Semiconductor processing method and process equipment
By recycling the first plasma gas removal and the second plasma gas regenerating the oxide layer, the problem of trench surface damage defects after etching is solved, and the surface flatness is improved and subsequent process optimization is achieved.
Patent Information
- Application Number
- CN202410713839.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-04
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-06-04
AI Technical Summary
In the etching process during semiconductor manufacturing, the trench or other etching termination interface of the wafer is prone to burr-like damage defects due to ion bombardment and gas reaction unevenness, which affects the subsequent process.
The oxide layer on the semiconductor substrate and the trench surface is removed using a first plasma gas, and then the oxide layer is regenerated on the target surface using a second plasma gas, and cycles until defects are eliminated.
It effectively eliminates damage defects in the trench or other etching termination interface after etching, improves the flatness of the trench surface, and ensures the smooth progress of the subsequent process.
Smart Images

Figure CN118610086B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductor technology, and in particular to a semiconductor processing method and process equipment. Background Art
[0002] In the semiconductor manufacturing process, the etching process is a crucial process in the chip manufacturing process. After the gas used for etching is excited into a plasma state, the required trenches or other interfaces are etched on the wafer surface through physical / chemical effects. In this process, due to ion bombardment and the unevenness of the gas reaction in the trench, burr-like damage defects will appear on the etched trench surface or other etching termination interfaces. Such a trench surface will have an adverse effect on the subsequent trench sidewall process and trench filling process, and this situation needs to be changed.
[0003] In view of this, the present application provides a semiconductor processing method and process equipment to solve the problem that damage defects in the groove or other etching stop interface are difficult to eliminate after ion bombardment of the wafer during the etching process.
[0004] To achieve the above objectives, according to the first aspect, the technical solution adopted is:
[0005] A semiconductor processing method, comprising:
[0006] Providing a semiconductor substrate, wherein the semiconductor substrate has a target groove formed by an etching process;
[0007] After removing the oxide layer on the target surface of the semiconductor substrate and the target groove by using the first plasma gas, the oxide layer is regenerated on the target surface by using the second plasma gas, wherein the first plasma gas includes plasma H after ions are filtered out. 2 , the second plasma gas includes an oxygen-containing gas in a plasma state after ions are filtered out, and the target surface includes a surface of the semiconductor substrate, a sidewall of the target trench, and a bottom of the target trench;
[0008] The first plasma gas and the second plasma gas are cyclically used to act on the target surface until defects on the target surface are eliminated.
[0009] The present application is further configured as follows: the first plasma gas includes: plasma H after ions are filtered out 2 、N 2 and / or inert gases.
[0010] The present application is further configured as follows: the second plasma gas includes: plasma oxygen-containing gas after ions are filtered out, N 2 and / or inert gases.
[0011] The present application is further configured as follows: the oxygen-containing gas includes O 2 , O 3 or water vapor.
[0012] The present application is further configured as follows: the cyclic use of the first plasma gas and the second plasma gas to act on the target surface has a set number of cycles.
[0013] The present application is further configured such that: the target surface has rough protrusions, and after the first plasma gas and the second plasma gas are cyclically used to act on the target surface, the rough protrusions are peeled off one by one.
[0014] The present application is further configured as follows: the cyclic use of the first plasma gas and the second plasma gas to act on the target surface is completed in the same process chamber.
[0015] According to the second aspect, the technical solution adopted is:
[0016] A semiconductor process equipment comprises a process chamber, an air intake assembly, an ICP power source assembly, a plasma filter grid plate, a heating support table and a controller, wherein the controller comprises at least one processor and at least one memory, wherein a computer program is stored in the memory, and when the computer program is executed by the processor, the method for preparing a semiconductor device described in any of the above embodiments is implemented.
[0017] In summary, compared with the prior art, the present application discloses a semiconductor processing method and process equipment, which uses a first plasma gas to remove the oxide layer on the target surface of the semiconductor substrate and the target groove formed on the semiconductor substrate after the etching process, and then regenerates the oxide layer on the target surface through a second plasma gas. The first plasma gas and the second plasma gas are cyclically used to act on the target surface until the defects on the target surface are eliminated, thereby solving the problem that it is difficult to eliminate damage defects in the grooves or other etching stop interfaces of the wafer after etching. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.
