A vacuum consumable arc melting method for NbZrTiAl series refractory high entropy alloy ingot
Through the vacuum consumable arc melting method of NbZrTiAl series refractory high-entropy alloy, the ingredients and process are optimized to solve the problem of uneven composition and segregation in large-sized ingots, and achieve efficient preparation of finished products and cost reduction.
Patent Information
- Application Number
- CN202411076121.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-08-07
AI Technical Summary
Existing refractory high-entropy alloys have problems such as uneven composition, severe segregation and long production cycle in the preparation of large-size ingots, especially volatilization caused by elements with large differences in melting points and densities such as Nb, Zr, Ti and Al. damage and segregation issues.
The vacuum consumable arc melting method of NbZrTiAl series refractory high-entropy alloy is adopted. By optimizing ingredients, mixing, pressing electrode blocks, welding consumable electrodes and smelting processes, it includes multiple vacuum consumable arc melting, electromagnetic stirring and Specific cooling water temperature control ensures composition uniformity and strength.
The composition accuracy and uniformity of large-size refractory high-entropy alloy ingots of hundreds of kilograms are achieved, reducing production costs and improving the overall strength of the ingots and the uniformity of finished products.
Smart Images

Figure CN118600261B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a vacuum consumable arc melting method for NbZrTiAl series refractory high entropy alloy ingots, belonging to the technical field of alloys. Background Art
[0002] Refractory high entropy alloys are mainly composed of refractory metal elements. Due to the high melting points and large differences of refractory metal elements, it is easy to cause volatilization and segregation of low melting point metal elements. They are currently mainly prepared by vacuum induction melting and vacuum non-consumable arc melting. Due to the low technical maturity of refractory high entropy alloys, it only remains in the laboratory stage. At present, only the preparation of small-sized ingots ranging from hundreds of grams to several kilograms has been achieved, which is difficult to apply in engineering. In order to promote the engineering application of refractory high entropy alloys, the preparation of large-scale ingots will inevitably become the mainstream trend. However, when the smelted high entropy alloy contains elements such as Nb, Zr, Ti and Al with large differences in melting point, density and vapor pressure, due to the difference in melting point of more than 550°C, the Al element with a low melting point will melt first, and the Nb, Zr, Ti and other elements with high melting points will melt later; due to the density difference of 1.8g / cm 3 As mentioned above, the low-density Al element is generally distributed in the upper part of the crucible, and its vapor pressure is much greater than that of other elements (except Mn element) at the same smelting temperature, resulting in serious volatilization and burning of the first-melted Al element, and the later-melted Ti, Zr, Nb and other elements are usually distributed in the middle and lower parts of the crucible, and unmelted blocks of Nb and other elements with the highest melting points may appear at the bottom of the crucible. The Al element with the lowest density and the lowest melting point is seriously volatilized and burned, and the elements with the highest density and the highest melting point, such as Nb, are seriously segregated. Multiple remelting increases the content of gas impurities, resulting in poor accuracy and uniformity of the alloy composition of the ingot after smelting. At the same time, for large-sized ingots, the temperature gradient differences and cooling rate gradient differences in various parts of the ingot increase, which can aggravate the component segregation at different positions of the ingot.
[0003] Chinese patent application CN116511429A discloses that a high-entropy alloy ingot with uniform composition and large size and no casting defects can be prepared by magnetic levitation smelting plus consumable smelting. However, this preparation method requires three magnetic levitation smeltings to obtain a single consumable electrode for consumable smelting. When the size and number of the final consumable ingot increase, the number and frequency of consumable electrodes prepared by magnetic levitation smelting further increase, which greatly increases the preparation cycle and production cost of large-size high-entropy alloy ingots, which is not conducive to industrial production. Summary of the invention
[0004] In view of this, the purpose of the present invention is to provide a vacuum consumable arc melting method for NbZrTiAl series refractory high entropy alloy ingots. By optimizing the batching and mixing process, the pressing and welding electrode process and the melting process, a one-time forming of a large-sized refractory high entropy alloy ingot with uniform composition and a weight of 100 kg is achieved.
[0005] To achieve the above objectives, the technical solution of the present invention is as follows.
