High-entropy alloy ceramic composite coating with wide temperature range and low thermal conductivity, preparation method and application thereof
By using a high-entropy alloy ceramic composite coating with wide temperature range and low thermal conductivity in diesel engines, and using atmospheric plasma spraying technology to form a disordered structure interface layer, the problem of increased thermal conductivity of metal-based thermal barrier coatings under high temperature conditions is solved. problem, achieving excellent thermal insulation and mechanical properties at medium and high temperatures, extending the service life of the coating.
Patent Information
- Application Number
- CN202411082659.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-08-08
AI Technical Summary
The thermal conductivity of existing metal-based thermal barrier coatings increases sharply under high temperature conditions, resulting in degradation of thermal insulation performance, making it difficult to effectively improve thermal efficiency and extend service life in diesel engines.
A high-entropy alloy ceramic composite coating with low thermal conductivity in a wide temperature range is used. High-entropy alloy powder and yttria-stabilized zirconia powder are mixed through atmospheric plasma spraying technology to form an interface layer rich in Al-Ti-Si-O disordered structure. , reduce the thermal conductivity of the coating, and ensure the thermal insulation and mechanical properties of the coating at medium and high temperatures through reasonable element composition and process parameter control.
It maintains low thermal conductivity above 1000°C, significantly improves thermal insulation performance and mechanical properties, and extends the service life of the coating. It is suitable for thermal insulation protection of hot-end components of diesel engines.
Smart Images

Figure CN118600362B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of thermal insulation and protection technology in surface engineering, and in particular to a high-entropy alloy ceramic composite coating with low thermal conductivity over a wide temperature range, and a preparation method and application thereof. Background Art
[0002] Diesel engines are widely used due to their high thermal efficiency, wide power range, safe operation, and long service life. However, excessive consumption of diesel not only brings about an energy crisis, but also seriously pollutes the environment with exhaust gas produced by its combustion. Preparing thermal barrier coatings (TBCs) on the hot end surfaces of high heat consumption components of diesel engines can effectively improve thermal efficiency and reduce exhaust emissions.
[0003] The successful application of thermal barrier coating technology in high-temperature fields such as aerospace has provided a good reference for the thermal protection of diesel engine-related components. At present, ceramic materials represented by YSZ are widely used, which have excellent thermal insulation properties and good high-temperature phase stability. However, when used in internal combustion engines, due to the inherent brittleness of ceramic materials, the coating is prone to high-frequency thermal fatigue under the coupling of thermal and mechanical loads, which can cause cracking and peeling of the coating in severe cases, affecting the service life of the coating.
[0004] Based on the possible problems in the application of ceramic-based thermal barrier coatings in internal combustion engines, a research team has proposed the design concept of metal-based thermal barrier coatings. At present, the research on related metal-based thermal barrier coatings is still mainly based on Fe-based amorphous coatings, such as the invention patents 201410128869.4, 201610024163.2, 201610024343.0, 201610025620.X and 201710811742.6 disclosed by Zhou Zheng's team. However, Fe-based amorphous alloys are metastable materials, which will crystallize at around 600°C, causing the thermal conductivity to rise sharply, thereby causing the thermal insulation performance of the coating to degrade. The temperature faced by the hot end surfaces such as the internal pistons of large ship-type heavy-duty diesel engines can reach more than 1000°C instantly, which is a huge challenge to the performance stability and reliability of Fe-based amorphous alloy coatings. Although Zhou Zheng's team designed a new type of high-entropy alloy as a candidate material for metal-based thermal barrier coatings, its room temperature thermal conductivity is about 3 W / mK, and the thermal conductivity of the coating has increased to about 10 W / mK at 900°C, which means that the thermal insulation performance of the coating has seriously degraded, and also limits the improvement of the thermal efficiency of diesel engines.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] In order to solve the above technical problems, the present invention provides a high-entropy alloy ceramic composite coating with low thermal conductivity over a wide temperature range, and a preparation method and application thereof.
