Copper embedded nitrogen doped carbon composite material, preparation method and application thereof
By using copper-embedded nitrogen-doped carbon composites as catalysts in microbial fuel cells, the problems of low cathode oxygen reduction efficiency and high cost are solved, achieving efficient energy conversion and efficient degradation of rhodamine B, which is significantly better than commercial platinum-based ones. catalyst.
Patent Information
- Application Number
- CN202411060131.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-08-05
AI Technical Summary
Existing microbial fuel cells have low oxygen reduction reaction efficiency at the cathode, and traditional precious metal catalysts are costly and resource scarce, making them difficult to be widely used, especially when dealing with organic pollutants such as rhodamine B.
Through ultrasonic mixing and co-pyrolysis methods, nitrogen is introduced into metal-organic framework-derived carbon materials to prepare copper-embedded nitrogen-doped carbon composites, and compounded with hollow fibrous polymers to form catalysts with high adsorption properties for Improve the electricity production capacity of microbial fuel cells and the degradation efficiency of rhodamine B.
It significantly improves the catalytic efficiency of the oxygen reduction reaction and the stability of the composite material, achieving efficient energy conversion and efficient degradation of rhodamine B. The catalytic efficiency is better than that of commercial platinum-based catalysts, and it has important potential for environmental purification applications.
Smart Images

Figure CN118588957B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of nanocomposite materials, and in particular to a copper-embedded nitrogen-doped carbon composite material, a preparation method and application thereof. Background Art
[0002] Rhodamine B, a widely used water-soluble dye, has attracted much attention due to its potential harm to the environment and human health. This dye is not only toxic to aquatic organisms, but may also cause liver and kidney damage and irritate the skin and respiratory system. With the acceleration of industrialization, the emission of organic pollutants such as Rhodamine B has continued to increase, causing serious pollution to the aquatic environment. Therefore, developing effective methods to degrade Rhodamine B and reduce its negative impact on ecosystems and human health has become an urgent task in the field of environmental governance.
[0003] To address this challenge, microbial fuel cells (MFCs), as an innovative environmental purification technology, provide a sustainable solution to convert organic pollutants into electrical energy. MFCs convert organic matter in wastewater into electrical energy through microbial metabolism, achieving pollutant reduction and energy recovery. However, the performance of microbial fuel cells is largely limited by the oxygen reduction reaction efficiency of their cathode. Traditional noble metal-based catalysts, such as platinum, have high catalytic activity, but their high cost and resource scarcity limit the widespread application of microbial fuel cells.
[0004] To address this problem, carbon materials derived from metal organic frameworks (MOFs) have become a hot topic of research due to their unique porous structure and tunable chemical composition. In particular, nitrogen-doped carbon materials have attracted much attention because they can provide more active sites and improve electronic conductivity. Copper has suitable biocompatibility. Therefore, it is worth further studying how to prepare copper-embedded nitrogen-doped carbon materials with high stability and high oxygen reduction reaction catalytic efficiency and use them as cathode catalysts in microbial fuel cells to enhance power generation and rhodamine B degradation capabilities. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a copper-embedded nitrogen-doped carbon composite material, a preparation method and an application thereof in view of the deficiencies in the above-mentioned prior art. Firstly, the element N is successfully introduced into the carbon material derived from the metal organic framework by ultrasonic mixing and co-pyrolysis, and graphite phase carbon nitride (g-C3N4) is used as a nitrogen source for doping. Subsequently, this nitrogen-doped carbon material is compounded with a polymer having a hollow fiber morphology to form a new composite material with enhanced adsorption properties, so as to achieve high power generation and Rhodamine B degradation capabilities of microbial fuel cells.
[0006] To achieve the above object, the technical solution adopted by the present invention is: In a first aspect of the present invention, a method for preparing a copper-embedded nitrogen-doped carbon composite material is provided, comprising the following steps:
[0007] S1. Preparation of Cu-based metal organic framework materials:
[0008] Copper (II) acetate monohydrate is dissolved to prepare solution A, 2,5-dihydroxyterephthalic acid is dissolved to prepare solution B, solution A is added dropwise to solution B, mixed evenly and allowed to stand, solids are collected by filtration, and the obtained solids are recrystallized to obtain a Cu-based metal organic framework material, which is recorded as CDA;
[0009] S2. Preparation of hollow fiber polymer LZU1:
[0010] The trimesic acid and trimesic acid are mixed and dissolved, and then p-phenylenediamine is added after ultrasonic and stirring treatment, and stirred, and glacial acetic acid is added, stirred, and allowed to stand, and the precipitate is collected by filtration, washed, dried, soaked in methanol, rotary evaporated, and vacuum dried to obtain a hollow fiber polymer LZU1;
[0011] S3. Preparation of copper embedded nitrogen doped carbon composite material:
[0012] The CDA and g-C3N4 prepared in step S1 are mixed evenly and then calcined to obtain a CDA / NC composite material; the CDA / NC composite material and the hollow fibrous polymer LZU1 prepared in step S2 are evenly mixed in a solution, stirred, and the solid product is collected and dried under vacuum to obtain a copper-embedded nitrogen-doped carbon composite material, which is recorded as CL / NC.