[0006] A vacuum consumable arc melting method for NbZrTiAl series refractory high entropy alloy ingots, the method steps comprising:
[0007] (1) Batching and mixing: weighing the raw materials of each component in the NbZrTiAl series refractory high entropy alloy according to atomic percentage, crushing the raw materials to obtain particles with a particle size of 5 to 10 mm, and then mixing them to obtain a mixed material;
[0008] (2) Pressing electrode blocks: Pressing the mixture into multiple cylindrical electrode blocks; the mass of each electrode block is 1 / 9 to 1 / 3 of the total mass of the mixture, the diameter of the electrode block is 100 to 300 mm, and the density of each electrode block is 3.0 to 5.0 g / cm 3 ;
[0009] (3) welding a consumable electrode: welding the electrode block into a consumable electrode;
[0010] (4) Melting: placing the consumable electrode into an arc furnace, and performing vacuum consumable arc melting for more than three times under an inert gas atmosphere, and obtaining a NbZrTiAl-based refractory high entropy alloy ingot after the melting is completed;
[0011] The atomic expression of the NbZrTiAl refractory high entropy alloy is: a Zr b Ti c Al d M x , M is one or more of V, Cr, Mn, Fe, Co, Ni, Mo, Hf and W, 10≤a≤25, 5≤b≤30, 40≤c≤70, 15≤d≤40, 0≤x≤10, and a+b+c+d+x=100;
[0012] In step (1), Zr is added in the form of single substance sponge zirconium, Ti is added in the form of single substance sponge titanium and AlTi master alloy, Nb, M and Al are added in the form of AlNb master alloy and AlM master alloy respectively; the volume of the single substance is more than 50% of the total volume;
[0013] In step (2), the pressing pressure is (electrode block surface pressure × π × electrode block radius squared) × 10 -4 Tons, the surface pressure of the electrode block is 250~350MPa;
[0014] In step (4), the melting voltage is 30-40V, the first melting current is 2-7KA, and starting from the second melting, the melting current is increased by 1-2KA compared with the previous melting current; the first and second melting times are 3-5min, and the circulating cooling water temperature is maintained at 55-65°C; the third and subsequent melting times are 6-10min, respectively, and the circulating cooling water temperature is maintained at 35-45°C; during the melting process, a single-winding spiral electromagnetic stirring device is used to electromagnetically stir the high-entropy alloy melt, and the deflection angle of the inclined magnetic yoke is 40°-60°.
[0015] Optimally, in step (1), Nb and Al are added in the form of Al-(60-75)Nb and Al-(5-10)Ti master alloys, respectively; V, Cr, Mn, Fe, Co, Ni, Mo, and Hf are added in the form of Al-(10-50)V, Al-(10-20)Cr, Al-(10-80)Mn, Al-(10-60)Fe, Al-(10-30)Co, Al-(10-20)Ni, Al-(20-60)Mo, Al-(10-20)Hf, and Al-(10-50)W master alloys, respectively. In the above master alloys, the values in brackets represent the mass fractions of the elements in the master alloy.
[0016] Preferably, in step (1), when the raw materials are crushed, a jaw crusher is first used to coarsely crush the titanium sponge and the intermediate alloy particles, respectively, and after the coarse crushing, a vibrating screen is used to screen the particles with a particle size of less than 150 mm; then a toothed roller crusher is used to medium crush the screened particles, and after the medium crushing, a vibrating screen is used to screen the particles with a particle size of less than 75 mm; finally, the screened particles are finely crushed 4 to 10 times by a toothed roller crusher, and after the fine crushing, a vibrating screen is used to screen the particles with a particle size of 5 to 10 mm.
[0017] Preferably, in step (1), the mixing is performed multiple times, the amount of a single mixing is sufficient to suppress the mass of an electrode block, and the single mixing time is 10 to 20 minutes.
