Automobile steering intermediate shaft and production process
Through mold forming and heat treatment technology, combined with dip-coating anti-carburization agent and carburizing treatment, the problems of complexity of intermediate shaft processing and unstable quality in the existing technology are solved, and high-precision and efficient intermediate shaft production is achieved.
Patent Information
- Application Number
- CN202411058178.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-08-02
AI Technical Summary
The split processing technology of the existing automobile steering intermediate shaft is complex, the processing precision is high, and the welding or riveting quality is prone to defects, resulting in low production efficiency and unstable quality.
The shaft fork and tube fork are integrally formed through a mold, and arc-shaped and inclined convex parts are formed through heat treatment and forging. Combined with dipping anti-carburizing agent and carburizing treatment, the surface hardness and accuracy are improved and quality defects caused by welding or riveting are avoided. .
It improves the accuracy and production efficiency of the shaft fork and tube fork, reduces the risk of quality defects, ensures the high precision and strength of the intermediate shaft, and simplifies the production process.
Smart Images

Figure CN118579133B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of automobile steering systems, in particular to an automobile steering intermediate shaft and a production process. Background Art
[0002] Reference Figure 1 As shown, the intermediate shaft is one of the core components of the automobile steering system. It is connected between the steering gear and the steering column to transmit steering motion and steering force. The intermediate shaft mainly includes a tube fork and a shaft fork, and the two are driven and connected by steel balls and splines.
[0003] The steel ball type shaft and fork adopted in the prior art are split type, and the steel ball type tube fork is also split type, that is, the shaft and fork of the steel ball type shaft fork are processed separately, and the shaft is treated with carburizing or carbonitriding to improve its surface hardness and increase its service life, while the fork does not need the above-mentioned heat treatment. The two are then initially positioned through spline matching, and then the shaft and fork are welded or riveted to connect the shaft and fork as one. Similarly, the steel ball type tube fork also has the tube and fork processed separately, and the tube is treated with nitrocarburizing, while the fork does not need the above-mentioned heat treatment, and then the two are directly welded or riveted to connect as one. The above-mentioned split processing method not only has many processes, but also requires high processing precision for the matching between the shaft and fork or the tube and fork, and has great processing difficulty, and the risk of quality defects in welding or riveting is high. Summary of the invention
[0004] The object of the present invention is to provide an automobile steering intermediate shaft and a production process to solve the problems raised in the above background technology.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: a production process of an automobile steering intermediate shaft, the intermediate shaft comprises a shaft fork and a tube fork, wherein the shaft fork is integrally formed by forging a shaft and a shaft yoke, and the tube fork is integrally formed by forging a tube and a tube yoke:
[0006] The one-piece molding process of the shaft fork and the tube fork includes the following steps:
[0007] After the raw material is subjected to the first heat treatment, the first forging is performed to form large and small diameters, wherein the shaft yoke / tube yoke area is the large diameter and the shaft / tube area is the small diameter;
[0008] After the semi-finished product after the first forging is subjected to a second heat treatment, a second forging is performed. The second forging is a forming forging. An arc-shaped convex portion is formed on the outer side of the shaft yoke / tube yoke punching position. The diameter of the arc-shaped convex portion is larger than the diameter of the hole to be punched. An inclined convex portion is formed on the inner side of the shaft yoke / tube yoke punching position. The width of the inclined convex portion is larger than the diameter of the hole to be punched.
[0009] The semi-finished product of the second forged shaft is forged for the third time to form a slideway for the steel balls to roll on the shaft / tube;
[0010] For the semi-finished product after the third forging, after cleaning, anti-carburizing agent is applied to the punching position of the shaft yoke / tube yoke by dipping;
[0011] Carry out the third heat treatment, using carburizing or carbonitriding to improve the surface hardness;
[0012] The shaft yoke / tube yoke is punched, and after the arc-shaped protrusion and the inclined protrusion are punched and material is removed, a reinforcing rib structure is formed around the hole.
