Conductive agent and preparation method thereof, positive electrode sheet, negative electrode sheet and solid-state battery
By coating the conductive carbon material with fast ion conductor, the problem of unsatisfactory ion and electron transport and chemical reactions in sulfide-based solid-state batteries is solved, and the electrochemical performance and service life of the battery are improved.
Patent Information
- Application Number
- CN202411083746.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-08
AI Technical Summary
Sulfide-based solid-state batteries have problems such as unsatisfactory ion and electron transport paths and easy chemical reactions between sulfide electrolytes and electrode materials, which affects the electrochemical performance and service life of the battery.
Fast ion conductors are used to coat conductive carbon materials, providing rich ion transmission channels, reducing the contact between conductive carbon materials and solid electrolytes, reducing interface reactions, and improving the electrochemical performance and service life of the battery.
The fast ion conductor coats the conductive carbon material, which improves the ion and electron transport efficiency of solid-state batteries, extends the service life, and improves the battery's magnification and cycling performance.
Smart Images

Figure CN118610468B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a conductive agent and a preparation method thereof, a positive electrode sheet, a negative electrode sheet and a solid-state battery. Background Art
[0002] The lithium batteries currently under development mainly use liquid electrolytes, which contain a large amount of organic solvents, resulting in a large safety hazard for liquid lithium batteries. Using a solid electrolyte layer instead of a liquid electrolyte can hopefully eliminate the safety hazard during use, which is more in line with the future development needs of electric vehicles and large-scale energy storage. Sulfide electrolytes combine the high ionic conductivity of oxide electrolytes with the high processing performance of polymer electrolytes, so sulfide-based solid-state batteries have broad prospects for industrialization.
[0003] However, current sulfide-based solid-state batteries have problems such as unsatisfactory transmission paths and efficiency of ions and electrons, and easy chemical reactions between sulfide electrolytes and electrode materials, which still need to be improved. Summary of the invention
[0004] The present application aims to solve at least one of the technical problems in the related art to a certain extent. To this end, one purpose of the present application is to propose a conductive agent and a preparation method thereof, a positive electrode sheet, a negative electrode sheet, a solid-state battery and an electrical device. The conductive agent of the present application can improve the interface stability of the solid-state battery, and at the same time provide abundant transmission channels for ions and electrons to improve the transmission efficiency of both, thereby improving the electrochemical performance and service life of the solid-state battery as a whole.
[0005] The first aspect of the present application provides a conductive agent. According to an embodiment of the present application, the conductive agent comprises: a core, the core comprises a conductive carbon material; and a shell, the shell covers at least a portion of the surface of the core, the shell comprises a fast ion conductor.
[0006] According to the conductive agent of the embodiment of the present application, the conductive carbon material is coated with a fast ion conductor, which can provide an ion transmission path to improve the ion transmission efficiency; it can also reduce the contact between the conductive carbon material and the solid electrolyte, reduce the occurrence of interfacial reactions, and improve the contact stability of the solid electrolyte. As a result, the electrochemical performance of the solid-state battery can be improved and the service life can be extended. In addition, the fast ion conductor has a higher electrochemical stability window, which can match the ternary high-nickel positive electrode, and finally realize the capacity and rate of the ternary positive electrode for the solid-state battery.
[0007] According to an embodiment of the present application, the conductive agent may also have the following additional technical features:
[0008] According to an embodiment of the present application, the fast ion conductor includes at least one of lithium aluminum titanium phosphate, lithium lanthanum titanium oxide and lithium zirconium oxide.
[0009] According to an embodiment of the present application, the fast ion conductor includes Li 1+x Al x Ti 2-x (PO 4 ) 3 , 0≤x≤0.5.
[0010] According to an embodiment of the present application, the conductive carbon material includes: at least one of carbon nanotubes, carbon fibers, acetylene black, carbon black, carbon black and graphene.
[0011] According to an embodiment of the present application, the conductive agent satisfies at least one of the following conditions:
[0012] The ratio of the diameter of the core to the thickness of the shell is (0.1-10):1;
[0013] The diameter of the core is 0.5 nm to 0.5 μm;
[0014] The thickness of the shell layer is 0.5 nm to 0.5 μm;
[0015] The specific surface area of the core is 10 m 2 / g~500 m 2 / g;
[0016] The specific surface area of the shell is 10 m 2 / g ~500 m 2 / g;
[0017] The shell layer has a porous structure, and the porosity of the shell layer is 50% to 80%;
[0018] The conductive agent is in a fibrous shape with an aspect ratio of (30-150):1.