[0018] Optimally, in step (3), the electrode blocks are welded in an inert atmosphere protection welding box. During welding, a pressure of 0.015 to 0.025 tons is applied to the electrode blocks at both ends, and the vacuum degree in the box is 2 to 6×10 -3 Pa, a weld is welded at the butt joint of the two electrode blocks; 2 to 6 longitudinal welds are evenly distributed in the direction perpendicular to the butt weld. More preferably, the weld width is 20 to 25 mm, the depth is 10 to 15 mm, the longitudinal weld length is 30 to 40 mm, and the solder is a Ti-Zr-Cu-Ni series solder with a composition of Ti-(13 to 37.5)Zr-(15 to 21)Cu-(9 to 15)Ni. The values in brackets represent the mass fraction of the element in the solder.
[0019] Optimally, in step (4), when the ingot is melted, the pressure is 1.3 to 1.5 times the vapor pressure of the Al element at the melt temperature.
[0020] Preferably, in step (4), during electromagnetic stirring, when the smelted weight is less than 1 / 50 of the total weight of the ingot, the rotating magnetic field in the electromagnetic stirring device is operated alone, and its intensity is 5-20 gauss, the stirring period is 5-20s, and the switching frequency is 5-20s / time; when the smelted weight is greater than or equal to 1 / 50 of the total weight of the ingot, the rotating magnetic field and the traveling wave magnetic field in the electromagnetic stirring device are operated simultaneously to form a spiral magnetic field, wherein the intensity of the rotating magnetic field is 25-50 gauss, the stirring period is 25-50s, the switching frequency is 25-50s / time, the intensity of the traveling wave magnetic field is 25-50 gauss, the stirring period is 25-50s, and the direction of the induced electromagnetic force is vertically upward along the axial direction of the ingot.
[0021] Optimally, in step (4), starting from the second smelting, a head of material having a length of 0.01 to 0.03 times the ingot length is cut off before each smelting and then the smelting direction is reversed.
[0022] Optimally, in step (4), the smelting times are 3 to 6 times.
[0023] Beneficial Effects
[0024] The present invention provides a vacuum consumable arc melting method for NbZrTiAl series refractory high entropy alloy ingots, which adopts the form of Al series master alloy to add high melting point and high density elements such as Nb, V, Cr and low melting point and low density Al elements, effectively avoiding the segregation of high melting point and high density elements and the volatilization and burning loss of low melting point and low density elements, and ensuring the accuracy and uniformity of alloy composition. In addition, combined with the good plasticity of sponge zirconium and sponge titanium and the poor plasticity of master alloy, a specific component ratio is used to ensure that the sum of the volumes of sponge titanium and sponge zirconium is 50% or more, which is conducive to the process of pressing the electrode, so that the two easily deformable single metals can fully cover the non-deformable master alloy, thereby improving the overall strength of the electrode block after pressing.
[0025] The invention provides a vacuum consumable arc melting method for NbZrTiAl series refractory high entropy alloy ingots. The particle sizes of sponge zirconium, sponge titanium and intermediate alloy particles are reasonably controlled within 5-10 mm through mechanical crushing and vibration screening processes, so as to avoid that after the uniformly mixed raw materials are poured into a mold cavity to press an electrode block, the raw materials are not evenly distributed in the electrode block due to large differences in particle size and shape, thereby affecting the uniformity of the alloy components.
[0026] The present invention provides a vacuum consumable arc melting method for NbZrTiAl series refractory high entropy alloy ingots. According to the characteristics of high activity and easy reaction of NbZrTiAl series refractory high entropy alloys, a vacuum inert atmosphere shielded welding method is adopted to effectively avoid the consumable electrode reacting with oxygen in the air to form oxides and introduce impurities during the welding process, thereby ensuring the cleanliness of the alloy components. In the process of pressing and welding the electrode block, a specific pressure is applied to the electrode block and a longitudinal weld is increased to ensure the strength of the consumable electrode, thereby avoiding the consumable electrode from falling off or breaking due to insufficient strength during the melting process.
[0027] The present invention provides a vacuum consumable arc melting method for NbZrTiAl series refractory high entropy alloy ingots, which strictly controls the power, time and cooling water temperature of each melting; under the condition of ensuring the normal cooling of the crucible, the temperature of the circulating cooling water is appropriately increased, the cooling rate of the solidified shell is reduced, the wall thickness of the solidified shell is reduced, and the volatilization and burning loss of the Al element are compensated. The cooling water temperature of the first and second melting cycles is set higher, so that the cooling water takes away less heat from the alloy melt, prolongs the time that the melt is in a high-temperature molten state, is more conducive to the melting and diffusion of high-melting-point elements, and thus reduces the tendency of ingot composition segregation. The introduction of argon gas at a specific pressure inhibits the reaction of liquid Al to gaseous Al, effectively reduces the volatilization and burning loss of the Al element, thereby ensuring the accuracy of the alloy composition.