[0013] Preferably, in the second forging, a precision forging die is used for precision forging, the precision forging die provides a die cavity with an arc-shaped protrusion and an inclined protrusion, a vent hole is provided on the precision forging die body, and after the upper and lower dies are closed, a closed forging process is used for forging.
[0014] Preferably, the first heat treatment is a spheroidizing annealing process, wherein the raw materials are first placed in layers in a vacuum annealing furnace, the vacuum annealing furnace is continuously evacuated, and then a carrier gas is introduced for re-pressurization and heating. The vacuuming, re-pressurization and heating cycles are continued at least twice, and the temperature is controlled between 730°C and 770°C during the entire cycle.
[0015] Preferably, the anti-carburizing agent is an inorganic anti-carburizing material with a viscosity of 5000mPa·s-6000mPa·s. The thickness of the anti-carburizing agent coating on the semi-finished product after dipping is 0.3-0.5mm.
[0016] Preferably, the third heat treatment is a carburizing process using a carburizing furnace. First, the semi-finished product coated with the anti-carburizing agent is placed in a carburizing container containing the carburizing agent, and then a step-by-step heating and insulation step is performed. Then, a carburizing atmosphere is introduced to perform a carburizing step, and finally, the semi-finished product is cooled to room temperature and taken out of the furnace.
[0017] Preferably, the arc-shaped protrusion is a teardrop-shaped structure, and the main body of the teardrop-shaped structure is provided with an extension section at the front end of the hemispherical structure, and the thickness and width of the extension section gradually decrease toward the outer end of the shaft yoke / tube yoke until the outer end edge of the shaft yoke / tube yoke.
[0018] Preferably, the thickness of the inclined protrusion is between 0.5 mm and 1.5 mm, and the thickness of the inclined protrusion gradually decreases toward the outer end of the shaft yoke / tube yoke.
[0019] Preferably, the semi-finished product after the third forging is coated with anti-carburizing agent by dipping, and a dipping device is used. The dipping device includes a dipping tank and a transfer robot. The transfer robot includes a rotating jaw, and the rotating jaw is fixed at the end of an arc-shaped mechanical arm. The bending arc of the arc-shaped mechanical arm is between 80° and 90°. One end of the arc-shaped mechanical arm is fixed on the circumferential side of the rotating shaft. In the starting position, the axial direction of the rotating jaw is horizontal in the X direction, and the semi-finished product is coaxially clamped. The rotating shaft starts to rotate. When the rotating jaw rotates to the bottom, the axial direction of the rotating jaw is inclined downward. The dipping tank is located at the bottom of the rotating jaw, and the semi-finished product enters the dipping tank in an inclined state. The punching position is in the anti-carburizing agent in the dipping tank. At this time, the rotating jaw is turned on and rotated 360 degrees so that the punching position is in full contact with the anti-carburizing agent. The rotating shaft continues to rotate to the end position. At the end position, the axial direction of the rotating jaw is horizontal in the Y direction.
[0020] Preferably, the transfer robot includes two sets of symmetrically arranged rotating jaws and a rotating shaft. The transfer robot also includes a gear and a rack structure arranged in the middle. Both ends of the gear are fixedly connected with a universal joint. The two rotating shafts are symmetrical and inclined at 45° to the horizontal X direction on both sides, and are respectively connected to the universal joints on both sides.
[0021] The present invention also provides an automobile steering intermediate shaft, which is produced by adopting the above process.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] The shaft and yoke of the process shaft fork provided by the present invention are integrally formed by a mold, and the entire shaft fork has high precision, avoiding quality defects caused by welding or riveting; during the heat treatment ring connection, anti-carburizing agent is applied to the punched holes of the yoke to avoid the shaft and fork being heat treated together, and the fork's own strength and rigidity at the punched holes are reduced due to the heat treatment; similarly, the tube and yoke of the steel ball type tube fork are also integrally formed by a mold, and the entire tube fork has high precision. During the heat treatment ring connection, anti-carburizing agent is also applied to the punched holes of the yoke.