[0007] Specifically, the technical solution of the present invention is as follows:
[0008] In the first aspect, the present invention provides a high-entropy alloy ceramic composite coating with low thermal conductivity over a wide temperature range, which is prepared by atmospheric plasma spraying of mixed high-entropy alloy powder and ceramic powder; the high-entropy alloy powder includes the following components in percentage by mass: Al: 3-8%; Co: 5-10%; Cr: 27-32%; Fe: 28-33%; Ni: 10-15%; Ti: 8-13%; Si: 0.1-3%; B: 0.1-1%; the ceramic powder is yttria-stabilized zirconia; by volume, the amount of the ceramic powder is 15-25% of the total amount of the high-entropy alloy powder and the ceramic powder.
[0009] Preferably, a disordered structure interface layer with Al-Ti-Si-O as the main elements is formed between the high-entropy alloy particles and the ceramic particles in the high-entropy alloy ceramic composite coating prepared by atmospheric plasma spraying of the present invention; the thickness of the disordered structure interface layer is 20 to 40 nm.
[0010] Preferably, the high entropy alloy powder of the present invention comprises the following components in percentage by mass: Al: 4-7%; Co: 6-9%; Cr: 26-30%; Fe: 29-32%; Ni: 10-15%; Ti: 9-12%; Si: 1-2%; B: 0.1-1%;
[0011] Preferably, the high entropy alloy powder of the present invention is a spherical powder with a particle size ranging from 38 to 80 μm.
[0012] Preferably, the ceramic powder of the present invention is agglomerated sintered powder with a particle size ranging from 25 to 75 μm.
[0013] In a second aspect, the present invention provides a method for preparing the high-entropy alloy ceramic composite coating with a wide temperature range and low thermal conductivity, which comprises the following steps: mixing high-entropy alloy powder and ceramic powder, and performing atmospheric plasma spraying.
[0014] Preferably, the process parameters of the atmospheric plasma spraying include: current 630-720A, argon flow rate 55±5L / min, hydrogen flow rate 5-10L / min, powder feeding rate 38±2g / min, and spraying distance 90-100mm.
[0015] More preferably, the process parameters of the atmospheric plasma spraying include: current 650±10A, argon flow rate 55±1L / min, hydrogen flow rate 8±1L / min, powder feeding rate 38±1g / min, and spraying distance 95±1mm.
[0016] In a third aspect, the present invention provides an application of the high-entropy alloy ceramic composite coating with low thermal conductivity over a wide temperature range or the high-entropy alloy ceramic composite coating with low thermal conductivity over a wide temperature range obtained by the preparation method in thermal insulation protection of hot end components of a diesel engine.
[0017] Preferably, the thermal insulation protection can maintain a thermal conductivity of 1.75 to 3.58 W / mK within 1000°C, and the wear rate at 600°C is as low as 2×10 -5 mm 3 N -1 m -1 the following.
[0018] Beneficial effects:
[0019] The present invention provides a high-entropy alloy ceramic composite coating with low thermal conductivity in a wide temperature range, and a preparation method and application thereof. The high-entropy alloy ceramic composite coating with low thermal conductivity in a wide temperature range is prepared by atmospheric plasma spraying of mixed high-entropy alloy powder and ceramic powder; the high-entropy alloy powder includes the following components in percentage by mass: Al: 3-8%; Co: 5-10%; Cr: 27-32%; Fe: 28-33%; Ni: 10-15%; Ti: 8-13%; Si: 0.1-3%; B: 0.1-1%; the ceramic powder is yttria-stabilized zirconia; by volume, the amount of the ceramic powder is 15-25% of the total amount of the high-entropy alloy powder and the ceramic powder. The coating provided by the present invention has excellent thermal insulation and mechanical properties, and has broad application prospects in the field of medium and high temperature thermal insulation protection. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be described below.
[0021] Figure 1 XRD spectra of the high entropy alloy / ceramic composite coating prepared in Example 4 and the iron-based amorphous / ceramic composite coating prepared in Comparative Example 5 after heat treatment at room temperature and 1000° C. for 2 hours.