[0028] The present invention provides a vacuum consumable arc melting method for NbZrTiAl series refractory high entropy alloy ingots. A single-winding spiral electromagnetic stirring device is used during the ingot melting process, so that the high entropy alloy melt moves downward in a spiral along the axial direction of the ingot. The effective flow range of the melt is larger than that of the traditional single rotating electromagnetic stirring device, thereby ensuring the uniformity of the alloy composition. At the same time, the induced electromagnetic force generated by the traveling wave magnetic field is vertically upward along the axial direction of the billet, which can slow down the downward flow of the melt, ensure that the high melting point elements are fully melted and diffused, and effectively improve the segregation of the ingot composition. The rotating magnetic field in the electromagnetic stirring device is operated separately when the smelted weight is within 1 / 50 of the total weight of the ingot, which is conducive to establishing a molten pool with uniform composition. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 is Nb in Example 1 10 Zr5Ti 65 Al 20 Schematic diagram of sampling for ingot chemical composition testing.
[0030] Figure 2 is Nb in Example 1 10 Zr5Ti 65 Al 20 Surface scanning results of energy spectrum analysis of ingot chemical composition. DETAILED DESCRIPTION
[0031] The present invention will be further described in detail below in conjunction with specific embodiments.
[0032] Example 1
[0033] Nb 10 Zr5Ti 65 Al 20 The vacuum consumable arc melting method for refractory high entropy alloy ingots is as follows:
[0034] Ingredients and mixing: According to the chemical formula Nb 10 Zr5Ti 65 Al 20 Weigh 3 portions of raw materials by atomic percentage with a balance, each portion weighing 40kg, with a total weight of 120kg. In each portion of raw materials, Al-75Nb particles are 9.839kg, Al-5Ti particles are 1.923kg, sponge zirconium is 3.623kg, and sponge titanium is 24.617kg. Before mixing, a jaw crusher is used to coarsely crush the sponge titanium and intermediate alloy particles respectively. After coarse crushing, a vibrating screen is used to screen particles with a particle size of less than 100mm. Then, a toothed roller crusher is used to medium crush the screened particles. After medium crushing, a vibrating screen is used to screen particles with a particle size of less than 50mm. Then, the screened particles are finely crushed 5 times with a toothed roller crusher. After fine crushing, a vibrating screen is used to screen particles with a particle size of about 5mm. Then, each portion of raw materials is placed in a rotary mixer for mixing in turn. The mixing time is 10min. After the mixing of the previous portion of raw materials is completed, it is taken out of the mixer and placed in a drying oven for standby use. Then, the mixing work of the next portion of raw materials is carried out.
[0035] Pressing electrode blocks: Take out the first batch of raw materials from the dryer and put them into an electrode block mold with a size of Φ150×450mm. Use a 2000-ton press to press out the first electrode block at a pressure of 450 tons (the surface pressure of the electrode block is 250MPa). Then press the remaining electrode blocks in sequence according to the pressing steps of the first electrode block. The density of each electrode block is 3.3g / cm 3 .
[0036] Welding consumable electrode: put three electrode blocks into the inert gas shielded welding box in turn, close the box door and evacuate the vacuum. When the vacuum degree reaches 6×10 -3 Argon welding was started at 90°C Pa. During the welding process, the hydraulic cylinders attached to both sides of the welding box were turned on, and a pressure of 0.015 tons was applied to the electrode blocks at both ends through their push rods. The pressure was maintained until the end of welding, and a weld was welded at the butt joint of the two electrode blocks; two longitudinal welds were evenly distributed in the direction of the vertical butt weld, all welds were 20mm wide, 10mm deep, and 30mm long. The solder composition used was Ti-13Zr-15Cu-9Ni. After the welding was completed, the consumable electrode was cooled to room temperature, the power of the hydraulic cylinder and the welding box was turned off, and the consumable electrode was taken out.