[0019] According to an embodiment of the present application, the conductive agent satisfies at least one of the following conditions:
[0020] The ratio of the diameter of the inner core to the thickness of the shell is (1-3):1;
[0021] The diameter of the core is 50 nm to 200 nm;
[0022] The thickness of the shell layer is 100 nm to 200 nm;
[0023] The specific surface area of the core is 10 m 2 / g~100 m 2 / g;
[0024] The specific surface area of the shell is 50 m 2 / g ~200 m 2 / g;
[0025] The shell layer has a porous structure, and the porosity of the shell layer is 50% to 80%;
[0026] The conductive agent is in a fibrous shape with an aspect ratio of (30-70):1.
[0027] The second aspect of the present application provides a method for preparing the conductive agent described in the first aspect. According to an embodiment of the present application, the method comprises:
[0028] The inner core spinning solution and the shell layer spinning solution are subjected to coaxial electrospinning to obtain a precursor;
[0029] The precursor is subjected to a heat treatment to obtain the conductive agent.
[0030] According to an embodiment of the present application, the method includes at least one of the following conditions:
[0031] The shell spinning solution comprises: lithium salt, aluminum salt, titanium salt, phosphonate, complexing agent, binder and organic solvent;
[0032] The solid content of the core spinning solution is 5% to 25% by mass;
[0033] The core spinning solution includes polyacrylonitrile and an organic solvent;
[0034] The solid content of the shell spinning solution is 5% to 25% by mass;
[0035] The injection speed of the core spinning solution is 0.2 ml / h ~1 ml / h;
[0036] The injection speed of the shell spinning solution is 0.3 ml / h to 0.8 ml / h;
[0037] The coaxial electrospinning treatment time is 5 min to 15 min.
[0038] According to an embodiment of the present application, the heating treatment includes: subjecting the precursor to a first heating treatment, a second heating treatment, and a third heating treatment in sequence;
[0039] The heating treatment satisfies at least one of the following conditions:
[0040] The temperature of the first heating treatment is 200°C to 300°C, and the time is 0.5 h to 4 h;
[0041] The second heating treatment is performed at a temperature of 650°C to 900°C and for a time of 6 h to 12 h;
[0042] The temperature of the third heat treatment is 1000° C. to 1500° C., and the time is 1 h to 4 h;
[0043] The heating rate of heating from the first heating treatment temperature to the second heating treatment temperature is 5°C / min to 10°C / min.
[0044] The third aspect of the present application provides a positive electrode plate. According to an embodiment of the present application, the positive electrode plate includes: a positive electrode active material layer, and the positive electrode active material layer includes:
[0045] Positive electrode active material;
[0046] And, the conductive agent described in the first aspect or the conductive agent obtained by the preparation method described in the second aspect.
[0047] According to an embodiment of the present application, the positive electrode active material includes lithium iron phosphate or nickel-cobalt-manganese ternary positive electrode material;
[0048] and / or, the positive electrode active material layer further comprises a sulfide electrolyte;
[0049] And / or, the mass of the conductive agent accounts for 0.5% to 7% of the mass of the positive electrode active material layer.
[0050] According to an embodiment of the present application, the mass of the conductive agent accounts for 0.5% to 1% of the mass of the positive electrode active material layer.
[0051] The fourth aspect of the present application provides a negative electrode plate. According to an embodiment of the present application, the negative electrode plate comprises: a negative electrode active material layer, and the negative electrode active material layer comprises:
[0052] Negative electrode active material;
[0053] And, the conductive agent described in the first aspect or the conductive agent obtained by the preparation method described in the second aspect.
[0054] The fifth aspect of the present application provides a solid-state battery. According to an embodiment of the present application, the solid-state battery comprises: a positive electrode sheet, a sulfide electrolyte layer and a negative electrode sheet, wherein the sulfide electrolyte layer is located between the positive electrode sheet and the negative electrode sheet;
[0055] The positive electrode sheet is selected from the positive electrode sheet described in the third aspect; and / or, the negative electrode sheet is selected from the negative electrode sheet described in the fourth aspect.
[0056] The sixth aspect of the present application provides an electric device. According to an embodiment of the present application, the electric device includes: the solid-state battery described in the fifth aspect.
[0057] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0059] Figure 1 A schematic diagram of the conductive agent structure according to an embodiment of the present application is shown;
[0060] Figure 2 A diagram showing the mechanism of fast ion conductor coating with conductive carbon material according to one embodiment of the present application is shown;
[0061] Figure 3 A schematic diagram of a process for preparing a conductive agent according to an embodiment of the present application is shown.