[0024] In addition, the present invention adopts a dipping method to apply the anti-carburizing agent, thereby improving production efficiency.
[0025] It is worth mentioning that the present application has specifically designed a unique blank (semi-finished product) structure, that is, in the second forging forming link, an arc-shaped protrusion is formed on the outside of the yoke, and an inclined protrusion is set on the inside. Due to the use of mold casting, burrs will be generated, especially the annular reinforcing rib structure will have more obvious burr phenomenon after forging is completed. This is because the width and thickness of this type of reinforcing rib are small, and the structure has multiple sections of ups and downs, which are prone to residual edges and burrs. These burrs will seriously affect the link of applying anti-carburizing agent. If an additional deburring process is added to solve the burr, production efficiency will be affected. Therefore, in the process of forming, the present invention forms a certain margin at the yoke punching place (also the key position for applying anti-carburizing agent), which can reduce the burrs here and facilitate application. The protrusion provided is conducive to the flow of coating, and is also conducive to the uniformity of coating during dip coating, avoiding the occurrence of local "air bags" and reducing the phenomenon of coating droplets hanging. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is an intermediate shaft structure in the prior art;
[0027] Figure 2 It is a schematic diagram of the main steps of the production process of the present invention;
[0028] Figure 3 It is a schematic diagram of the structure of the forging blank;
[0029] Figure 4 This is a schematic diagram of the structure of the transfer robot of the present invention;
[0030] Figure 5 This is a schematic diagram of the operating steps of the dip coating of the present invention;
[0031] Figure 6 This is a metallographic diagram of the carburizing position mentioned in the embodiment of the present invention.
[0032] In the figure: 1, shaft fork; 2, tube fork; 21, yoke; 22, arc-shaped protrusion; 23, inclined protrusion; 24, avoidance groove; 3, rack; 4, gear; 5, arc-shaped mechanical arm; 6, rotating claw; 7, universal joint; 8, rotating shaft. DETAILED DESCRIPTION
[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] See also Figure 2As shown in, this embodiment provides an automobile steering intermediate shaft and a production process, 1. The intermediate shaft includes a shaft fork 1 and a tube fork 2, wherein the shaft fork 1 is formed into one piece by forging a shaft and a shaft yoke, and the tube fork 2 is formed into one piece by forging a tube and a tube yoke:
[0035] The one-piece molding process of the shaft fork and the tube fork includes the following steps:
[0036] After the first heat treatment of the raw materials, spheroidizing annealing, first the raw materials are placed in layers in a vacuum annealing furnace, the vacuum annealing furnace is continuously evacuated, and then a carrier gas (usually nitrogen) is introduced for re-pressurization and heating. The vacuum evacuation, re-pressurization and heating cycle is continued for at least two times. During the entire cycle, the temperature is controlled between 730℃-770℃.
[0037] The first forging is performed to form large and small diameters, wherein the shaft yoke / tube yoke area is the large diameter and the shaft / tube area is the small diameter.
[0038] After the semi-finished product after the first forging is subjected to a second heat treatment, a second forging is performed; the difference between the second heat treatment step and the first heat treatment step is that the temperature of the second heat treatment is controlled between 650°C and 700°C.
[0039] The second forging process is to form an arc-shaped protrusion 22 on the outside of the punching position of the shaft yoke / tube yoke through a forging die, and the diameter of the arc-shaped protrusion 22 is larger than the diameter of the hole to be punched, and an inclined protrusion 23 is formed on the inside of the punching position of the shaft yoke / tube yoke, and the width of the inclined protrusion 23 is larger than the diameter of the hole to be punched;
[0040] In the second forging, a precision forging die is used for precision forging. The precision forging die provides a die cavity with an arc-shaped protrusion 22 and an inclined protrusion 23. A vent hole is provided on the precision forging die body. After the upper and lower dies are closed, a closed forging process is used for forging. Flash-free forging can be achieved, and the flash of the outer contour can be reduced (that is, the burr generation can be minimized), which is convenient for subsequent processes and improves the qualified rate.