[0037] Melting: Use a crane to hoist the consumable electrode to the side of the arc furnace, load it into the furnace and start to evacuate. When the vacuum is less than 5Pa, open the gas valve and introduce argon into the arc furnace. When the furnace pressure reaches 7534Pa, close the gas valve, introduce cooling water and start melting. The cooling water temperature is maintained at 50~60℃ during the whole melting process. Three vacuum consumable arc melting is adopted, the melting voltage is 36V, the melting current of the first melting is 3KA, the melting time is 3min, after the melting is completed, the 11mm material head is cut off, the ingot direction is turned to install the electrode and start the second melting. The current of the second melting is 4KA, the melting time is 3min, after the melting is completed, the 11mm material head is cut off, the ingot direction is turned to install the electrode and start the third melting. The circulating cooling water temperature during the first two meltings is 55℃. The third smelting current is 5KA, the smelting time is 6min, the circulating cooling water temperature is 35℃, and after the smelting is completed, the 11mm material head is cut off, the ingot is peeled 5mm, and the surface oxide skin is removed and samples are taken for chemical composition detection. During the smelting of the ingot, when the smelted weight is within 2.4kg, the rotating magnetic field in the electromagnetic stirring device is operated alone, and its intensity is 6 gauss, the stirring cycle is 6s, and the commutation frequency is 6s / time; when the smelted weight is beyond 2.4kg, the rotating magnetic field and the traveling magnetic field in the electromagnetic stirring device are operated simultaneously to form a spiral magnetic field, wherein the deflection angle of the inclined magnetic yoke is 50°, the intensity of the rotating magnetic field is 26 gauss, the stirring cycle is 26s, the commutation frequency is 26s / time, the intensity of the traveling magnetic field is 26gauss, the stirring cycle is 26s, and the direction of the induced electromagnetic force is vertically upward along the axial direction of the ingot.
[0038] The chemical composition test results show that the deviation values of Nb, Zr and Ti from the nominal composition are all within the range of 0~0.40wt.%, and the deviation value of Al from the nominal composition is within the range of 0~0.5wt.%. Figure 1 The results of the spectrum analysis show that the four elements Nb, Zr, Ti and Al are evenly distributed inside the ingot. Figure 2 shown.
[0039] Embodiment 2:
[0040] Nb 16 Zr 12 Ti 45 Al 27 The vacuum consumable arc melting method for refractory high entropy alloy ingots is as follows:
[0041] Based on Example 1, only the atomic ratio of each element is changed, and the other steps remain unchanged. 16 Zr 12 Ti 45 Al 27Three portions of raw materials were weighed by a balance according to atomic percentage, each portion weighing about 40 kg, with a total weight of about 120 kg. In each portion of raw materials, Al-75Nb particles weighed 14.511 kg, Al-5Ti particles weighed 1.796 kg, sponge zirconium weighed 8.014 kg, and sponge titanium weighed 15.681 kg.
[0042] The chemical composition test results show that the deviations of the four elements Nb, Zr, Ti and Al from the nominal composition are all within the range of 0~0.40wt.%. The surface scan results of the energy spectrum analysis show that the four elements Nb, Zr, Ti and Al are evenly distributed inside the ingot.
[0043] Embodiment 3:
[0044] Nb 11 Zr 11 Ti 45 Al 26 The vacuum consumable arc melting method of V7 refractory high entropy alloy ingot is as follows:
[0045] On the basis of Example 1, the atomic ratio of each element is changed, and V element is added, and the other steps remain unchanged. 11 Zr 11 Ti 45 Al 26 V7 weighs 3 portions of raw materials by atomic percentage using a balance, each portion is about 40 kg, and the total weight is about 120 kg. In each portion of raw materials, Al-75Nb particles are 10.407 kg, Al-5Ti particles are 0.035 kg, Al-50V particles are 5.447 kg, sponge zirconium is 7.664 kg, and sponge titanium is 16.452 kg.
[0046] The chemical composition test results show that the deviations of the five elements Nb, Zr, Ti, Al, and V from the nominal composition are all within the range of 0~0.42wt.%. The surface scan results of the energy spectrum analysis show that the five elements Nb, Zr, Ti, Al, and V are evenly distributed inside the ingot.