[0013] Preferably, step S1 specifically comprises:
[0014] S1-1, dissolving 104-419 mg of copper (II) acetate monohydrate in 10-20 mL of a mixed solvent 1 consisting of N,N-dimethylformamide (DMF) and acetonitrile (CH3CN) to obtain a solution A, wherein the volume ratio of N,N-dimethylformamide to acetonitrile is 1:1-1:4;
[0015] Dissolve 46.8-187.2 mg of 2,5-dihydroxyterephthalic acid in 10-20 mL of a mixed solvent 2 consisting of DMF, CH3CN and deionized water to obtain a solution B, wherein the volume ratio of DMF:CH3CN:deionized water is 1-4:0.5-2:0.1-0.3;
[0016] S1-2, under stirring, according to the volume ratio of solution A: solution B of 1:2-1:10, solution A is added dropwise to solution B at a rate of 3-12 μL / s, and stirring is maintained for 1-4 hours after the addition is completed. The resulting mixed solution is allowed to stand at room temperature for 20-28 hours, filtered, and the solid is collected to obtain a precursor;
[0017] S1-3. Add 5-20 mg of the precursor to a mixed solution containing 10-40 mg of sodium dodecylbenzene sulfonate, 6-24 mL of methanol and 0.5-2 mL of deionized water, let stand at room temperature for 4-16 hours for recrystallization, collect the precipitate by filtration, wash with deionized water, and vacuum dry at 50-80°C for 6-24 hours to obtain a Cu-based metal organic framework material, recorded as CDA.
[0018] Preferably, step S2 specifically comprises:
[0019] S2-1, dissolve 40-160 mg of trimesic acid and 20-80 mg of trimesic acid in 5-20 mL of 1,4-dioxane, and disperse by ultrasonication for 5-15 min. After stirring for 5-15 min, add 80-320 mg of p-phenylenediamine to the resulting solution, continue stirring for 5-15 min, add 0.1-0.4 mL of 1.5-6 mol / L glacial acetic acid, continue stirring for 20-28 hours, and then seal and stand at room temperature for 45-51 h;
[0020] S2-2. Collect the precipitate by filtration, wash it three times with tetrahydrofuran and acetone respectively, and dry it under vacuum at 50-70°C for 20-28h; soak the obtained solid in methanol, and then rotary evaporate it, repeat 2-6 times, and finally vacuum dry it at 50-70°C for 20-28h to obtain a hollow fiber polymer LZU1.
[0021] Preferably, step S3 specifically comprises:
[0022] S3-1, adding 25-100 mg of CDA prepared in step S1 to 10-40 mL of methanol, ultrasonically dispersing for 5-15 min, adding 50-200 mg of g-C3N4 to the resulting solution, ultrasonically dispersing for 0.5-2 h, rotary evaporation to remove the solvent, vacuum drying the resulting mixture powder at 50-70 ° C for 6-24 hours, and calcining at 600-900 ° C for 1-3 h under nitrogen protection to obtain a CDA / NC composite material;
[0023] S3-2, disperse 15-60 mg of CDA / NC in 10-40 mL of methanol, then add 6-24 mg of the hollow fibrous polymer LZU1 prepared in step S2, ultrasonically disperse for 20-40 min, stir at room temperature for 12-48 h, and vacuum dry the resulting mixture at 50-70 ° C for 1-4 hours to obtain a copper-embedded nitrogen-doped carbon composite material, recorded as CL / NC.
[0024] Preferably, in step S3-1, the calcination temperature is 700°C.
[0025] Preferably, the method for preparing the copper-embedded nitrogen-doped carbon composite material comprises the following steps:
[0026] S1. Preparation of Cu-based metal organic framework materials:
[0027] S1-1, dissolving 209.63 mg of copper (II) acetate monohydrate in 15 mL of a mixed solvent 1 consisting of N,N-dimethylformamide (DMF) and acetonitrile (CH3CN) to obtain a solution A, wherein the volume ratio of N,N-dimethylformamide to acetonitrile is 1:2;
[0028] 93.62 mg of 2,5-dihydroxyterephthalic acid was dissolved in 15.75 mL of a mixed solvent 2 consisting of DMF, CH3CN and deionized water to obtain a solution B, wherein the volume ratio of DMF:CH3CN:deionized water was 2:1:0.15;
[0029] S1-2, under stirring at a speed of 200 rpm, according to the volume ratio of solution A:solution B of 1:5, solution A was added dropwise to solution B at a speed of 6 μL / s, and stirring was maintained for 2 hours after the addition was completed. The resulting mixed solution was allowed to stand at room temperature for 24 hours, filtered, and the solid was collected to obtain a precursor;
[0030] S1-3, adding 10 mg of the precursor to a mixed solution containing 20 mg of sodium dodecylbenzene sulfonate, 12 mL of methanol and 1 mL of deionized water, standing at room temperature for 8 h for recrystallization, collecting the precipitate by filtration, washing with deionized water, and vacuum drying at 65 ° C for 12 hours to obtain a Cu-based metal organic framework material, recorded as CDA;
[0031] S2. Preparation of hollow fiber polymer LZU1:
[0032] S2-1, dissolve 80 mg of trimesaldehyde and 40 mg of trimesic acid in 10 mL of 1,4-dioxane, and disperse by ultrasonication for 10 min. After stirring for 10 min, add 160 mg of p-phenylenediamine to the resulting solution, continue stirring for 10 min, add 0.2 mL of 3 mol / L glacial acetic acid, continue stirring for 24 hours, and then seal and stand at room temperature for 2 days;
[0033] S2-2. Collect the precipitate by filtration, wash it three times with tetrahydrofuran and acetone respectively, and dry it under vacuum at 60°C for 24 hours; soak the obtained solid in methanol, and then rotary evaporate it, repeat three times, and finally dry it under vacuum at 60°C for 24 hours to obtain a hollow fiber polymer LZU1.