[0041] The function of the arc-shaped protrusion 22 is to reduce burrs. Since paint needs to be applied here later, a larger arc-shaped protrusion is formed during forging. Due to its large surface area, the burrs generated during forging are less than those of the circular and narrow reinforcing ribs, which is convenient for applying paint. And after drilling, a circular reinforcing rib structure is naturally formed through the arc-shaped protrusion 22. The structure of the arc-shaped protrusion 22 can be a hemispherical structure. Since its radius is larger than the radius of the hole to be drilled, a circle of reinforcing ribs is formed after drilling. In addition, in another preferred embodiment, referring to Figure 3 As shown ( Figure 3In the figure, the tube fork 2 is taken as an example, but in fact, the yoke 21 of the shaft fork 1 and the tube fork 2 is the same), the arc-shaped protrusion 22 is a teardrop-shaped structure, and its main body is provided with an extension section at the front end of the hemispherical structure, and the thickness and width of the extension section are gradually reduced toward the outer end of the yoke 21 until the outer end edge of the shaft yoke / tube yoke. After drilling, the teardrop-shaped structure, in addition to forming a reinforcing rib on the outer circle of the hole, also forms a rib block structure at the front end, which can improve the strength of the fork mouth.
[0042] The function of the inclined protrusion 23 is similar to that of the arc-shaped protrusion 22, except that the inclined protrusion 23 with a low thickness (0.5mm-1.5mm) is located on the inner side, which is more convenient for dip coating. If the inner side is also provided with an arc-shaped high protrusion, the paint will be retained in the middle, which will cause inconvenience to subsequent work, such as affecting the drying of the paint, causing stress in the high temperature link to cause the paint to fall off, etc. The specific structure of the inclined protrusion 23 can be found in Figure 3 As shown, the thickness of the inclined protrusion 23 gradually decreases toward the outer end of the shaft yoke / tube yoke. In addition, the inner side of the outer end of the yoke 21 has a reduced thickness escape groove 24, which is located at the end of the inclined protrusion 23. The escape groove 24 is for the convenience of subsequent universal joint installation. It can be directly formed during forging.
[0043] The semi-finished product after the second forging is subjected to surface phosphorus saponification treatment. Surface phosphorus saponification treatment specifically refers to placing the semi-finished product in a phosphating solution (phosphate solution, such as zinc phosphate, calcium phosphate) to form a phosphating film on the surface, and then placing the semi-finished product with the phosphating film in a soap solution, in which the saturated fatty acid soap reacts with the phosphating film to form a fatty acid film (fatty acid zinc, fatty acid calcium) and a soap film layer. The workpiece treated with the above phosphorus saponification treatment has increased plastic thickness, and the formed film layer has a lubricating effect, which can greatly reduce heat and prevent metal sintering and melting.
[0044] After the surface is phosphorus saponified, the third forging is performed to form the inner / outer spline slideway for the steel ball to roll on the shaft / tube; the slideway on the shaft fork 1 is located on the outer surface and is forged in one step using a forging die and a press. The slideway of the tube fork 2 is located inside, so the third forging of the tube fork 2 can be completed in two forging steps, that is, after the first forging step is completed, it is properly cooled, and then heated for the second time and forged again to ensure the accuracy of the slideway.
[0045] After the third forging is completed, the semi-finished product is turned, mainly for processing the shape and structure, such as turning off excess length or small flash around the shape to meet the size requirements.