[0047] Embodiment 4:
[0048] Nb 14 Zr 25 Ti 40 Al 20 The vacuum consumable arc melting method for Mo1 refractory high entropy alloy ingot is as follows:
[0049] Based on Example 1, the atomic ratio of each element is changed, and Mo element is added, and the other steps remain unchanged. 14 Zr 25 Ti 40 Al 20Mo1 was weighed in 3 portions by atomic percentage using a balance, each portion was about 40 kg, and the total weight was about 120 kg. In each portion of the raw material, Al-75Nb particles were 11.315 kg, Al-5Ti particles were 0.289 kg, Al-60Mo particles were 1.044 kg, sponge zirconium was 14.878 kg, and sponge titanium was 12.492 g.
[0050] The chemical composition test results show that the deviations of the five elements Nb, Zr, Ti, Al and Mo from the nominal composition are all within the range of 0~0.44wt.%. The surface scan results of energy spectrum analysis show that the five elements Nb, Zr, Ti, Al and Mo are evenly distributed inside the ingot.
[0051] Embodiment 5:
[0052] On the basis of Example 1, the screened particles were crushed 10 times with a toothed roller crusher, the mixing time was changed to 20 min, the electrode block pressing pressure was changed to 620 tons (the electrode block surface pressure was 350 MPa), the pressure applied by the electrode blocks at both ends during welding was changed to 0.025 tons, and the vacuum degree in the welding box was changed to 2×10 -3 Pa, 6 longitudinal welds are evenly distributed in the direction perpendicular to the butt weld, all welds are 25mm wide, 15mm deep, 40mm long, the melting voltage is 40V, the melting current of the first melting is 7KA, and the melting currents of the second, third, fourth, fifth and sixth meltings are 9KA, 10KA, 11KA, 12KA and 13KA respectively; the first and second melting times are 5min, and the melting time of more than three meltings is 10min. The rotating magnetic field in the electromagnetic stirring device is operated alone, with an intensity of 20gauss, a stirring cycle of 20s, and a commutation frequency of 20s / time; the rotating magnetic field and the traveling wave magnetic field in the electromagnetic stirring device are operated simultaneously to form a spiral magnetic field, wherein the deflection angle of the inclined magnetic yoke is 50°, the intensity of the rotating magnetic field is 50gauss, the stirring cycle is 50s, the commutation frequency is 50s / time, the intensity of the traveling wave magnetic field is 50gauss, and the stirring cycle is 50s.
[0053] The chemical composition test results show that the deviations of the four elements Nb, Zr, Ti and Al from the nominal composition are all within the range of 0~0.1wt.%. The surface scan results of the energy spectrum analysis show that the four elements Nb, Zr, Ti and Al are evenly distributed inside the ingot.
[0054] Embodiment 6:
[0055] On the basis of Example 1, the number of pressed electrode blocks is changed to 6, and the other steps remain unchanged. 10 Zr5Ti 65 Al 20A total of 6 portions of raw materials were weighed by a balance according to atomic percentage, each portion weighing 20 kg, with a total weight of 120 kg. In each portion of raw materials, Al-75Nb particles weighed 10.407 kg, Al-5Ti particles weighed 0.063 kg, sponge zirconium weighed 1.660 kg, and sponge titanium weighed 7.866 kg.
[0056] The chemical composition test results show that the deviations of Nb, Zr and Ti from the nominal composition are all within the range of 0~0.38wt.%, and the deviations of Al from the nominal composition are within the range of 0~0.46wt.%. The surface scan results of energy spectrum analysis show that the four elements Nb, Zr, Ti and Al are evenly distributed inside the ingot.
[0057] Comparative Example 1:
[0058] Based on Example 1, according to the chemical formula Nb 10 Zr5Ti 65 Al 20 Three portions of raw materials were weighed on a balance according to atomic percentage, each portion weighing 40 kg, with a total weight of 120 kg. Nb and Al were not added in the form of intermediate alloys, but in the form of single substances. Among them, Nb particles were 7.400 kg, sponge zirconium was 3.600 kg, Ti particles were 24.700 kg, and Al particles were 4.300 kg.