[0019] Figure 1 is a flow chart of the semiconductor processing method of this embodiment;
[0020] Figure 2 is a schematic structural diagram of the semiconductor processing method of this embodiment;
[0021] Figure 3 It is a schematic structural diagram of the semiconductor process equipment of this embodiment. DETAILED DESCRIPTION
[0022] Here, exemplary embodiments will be described in detail, examples of which are shown in the accompanying drawings. When the following description refers to the drawings, unless otherwise indicated, the same numbers in different drawings represent the same or similar elements. The implementations described in the following exemplary embodiments do not represent all implementations consistent with the present application. Instead, they are only examples of devices and methods consistent with some aspects of the present application as detailed in the attached claims.
[0023] It should be noted that, in this article, the terms "include", "comprises" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the sentence "includes a ..." does not exclude the existence of other identical elements in the process, method, article or device including the element. In addition, components, features, and elements with the same name in different embodiments of the present application may have the same meaning or different meanings, and their specific meanings need to be determined by their explanation in the specific embodiment or further combined with the context of the specific embodiment.
[0024] It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0025] In the subsequent description, the suffixes such as "module", "component" or "unit" used to represent elements are only used to facilitate the description of the present application, and have no specific meanings. Therefore, "module", "component" or "unit" can be used in a mixed manner.
[0026] In the description of the present application, it should be noted that the terms "upper", "lower", "left", "right", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present application. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.
[0027] The technical solutions shown in this application will be described in detail below through specific embodiments. It should be noted that the description order of the following embodiments is not intended to limit the priority order of the embodiments.
[0028] As described in the background technology, the gas used in the existing etching is excited into a plasma state and then a desired trench or other interface is etched on the wafer surface through physical / chemical action. In this process, due to ion bombardment and the unevenness of the gas reaction in the trench, burr-like damage defects will appear on the etched trench surface or other etching stop interface. Such a trench surface will have an adverse effect on the subsequent trench sidewall process and trench filling process. Based on this, the present embodiment discloses a semiconductor processing method and process equipment.
[0029] Please refer to Figure 1 , Figure 1 is a flow chart of a semiconductor processing method of this embodiment, the semiconductor processing method comprising:
[0030] S101, providing a semiconductor substrate, wherein the semiconductor substrate has a target groove formed by an etching process.
[0031] The material of the semiconductor substrate of this embodiment can be single crystal silicon, silicon carbide, gallium arsenide, indium phosphide or silicon germanium and the like. The semiconductor substrate can also be a silicon germanium substrate, a III-V group element compound substrate, a silicon carbide substrate or its stacked structure, or a silicon-on-insulator structure. It can also be a diamond substrate or other semiconductor material substrates known to those skilled in the art.
[0032] The formation of the target groove may specifically include the following steps:
[0033] First, a layer of photoresist is coated on the semiconductor substrate, and then a photolithography machine is used to expose the photoresist to a specific mask template. The photoresist is patterned and defined through the photolithography process, and the exposed area in the photoresist is the position and shape of the target groove;
[0034] Secondly, etching equipment is used to etch the exposed areas defined by the photoresist. During the etching process, etching gas is introduced into the process chamber and physically / chemically reacts with the substrate surface through high-energy plasma, so that the substrate material is gradually removed.
[0035] Finally, after the etching is completed, the photoresist residue is removed to obtain a target trench on the semiconductor substrate.
[0036] On the other hand, before forming the target groove on the semiconductor substrate, the surface particles or natural contaminants on the surface of the semiconductor substrate may be cleaned. In one embodiment, the semiconductor substrate may be cleaned using a wet cleaning process. For example, the semiconductor substrate may be cleaned using a chemical reagent to remove contaminants on the surface of the semiconductor substrate. The chemical reagent may include a combination of one or more of sulfuric acid, hydrochloric acid, nitric acid, and hydrofluoric acid. That is, the acidic solution may include any one of the above solutions, or may include a combination of any two or more of the above solutions. This embodiment does not limit this.
[0037] S102, after removing the oxide layer on the target surface of the semiconductor substrate and the target groove using the first plasma gas, regenerating the oxide layer on the target surface using the second plasma gas, wherein the first plasma gas includes plasma H after ions are filtered out. 2 The second plasma gas includes an oxygen-containing gas in a plasma state after ions are filtered out, and the target surface includes a surface of a semiconductor substrate, a sidewall of a target trench, and a bottom of a target trench.