[0062] Reference numerals:
[0063] 1: conductive agent; 100: core; 200: shell. DETAILED DESCRIPTION
[0064] The embodiments of the present application are described in detail below. The embodiments described below are exemplary and are only used to explain the present application, and cannot be understood as limiting the present application.
[0065] It should be noted that the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. Further, in the description of this application, unless otherwise specified, the meaning of "plurality" is two or more.
[0066] The endpoints and any values of the ranges disclosed in this application are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in this application.
[0067] In the present application, the terms "comprise" or "include" are open expressions, that is, including the contents specified in the present application but not excluding other contents.
[0068] At present, there are still many major challenges for the large-scale application of sulfide-based solid-state batteries. On the one hand, the ion and electron transmission paths and transmission efficiency inside the electrodes of sulfide all-solid-state batteries are not ideal, especially inside the positive electrode. On the other hand, some sulfide electrolytes have high chemical reactivity with conductive carbon materials (such as carbon nanotubes, carbon black, and SuperP, etc.), which are prone to interfacial reactions, and the electron transmission between the conductive carbon material and the sulfide electrolyte will aggravate the reaction, resulting in the rate performance and cycle performance of sulfide-based solid-state batteries. It is difficult to meet commercial requirements. The main reasons are as follows: In order to achieve the maximum capacity of the electrode active material, conductive carbon materials need to be added to the positive electrode to ensure sufficient electron transmission. However, this approach increases the contact area between the conductive carbon and the sulfide electrolyte, thereby accelerating the decomposition reaction of the electrolyte.
[0069] One strategy currently used is to coat the surface of conductive carbon materials with Al 2 O 3 , ZnO and other inert oxides to reduce the interfacial reaction between them and the sulfide electrolyte. Although this method can effectively slow down the chemical reaction, the ionic conductivity of these inert oxide modified materials is significantly lower than that of the sulfide electrolyte itself, resulting in limited electrochemical performance of the composite electrode material at room temperature, especially affecting its capacity.
[0070] In view of this, the present application not only effectively reduces the contact area between the conductive carbon and the sulfide electrolyte by coating the fast ion conductor on the surface of the conductive carbon material, thereby reducing the interface reaction and enhancing the stability of the battery; but also improves the ion transmission efficiency due to the high ion conductivity of the fast ion conductor. 2 O 3 , ZnO) coating materials, can also be combined with sulfide solid electrolytes to improve the overall electrochemical properties of solid-state batteries, such as cycle performance and rate performance, thereby extending the service life of solid-state batteries.
[0071] To this end, the first aspect of the present application proposes a conductive agent. According to the embodiments of the present application, see Figure 1 The conductive agent 1 includes: a core 100 and a shell 200, wherein the core 100 includes a conductive carbon material, the shell 200 covers at least a portion of the surface of the core 100, and the shell 200 includes a fast ion conductor.
[0072] Combine the following Figure 2 Explain the mechanism of fast ion conductor coated with conductive carbon material:
[0073] By coating the surface of the conductive carbon material with a fast ion conductor, lithium ions can be transported between the active material, solid electrolyte and conductive agent inside the electrode through the shell mesh fast ion conductor, thus improving the ion transmission efficiency. Electrons are mainly transported between the active material and conductive agent inside the electrode through the conductive material in the core, while the shell mesh fast ion conductor can effectively reduce the contact area between the conductive carbon and the sulfide electrolyte, slowing down the interface side reactions. This improves the electrochemical performance of the solid-state battery and extends its service life.
[0074] According to an embodiment of the present invention, the fast ion conductor includes at least one of lithium aluminum titanium phosphate, lithium lanthanum titanium oxide and lithium zirconium oxide. 1.3 Al 0.3 Ti 1.7 (PO 4 ) 3 , referred to as LATP), lithium lanthanum titanium oxide (Li 0.33 La 0.56 TiO 3 , LLTO) and lithium zirconium oxide (Li 7 La 3 Zr 2 O 12 , referred to as LLZO) not only has excellent ionic conductivity, which is conducive to the rapid transmission of ions during the battery charging and discharging process; it also has relatively stable chemical properties, is not easy to react chemically with sulfide electrolytes, has strong interface stability, reduces the performance degradation caused by interface reactions, and further improves the battery's rate performance and cycle performance. In addition, the above-mentioned fast ion conductor has a high electrochemical stability window, which can match the ternary high-nickel positive electrode, and ultimately achieve the capacity and rate performance of the ternary positive electrode for solid-state batteries.