[0059] The chemical composition test results show that the deviations of the four elements Nb, Zr, Ti and Al from the nominal composition are within the range of 1~3wt.%, the Al element is seriously volatilized and burned, and the Nb and Zr elements at the bottom of the ingot are seriously segregated. The surface scan results of the energy spectrum analysis show that the four elements Nb, Zr, Ti and Al are extremely unevenly distributed inside the ingot.
[0060] Comparative Example 2:
[0061] On the basis of Example 1, the process combining mechanical crushing and vibration screening was not used to treat the sponge zirconium, sponge titanium and intermediate alloy particles before mixing, and the other steps remained unchanged.
[0062] The chemical composition test results show that the deviations of Nb, Zr and Ti from the nominal composition are all within the range of 1~1.5wt.%, and the deviations of Al from the nominal composition are within the range of 1~1.5wt.%. The surface scan results of energy spectrum analysis show that the four elements Nb, Zr, Ti and Al are unevenly distributed inside the ingot.
[0063] Comparative Example 3:
[0064] On the basis of Example 1, the temperature of cooling water was changed to 25° C., argon gas was not introduced during smelting, a single-winding spiral electromagnetic stirring device was not used, and the remaining steps remained unchanged.
[0065] The chemical composition test results show that the deviations of Nb, Zr and Ti from the nominal composition are all within the range of 0~0.3wt.%, and the deviations of Al from the nominal composition are within the range of 0.5~1wt.%, and Al volatilization and burning loss are serious. The surface scanning results of energy spectrum analysis show that Nb, Zr, Ti and Al are not evenly distributed inside the ingot, among which the uneven distribution of Al is more obvious, and the segregation of Nb is serious.
[0066] In summary, the invention includes but is not limited to the above embodiments. Any equivalent substitution or partial improvement made under the spirit and principle of the invention shall be deemed to be within the protection scope of the invention.
Claims
1. A vacuum consumable arc melting method for NbZrTiAl refractory high entropy alloy ingots, characterized in that: The method steps include: (1) Batching and mixing: weighing the raw materials of each component in the NbZrTiAl series refractory high entropy alloy according to atomic percentage, crushing the raw materials to obtain particles with a particle size of 5 to 10 mm, and then mixing them to obtain a mixed material; (2) Pressing electrode blocks: Pressing the mixture into multiple cylindrical electrode blocks; the mass of each electrode block is 1 / 9 to 1 / 3 of the total mass of the mixture, the diameter of the electrode block is 100 to 300 mm, and the density of each electrode block is 3.0 to 5.0 g / cm 3 ; (3) welding a consumable electrode: welding the electrode block into a consumable electrode; (4) Melting: placing the consumable electrode into an arc furnace, and performing vacuum consumable arc melting for more than three times under an inert gas atmosphere, and obtaining a NbZrTiAl-based refractory high entropy alloy ingot after the melting is completed; The atomic expression of the NbZrTiAl refractory high entropy alloy is: a Zr b Ti c Al d M x , M is one or more of V, Cr, Mn, Fe, Co, Ni, Mo, Hf and W, 10≤a≤25, 5≤b≤30, 40≤c≤70, 15≤d≤40, 0≤x≤10, and a+b+c+d+x=100; In step (1), Zr is added in the form of single substance sponge zirconium, Ti is added in the form of single substance sponge titanium and AlTi master alloy, Nb, M and Al are added in the form of AlNb master alloy and AlM master alloy respectively; the volume of the single substance is more than 50% of the total volume; In step (2), the pressing pressure is (electrode block surface pressure × π × electrode block radius squared) × 10 -4 Tons, the surface pressure of the electrode block is 250~350MPa; In step (4), the smelting voltage is 30-40 V, the first smelting current is 2-7 kA, and starting from the second smelting, the smelting current is increased by 1-2 kA compared with the previous smelting current; the first and second smelting times are 3-5 min, and the circulating cooling water temperature is maintained at 55-65 ° C; the third and subsequent smelting times are 6-10 min, respectively, and the circulating cooling water temperature is maintained at 35-45 ° C; during the smelting process, a single-winding spiral electromagnetic stirring device is used to electromagnetically stir the high-entropy alloy melt, and the deflection angle of the inclined magnetic yoke is 40°-60°.