[0038] In this step, it should be noted that when the semiconductor substrate, i.e. the wafer, is exposed to air, its surface reacts with oxygen to form a thin oxide layer. For a silicon substrate, this oxide layer is usually silicon dioxide (SiO 2 ), the first plasma gas of this embodiment acts on the oxide layer on the target surface of the semiconductor substrate and the target groove to remove the oxide layer.
[0039] Furthermore, the present embodiment continues to use the second plasma gas to fill the defective area on the target surface, that is, the oxide layer is re-formed on the target surface by the second plasma gas. Thus, by removing and regenerating the oxide layer, the damage defects on the target surface caused by the aforementioned etching can be reduced, that is, the burr-like structural damage on the target surface can be reduced, thereby ensuring that the target surface is smooth.
[0040] S103, cyclically using the first plasma gas and the second plasma gas to act on the target surface until the defects on the target surface are eliminated.
[0041] In some embodiments, a buried layer and an epitaxial layer stacked in sequence may be formed on the semiconductor substrate. It should be noted that the target surface may represent the structural surface of the target groove, or the surface of the semiconductor substrate or the etching stop interface of the semiconductor substrate.
[0042] In this embodiment, after the oxide layer on the target surface of the semiconductor substrate and the target groove formed on the semiconductor substrate after the etching process is removed by the first plasma gas, the oxide layer is regenerated on the target surface by the second plasma gas. The first plasma gas and the second plasma gas are cyclically used to act on the target surface, which can eliminate the defect damage on the target surface. Therefore, the problem of difficult to eliminate damage defects in the groove or other etching stop interface after ion bombardment of the wafer during the etching process is solved.
[0043] The semiconductor processing method of this embodiment is described in detail below with reference to the structural schematic diagram of the semiconductor device.
[0044] Please refer to Figure 2 , Figure 2 It is a structural schematic diagram of the semiconductor processing method of this embodiment.
[0045] In a specific implementation process, a semiconductor substrate 1 is provided, and a target trench 2 is formed on the semiconductor substrate 1 after being processed by an etching process.
[0046] It is understandable that due to the ion bombardment and the non-uniformity of the gas reaction in the target groove 2 , burr-like damage defects may appear on the surface of the etched target groove 2 or the surface of the semiconductor substrate 1 or the etching stop interface of the semiconductor substrate 1 .
[0047] Furthermore, the first plasma gas is used to remove the oxide layer 4 on the target surface 3 of the semiconductor substrate 1 and the target trench 2 .
[0048] The target surface 3 of this embodiment may include the surface of the semiconductor substrate 1 , the sidewalls of the target trench 2 , and the bottom of the target trench 2 .
[0049] In one embodiment, the target surface 3 may also include an etch stop interface of the semiconductor substrate 1 .
[0050] The first plasma gas is then used to remove the oxide layer 4 on the target surface 3 of the semiconductor substrate 1 and the target trench 2 . The oxide layer 4 here may include the natural oxide layer described above.
[0051] The first plasma gas may include plasma H after ions are filtered out. 2 .
[0052] It should be noted that, in the process of removing the oxide layer 4 of the target surface 3 of the semiconductor substrate 1 and the target trench 2 by the first plasma gas, H 2 The chemical reaction of the treatment target is:
[0053] SiO 2 +H 2 →Si+H2 +O 2
[0054] That is, this embodiment uses the plasma state H after filtering out the ions. 2 After removing the oxide layer 4 of the target surface 3 of the target groove 2 formed on the semiconductor substrate 1 by the etching process, the oxide layer 4 is regenerated on the target surface 3 by the second plasma gas, and the plasma H after the ions are filtered out is recycled. 2 The second plasma gas acts on the target surface 3 to eliminate the defect damage on the target surface 3, thereby solving the problem that the damage defects in the groove or other etching stop interface of the wafer after ion bombardment during the etching process are difficult to eliminate.
[0055] In one embodiment, the first plasma gas includes: plasma H after ions are filtered out. 2 、N 2 And / or inert gas, wherein the inert gas in this embodiment refers to a gas with high stability and low reactivity, including helium (He), neon (Ne), argon (Ar), krypton (Kr) and xenon (Xe) and the like.