[0034] S3. Preparation of copper embedded nitrogen doped carbon composite material:
[0035] S3-1, adding 50 mg of CDA prepared in step S1 to 20 mL of methanol, ultrasonically dispersing for 10 min, adding 100 mg of g-C3N4 to the obtained solution, ultrasonically dispersing for 1 h, and removing the solvent by rotary evaporation. The obtained mixture powder was vacuum dried at 60 ° C for 12 h, heated to 700 ° C at a heating rate of 5 ° C / min under nitrogen protection, and calcined for 2 h to obtain a CDA / NC composite material;
[0036] S3-2, 30 mg of CDA / NC was dispersed in 20 mL of methanol, and then 12 mg of the hollow fibrous polymer LZU1 prepared in step S2 was added, ultrasonically dispersed for 30 min, stirred at room temperature for 12 h, and the resulting mixture was vacuum dried at 60 ° C for 2 hours to obtain a copper-embedded nitrogen-doped carbon composite material: CL / NC.
[0037] A second aspect of the present invention provides a copper-embedded nitrogen-doped carbon composite material, which is prepared by the method as described above.
[0038] The third aspect of the present invention provides an application of the copper embedded nitrogen doped carbon composite material as described above in a microbial fuel cell, and the application method is: the copper embedded nitrogen doped carbon composite material is coated on the cathode surface as a catalyst, and then the obtained cathode is used to assemble a microbial fuel cell. Further preferably, the application method is: the copper embedded nitrogen doped carbon composite material, deionized water, Nafion solution and isopropanol are mixed evenly, and the obtained slurry is evenly coated on the surface of the carbon cloth as a catalyst as a cathode; the carbon brush is used as an anode, and then assembled into a microbial fuel cell.
[0039] In a fourth aspect of the present invention, there is provided an application of the copper embedded nitrogen doped carbon composite material as described above in the degradation of rhodamine B, the application method being: coating the copper embedded nitrogen doped carbon composite material as a catalyst on the surface of a cathode, and then using the obtained cathode to assemble a microbial fuel cell, and using the microbial fuel cell to degrade rhodamine B.
[0040] The beneficial effects of the present invention are:
[0041] The present invention provides a copper-embedded nitrogen-doped carbon composite material, a preparation method thereof and an application thereof in a microbial fuel cell and in the degradation of rhodamine B. The copper-embedded nitrogen-doped carbon composite material CL / NC prepared by the present invention has a unique hollow fiber morphology, significantly improves the specific surface area and the distribution of active sites, which is beneficial to the diffusion and adsorption of active oxygen species and organic pollutant molecules; the introduction of nitrogen doping greatly improves the conductivity and catalytic activity of the composite material, and promotes the kinetics of the oxygen reduction reaction; the embedding of copper not only enhances the stability of the composite material, but also combines with nitrogen doping and the hollow fiber morphology to produce a synergistic enhancement effect, optimizes mass transfer and provides abundant active sites for the oxygen reduction reaction; the composite material of the present invention exhibits excellent performance in microbial fuel cells (MFCs), and also exhibits excellent catalytic effect in the degradation of rhodamine B, and its catalytic efficiency and stability are better than those of commercial platinum-based catalysts, realizing efficient energy conversion in microbial fuel cells (MFCs) and efficient degradation of the organic pollutant rhodamine B, having important application potential in treating industrial wastewater and purifying the environment, and can expand the application scenarios of MFCs.
[0042] In some preferred embodiments, the copper embedded nitrogen-doped carbon composite material prepared by the present invention is used as a cathode catalyst in a microbial fuel cell, and the maximum power density reaches 2291.67±27.75 mW m −2 , a degradation efficiency of over 96% was achieved for various concentrations of Rhodamine B. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 SEM images and TEM images of CDA / NC, LZU1, and CL / NC prepared in Examples 2 and 3;
[0044] Figure 2 The Tafel curves of CL / NC-600 electrode, CL / NC-700 electrode, CL / NC-800 electrode, CL / NC-900 electrode and 20% Pt / C electrode;
[0045] Figure 3 Polarization and power density curves of five groups of microbial fuel cells: CL / NC-600 battery group, CL / NC-700 battery group, CL / NC-800 battery group, CL / NC-900 battery group, and 20% Pt / C battery group;
[0046] Figure 4 These are the test results of the degradation efficiency of Rhodamine B for CL / NC-600 battery pack, CL / NC-700 battery pack, CL / NC-800 battery pack, CL / NC-900 battery pack, and 20% Pt / C battery pack. DETAILED DESCRIPTION
[0047] The present invention is further described in detail below in conjunction with embodiments so that those skilled in the art can implement the invention with reference to the description.
[0048] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.
[0049] The test methods used in the following examples are conventional methods unless otherwise specified. The materials and reagents used in the following examples are all commercially available unless otherwise specified. In the following examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are all conventional products that can be purchased commercially.