[0022] Figure 2 This is the SEM morphology of the high entropy alloy and ceramic composite coating prepared in Example 4.
[0023] Figure 3 This is the TEM morphology of the high entropy alloy and ceramic composite coating prepared in Example 4.
[0024] Figure 4 The results of the thermal conductivity of the high entropy alloy ceramic composite coating prepared in Example 4 changing with temperature. DETAILED DESCRIPTION
[0025] The invention provides a high entropy alloy / ceramic composite coating with low thermal conductivity in a wide temperature range, and a preparation method and application thereof. The composite coating is mainly composed of high entropy alloy particles with a BCC phase structure, ceramic particles, and a heterogeneous particle interface layer. Specifically, the high entropy alloy and ceramic composite powder are sprayed by atmospheric plasma spraying technology to form a disordered structure interface layer rich in Al-Ti-Si-O between the high entropy alloy particles and the ceramic particles, thereby reducing the thermal conductivity of the composite coating and greatly improving the thermal insulation performance of the coating.
[0026] In a more specific embodiment provided by the present invention, the high entropy alloy powder is AlCoCrFeNiTiSiB with a particle size of 38 to 80 μm, which is prepared by a high-pressure argon gas atomization method. The ceramic powder is YSZ with a particle size of 25 to 75 μm, which is prepared by agglomeration sintering. The high entropy alloy powder and the YSZ powder are mixed in a certain volume ratio to finally obtain a composite powder with good sphericity. The preparation method is atmospheric plasma spraying technology. The composite coating prepared by the present invention has a disordered structure interface layer rich in Al-Ti-Si-O, and under the action of YSZ, the composite coating maintains a low thermal conductivity in a wide temperature range, and can be used for thermal insulation protection of hot end components of diesel engines.
[0027] More specifically, the present invention adopts the following technical solutions:
[0028] A high entropy alloy / ceramic composite coating material with low thermal conductivity over a wide temperature range, wherein the raw material powder contains two components, namely, a high entropy alloy and a ceramic; the high entropy alloy components are as follows in terms of mass percentage: Al: 3-8%; Co: 5-10%; Cr: 27-32%; Fe: 28-33%; Ni: 10-15%; Ti: 8-13%; Si: 0.1-3%; B: 0.1-1%; the ceramic is YSZ, i.e., yttria-stabilized zirconia, and the volume of the YSZ ceramic powder accounts for 15%-25% of the total amount of the high entropy alloy and ceramic composite powder.
[0029] As a preferred solution, the composition of the elements in the high entropy alloy / ceramic composite coating in terms of mass percentage is as follows: Al: 4-7%; Co: 6-9%; Cr: 26-30%; Fe: 29-32%; Ni: 10-15%; Ti: 9-12%; Si: 1-2%; B: 0.1-1%.
[0030] The method of the present invention for preparing a high entropy alloy / ceramic composite coating with low thermal conductivity over a wide temperature range using the above-mentioned materials preferably comprises the following steps:
[0031] Step 1: prepare high entropy alloy powder and ceramic powder by argon atomization method and agglomeration sintering method respectively, and then mix the two powders to obtain composite powder.
[0032] Step 2: Remove the oxide film and dirt on the surface of the metal substrate, and then sandblast it. Then use atmospheric plasma spraying technology to prepare a high entropy alloy / ceramic composite coating on the surface of the metal substrate. The process parameters are: current 630-720A, argon flow rate 55L / min, hydrogen flow rate 5-10L / min, powder feeding rate: 38g / min, spraying distance: 90-100mm.
[0033] The high entropy alloy / ceramic composite coating prepared by the above method can maintain low thermal conductivity, stable thermal insulation performance and good fracture toughness in a wide temperature range; the improvement of the thermal insulation performance of the composite coating is mainly determined by its own organizational structure.
[0034] The composite coating material of the present invention comprises two parts: a high entropy alloy and ceramics.