[0056] That is, through N 2 and / or inert gas to maintain plasma 2 stability.
[0057] In this embodiment, the plasma state H after filtering out the ions is used. 2 、N 2 After the oxide layer 4 on the target surface 3 of the target groove 2 formed on the semiconductor substrate 1 by the etching process is removed by the inert gas and / or the inert gas, the oxide layer 4 is regenerated on the target surface 3 by the second plasma gas, and the plasma H after the ions are filtered out is recycled. 2 The second plasma gas acts on the target surface 3 to eliminate the defect damage on the target surface 3, thereby solving the problem that the damage defects in the groove or other etching stop interface of the wafer after ion bombardment during the etching process are difficult to eliminate.
[0058] Furthermore, after using the first plasma gas to remove the oxide layer 4 on the target surface 3 of the semiconductor substrate 1 and the target groove 2, the present embodiment uses a second plasma gas to regenerate the oxide layer 4 on the target surface 3. Specifically, the second plasma gas may include a plasma oxygen-containing gas after ions are filtered out.
[0059] The second plasma gas regenerates an oxide layer 4 on the target surface 3. The chemical reaction of the plasma oxygen-containing gas treating the target is:
[0060] Si+O 2 →SiO2
[0061] That is, the second plasma gas is used to regenerate the oxide layer 4 on the target surface 3, which may include: plasma O 2 It reacts with defective areas of the target surface 3 to form an oxide layer 4 .
[0062] In one embodiment, the oxygen-containing gas in the plasma state may further include O 3 or water vapor.
[0063] That is, this embodiment uses the plasma state H after filtering out the ions. 2 (or plasma H after filtering out ions 2 、N 2 After removing the oxide layer 4 of the target surface 3 of the target groove 2 formed on the semiconductor substrate 1 by etching process, the oxygen-containing gas (O 2 , O 3 or water vapor) to regenerate an oxide layer 4 on the target surface 3, and the plasma H after filtering out the ions is recycled. 2 The oxygen-containing gas in a plasma state acts on the target surface 3 to eliminate the defect damage on the target surface 3, thereby solving the problem that the damage defects in the grooves or other etching stop interfaces of the wafer are difficult to eliminate after ion bombardment during the etching process.
[0064] In one embodiment, the second plasma gas includes: plasma-state oxygen-containing gas after ions are filtered out, N 2 and / or inert gas, wherein the inert gas includes He, Ne, Ar, Kr and Xe, etc.
[0065] The first plasma gas and the second plasma gas are cyclically used to act on the target surface 3 until the defects of the target surface 3 are eliminated.
[0066] Preferably, the plasma H 2 (or plasma H after filtering out ions 2 、N 2 and / or inert gas) and plasma O 2 (Plasma O 2 、N 2 and / or inert gas) acts on the target surface 3 until the defects of the target surface 3 are eliminated.
[0067] In one embodiment, the first plasma gas and the second plasma gas are cyclically used to act on the target surface 3 for a set number of cycles, that is, the defects and damages on the target surface 3 are eliminated within the limit of the set number of cycles.
[0068] Preferably, the number of cycles is set to include 2-3 times.
[0069] In this embodiment, the plasma state H after filtering out the ions is used. 2 (or plasma H after filtering out ions 2 、N 2 After removing the oxide layer 4 of the target surface 3 of the target groove 2 formed on the semiconductor substrate 1 after the etching process by using the inert gas (or the inert gas, N 2 and / or inert gas) to regenerate an oxide layer 4 on the target surface 3, and this cycle can be repeated 2-3 times to eliminate the defect damage on the target surface 3, thereby solving the problem that damage defects in the groove or other etching stop interfaces are difficult to eliminate after ion bombardment during the etching process of the wafer.