[0046] After cleaning, the semi-finished product is coated with anti-carburizing agent at the punching position of the shaft yoke / tube yoke by dipping; in this step, a dipping device is used, referring to Figure 4 as well as Figure 5 As shown, the dipping device includes a dipping pool and a transfer robot. The transfer robot includes a rotating jaw 6. The rotating jaw 6 is fixed at the end of the arc-shaped mechanical arm 5. The bending arc of the arc-shaped mechanical arm 5 is between 80° and 90°. One end of the arc-shaped mechanical arm 5 is fixed on the circumferential side of the rotating shaft 8. In the starting position, the axial direction of the rotating jaw 6 is in an X-direction horizontal state, the semi-finished product is coaxially clamped, and the rotating shaft 8 starts to rotate. When the rotating jaw 6 rotates to the bottom, the axial direction of the rotating jaw 6 is in an inclined downward state. The dipping pool is located at the bottom of the rotating jaw 6, and the semi-finished product enters the dipping pool in an inclined state. The punching position is in the anti-carburizing agent in the dipping pool. At this time, the rotating jaw 6 is opened and rotated 360 degrees so that the punching position is in full contact with the anti-carburizing agent. The rotating shaft 8 continues to rotate to the end position. At the end position, the axial direction of the rotating jaw 6 is in a Y-direction horizontal state.
[0047] The specific structure is as follows Figure 4 The transfer robot includes two symmetrically arranged groups of rotating jaws 6 and a rotating shaft 8. The transfer robot also includes a gear 4 and a rack 3 structure arranged in the middle. Both ends of the gear 4 are fixedly connected with a universal joint 7. The two rotating shafts 8 are symmetrical and arranged on both sides at an angle of 45° to the horizontal X direction, and are respectively connected to the universal joints 7 on both sides. Two groups of dipping pools are provided, corresponding to two groups of rotating jaws 6, and the two groups of dipping pools are connected to each other, and the anti-carburizing agent in the dipping pool forms a flow cycle.
[0048] Traditional dip coating usually adopts a suspended assembly line, with a dip coating pool at the bottom. By setting the workpiece suspension height of the assembly line, the workpiece enters the dip coating pool to complete the dip coating. However, this type of assembly line is more suitable for large workpieces or coating dip coating work that requires a long time to dry. The production subject of this application is to mention smaller hardware workpieces, and the anti-carburizing agent itself does not need to be dried for a long time, so there is no need for a long assembly line operation, only a simple transfer is required.
[0049] The transfer robot structure disclosed in this embodiment has the following design features: First, according to the three-dimensional coordinate axis, the transfer station path is set in the three directions of XYZ. Figure 5As shown, the loading station is arranged along the X direction, the dipping station is arranged along the Z direction, and the unloading station is arranged along the Y direction. According to the three stations in different directions, the production rhythm can be reasonably arranged to improve production efficiency, and the equipment installation of the corresponding process can also be reasonably arranged. Secondly, the rotating jaw 6 of the transfer robot swings along an arc path during operation, and the workpiece will have a centrifugal force on it. With the arc-shaped protrusion 22 and the inclined protrusion 23 set on the workpiece itself, the excess paint can be smoothly thrown off. For example, the arc-shaped protrusion of the water drop-shaped structure has a relatively smooth arc transition, and it plays a role in guiding the paint on the outer side in the extension section, which can accelerate the outflow and avoid the formation of droplets at the end. The inclined protrusion 23 cooperates with the avoidance groove 24 to allow the excess paint on the inside to be discharged. Finally, refer to Figure 5 As shown, the workpiece is tilted in the dipping pool. When the workpiece is stopped, the rotating clamp 6 rotates around its own axis, and the workpiece also rotates around its own axis. Because the coating of the workpiece is a symmetrical structure with an inner and outer side, the rotating action can make the outer and inner surfaces more evenly and thoroughly coated. At the same time, the workpiece is tilted into the dipping pool, which can make the depth of the dipping pool smaller. The smaller the depth of the dipping pool, the smaller the depth of the internal coating, which is not easy to produce precipitation and affect the anti-carburization effect of the coating.