[0035] The high entropy alloy part is a multi-principal alloy containing aluminum, cobalt, chromium, iron, nickel, titanium, silicon, and boron. Among them, the atomic radius of several transition metals is relatively close, the difference in atomic size is relatively small, the substitution between the component atoms is relatively simple, and there is a similar probability to occupy the lattice, which helps to form a disordered solid solution. Iron and chromium elements can promote the formation of disordered BCC phases in the coating, and relatively high content can also increase the disorder degree of the coating, which is conducive to increasing the scattering effect on electrons and phonons. Adding nickel and cobalt elements increases the entropy value of the alloy system to promote the formation of a single-phase solid solution, and at the same time provides a guarantee for the high-temperature mechanical stability of the coating. The present invention not only promotes the system to generate BCC phases by adding a certain amount of titanium elements, but also has a larger atomic radius relative to other elements. The same large-sized aluminum element can increase the degree of lattice distortion and further increase the scattering effect on electrons and phonons. Aluminum elements are easy to react with nickel elements and the like to form intermetallic compounds, which increases the brittleness of the coating. The present invention mainly solves this problem by coordinating element content and process. The present invention adds a small amount of silicon element to the alloy composition, controls the solidification conditions through the preparation process, so that a part of the silicon element can be dissolved in the lattice as small-sized atoms, increases the lattice friction, and then reduces the phonon thermal conductivity. At the same time, another part of the silicon element can diffuse rapidly to the particle interface, and jointly with aluminum and titanium elements to form an interface layer with a disordered structure at the interface between ceramic and metal particles. The formation of the interface layer can not only effectively increase the interface wettability of the ceramic particles, but also increase the scattering effect of the heat transfer carrier by using the disordered structure, further reduce the overall thermal conductivity of the coating, and increase the thermal insulation effect. The thickness of the interface layer is crucial to the overall performance of the coating. If the interface layer is too thin, it is difficult to play a wetting role. If it is too thick, it will affect the interface bonding force of the deformed particles, reduce the bonding strength between the coating and the substrate, and even cause particle peeling or fracture. The present invention strictly controls the thickness and quality of the interface layer, especially by introducing a small amount of boron element to reduce the oxidation degree of the metal elements in the coating, and at the same time, it inhibits the excessive growth of the thickness of the interface layer of heterogeneous particles, thereby ensuring the mechanical properties of the coating. In addition, the mixing enthalpy of boron with iron and chromium is relatively negative, and brittle boride is easily formed. The present invention solves this technical problem by precisely regulating its content and controlling the effect of boron with the spraying process.
[0036] YSZ is selected as the ceramic part. YSZ has low thermal conductivity and good high-temperature phase stability. Its addition can reduce the thermal conductivity of the composite coating. However, ceramics have intrinsic brittleness, and excessive content will significantly reduce the mechanical properties of the coating. At the same time, the coordinated deformation of the high-melting-point ceramic phase and the low-melting-point metal particles is also a difficulty in process control. The method provided by the present invention controls the content of ceramic particles and the spraying process to regulate the coordinated deformation with metal particles, and finally obtains a composite coating with better comprehensive performance.
[0037] In the present invention, the disordered BCC phase structure rich in FeCr elements is relatively stable and almost no phase change occurs. At the same time, the micrometer-scale ceramic phase structure is also relatively stable within 1170°C, and the nanometer-scale disordered interface layer enhances the interface stability of the heterogeneous phase structure. Therefore, the obtained composite coating can maintain a stable phase structure under a wide temperature range, show low thermal conductivity, and have good mechanical properties and high temperature wear resistance.
[0038] In summary, the high entropy alloy / ceramic composite coating provided by the present invention has low thermal conductivity in a wide temperature range, good fracture toughness and high temperature wear resistance, which is mainly achieved by the synergistic effect of factors such as reasonable metal matrix composition, suitable metal / ceramic design and reasonable process parameters. Each element in the composite coating plays a vital role and is indispensable. Of course, it cannot be obtained by just a limited number of tests.