[0070] It should be noted that the target surface 3 of the present embodiment includes the surface of the semiconductor substrate 1, the sidewall of the target groove 2 and the bottom of the target groove 2, wherein the target surface 3 has rough protrusions (burr-shaped damage defects). After the first plasma gas and the second plasma gas are cyclically used to act on the target surface 3, the rough protrusions are peeled off one by one. Specifically, the first plasma gas removes the oxide layer 4 of the target surface 3, and the second plasma gas regenerates the oxide layer 4 on the target surface 3, and this is repeated. The plasma oxygen-containing gas oxidizes the target surface 3 and the plasma H 2 The oxide layer 4 on the target surface 3 is processed and removed. Based on the anisotropic and surface-oriented properties of the oxide layer 4 during its formation, the raised portion of the target surface 3 is gradually peeled off along with the removal-generation-removal of the oxide layer 4, thereby reducing the roughness and eliminating surface defects.
[0071] Among them, the cyclic use of the first plasma gas and the second plasma gas in this embodiment to act on the target surface 3 are all completed in the same process chamber, that is, multiple steps of reaction are combined in the same process chamber, which can simplify the semiconductor processing process and reduce the complexity of equipment and process, and is also conducive to more precise control of the parameters and conditions of the processing process, which helps to improve production efficiency. At the same time, the cyclic formation and removal of the oxide layer 4 in the same process chamber can better eliminate the rough protrusions on the target surface 3 and avoid it from being affected by other environmental conditions during the etching process, which helps to ensure the integrity and consistency of the device structure, realize the morphology protection of the semiconductor, and optimize the electrical properties of the semiconductor device.
[0072] It should be noted that, in this embodiment, the first plasma gas and the second plasma gas are cyclically used to act on the target surface 3, and the cycle termination step may be that the first plasma gas acts on the target surface 3, and the semiconductor substrate 1 and the target groove 2 with the defect damage of the target surface 3 eliminated are obtained, and the oxide layer 4 generated by the second plasma gas is removed from the target surface 3;
[0073] Alternatively, the cycle termination step may be that the second plasma gas acts on the target surface 3, that is, the semiconductor substrate 1 and the target groove 2 obtained by eliminating the defect damage of the target surface 3, and the target surface 3 may still have an oxide layer 4 generated by the reaction of the plasma oxygen-containing gas and the target surface 3.
[0074] It can be understood that by using the first plasma gas to act on the target surface 3 as the cycle termination step, the target surface 3 of the semiconductor substrate 1 and the target groove 2 can still be in contact with the natural environment to form a natural oxide layer. Of course, the specific selection of the cycle termination step of this embodiment can be formulated according to actual production needs to adapt to different environmental requirements, and will not be repeated here.
[0075] This embodiment also discloses a semiconductor process equipment, referring to Figure 3 , Figure 3 It is a schematic diagram of the structure of the semiconductor process equipment of this embodiment, which includes a process chamber 20, an air intake assembly 21, an ICP power source assembly 22, a plasma filter grid plate 23, a heating support platform 24 and a controller (not shown).
[0076] The controller includes at least one processor and at least one memory, wherein a computer program is stored in the memory, and when the computer program is executed by the processor, the semiconductor processing method of any one of the above embodiments is implemented.
[0077] Exemplarily, the air inlet component 21 can be connected to the top of the process chamber 20, and the controller can be a host computer or a slave computer, wherein the controller can control the valve of the air inlet component 21 to open so as to introduce corresponding process gases into the interior of the process chamber 20. Specifically, under the control of the controller, in the process chamber 20, a first plasma gas is used to remove the oxide layer on the target surface of the semiconductor substrate and the target groove formed on the semiconductor substrate after the etching process, and then a second plasma gas is used to repair the defective area on the target surface. In this way, the first plasma gas and the second plasma gas are cyclically used to act on the target surface until the defects on the target surface are eliminated, thereby solving the problem that damage defects in the grooves or other etching termination interfaces of the wafer after etching are difficult to eliminate.
[0078] The controller can also control the opening and closing degree of the valve of the air inlet component 21 to control the flow rate of the process gas. The controller can also control the exhaust component to exhaust the interior of the process chamber 20 to control the pressure inside the process chamber 20 and discharge reaction by-products.
[0079] The ICP power source assembly 22 is connected to the process chamber 20, and includes a radio frequency coil, a radio frequency power supply and a matcher. The controller is also used to control the radio frequency power supply to provide electrode power to the radio frequency coil through the matcher, so that the radio frequency coil excites the process gas inside the process chamber 20 to generate plasma.