[0050] The anti-carburizing agent uses inorganic anti-carburizing material with a viscosity of 5000mPa·s-6000mPa·s. The viscosity cannot be too small, otherwise the adhesion effect is poor and it is not suitable for the dip coating process. It cannot be too large, otherwise the coating thickness will become thicker and easy to fall off after drying. The thickness of the anti-carburizing agent coating of the semi-finished product after dip coating is 0.3-0.5mm.
[0051] The third heat treatment is carried out, and carburizing or carbonitriding treatment is used to improve the surface hardness; the third heat treatment is a carburizing process using a carburizing furnace. First, the semi-finished product coated with anti-carburizing agent is placed in a carburizing container containing a carburizing agent, and then a step-by-step heating and insulation step is performed (the temperature is raised from 300 degrees to 900 degrees, and each stage is kept warm for at least 30 minutes, such as 300 degrees for 30 minutes, then raised to 500 degrees, continued to be kept warm for 30 minutes, and then heated again...), and then a carburizing atmosphere is introduced (usually acetylene and nitrogen are alternately introduced) for the carburizing step, and finally cooled to room temperature and taken out of the furnace. The hardness requirement at the punching point is Hv160-320, and the hardness requirement at other carburizing positions is Hv600-700. Refer to the metallographic diagram of the carburizing position after the third heat treatment Figure 6 shown.
[0052] The shaft yoke / tube yoke is punched, and the arc-shaped protrusion 22 and the inclined protrusion 23 are punched and removed. When the shaft hole is formed, a reinforcing rib structure is naturally formed around the shaft hole. Finally, the workpiece is finely ground to form a finished product.
[0053] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A production process for an automobile steering intermediate shaft, Features: The intermediate shaft comprises a shaft fork (1) and a tube fork (2), wherein the shaft fork (1) is formed into one piece by forging a shaft and a shaft fork, and the tube fork (2) is formed into one piece by forging a tube and a tube fork: The one-piece molding process of the shaft fork and the tube fork includes the following steps: After the raw material is subjected to the first heat treatment, the first forging is performed to form large and small diameters, wherein the shaft yoke / tube yoke area is the large diameter and the shaft / tube area is the small diameter; The first heat treatment is spheroidizing annealing. First, the raw materials are placed in layers in a vacuum annealing furnace, the vacuum annealing furnace is continuously evacuated, and then nitrogen is introduced for re-pressurization and heating. The vacuum evacuation, re-pressurization and heating cycle are continued for at least two times. During the entire cycle, the temperature is controlled between 730°C and 770°C. After the semi-finished product after the first forging is subjected to a second heat treatment, a second forging is performed; The difference between the second heat treatment step and the first heat treatment step is that the temperature of the second heat treatment is controlled between 650°C and 700°C; The second forging is a forming forging, forming an arc-shaped protrusion (22) on the outside of the shaft yoke / tube yoke punching position, the diameter of the arc-shaped protrusion (22) is larger than the diameter of the hole to be punched, and forming an inclined protrusion (23) on the inside of the shaft yoke / tube yoke punching position, the width of the inclined protrusion (23) is larger than the diameter of the hole to be punched; In the second forging, a precision forging die is used for precision forging. The precision forging die provides a die cavity with an arc-shaped protrusion (22) and an inclined protrusion (23). A vent hole is provided on the precision forging die body. After the upper and lower dies are closed, a closed forging process is used for forging. The semi-finished product after the second forging is subjected to surface phosphorus saponification treatment; After the surface is treated with phosphorus saponification, the third forging is performed to form the inner / outer spline slideways for the steel balls to roll on the shaft / tube; After the third forging is completed, the semi-finished product is turned; After cleaning, the semi-finished product is coated with an anti-carburizing agent at the position where the holes on