[0075] According to an embodiment of the present invention, the fast ion conductor includes Li 1+x Al x Ti 2-x (PO 4 ) 3 , 0≤x≤0.5. Exemplarily, x is 0, 0.1, 0.2, 0.3, 0.4, 0.5. As a result, it is conducive to the rapid transmission of ions during the charging and discharging process of the battery, and has relatively stable chemical properties, is not easy to react chemically with sulfide electrolytes, has strong interface stability, reduces the performance degradation caused by interface reactions, and further improves the rate performance and cycle performance of the battery. In addition, the above-mentioned fast ion conductor has a higher electrochemical stability window, which can match the ternary high-nickel positive electrode, and ultimately achieves the capacity and rate performance of the ternary positive electrode for high-area capacity solid-state batteries. When x is 0.4, the ion transmission capacity of the fast ion conductor is optimal.
[0076] According to an embodiment of the present invention, the conductive carbon material includes at least one of carbon nanotubes, carbon fibers, acetylene black, carbon black, carbon black and graphene, thereby having excellent electron transport capability.
[0077] According to an embodiment of the present invention, the ratio of the diameter of the inner core to the thickness of the shell is (0.1-10): 1, for example, it can be 0.1: 1, 0.5: 1, 1: 1, 2: 1, 3: 1, 4: 1, 5: 1, 6: 1, 7: 1, 8: 1, 9: 1, 10: 1, preferably (1-3): 1. The ratio of the diameter of the inner core to the thickness of the shell satisfies the above conditions, which can not only make the conductive carbon material and the sulfide electrolyte sufficiently isolated, reduce the direct contact area, thereby reducing the occurrence of interfacial reactions and enhancing the chemical stability of the battery; secondly, it takes into account the transmission efficiency of ions and electrons, and reduces the influence of excessive increase in shell thickness on electron transmission.
[0078] According to an embodiment of the present invention, the diameter of the core is 0.5 nm to 0.5 μm, for example, 0.5 nm, 1 nm, 10 nm, 50 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, preferably 50 nm to 200 nm. The diameter of the core meets the above conditions, and the conductive carbon material has sufficient volume to achieve efficient electron transmission, which is conducive to high power output and fast charge and discharge capabilities without sacrificing energy density; at the same time, the use of the above core thickness also helps to maintain the structural integrity of the electrode material, reduce the stress caused by volume expansion and contraction during the charge and discharge process, and improve the mechanical stability and cycle life of the battery.
[0079] According to an embodiment of the present invention, the thickness of the shell layer is 0.5 nm to 0.5 μm, for example, 0.5 nm, 1 nm, 10 nm, 50 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, preferably 100 nm to 200 nm. The shell layer thickness meets the above conditions, can effectively isolate the direct contact between the conductive carbon material and the sulfide electrolyte, reduce the interface reaction, thereby enhancing the chemical stability and cycle life of the battery; secondly, it helps to form an efficient ion transmission channel, ensure the rapid migration of ions during the charge and discharge process, and does not sacrifice the energy density, thereby improving the charge and discharge efficiency and rate performance of the battery.
[0080] According to an embodiment of the present invention, the specific surface area of the core is 10 m 2 / g~500 m 2 / g, for example, 10 m 2 / g, 50 m2 / g, 100 m 2 / g, 150 m 2 / g, 200 m 2 / g, 250 m 2 / g, 300 m 2 / g, 350 m 2 / g, 400 m 2 / g, 450 m 2 / g, 500 m 2 / g, preferably 10 m 2 / g~100 m 2 / g. As a result, the contact area and transmission path between the inner components of the electrode are increased, which helps to improve the transmission efficiency of electrons inside the electrode, while reducing the side reactions between the inner core and the conductive carbon material.
[0081] According to an embodiment of the present invention, the specific surface area of the shell layer is 10 m 2 / g ~500 m 2 / g, for example, 10 m 2 / g, 50 m 2 / g, 100 m 2 / g, 150 m 2 / g, 200 m 2 / g, 250 m 2 / g, 300 m 2 / g, 350 m 2 / g, 400 m 2 / g, 450 m 2 / g, 500 m 2 / g, preferably 50 m 2 / g ~200 m 2 The specific surface area that meets the above conditions is conducive to providing an appropriate number of pores for the shell layer, which not only helps to reduce the contact area between the conductive carbon material and the solid electrolyte and slow down the side reaction between the solid electrolyte and the conductive carbon material, but also can meet the needs of electron transmission.