2. A vacuum consumable arc melting method for NbZrTiAl refractory high entropy alloy ingots as claimed in claim 1, characterized in that: In step (1), Nb and Al are added in the form of Al-(60~75)Nb and Al-(5~10)Ti master alloys, respectively; V, Cr, Mn, Fe, Co, Ni, Mo, Hf and W are added in the form of Al-(10~50)V, Al-(10~20)Cr, Al-(10~80)Mn, Al-(10~60)Fe, Al-(10~30)Co, Al-(10~20)Ni, Al-(20~60)Mo, Al-(10~20)Hf and Al-(10~50)W master alloys, respectively.
3. A vacuum consumable arc melting method for NbZrTiAl refractory high entropy alloy ingots as claimed in claim 1, characterized in that: In step (1), when the raw materials are crushed, a jaw crusher is first used to coarsely crush the sponge zirconium, sponge titanium and intermediate alloy particles, and after the coarse crushing, a vibrating screen is used to screen the particles with a particle size of less than 150 mm; then a toothed roller crusher is used to medium crush the screened particles, and after the medium crushing, a vibrating screen is used to screen the particles with a particle size of less than 75 mm; finally, the screened particles are finely crushed 4 to 10 times by a toothed roller crusher, and after the fine crushing, a vibrating screen is used to screen the particles with a particle size of 5 to 10 mm.
4. A vacuum consumable arc melting method for NbZrTiAl refractory high entropy alloy ingots as claimed in claim 1, characterized in that: In step (1), the mixing is performed multiple times, the amount of a single mixing is sufficient to suppress the mass of an electrode block, and the single mixing time is 10 to 20 minutes.
5. A vacuum consumable arc melting method for NbZrTiAl refractory high entropy alloy ingots as claimed in claim 1, characterized in that: In step (3), the electrode blocks are welded in an inert atmosphere protection welding box. During welding, a pressure of 0.015 to 0.025 tons is applied to the electrode blocks at both ends, and the vacuum degree in the box is 2 to 6×10 -3 Pa, a weld is made at the butt joint of the two electrode blocks; 2 to 6 longitudinal welds are evenly distributed in the direction perpendicular to the butt weld.
6. A vacuum consumable arc melting method for NbZrTiAl refractory high entropy alloy ingots as claimed in claim 5, characterized in that: The weld width is 20~25mm, the depth is 10~15mm, the longitudinal weld length is 30~40mm, the solder is Ti-Zr-Cu-Ni series solder, and the composition is Ti-(13~37.5)Zr-(15~21)Cu-(9~15)Ni.
7. A vacuum consumable arc melting method for NbZrTiAl refractory high entropy alloy ingots as claimed in claim 1, characterized in that: In step (4), when the ingot is melted, the pressure is 1.3 to 1.5 times the vapor pressure of the Al element at the melt temperature.
8. A vacuum consumable arc melting method for NbZrTiAl refractory high entropy alloy ingots as claimed in claim 1, characterized in that: In step (4), during electromagnetic stirring, when the smelted weight is less than 1 / 50 of the total weight of the ingot, the rotating magnetic field in the electromagnetic stirring device is operated alone, and its intensity is 5-20 gauss, the stirring period is 5-20s, and the switching frequency is 5-20s / time; when the smelted weight is greater than or equal to 1 / 50 of the total weight of the ingot, the rotating magnetic field and the traveling wave magnetic field in the electromagnetic stirring device are operated simultaneously to form a spiral magnetic field, wherein the intensity of the rotating magnetic field is 25-50 gauss, the stirring period is 25-50s, the switching frequency is 25-50s / time, the intensity of the traveling wave magnetic field is 25-50 gauss, the stirring period is 25-50s, and the direction of the induced electromagnetic force is vertically upward along the axial direction of the ingot.
9. A vacuum consumable arc melting method for NbZrTiAl refractory high entropy alloy ingots as claimed in claim 1, characterized in that: In step (4), starting from the second smelting, a head of material having a length of 0.01 to 0.03 times the ingot length is cut off before each smelting and then the smelting direction is reversed.