the shaft yoke / tube yoke are punched by dipping. In this step, a dipping device is used, which includes a dipping tank and a transfer robot. The transfer robot includes a rotating clamp (6), which is fixed at the end of an arc-shaped mechanical arm (5). The bending arc of the arc-shaped mechanical arm (5) is between 80° and 90°. One end of the arc-shaped mechanical arm (5) is fixed to the circumference of the rotating shaft (8). When in the starting position, the axial direction of the rotating clamp (6) is the X-axis direction. In a flat state, the semi-finished product is coaxially clamped, and the rotating shaft (8) starts to rotate. When the rotating jaw (6) rotates to the bottom, the axial direction of the rotating jaw (6) is in an inclined downward state, and the dipping pool is located at the bottom of the rotating jaw (6). The semi-finished product enters the dipping pool in an inclined state, and the punching position is in the anti-carburizing agent in the dipping pool. At this time, the rotating jaw (6) is opened and rotated 360 degrees, so that the punching position is fully in contact with the anti-carburizing agent, and the rotating shaft (8) continues to rotate to the end position. At the end position, the axial direction of the rotating jaw (6) is in a Y-direction horizontal state; The transfer robot comprises two sets of symmetrically arranged rotating jaws (6) and a rotating shaft (8), and the transfer robot also comprises a gear (4) and a rack (3) structure arranged in the middle, both ends of the gear 4 are fixedly connected with a universal joint (7), the two rotating shafts (8) are symmetrically arranged on both sides and inclined at 45 degrees with respect to the horizontal X direction, and are respectively connected to the universal joints (7) on both sides by transmission, and two sets of dipping pools are arranged, corresponding to the two sets of rotating jaws (6), and the two sets of dipping pools are connected to each other, and the anti-carburizing agent in the dipping pool forms a flow circulation; Carry out the third heat treatment, using carburizing or carbonitriding to improve the surface hardness; The third heat treatment is a carburizing process using a carburizing furnace. First, the semi-finished product coated with anti-carburizing agent is placed in a carburizing container containing a carburizing agent, and then a step-by-step heating and insulation step is performed, with the temperature rising from 300 degrees to 900 degrees, and the temperature is kept at least 30 minutes in each stage. Then, acetylene and nitrogen are alternately introduced to perform the carburizing step, and finally cooled to room temperature before being taken out of the furnace. The hardness requirement for the subsequent drilling position is Hv160-320, and the hardness requirement for other carburizing positions is Hv600-700; The shaft yoke / tube yoke is punched, and after the arc-shaped protrusion (22) and the inclined protrusion (23) are punched and material is removed, a reinforcing rib structure is formed around the hole.
2. A production process for an automobile steering intermediate shaft according to claim 1, Features: The anti-carburizing agent adopts inorganic anti-carburizing material with a viscosity of 5000mPa·s-6000mPa·s. The thickness of the anti-carburizing agent coating of the semi-finished product after dipping is 0.3-0.5mm.
3. The production process of an automobile steering intermediate shaft according to claim 1, Features: The arc-shaped raised portion (22) is a teardrop-shaped structure. The main body of the teardrop-shaped structure is provided with an extension section at the front end of the hemispherical structure. The thickness and width of the extension section gradually decrease toward the outer end of the shaft yoke / tube yoke until reaching the outer end edge of the shaft yoke / tube yoke.
4. A production process for an automobile steering intermediate shaft according to claim 1, Features: The thickness of the inclined protrusion (23) is between 0.5 mm and 1.5 mm, and the thickness of the inclined protrusion (23) gradually decreases towards the outer end of the shaft yoke / tube yoke.
5. An automobile steering intermediate shaft, Features: The invention is produced by adopting the automobile steering intermediate shaft production process described in any one of claims 1 to 4.
Citation Information
Patent Citations
Driver and a method and arrangement to produce it
CN101557890A
Processing method for universal-joint flange yoke of transmission shaft of heavy-duty car
CN102107345A