[0050] The present invention provides a copper-embedded nitrogen-doped carbon composite material and a preparation method thereof, the method comprising the following steps:
[0051] S1. Preparation of Cu-based metal organic framework materials:
[0052] S1-1, dissolving 104-419 mg of copper (II) acetate monohydrate in 10-20 mL of a mixed solvent 1 consisting of N,N-dimethylformamide (DMF) and acetonitrile (CH3CN) to obtain a solution A, wherein the volume ratio of N,N-dimethylformamide to acetonitrile is 1:1-1:4;
[0053] Dissolve 46.8-187.2 mg of 2,5-dihydroxyterephthalic acid in 10-20 mL of a mixed solvent 2 consisting of DMF, CH3CN and deionized water to obtain a solution B, wherein the volume ratio of DMF:CH3CN:deionized water is 1-4:0.5-2:0.1-0.3;
[0054] S1-2, under stirring, according to the volume ratio of solution A: solution B of 1:2-1:10, solution A is added dropwise to solution B at a rate of 3-12 μL / s, and stirring is maintained for 1-4 hours after the addition is completed. The resulting mixed solution is allowed to stand at room temperature for 20-28 hours, filtered, and the solid is collected to obtain a precursor;
[0055] S1-3. Add 5-20 mg of the precursor to a mixed solution containing 10-40 mg of sodium dodecylbenzene sulfonate, 6-24 mL of methanol and 0.5-2 mL of deionized water, let stand at room temperature for 4-16 hours for recrystallization, collect the precipitate by filtration, wash with deionized water, and vacuum dry at 50-80°C for 6-24 hours to obtain a Cu-based metal organic framework material, recorded as CDA.
[0056] Copper (II) acetate monohydrate is used as a copper source, and its chemical formula is Cu(CH3COO)2·H2O. The prepared Cu-based metal organic framework material can make copper evenly distributed on the carbon material.
[0057] In a preferred embodiment, the molar ratio of copper (II) acetate monohydrate to 2,5-dihydroxyterephthalic acid in the raw material for preparing CDA is 2.2:1.
[0058] S2. Preparation of hollow fiber polymer LZU1:
[0059] S2-1, dissolve 40-160 mg of trimesic acid and 20-80 mg of trimesic acid in 5-20 mL of 1,4-dioxane, and disperse by ultrasonication for 5-15 min. After stirring for 5-15 min, add 80-320 mg of p-phenylenediamine to the resulting solution, continue stirring for 5-15 min, add 0.1-0.4 mL of 1.5-6 mol / L glacial acetic acid, continue stirring for 20-28 hours, and then seal and stand at room temperature for 45-51 h;
[0060] S2-2. Collect the precipitate by filtration, wash it three times with tetrahydrofuran and acetone respectively, and dry it under vacuum at 50-70°C for 20-28h; soak the obtained solid in methanol, and then rotary evaporate it, repeat 2-6 times, and finally vacuum dry it at 50-70°C for 20-28h to obtain a hollow fiber polymer LZU1.
[0061] In a preferred embodiment, the mass ratio of trimesic acid to trimesic acid in the raw materials for preparing the hollow fiber polymer LZU1 is 2:1.
[0062] S3. Preparation of copper embedded nitrogen doped carbon composite material:
[0063] S3-1, adding 25-100 mg of CDA prepared in step S1 to 10-40 mL of methanol, ultrasonically dispersing for 5-15 min, adding 50-200 mg of g-C3N4 to the resulting solution, ultrasonically dispersing for 0.5-2 h, rotary evaporation to remove the solvent, vacuum drying the resulting mixture powder at 50-70 ° C for 6-24 hours, and calcining at 600-900 ° C for 1-3 h under nitrogen protection to obtain a CDA / NC composite material;
[0064] S3-2, disperse 15-60 mg of CDA / NC in 10-40 mL of methanol, then add 6-24 mg of the hollow fibrous polymer LZU1 prepared in step S2, ultrasonically disperse for 20-40 min, stir at room temperature for 12-48 h, and vacuum dry the resulting mixture at 50-70 ° C for 1-4 hours to obtain a copper-embedded nitrogen-doped carbon composite material, recorded as CL / NC.
[0065] In a preferred embodiment, in step S3-1, the calcination temperature is 700°C.
[0066] The present invention also provides an application of the above copper embedded nitrogen doped carbon composite material in a microbial fuel cell, and the application method is: the copper embedded nitrogen doped carbon composite material is coated on the cathode surface as a catalyst, and then the obtained cathode is used to assemble a microbial fuel cell. In a more preferred embodiment, the application method is: the above copper embedded nitrogen doped carbon composite material, deionized water, Nafion solution and isopropanol are mixed evenly, and the obtained slurry is evenly coated on the surface of the carbon cloth as a catalyst as a cathode; the carbon brush is used as an anode, and then assembled into a microbial fuel cell.
[0067] The present invention also provides another application of the above copper-embedded nitrogen-doped carbon composite material in the degradation of rhodamine B. The application method is: the copper-embedded nitrogen-doped carbon composite material is coated on the cathode surface as a catalyst, and then the obtained cathode is assembled into a microbial fuel cell, and the microbial fuel cell is used to degrade rhodamine B.
[0068] The present invention firstly adopts the recrystallization method to prepare the Cu-based metal organic framework material, and uses it as a precursor to make copper evenly distributed on the carbon material. The present invention uses ultrasonic mixing and co-pyrolysis technology to use g-C3N4 as a nitrogen source to introduce nitrogen into the Cu-based metal organic framework material, thereby realizing nitrogen doping; nitrogen doping not only increases the conductivity of the catalyst, but also further provides more active sites for the oxygen reduction reaction by forming CN bonds. In addition, the present invention finally prepares a copper-embedded nitrogen-doped carbon composite material: CL / NC-700 by compounding the nitrogen-doped Cu-based metal organic framework material with the hollow fiber-shaped polymer LZU1; this composite structure not only maintains the hollow fiber morphology of LZU1, but also optimizes the electronic structure of the material through nitrogen doping, further improving its adsorption capacity and catalytic activity as a catalyst.