[0082] According to an embodiment of the present invention, the shell has a porous structure, and the porosity of the shell is 50% to 80%. When preparing the conductive agent, the raw material of the conductive carbon material undergoes a thermal decomposition reaction during the high-temperature carbonization process, releasing a large amount of small molecule gas to form a porous structure on the shell. On the one hand, these porous structures can provide ion and electron transmission pathways to improve the efficiency of ion and electron transmission, and on the other hand, they can increase the risk of porous contact between the conductive carbon material and the sulfide electrolyte to a certain extent. The porous structure with the above-mentioned porosity can take into account the excellent ion and electron transmission performance and interface stability, which not only promotes the rapid transmission of ions and electrons, but also improves the charge and discharge efficiency of the battery, and reduces the chance of direct contact between the conductive carbon material and the sulfide electrolyte, effectively avoiding possible adverse reactions. Improve the electrochemical performance of the battery.
[0083] According to an embodiment of the present application, the conductive agent is in a fibrous shape, and the aspect ratio is (30-150):1, for example, 30:1, 50:1, 70:1, 100:1, 120:1, 140:1, preferably (30-70):1. Compared with the spherical structure, the fibrous structure provides more contact area and longer transmission path, which helps to improve the transmission efficiency of electrons and ions in the electrode material. The aspect ratio meets the above conditions, which is better for electron and ion transmission.
[0084] The second aspect of the present application provides a method for preparing the conductive agent described in the first aspect. Figure 2 The method includes: S100 coaxial electrospinning treatment and S200 heating treatment, which will be described in detail below.
[0085] S100 Coaxial Electrospinning Process
[0086] In this step, the inner core spinning solution and the shell layer spinning solution are subjected to coaxial electrospinning to obtain a precursor. Through the coaxial electrospinning process, a precursor having a core-shell structure can be obtained.
[0087] In the present application, coaxial electrospinning refers to the formation of a precursor having a core-shell structure on a drum receiver by the coaxial spinning solution under the traction effect of the electrostatic force at the coaxial spinning head in a high voltage electric field.
[0088] According to an embodiment of the present application, the shell spinning solution includes: a lithium salt (e.g., lithium nitrate (LiNO 3 )), aluminum salts (e.g. aluminum nitrate nonahydrate (Al(NO 3 ) 3 9H 2 O)), titanium salts (tetrabutyl titanate (Ti(OC 4 H 9 ) 4)), phosphonates (e.g. phenylphosphonic acid (C 6 H 7 O 3 P) ), a complexing agent, a binder and an organic solvent. Thus, the precursor obtained by electrospinning contains a precursor of lithium aluminum titanium phosphate, and the precursor can form lithium aluminum titanium phosphate with high ionic conductivity and chemical stability after subsequent heating treatment.
[0089] In some embodiments, the binder may include one or more of acetic acid, ethylenediaminetetraacetic acid (EDTA), ammonia water, citric acid, and tartaric acid; the adhesive may include one or more of polyvinyl pyrrolidone (PVP), vinylidene fluoride (PVDF), sodium carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR), and polyimide (PI); the organic solvent may include one or more of NN dimethylformamide (DMF), dimethylformamide (DMF), dimethyl sulfoxide (DMSO), ethanol, acetone, anisole, and butyl acetate.
[0090] According to an embodiment of the present application, the solid content of the core spinning solution is 5% to 25% by mass. For example, the solid content of the core spinning solution is 5%, 10%, 15%, 20%, or 25% by mass. This is conducive to obtaining a core that meets the aforementioned diameter.
[0091] According to an embodiment of the present application, the solid content of the shell spinning solution is 5% to 25% by mass. For example, the solid content of the shell spinning solution is 5%, 10%, 15%, 20%, or 25% by mass. This is conducive to obtaining a shell layer that meets the aforementioned thickness.
[0092] According to an embodiment of the present application, the injection speed of the core spinning solution is 0.2 ml / h to 1 ml / h. Exemplarily, the injection speed of the core spinning solution is 0.2 ml / h, 0.4 ml / h, 0.6 ml / h, 0.8 ml / h, and 1 ml / h. This is conducive to obtaining a core that meets the aforementioned diameter.
[0093] According to an embodiment of the present application, the injection speed of the shell spinning solution is 0.3 ml / h to 0.8 ml / h. Exemplarily, the injection speed of the shell spinning solution is 0.3 ml / h, 0.4 ml / h, 0.5 ml / h, 0.6 ml / h, 0.7 ml / h, and 0.8 ml / h. This is conducive to obtaining a core that meets the aforementioned thickness.