[0039] Compared with the prior art, the present invention has the following advantages:
[0040] The high entropy alloy and ceramic composite coating prepared by the present invention has excellent thermal insulation performance and good mechanical properties, and has broad application prospects in the field of medium and high temperature thermal insulation protection. First, an interface layer with a disordered structure is generated at the interface between the metal particles and the ceramic particles in the coating; secondly, the thermal conductivity of the coating is low, and it can be as low as 1.75W / mK at room temperature without post-treatment; thirdly, compared with the disclosed metal-based thermal barrier coatings, the high entropy alloy and ceramic composite coating has lower thermal conductivity and better thermal stability at medium and high temperatures, and there is no obvious mutation within 1000°C; finally, the fracture toughness of the coating is good, which can reach 4.41MPa / mm 1 / 2 The friction and wear rate at 600°C is as low as 1.76×10 -5 mm 3 N -1 m -1 .
[0041] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0043] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "specific implementations", or "some specific implementations" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the embodiment of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0044] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased through regular channels.
[0045] In the following embodiments, the coating is prepared by the following steps:
[0046] Step 1: prepare high entropy alloy powder and ceramic powder by argon atomization method and agglomeration sintering method respectively, and then mix the two powders to obtain composite powder.
[0047] Step 2: Remove the oxide film and dirt on the surface of the metal substrate, and then sandblast it. Then use atmospheric plasma spraying technology to prepare a high entropy alloy / ceramic composite coating on the surface of the metal substrate. The process parameters are: current 630-720A, argon flow rate 55L / min, hydrogen flow rate 5-10L / min, powder feeding rate: 38g / min, spraying distance: 90-100mm.
[0048] Example 1
[0049] The mass percentages of the elements in the high entropy alloy powder are as follows: Al: 3%; Co: 9%; Cr: 31%; Fe: 33%; Ni: 13%; Ti: 10%; Si: 0.9%; B: 0.1%; and unavoidable impurities < 0.5%. The volume of YSZ accounts for 15% of the total amount of high entropy alloy and ceramic composite powder. The spraying process parameters are: current: 600A, argon flow rate: 55L / min, hydrogen flow rate: 8L / min, powder feeding rate: 38g / min, spraying distance: 90mm.
[0050] Example 2
[0051] The mass percentages of the elements in the high entropy alloy powder are as follows: Al: 5%; Co: 9%; Cr: 28%; Fe: 31%; Ni: 15%; Ti: 11%; Si: 0.9%; B: 0.1%; and unavoidable impurities < 0.5%. The volume of YSZ accounts for 15% of the total amount of high entropy alloy and ceramic composite powder. The spraying process parameters are: current: 600A, argon flow rate: 55L / min, hydrogen flow rate: 8L / min, powder feeding rate: 38g / min, spraying distance: 90mm.
[0052] Example 3
[0053] The mass percentages of the elements in the high entropy alloy powder are as follows: Al: 8%; Co: 10%; Cr: 27%; Fe: 32%; Ni: 11%; Ti: 10%; Si: 1.5%; B: 0.5%; and unavoidable impurities < 0.5%. The volume of YSZ accounts for 15% of the total amount of high entropy alloy and ceramic composite powder. The spraying process parameters are: current: 630A, argon flow rate: 55L / min, hydrogen flow rate: 8L / min, powder feeding rate: 38g / min, spraying distance: 90mm.
[0054] Example 4
[0055] The mass percentages of the elements in the high entropy alloy powder are as follows: Al: 6%; Co: 7%; Cr: 30%; Fe: 31%; Ni: 13%; Ti: 11%; Si: 1.5%; B: 0.5%; and unavoidable impurities < 0.5%. The volume of YSZ accounts for 20% of the total amount of high entropy alloy and ceramic composite powder. The spraying process parameters are: current: 650A, argon flow rate: 55L / min, hydrogen flow rate: 8L / min, powder feeding rate: 38g / min, spraying distance: 95mm.