[0069] The above is the overall concept of the present invention, and detailed embodiments and comparative examples are provided below on the basis of the overall concept of the present invention to further illustrate the present invention.
[0070] The sources of the main raw materials or products involved in the following examples are described as follows:
[0071] g-C3N4, homemade, preparation method: take 2g of dicyandiamide and heat it to 550℃ at a rate of 5℃ / min under nitrogen atmosphere, maintain it for 5h, and obtain g-C3N4.
[0072] Commercial platinum carbon, 20% Pt / C, Sigma-Aldrich;
[0073] Nafion solution, Sigma-Aldrich;
[0074] Copper(II) acetate monohydrate, TCI
[0075] 2,5-Dihydroxyterephthalic acid, Beijing Huawei Ruike Chemical Technology Co., Ltd.
[0076] Trimethylenediamine, Aladdin;
[0077] Trimesic acid, Aladdin;
[0078] p-phenylenediamine, Aladdin;
[0079] Dicyandiamide, Aladdin.
[0080] Example 1 Preparation of Cu-based metal organic framework materials
[0081] S1-1, dissolving 209.63 mg of copper (II) acetate monohydrate in 15 mL of a mixed solvent 1 consisting of N,N-dimethylformamide (DMF) and acetonitrile (CH3CN) to obtain a solution A, wherein the volume ratio of N,N-dimethylformamide to acetonitrile is 1:2;
[0082] 93.62 mg of 2,5-dihydroxyterephthalic acid was dissolved in 15.75 mL of a mixed solvent 2 consisting of DMF, CH3CN and deionized water to obtain a solution B, wherein the volume ratio of DMF:CH3CN:deionized water was 2:1:0.15;
[0083] S1-2. Under stirring at a speed of 200 rpm, according to the volume ratio of solution A to solution B of 1:5, solution A was slowly added dropwise at a rate of 6 μL / s. After the addition was completed, stirring was maintained for 2 hours. The resulting mixed solution was allowed to stand at room temperature for 24 hours, filtered, and a green solid was collected to obtain a precursor;
[0084] S1-3. Add 10 mg of the precursor to a mixed solution containing 20 mg of sodium dodecylbenzene sulfonate, 12 mL of methanol and 1 mL of deionized water, let stand at room temperature for 8 h for recrystallization, collect the precipitate by filtration, wash with deionized water, and vacuum dry at 65°C for 12 h to obtain a black Cu-based metal organic framework material, denoted as CDA.
[0085] Example 2 Preparation of hollow fiber polymer LZU1
[0086] S2-1, dissolve 80 mg of trimesaldehyde and 40 mg of trimesic acid in 10 mL of 1,4-dioxane, and disperse by ultrasonication for 10 min. After stirring for 10 min, add 160 mg of p-phenylenediamine to the resulting solution, continue stirring for 10 min, add 0.2 mL of 3 mol / L glacial acetic acid, continue stirring for 24 hours, and then seal and stand at room temperature for 2 days;
[0087] S2-2. Collect the green precipitate by filtration, wash it three times with tetrahydrofuran and acetone respectively, and dry it under vacuum at 60°C for 24 hours; soak the obtained solid in methanol, and then rotary evaporate it, repeat three times, and finally dry it under vacuum at 60°C for 24 hours to obtain a hollow fiber polymer LZU1.
[0088] Example 3 Preparation of copper-embedded nitrogen-doped carbon composite material
[0089] S3-1, add 50 mg of CDA prepared in step S1 to 20 mL of methanol, ultrasonically disperse for 10 min, add 100 mg of g-C3N4 to the resulting solution, ultrasonically disperse for 1 h, and remove the solvent by rotary evaporation. The resulting mixture powder is vacuum dried at 60 ° C for 12 h, heated to the set temperature at a heating rate of 5 ° C / min under nitrogen protection, and calcined for 2 h to obtain a CDA / NC composite material;
[0090] S3-2, 30 mg of CDA / NC was dispersed in 20 mL of methanol, and then 12 mg of the hollow fibrous polymer LZU1 prepared in step S2 was added, ultrasonically dispersed for 30 min, stirred at room temperature for 12 h, and the resulting mixture was vacuum dried at 60 ° C for 2 hours to remove the residual solvent and solidify the structure of the composite material, and finally a copper-embedded nitrogen-doped carbon composite material with hollow fiber morphology and nitrogen-doping characteristics was obtained: CL / NC.
[0091] In step S3-1, four set temperatures are set at 600, 700, 800, and 900°C, respectively. The four copper-embedded nitrogen-doped carbon composite materials prepared at the four calcination temperatures are respectively recorded as: CL / NC-600, CL / NC-700, CL / NC-800, and CL / NC-900, in order to compare the effects of different calcination temperatures on product performance.
[0092] Reference Figure 1, where a and d are the SEM image and TEM image of CDA / NC prepared in Example 3, respectively. It can be seen that CDA is successfully dispersed on the flaky g-C3N4. B and e are the SEM image and TEM image of the hollow fiber polymer LZU1 prepared in Example 2, respectively. It can be clearly seen that it has a hollow structure, indicating the successful preparation of LZU1. C and f are the SEM image and TEM image of CL / NC prepared in Example 3, respectively. It can be seen that LZU1 is successfully grown on CDA, and the hollow structure of LZU1 is well preserved without being destroyed.