[0094] According to an embodiment of the present application, the coaxial electrospinning treatment time is 5 min to 15 min. Exemplarily, the coaxial electrospinning treatment time is 5 min, 6 min, 8 min, 10 min, 12 min, and 15 min. This is conducive to obtaining a fibrous conductive agent that satisfies the aforementioned aspect ratio.
[0095] S200 heat treatment
[0096] In this step, the precursor is subjected to a heat treatment to obtain a conductive agent, thereby causing the raw material of the conductive carbon material to be thermally decomposed and carbonized to form a conductive carbon material, thereby obtaining a conductive agent with a stable structure.
[0097] According to an embodiment of the present application, the S200 heating treatment includes: sequentially performing a first heating treatment, a second heating treatment, and a third heating treatment on the precursor, and the S200 heating treatment satisfies at least one of the following conditions:
[0098] The first heat treatment is performed at a temperature of 200° C. to 300° C. for 0.5 h to 4 h, for example, at a temperature of 200° C., 220° C., 240° C., 250° C., 260° C., 280° C., 300° C. for 0.5 h, 1 h, 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, 4 h.
[0099] The second heat treatment is performed at a temperature of 650° C. to 900° C. for 6 h to 12 h, for example, at a temperature of 650° C., 700° C., 750° C., 800° C., 850° C., 900° C. for 6 h, 8 h, 10 h, 12 h.
[0100] The third heat treatment is performed at a temperature of 1000° C. to 1500° C. for a time of 1 h to 4 h, for example, at a temperature of 1000° C., 1100° C., 1200° C., 1300° C., 1400° C., 1500° C. for a time of 1 h, 2 h, 3 h, 4 h;
[0101] After the first heat treatment is completed, the heating rate from heating to the second heat treatment temperature is 5°C / min to 10°C / min, for example, the heating rate is 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min, and 10°C / min.
[0102] Taking the core spinning solution including polyacrylonitrile (PAN) as an example, the above-mentioned first heating treatment is performed to pre-oxidize the polyacrylonitrile so that it initially forms a cross-linked structure. Then, the above-mentioned second heating treatment is performed so that PAN begins to thermally decompose and generate small molecular gases. These gases are released from the material to form holes in the outer shell, increase the porosity of the material, and facilitate ion transmission. At the same time, the precursor in the shell undergoes chemical reaction and sintering at high temperature to form a fast ion conductor with a porous structure. Then, the above-mentioned third heating treatment is performed so that PAN is completely carbonized and converted into a carbon material to form a fast ion conductor coated with a conductive carbon material structure. The use of the above-mentioned heating rate helps to obtain a shell that meets the aforementioned porosity.
[0103] According to an embodiment of the present application, the method for preparing the conductive agent according to the first aspect includes:
[0104] (1) Different coaxial spinning solutions, namely the shell spinning solution and the core spinning solution, are placed in the microinjection pumps of the core and shell of the coaxial spinning head respectively.
[0105] Shell spinning solution: LiNO 3 、Al(NO 3 ) 3 9H 2 O、Ti(OC 4 H 9 ) 4 , C 6 H 7 O 3 P, acetic acid and PVP are dissolved in DMF, wherein the solid content of the shell spinning solution is 5%-25%, and it is necessary to stir at room temperature for more than 8 h to obtain a uniform transparent solution;
[0106] Core spinning solution: PAN is dispersed in N,N-dimethylformamide solvent, wherein the solid content of the core spinning solution is 5-25%, and it needs to be stirred at room temperature for more than 8 hours to obtain a uniform solution;
[0107] (2) The distance between the coaxial spinning head and the receiving plate is 10 cm-20 cm, the rotation speed of the drum receiver is 500 rpm-3000 rpm; the pushing speed of the core and shell microinjection pumps is 0.01 ml / h-1 ml / h;
[0108] (3) Coaxially electrospinning the obtained shell spinning solution and core spinning solution to obtain the precursor of the desired coating material, wherein the coating material precursor nanowires of different lengths are obtained by controlling the electrospinning time to 5 s-5 min, and the diameter of the nanowires is controlled to be 1 nm-1 µm;
[0109] (4) After drying the obtained coating material precursor, it is first subjected to a pre-oxidation treatment at 200-300°C for 0.5 h~4 h, and then placed in a tubular furnace in an argon atmosphere and heated to 650°C-900°C at a heating rate of 5°C / min~10°C / min, and treated at high temperature for 6 h~12 h. At a high temperature of 650-900°C, the thermal decomposition reaction of PAN in the inner core begins, releasing a large amount of small molecular gas to form holes in the outer shell. The precursor in the shell forms a porous fast ion conductor LATP (Li 1.4 Al 0.4 Ti 1.6 (PO 4 ) 3 ) shell, and finally keep the temperature at 1000℃-1500℃ for 1-4 hours to completely carbonize PAN to obtain a fast ion conductor coated carbon fiber material (LATP@C coated material).