[0056] Example 5
[0057] The mass percentages of the elements in the high entropy alloy powder are as follows: Al: 7%; Co: 5%; Cr: 31%; Fe: 29%; Ni: 14%; Ti: 12%; Si: 1.7%; B: 0.3%; and unavoidable impurities < 0.5%. The volume of YSZ accounts for 20% of the total amount of high entropy alloy and ceramic composite powder. The spraying process parameters are: current: 650A, argon flow rate: 55L / min, hydrogen flow rate: 8L / min, powder feeding rate: 38g / min, spraying distance: 95mm.
[0058] Example 6
[0059] The mass percentages of the elements in the high entropy alloy powder are as follows: Al: 7%; Co: 8%; Cr: 29%; Fe: 31%; Ni: 10%; Ti: 13%; Si: 1.7%; B: 0.3%; and unavoidable impurities < 0.5%. The volume of YSZ accounts for 20% of the total amount of high entropy alloy and ceramic composite powder. The spraying process parameters are: current: 690A, argon flow rate: 55L / min, hydrogen flow rate: 8L / min, powder feeding rate: 38g / min, spraying distance: 95mm.
[0060] Example 7
[0061] The mass percentages of the elements in the high entropy alloy powder are as follows: Al: 8%; Co: 6%; Cr: 32%; Fe: 28%; Ni: 13%; Ti: 10%; Si: 2.3%; B: 0.7%; and unavoidable impurities < 0.5%. The volume of YSZ accounts for 20% of the total amount of high entropy alloy and ceramic composite powder. The spraying process parameters are: current: 690A, argon flow rate: 55L / min, hydrogen flow rate: 8L / min, powder feeding rate: 38g / min, spraying distance: 100mm.
[0062] Example 8
[0063] The mass percentages of the elements in the high entropy alloy powder are as follows: Al: 6%; Co: 9%; Cr: 30%; Fe: 29%; Ni: 12%; Ti: 11%; Si: 2.3%; B: 0.7%; and unavoidable impurities < 0.5%. The volume of YSZ accounts for 25% of the total amount of high entropy alloy and ceramic composite powder. The spraying process parameters are: current: 690A, argon flow rate: 55L / min, hydrogen flow rate: 8L / min, powder feeding rate: 38g / min, spraying distance: 100mm.
[0064] Example 9
[0065] The mass percentages of the elements in the high entropy alloy powder are as follows: Al: 5%; Co: 10%; Cr: 27%; Fe: 32%; Ni: 10%; Ti: 13%; Si: 2.1%; B: 0.9%; and unavoidable impurities < 0.5%. The volume of YSZ accounts for 25% of the total amount of high entropy alloy and ceramic composite powder. The spraying process parameters are: current: 720A, argon flow rate: 55L / min, hydrogen flow rate: 8L / min, powder feeding rate: 38g / min, spraying distance: 100mm.
[0066] Example 10
[0067] The mass percentages of the elements in the high entropy alloy powder are as follows: Al: 3%; Co: 8%; Cr: 32%; Fe: 28%; Ni: 15%; Ti: 11%; Si: 2.1%; B: 0.9%; and unavoidable impurities < 0.5%. The volume of YSZ accounts for 25% of the total amount of high entropy alloy and ceramic composite powder. The spraying process parameters are: current: 720A, argon flow rate: 55L / min, hydrogen flow rate: 8L / min, powder feeding rate: 38g / min, spraying distance: 100mm.
[0068] Comparative Example 1
[0069] The mass percentages of the elements in the high entropy alloy powder are as follows: Al: 8%; Co: 15%; Cr: 20%; Fe: 20%; Ni: 15%; Ti: 14%; Si: 7%; B: 1%; and unavoidable impurities < 0.5%. The volume of YSZ accounts for 20% of the total amount of high entropy alloy and ceramic composite powder. The spraying process parameters are: current: 600A, argon flow rate: 45L / min, hydrogen flow rate: 10L / min, powder feeding rate: 38g / min, spraying distance: 130mm.