[0093] Example 4 Application of the copper embedded nitrogen-doped carbon composite material prepared in Example 3 to microbial fuel cells and degradation of rhodamine B
[0094] Assembling the Microbial Fuel Cell:
[0095] Take 21 mg of the copper embedded nitrogen-doped carbon composite material prepared in Example 3, 17.5 μL of deionized water, 140 μL of Nafion solution (mass concentration of 5%), and 70 μL of isopropanol, mix and stir for 1 hour, and the resulting slurry is evenly coated on the carbon cloth as a catalyst as a cathode; the carbon brush is used as an anode, and 3 mL of sludge (sludge containing anaerobic microorganisms taken from the Shishan Water Purification Plant of Suzhou High-tech Water Purification Co., Ltd.) and 3 mL of effluent without rhodamine B (this effluent is the effluent after adding 50 mmol / L PBS and 1 g / L sodium acetate to the microbial fuel cell in the past and running smoothly) are added to the reactor with a total volume of 28 mL, and filled with 50 mmol / L PBS solution containing 1 g / L sodium acetate to assemble a microbial fuel cell. When the degradation rate is tested later, rhodamine B is also added to make the concentration of rhodamine B reach 10, 15, 20 and 30 ppm respectively.
[0096] Among them, four different copper-embedded nitrogen-doped carbon composite materials CL / NC-600, CL / NC-700, CL / NC-800, and CL / NC-900 were used as catalysts to prepare cathodes, which were recorded as CL / NC-600 electrode, CL / NC-700 electrode, CL / NC-800 electrode, and CL / NC-900 electrode, respectively; these electrodes were used to assemble microbial fuel cells, and commercial platinum carbon electrode 20% Pt / C was used as cathode to assemble microbial fuel cells for comparison. The five groups of microbial fuel cells were recorded as CL / NC-600 battery group, CL / NC-700 battery group, CL / NC-800 battery group, CL / NC-900 battery group, and 20% Pt / C battery group.
[0097] The Tafel slope was directly tested on the CL / NC-600 electrode, CL / NC-700 electrode, CL / NC-800 electrode, CL / NC-900 electrode and commercial platinum carbon electrode 20% Pt / C using an electrochemical workstation.
[0098] For the above five groups of microbial fuel cells, the voltage of the microbial fuel cell was detected by a Keithley 2700 data logger (during the experiment, an external resistor was connected to the microbial fuel cell, and the MFC voltage was recorded every 600 seconds using a Keithley 2700 data logger), and residual rhodamine B was detected using UV-3600. It was run for 20 days without adding rhodamine B, and its polarization and power density curves were tested on the 8th day. Then, different concentrations of rhodamine B were added starting from the 20th day of operation, and the degradation efficiency of rhodamine B was tested after one cycle (2 days).
[0099] Reference Figure 2 The electrochemical performance was measured using a three-electrode configuration on a CHI 760D electrochemical workstation. A silver / silver chloride electrode was used as the reference electrode and a platinum electrode was used as the counter electrode. The sample was loaded with 0.30 mg cm-1 of sodium bicarbonate in 50 mM phosphate buffer (PBS). -2 The performance of the samples was evaluated on a rotating disk electrode (radius 4.0 mm) of catalyst ink, and the Tafel slopes of different electrodes CL / NC-600, CL / NC-700, CL / NC-800, CL / NC-900, and 20% Pt / C were obtained; it can be seen that the CL / NC-700 electrode has a Tafel slope of 128.7 mV dec. -1 The Tafel value is the lowest among all samples and lower than that of the commercial platinum carbon electrode 20% Pt / C, indicating that it has the fastest oxygen reduction reaction kinetic rate; this is attributed to the fact that the CL / NC-700 material is calcined at 700°C, which can form more carbon defects as active sites and enhance its oxygen reduction reaction ability.
[0100] Reference Figure 3 , are the polarization and power density curves of five groups of microbial fuel cells: CL / NC-600 battery group, CL / NC-700 battery group, CL / NC-800 battery group, CL / NC-900 battery group, and 20% Pt / C battery group on the eighth day of stable operation. Compared with other groups, the CL / NC-700 group of microbial fuel cells showed the highest power output, with 2291.67±27.75 mW m −2 The maximum power density is that of the commercial platinum carbon electrode 20% Pt / C group (1375.77±12.22 mW m −2 ) is about 1.66 times that of Figure 2This is consistent with the results shown to have the best oxygen reduction reaction kinetics rate.
[0101] Reference Figure 4 , are the test results of the degradation efficiency of Rhodamine B for CL / NC-600 battery pack, CL / NC-700 battery pack, CL / NC-800 battery pack, CL / NC-900 battery pack, and 20% Pt / C battery pack.
[0102] The calculation formula of the degradation efficiency η of rhodamine B is: , C0 and C1 represent the initial concentration and concentration after degradation of rhodamine B, respectively.
[0103] In the degradation test, different concentrations of rhodamine B solution (10, 15, 20 and 30 ppm) were introduced into the microbial fuel cell (MFC). The MFC of the CL / NC-700 battery group achieved degradation rates of 99.45%, 99.30%, 98.70%, and 96.59% when degrading different concentrations of rhodamine B solution (10, 15, 20 and 30 ppm), respectively; these results are significantly better than the 20% Pt / C battery group using commercial platinum carbon electrodes (degradation rates are 99.05%, 90.31%, 89.01%, and 86.29%, respectively). It can be shown that the copper embedded nitrogen-doped carbon composite material prepared by the present invention can be used as a cathode catalyst for microbial fuel cells, and can provide a reliable solution for improving the performance of microbial fuel cells and the degradation rate of rhodamine B.