[0110] It should be noted that the features and advantages described above for the conductive agent of the first aspect are also applicable to the conductive agent preparation method of the second aspect, and will not be repeated here. In addition, the preparation method of the present application has a simple process, low cost, and is suitable for large-scale production.
[0111] The third aspect of the present application provides a positive electrode sheet. According to an embodiment of the present application, the positive electrode sheet comprises: a positive electrode active material layer, the positive electrode active material layer comprises: a positive electrode active substance; and the conductive agent described in the first aspect or the conductive agent obtained by the preparation method described in the second aspect.
[0112] The fast ion conductor of the conductive agent can provide more ion transmission channels, reduce the transmission resistance of lithium ions in the electrode material, thereby improving the charge and discharge rate and rate performance of the battery; at the same time, the conductive carbon material of the conductive agent is conducive to electron transmission; the fast ion shell also helps to reduce the direct contact between the conductive carbon material and the sulfide electrolyte, slows down possible interfacial side reactions, and improves the chemical stability and cycle life of the battery; in addition, the conductive carbon material structure with fast ion coating can also provide additional mechanical support during the battery charging and discharging process, reduce the stress caused by the volume expansion and contraction of the active material, thereby improving the long-term reliability and durability of the battery.
[0113] According to an embodiment of the present application, the positive electrode active material includes lithium iron phosphate or nickel cobalt manganese ternary positive electrode material. For example, lithium nickel cobalt manganese oxide includes LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 (Also referred to as NCM 333 )、LiNi 0.5 Co 0.2 Mn 0.3 O2 (Also referred to as NCM 523 )、LiNi 0.5 Co 0.25 Mn 0.25 O 2 (Also referred to as NCM 211 )、LiNi 0.6 Co 0.2 Mn 0.2 O 2 (Also referred to as NCM 622 )、LiNi 0.8 Co 0.1 Mn 0.1 O 2 (Also referred to as NCM 811 ) etc. Since fast ion conductors have a high electrochemical stability window, they can match the ternary high nickel cathode, and ultimately achieve the capacity and rate performance of the ternary cathode for high surface capacity solid-state batteries.
[0114] According to an embodiment of the present application, the positive electrode active material layer may further include a sulfide electrolyte. The sulfide electrolyte includes a glass ceramic Li-PS system, an argyrodite Li 6 PS 5 X or LiGeP 10 G 2 S 12 wherein X is Cl, Br or I.
[0115] According to an embodiment of the present application, the mass of the conductive agent accounts for 0.5% to 7% of the mass of the positive electrode active material layer, for example, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, preferably 0.5% to 1%. Thus, the electron and ion transport performance and interface stability can be improved, thereby improving the rate performance and cycle performance of the solid-state battery.
[0116] According to an embodiment of the present application, the positive electrode sheet may further include a positive electrode current collector located on at least one side of the positive electrode active material layer.
[0117] According to an embodiment of the present application, the positive electrode current collector may include a metal foil or a composite positive electrode current collector. For example, the metal foil may be aluminum foil. The composite positive electrode current collector may include a polymer material base and a metal layer formed on at least one side of the polymer material base. For example, the composite negative electrode current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, etc.) on a polymer material substrate (such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT) and other substrates).
[0118] According to an embodiment of the present application, the positive electrode active material layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), butyl rubber (NBR), styrene butadiene latex (SBR), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin.
[0119] According to the embodiments of the present application, the positive electrode sheet can be prepared in the following manner: the components for preparing the positive electrode sheet (such as positive electrode active material, conductive agent, binder) are dispersed in a solvent (such as N-methylpyrrolidone, anisole, xylene, butyl butyrate, etc.) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0120] The fourth aspect of the present application provides a negative electrode sheet. According to an embodiment of the present application, the negative electrode sheet comprises: a negative electrode active material layer, the negative electrode active material layer comprises: a negative electrode active substance; and the conductive agent described in the first aspect or the conductive agent obtained by the preparation method described in the second aspect.