[0070] Comparative Example 2
[0071] Referring to the existing iron-based-ceramic composite coating patent (ZL201710811742.6), the mass percentage of raw materials in the iron-based-ceramic composite powder is as follows: iron-based alloy powder raw materials: ferroboron (B: 18%): 24%, ferroniobium (Nb: 65%): 13%, ferrosilicon (Si: 75%): 3%, pure chromium: 17% and pure iron 43%; mixed with TiO2 (TiO2 accounts for 18% of the total mass). The coating was prepared by atmospheric plasma spraying technology, and the spraying process parameters were: current: 600A, argon flow rate: 35L / min, hydrogen flow rate: 10L / min, powder feeding rate: 54g / min, spraying distance: 130mm.
[0072] Comparative Example 3
[0073] Referring to the existing high entropy alloy coating patent (ZL201810317100.5), the molar percentages of the elements in the coating are as follows: Al: 12.7%; Co: 15%; Cr: 17.5%; Fe: 18.6%; Ni: 17%; Ti: 19.2%; and unavoidable impurities: <0.5%. The coating was prepared by atmospheric plasma spraying technology, and the spraying process parameters were: current 550-650A, argon flow rate: 35L / min, hydrogen flow rate: 10L / min, powder feeding rate: 54g / min, spraying distance: 115-135mm.
[0074] Comparative Example 4
[0075] Referring to the existing patented iron-based amorphous-ceramic laminated thermal insulation coating (ZL201911215196.5), the raw materials of the iron-based amorphous layer are: ferroboron: 22%, ferroniobium: 12%, ferrosilicon: 4%, pure chromium: 20% and pure iron 42%. The thickness of the iron-based amorphous layer is about 100μm. The raw material of the ceramic layer is: TiO2. The thickness of the ceramic layer is about 50μm. The total thickness of the ceramic laminated coating is about 400μm. The laminated coatings were prepared by atmospheric plasma spraying technology, wherein the spraying process parameters of the iron-based amorphous layer are: current: 600A, argon flow rate: 45L / min, hydrogen flow rate: 4L / min, powder feeding rate: 58g / min, spraying distance: 135mm; the spraying process parameters of the ceramic layer are: current: 630A, argon flow rate: 25L / min, hydrogen flow rate: 8L / min, powder feeding rate: 48g / min, spraying distance: 135mm. The total thickness of the obtained double ceramic layer stacked coating of iron-based amorphous layer-ceramic layer-iron-based amorphous layer-ceramic layer-iron-based amorphous layer is 400 μm.
[0076] Comparative Example 5
[0077] Referring to the iron-based amorphous / ceramic composite coating in the existing patent (ZL202010525583.5), the raw material mass composition of the iron-based amorphous alloy powder is: ferroboron (B: 18%): 24%, ferroniobium (Nb: 65%): 13%, ferrosilicon (Si: 75%): 3%, pure chromium: 17% and pure iron 43%; mixed with YSZ containing 7wt% ZrO2 (YSZ accounts for 20% of the total volume). The coating was prepared by atmospheric plasma spraying technology, and the spraying process parameters were: current: 600A, argon flow rate: 45L / min, hydrogen flow rate: 4L / min, powder feeding rate: 42-60g / min, spraying distance: 135mm. The heat treatment of the prepared metal-based-ceramic composite coating specifically includes pre-annealing at 300°C for 5min in an argon atmosphere, and then heating to 400°C for annealing for 120min.
[0078] The coatings prepared in each embodiment and comparative example were subjected to XRD, SEM, TEM and fracture toughness tests; the thermal conductivity of the coatings prepared in each embodiment and comparative example was analyzed using a laser thermal conductivity analyzer; the friction and wear behavior of the coatings at different temperatures was tested using a reciprocating friction and wear device, and the wear volume was measured using a laser confocal microscope. Among them, comparative examples 2 to 5 were prepared according to the materials and methods described in the disclosed patents, and the thermal conductivity of the coatings from room temperature to 1000°C and the wear rate of the coatings were tested under the same conditions, and the results are shown in Table 1.