[0104] The present invention prepared CDA by recrystallization and successfully carried out nitrogen doping by co-pyrolysis, which increased the active sites of the composite material and enhanced its conductivity; then, it was compounded with the hollow fiber polymer LZU1 by simple ultrasound, stirring and other processes. This unique hollow fiber morphology was used to optimize mass transfer and enrich the active sites required for oxygen reduction reaction. The experimental results show that the CL / NC-700 battery pack achieved 2291.67±27.75mWm in MFCs. −2 The peak power density of the CL / NC prepared by the present invention is 1.34 W / m, and the degradation efficiency of the CL / NC is 2.33 W / m, which is significantly better than the 20% Pt / C battery pack of the commercial platinum carbon electrode. These results are attributed to the synergistic enhancement effect of nitrogen doping, hollow fiber morphology and copper embedding in the CL / NC prepared by the present invention on improving its catalyst performance. Therefore, the present invention provides a new idea for the development of efficient, low-cost and environmentally friendly catalysts, as well as their application in the fields of energy production and environmental remediation.
[0105] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to specific details.
Claims
1. A method for preparing a copper-embedded nitrogen-doped carbon composite material, characterized in that: The following steps are involved: S1. Preparation of Cu-based metal organic framework materials: Copper (II) acetate monohydrate is dissolved to prepare solution A, 2,5-dihydroxyterephthalic acid is dissolved to prepare solution B, solution A is added dropwise to solution B, mixed evenly and allowed to stand, solids are collected by filtration, and the obtained solids are recrystallized to obtain a Cu-based metal organic framework material, which is recorded as CDA; S2. Preparation of hollow fiber polymer LZU1: The trimesic acid and trimesic acid are mixed and dissolved, and then p-phenylenediamine is added after ultrasonic and stirring treatment, and stirred, and glacial acetic acid is added, stirred, and allowed to stand, and the precipitate is collected by filtration, washed, dried, soaked in methanol, rotary evaporated, and vacuum dried to obtain a hollow fiber polymer LZU1; S3. Preparation of copper embedded nitrogen doped carbon composite material: The CDA and g-C3N4 prepared in step S1 are mixed evenly and then calcined to obtain a CDA / NC composite material; the CDA / NC composite material and the hollow fibrous polymer LZU1 prepared in step S2 are evenly mixed in a solution, stirred, and the solid product is collected and dried under vacuum to obtain a copper-embedded nitrogen-doped carbon composite material, which is recorded as CL / NC.
2. The method for preparing the copper-embedded nitrogen-doped carbon composite material according to claim 1, characterized in that: Step S1 is specifically as follows: S1-1, dissolving 104-419 mg of copper (II) acetate monohydrate in 10-20 mL of a mixed solvent 1 consisting of N,N-dimethylformamide and acetonitrile to obtain a solution A, wherein the volume ratio of N,N-dimethylformamide to acetonitrile is 1:1-1:4; Dissolve 46.8-187.2 mg of 2,5-dihydroxyterephthalic acid in 10-20 mL of a mixed solvent 2 consisting of DMF, CH3CN and deionized water to obtain a solution B, wherein the volume ratio of DMF:CH3CN:deionized water is 1-4:0.5-2:0.1-0.3; S1-2, under stirring, according to the volume ratio of solution A: solution B of 1:2-1:10, solution A is added dropwise to solution B at a rate of 3-12 μL / s, and stirring is maintained for 1-4 hours after the addition is completed. The resulting mixed solution is allowed to stand at room temperature for 20-28 hours, filtered, and the solid is collected to obtain a precursor; S1-3. Add 5-20 mg of the precursor to a mixed solution containing 10-40 mg of sodium dodecylbenzene sulfonate, 6-24 mL of methanol and 0.5-2 mL of deionized water, let stand at room temperature for 4-16 hours for recrystallization, collect the precipitate by filtration, wash with deionized water, and vacuum dry at 50-80°C for 6-24 hours to obtain a Cu-based metal organic framework material, recorded as CDA.
3. The method for preparing the copper-embedded nitrogen-doped carbon composite material according to claim 1, characterized in that: Step S2 is specifically as follows: S2-1, dissolve 40-160 mg of trimesic acid and 20-80 mg of trimesic acid in 5-20 mL of 1,4-dioxane, and disperse by ultrasonication for 5-15 min. After stirring for 5-15 min, add 80-320 mg of p-phenylenediamine to the resulting solution, continue stirring for 5-15 min, add 0.1-0.4 mL of 1.5-6 mol / L glacial acetic acid, continue stirring for 20-28 hours, and then seal and stand at room temperature for 45-51 h; S2-2. Collect the precipitate by filtration, wash it three times with tetrahydrofuran and acetone respectively, and dry it under vacuum at 50-70°C for 20-28h; soak the obtained solid in methanol, and then rotary evaporate it, repeat 2-6 times, and finally vacuum dry it at 50-70°C for 20-28h to obtain a hollow fiber polymer LZU1.
