min, charge to 3.8V at 0.1C, let it sit for 30min; then discharge to 2.0V at 1 / 3C constant current, let it sit for 30min; repeat the charge and discharge three times and record the third discharge capacity as C0. Then charge to 3.8V at 1 / 3C constant current, let it sit for 5min, charge to 3.8V at 0.1C, let it sit for 30min, adjust the load to 100% SOC, store at 60℃ for 7D, and use the displacement volume device to test the gas production.
[0092] Low temperature power test: At -10℃, the battery was tested after acclimating to the environment for 6 hours. At -10℃, the battery was discharged at 0.2C to the cut-off voltage and left for 30 minutes; charged at 1 / 3C constant current to 3.8V, left for 5 minutes, charged at 0.1C to 3.8V, left for 30 minutes; discharged at 0.2C / 1 / 3C / 1C / 1.5C / 2C / 3C current to the cut-off voltage, left for 30 minutes (current ≥1C needs to be left for 1 hour); record the capacity / energy / median voltage / temperature rise of the charge and discharge steps, capacity ratio = discharge capacity at the discharge current / discharge capacity at the 0.2C discharge current.
[0093] Table 1
[0094]
[0095] As can be seen from Table 1, the positive electrode sheet prepared in the embodiment has higher capacity, cycle capacity retention rate and low-temperature rate discharge ratio, and lower full-charge storage gas production rate, showing excellent electrical performance and safety performance.
[0096] The preferred embodiments of the present disclosure are described in detail above in conjunction with the accompanying drawings; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.
[0097] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0098] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. A positive electrode lithium supplement current collector, characterized in that: The invention comprises a porous current collector, wherein pores of the porous current collector contain an oxygen capture agent and a lithium supplement agent, and the oxygen capture agent comprises at least one of methyl cinnamate, diphenylacetone and diphenylanthracene.
2. The positive electrode lithium supplement current collector according to claim 1, wherein: The lithium supplement includes at least one of lithium ferrite, lithium oxalate, lithium nickelate and lithium carbonate.
3. The positive electrode lithium supplement current collector according to claim 1, wherein: The porosity of the porous current collector is 20-70%.
4. The positive electrode lithium supplement current collector according to claim 1, wherein: The porous current collector has first pores with a pore size of 50nm-100nm and second pores with a pore size of 10μm-100μm, the pore volume of the first pores accounts for 10-30% of the total pore volume, and the pore volume of the second pores accounts for 70-90% of the total pore volume.
5. The positive electrode lithium supplement current collector according to claim 4, wherein: The oxygen capture agent is accommodated in the first pores, and the lithium supplement agent is accommodated in the second pores.
6. The positive electrode lithium supplement current collector according to claim 1, wherein: Based on 100 parts by weight of the positive electrode lithium replenishing current collector, the content of the oxygen capture agent is 0.1 to 5 parts by weight, and the content of the lithium replenishing agent is 1 to 50 parts by weight.
7. The positive electrode lithium supplement current collector according to claim 1, wherein: The pores of the porous current collector further contain a binder and a conductive agent, and the weight ratio of the lithium supplement, the binder and the conductive agent is 100: (1-20): (0.5-20).
8. The positive electrode lithium supplement current collector according to claim 7, wherein: The conductive agent includes at least one of carbon black, carbon tube and graphene.
9. The method for preparing the positive electrode lithium supplement current collector according to any one of claims 1 to 8, characterized in that: The method includes: A porous current collector is obtained, and a mixed slurry containing an oxygen capture agent, a lithium supplement agent and a solvent is prepared; The mixed slurry is loaded into the pores of the porous current collector, and then the solvent is removed to obtain a positive electrode lithium supplement current collector.
10. The method according to claim 9, wherein: Based on 100 parts by weight of the mixed slurry, the content of the solvent is 40 to 80 parts by weight; And / or, the method of loading the mixed slurry into the pores of the porous current collector is a vacuum impregnation method, and the conditions of the vacuum impregnation method include: a vacuum degree of 5-50 Pa, a temperature of 20-50° C., and an impregnation time of 5-15 h.
11. The method according to claim 9, wherein: The porous current collector has a first pore with a pore size of 50 nm to 100 nm and a second pore with a pore size of 10 μm to 100 μm, the pore volume of the first pore accounts for 10 to 30% of the total pore volume, and the pore volume of the second pore accounts for 70 to 90% of the total pore volume; The method for preparing the positive electrode lithium supplement current collector comprises: The foil-shaped current collector is subjected to a first etching treatment to obtain a current collector containing the first hole; wherein the conditions of the first etching treatment include: an ion beam current of 10-30 pA, a dwell time of 100-300 μs, a laser drilling frequency of 100-200 Hz, and a drilling speed of 1-2 m / min; Prepare a first slurry containing the oxygen capture agent, and load the first slurry into the first hole of the current collector containing the first hole by a first vacuum impregnation to obtain a current collector after the first vacuum impregnation; wherein the conditions of the first vacuum impregnation include: a vacuum degree of 5-50 Pa, a temperature of 20-50° C., and an impregnation time of 5-15 h; The current collector after the first vacuum impregnation is subjected to a second etching treatment to obtain a current collector containing the second hole; wherein the conditions of the second etching treatment include: an ion beam current of 10-30 pA, a dwell time of 300-500 μs, a laser drilling frequency of 100-200 Hz, and a drilling speed of 0.5-1.5 m / min; A second slurry containing the lithium replenishing agent and a solvent is prepared, and the second slurry is loaded into the second hole of the current collector containing the second hole by a second vacuum impregnation, and then the solvent is removed to obtain a positive electrode lithium replenishing current collector; wherein the conditions of the second vacuum impregnation include: a vacuum degree of 5-50 Pa, a temperature of 20-50° C., and an impregnation time of 5-15 h.
12. A positive electrode sheet, characterized in that: The invention comprises the positive electrode lithium replenishing current collector as claimed in any one of claims 1 to 8 and a positive electrode active material layer arranged on the surface of the positive electrode lithium replenishing current collector.
13. A lithium ion battery, characterized in that: Including the positive electrode sheet as described in claim 12.
14. An electrical device, characterized in that: Including the lithium ion battery as claimed in claim 13.