[0079] XRD test results of high entropy alloy / ceramic composite coating are as follows: Figure 1 As shown, the SEM morphology is Figure 2 As shown, the TEM morphology is Figure 3 The thermal conductivity curve with temperature is shown in Figure 4 The thermal conductivity, fracture toughness and wear rate of the composite coating are shown in Table 1.
[0080] Table 1 Test results of thermal conductivity, fracture toughness and wear rate of composite coatings of embodiments and comparative examples
[0081]
[0082] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A high-entropy alloy ceramic composite coating with a wide temperature range and low thermal conductivity, characterized in that: The invention is prepared by atmospheric plasma spraying of mixed high entropy alloy powder and ceramic powder; the high entropy alloy powder comprises the following components in percentage by mass: Al: 3-8%; Co: 5-10%; Cr: 27-32%; Fe: 28-33%; Ni: 10-15%; Ti: 8-13%; Si: 0.1-3%; B: 0.1-1%; the ceramic powder is yttria-stabilized zirconia; by volume, the amount of the ceramic powder is 15-25% of the total amount of the high entropy alloy powder and the ceramic powder.
2. According to claim 1, the high-entropy alloy ceramic composite coating with wide temperature range and low thermal conductivity is characterized in that: A disordered structure interface layer with Al-Ti-Si-O as main elements is formed between high entropy alloy particles and ceramic particles in the high entropy alloy ceramic composite coating prepared by atmospheric plasma spraying; the thickness of the disordered structure interface layer is 20-40nm.
3. The high-entropy alloy ceramic composite coating with a wide temperature range and low thermal conductivity according to claim 1, characterized in that: The high entropy alloy powder includes the following components in percentage by mass: Al: 4-7%, Co: 6-9%, Cr: 26-30%, Fe: 29-32%, Ni: 10-15%, Ti: 9-12%, Si: 1-2%, and B: 0.1-1%.
4. The high-entropy alloy ceramic composite coating with a wide temperature range and low thermal conductivity according to claim 1, characterized in that: The high entropy alloy powder is spherical powder with a particle size range of 38-80 μm.
5. The high-entropy alloy ceramic composite coating with a wide temperature range and low thermal conductivity according to claim 1, characterized in that: The ceramic powder is agglomerated sintered powder with a particle size ranging from 25 to 75 μm.
6. The method for preparing the high entropy alloy ceramic composite coating with wide temperature range and low thermal conductivity according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: mixing high entropy alloy powder and ceramic powder, and performing atmospheric plasma spraying.
7. The preparation method according to claim 6, characterized in that: The process parameters of the atmospheric plasma spraying include: current 630-720A, argon flow rate 55±5L / min, hydrogen flow rate 5-10L / min, powder feeding rate 38±2g / min, and spraying distance 90-100mm.
8. The preparation method according to claim 7, characterized in that: The process parameters of the atmospheric plasma spraying include: current 650±10A, argon flow rate 55±1L / min, hydrogen flow rate 8±1L / min, powder feeding rate 38±1g / min, and spraying distance 95±1mm.
9. Application of the high-entropy alloy ceramic composite coating with low thermal conductivity over a wide temperature range as described in any one of claims 1 to 5 or the high-entropy alloy ceramic composite coating with low thermal conductivity over a wide temperature range obtained by the preparation method described in any one of claims 6 to 8 in thermal insulation protection of hot end components of diesel engines.
10. The use according to claim 9, characterized in that: The thermal insulation protection can maintain a thermal conductivity of 1.75 to 3.58 W / mK within 1000°C, and the wear rate at 600°C is as low as 2×10 -5 mm 3 N -1 m -1 the following.
Citation Information
Patent Citations
Heat-insulating coating material for preventing hot-end component of automobile engine, and preparation method thereof
CN103898434A
Coating material for thermal insulation protection and coating preparing method of coating material
CN105568167A
Iron-based coating material for heat insulating protection and coating preparation method thereof
CN105603350A
Cored wire used for preparing iron-based coating and coating preparation method of cored wire
CN105648384A
Composite material for heat insulating coating and coating preparing method of composite material
CN107604299A