4. The method for preparing the copper-embedded nitrogen-doped carbon composite material according to claim 1, characterized in that: Step S3 is specifically as follows: S3-1, adding 25-100 mg of CDA prepared in step S1 to 10-40 mL of methanol, ultrasonically dispersing for 5-15 min, adding 50-200 mg of g-C3N4 to the resulting solution, ultrasonically dispersing for 0.5-2 h, rotary evaporation to remove the solvent, vacuum drying the resulting mixture powder at 50-70 ° C for 6-24 hours, and calcining at 600-900 ° C for 1-3 h under nitrogen protection to obtain a CDA / NC composite material; S3-2, disperse 15-60 mg of CDA / NC in 10-40 mL of methanol, then add 6-24 mg of the hollow fibrous polymer LZU1 prepared in step S2, ultrasonically disperse for 20-40 min, stir at room temperature for 12-48 h, and vacuum dry the resulting mixture at 50-70 ° C for 1-4 hours to obtain a copper-embedded nitrogen-doped carbon composite material, recorded as CL / NC.
5. The method for preparing the copper-embedded nitrogen-doped carbon composite material according to claim 4, characterized in that: In step S3-1, the calcination temperature is 700°C.
6. The method for preparing the copper-embedded nitrogen-doped carbon composite material according to claim 1, characterized in that: The following steps are involved: S1. Preparation of Cu-based metal organic framework materials: S1-1, dissolving 209.63 mg of copper (II) acetate monohydrate in 15 mL of a mixed solvent 1 consisting of N,N-dimethylformamide and acetonitrile to obtain a solution A, wherein the volume ratio of N,N-dimethylformamide to acetonitrile is 1:2; 93.62 mg of 2,5-dihydroxyterephthalic acid was dissolved in 15.75 mL of a mixed solvent 2 consisting of DMF, CH3CN and deionized water to obtain a solution B, wherein the volume ratio of DMF:CH3CN:deionized water was 2:1:0.15; S1-2, under stirring at a speed of 200 rpm, according to the volume ratio of solution A:solution B of 1:5, solution A was added dropwise to solution B at a speed of 6 μL / s, and stirring was maintained for 2 hours after the addition was completed. The resulting mixed solution was allowed to stand at room temperature for 24 hours, filtered, and the solid was collected to obtain a precursor; S1-3, adding 10 mg of the precursor to a mixed solution containing 20 mg of sodium dodecylbenzene sulfonate, 12 mL of methanol and 1 mL of deionized water, standing at room temperature for 8 h for recrystallization, collecting the precipitate by filtration, washing with deionized water, and vacuum drying at 65 ° C for 12 hours to obtain a Cu-based metal organic framework material, recorded as CDA; S2. Preparation of hollow fiber polymer LZU1: S2-1, dissolve 80 mg of trimesaldehyde and 40 mg of trimesic acid in 10 mL of 1,4-dioxane, and disperse by ultrasonication for 10 min. After stirring for 10 min, add 160 mg of p-phenylenediamine to the resulting solution, continue stirring for 10 min, add 0.2 mL of 3 mol / L glacial acetic acid, continue stirring for 24 hours, and then seal and stand at room temperature for 2 days; S2-2, collecting the precipitate by filtration, washing it three times with tetrahydrofuran and acetone respectively, and drying it under vacuum at 60°C for 24 hours; soaking the obtained solid in methanol, and then rotary evaporation, repeating three times, and finally vacuum drying it at 60°C for 24 hours to obtain a hollow fiber polymer LZU1; S3. Preparation of copper embedded nitrogen doped carbon composite material: S3-1, adding 50 mg of CDA prepared in step S1 to 20 mL of methanol, ultrasonically dispersing for 10 min, adding 100 mg of g-C3N4 to the obtained solution, ultrasonically dispersing for 1 h, and removing the solvent by rotary evaporation. The obtained mixture powder was vacuum dried at 60 ° C for 12 h, heated to 700 ° C at a heating rate of 5 ° C / min under nitrogen protection, and calcined for 2 h to obtain a CDA / NC composite material; S3-2, 30 mg of CDA / NC was dispersed in 20 mL of methanol, and then 12 mg of the hollow fibrous polymer LZU1 prepared in step S2 was added, ultrasonically dispersed for 30 min, stirred at room temperature for 12 h, and the resulting mixture was vacuum dried at 60 ° C for 2 hours to obtain a copper-embedded nitrogen-doped carbon composite material, recorded as CL / NC.
7. A copper-embedded nitrogen-doped carbon composite material, characterized in that: It is prepared by the method according to any one of claims 1 to 6.
8. Use of the copper embedded nitrogen doped carbon composite material as claimed in claim 7 in a microbial fuel cell, characterized in that: The application method is: coating the copper-embedded nitrogen-doped carbon composite material as a catalyst on the cathode surface, and then assembling a microbial fuel cell using the obtained cathode.
9. The use according to claim 8, characterized in that: The application method is: the copper-embedded nitrogen-doped carbon composite material, deionized water, Nafion solution and isopropanol are mixed evenly, the obtained slurry is used as a catalyst and evenly coated on the surface of the carbon cloth as a cathode; the carbon brush is used as an anode, and then assembled into a microbial fuel cell.
10. Use of the copper embedded nitrogen doped carbon composite material as claimed in claim 7 in the degradation of rhodamine B, characterized in that: The application method is: coating the copper-embedded nitrogen-doped carbon composite material as a catalyst on the cathode surface, then assembling a microbial fuel cell using the obtained cathode, and using the microbial fuel cell to degrade rhodamine B.