[0080] The plasma filter grid plate 23 and the heating support platform 24 are connected in the process chamber 20. The plasma filter grid plate 23 is located above the heating support platform 24. The heating support platform 24 carries the semiconductor substrate, that is, the wafer to be processed. The plasma filter grid plate 23 is kept at a distance above the semiconductor substrate, and the heating support platform 24 is also used to provide heating for the wafer to be processed. By controlling the temperature of the heater, the temperature control of the semiconductor substrate can be achieved to affect parameters such as the etching rate and surface reaction.
[0081] The plasma filter grid plate 23 is usually connected to the ground potential and is used to adjust the plasma density and energy distribution. The plasma filter grid plate 23 of this embodiment filters the plasma H 2 ions, that is, the first plasma gas can include the plasma H after the ions are filtered out. 2 , thereby avoiding ion bombardment damage to the semiconductor substrate and the target surface of the target groove formed on the semiconductor substrate after the etching process.
[0082] The semiconductor process equipment in the embodiment of the present application is an inductively coupled plasma (ICP) etching equipment.
[0083] In some embodiments, it may also be a capacitively coupled plasma (CCP) etching device. The embodiments of the present application do not limit the type of semiconductor process equipment.
[0084] For other working principles and processes of the process equipment of this embodiment, please refer to the description of the semiconductor processing method in the aforementioned embodiment of the present invention, which will not be repeated here.
[0085] The above is a detailed introduction to a semiconductor device processing method and process equipment provided by the present application. This article uses specific examples to illustrate the principles and implementation methods of the present application. It should be noted that in the present application, the descriptions of each embodiment have their own emphasis. For parts that are not described or recorded in detail in a certain embodiment, please refer to the relevant descriptions of other embodiments.
[0086] The above are only preferred embodiments of the present application, and the patent scope of the present application is not limited thereto. The various technical features of the technical solution of the present application can be arbitrarily combined. In order to make the description concise, not all possible combinations of the various technical features in the above embodiments are described. Any equivalent structure or equivalent process transformation made using the contents of the specification and drawings of this application, or directly or indirectly used in other related technical fields, as long as there is no contradiction in the combination of these technical features, are equally included in the patent protection scope of the present application.
Claims
1. A semiconductor processing method, characterized in that: include: Providing a semiconductor substrate, wherein the semiconductor substrate has a target groove formed by an etching process; After removing the oxide layer on the target surface of the semiconductor substrate and the target groove by using a first plasma gas, regenerating the oxide layer on the target surface by using a second plasma gas, wherein the first plasma gas includes plasma H2 after ions are filtered out, the second plasma gas includes plasma oxygen-containing gas after ions are filtered out, and the target surface includes the surface of the semiconductor substrate, the sidewall of the target groove, and the bottom of the target groove; The first plasma gas and the second plasma gas are cyclically used to act on the target surface until defects on the target surface are eliminated.
2. The semiconductor processing method according to claim 1, wherein: The first plasma gas includes: plasma H2, N2 and / or inert gas after ions are filtered out.
3. The semiconductor processing method according to claim 1, wherein: The second plasma gas includes: plasma-state oxygen-containing gas, N2 and / or inert gas after ions are filtered out.
4. The semiconductor processing method according to claim 1 or 3, characterized in that: The oxygen-containing gas includes O2, O3 or water vapor.
5. The semiconductor processing method according to claim 1, wherein: The cyclic use of the first plasma gas and the second plasma gas to act on the target surface has a set number of cycles.
6. The semiconductor processing method according to claim 1, wherein: The target surface has rough protrusions, and after the first plasma gas and the second plasma gas are cyclically used to act on the target surface, the rough protrusions are peeled off one by one.
7. The semiconductor processing method according to claim 1, wherein: The cyclic use of the first plasma gas and the second plasma gas to act on the target surface is completed in the same process chamber.
8. A semiconductor process equipment, comprising a process chamber, an air intake assembly, an ICP power source assembly, a plasma filter grid plate, a heating support table and a controller, characterized in that: The controller includes at least one processor and at least one memory, wherein a computer program is stored in the memory, and when the computer program is executed by the processor, the semiconductor processing method according to any one of claims 1 to 7 is implemented.
Citation Information
Patent Citations
Semiconductor treatment technology and semiconductor device preparation method
CN103871902A
Method for forming shallow trench isolation structure
CN111933566A