[0121] The fast ion conductor of the conductive agent can provide more ion transmission channels, reduce the transmission resistance of lithium ions in the electrode material, thereby improving the charge and discharge rate and rate performance of the battery; at the same time, the conductive carbon material of the conductive agent is conducive to electron transmission; the fast ion shell also helps to reduce the direct contact between the conductive carbon material and the sulfide electrolyte, slows down possible interfacial side reactions, and improves the chemical stability and cycle life of the battery; in addition, the conductive carbon material structure with fast ion coating can also provide additional mechanical support during the battery charging and discharging process, reduce the stress caused by the volume expansion and contraction of the active material, thereby improving the long-term reliability and durability of the battery.
[0122] According to an embodiment of the present application, the negative electrode sheet includes a negative electrode current collector disposed on at least one side of the negative electrode active material layer.
[0123] According to an embodiment of the present application, the negative electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, a copper foil may be used. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), etc.).
[0124] According to an embodiment of the present application, the negative electrode active material may adopt a negative electrode active material for a battery known in the art. As an example, the negative electrode active material may include at least one of the following materials: graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, etc. The silicon-based material may include at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may include at least one of elemental tin, tin oxide compounds, and tin alloys.
[0125] According to an embodiment of the present application, the negative electrode active material layer may further optionally include a binder. The binder may include at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0126] According to an embodiment of the present application, the negative electrode active material layer may further include a conductive agent, which may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0127] According to an embodiment of the present application, the negative electrode active material layer may further optionally include other auxiliary agents, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).
[0128] According to an embodiment of the present application, the negative electrode sheet can be prepared in the following manner: the components for preparing the negative electrode sheet (such as negative electrode active material, conductive agent, binder and any other components) are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.
[0129] It should be noted that the features and advantages described above for the conductive agent and its preparation method are also applicable to the positive electrode sheet and the negative electrode sheet, and will not be repeated here.
[0130] The fifth aspect of the present application proposes a solid-state battery. According to an embodiment of the present application, the solid-state battery comprises: a positive electrode sheet, a sulfide electrolyte layer and a negative electrode sheet, wherein the sulfide electrolyte layer is located between the positive electrode sheet and the negative electrode sheet; the positive electrode sheet is selected from the positive electrode sheet described in the third aspect; and / or the negative electrode sheet is selected from the negative electrode sheet described in the fourth aspect. The solid-state battery of the present application has excellent rate performance, cycle performance and thermal stability, and has a long service life.
[0131] According to an embodiment of the present application, the sulfide electrolyte layer includes a glass-ceramic Li-PS system, a sulfide germanium ore Li 6 PS 5 X or LiGeP 10 G2 S 12 wherein X is Cl, Br or I.
[0132] The battery of the present application may include a battery cell form, a battery module form and a battery pack form. In some embodiments, the battery cells can be assembled into a battery module, and the number of battery cells contained in the battery module can be one or more, and the specific number can be selected by those skilled in the art according to the application and capacity of the battery module. In some embodiments, the battery modules can also be assembled into a battery pack, and the number of battery modules contained in the battery pack can be one or more, and the specific number can be selected by those skilled in the art according to the application and capacity of the battery pack.
[0133] It should be noted that the characteristics and advantages described above for the positive electrode plate and the negative electrode plate are also applicable to the solid-state battery and will not be repeated here.
[0134] The sixth aspect of the present application provides an electric device. According to an embodiment of the present application, the electric device includes: the solid-state battery described in the fifth aspect. Therefore, the electric device of the present application has high-efficiency energy output and excellent service life and safety performance.
[0135] Battery cells, battery modules, and battery packs can be used as power sources for electrical devices or as energy storage units for electrical devices. Electrical devices may include, but are not limited to, mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships, satellites, energy storage systems, etc.
[0136] As an electrical device, a battery cell, battery module or battery pack can be selected according to its usage requirements.
[0137] As an embodiment, the electric device may be a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, etc. In order to meet the requirements of the electric device for high power and high energy density of the battery, a battery pack or a battery module may be used.
[0138] As another embodiment, the device may be a mobile phone, a tablet computer, a notebook computer, etc. The device is usually required to be light and thin, and a battery cell may be used as a power source.
[0139] It should be noted that the characteristics and advantages described above for solid-state batteries are also applicable to this electrical equipment and will not be repeated here.
[0140] The scheme of the present application will be explained below in conjunction with the embodiments. It will be appreciated by those skilled in the art that the following embodiments are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If no specific technology or conditions are indicated in the embodiments, the technology or conditions described in the literature in this area or the product specification are carried out. The reagents used or the instruments that do not indicate the manufacturer are all conventional products that can be obtained commercially.
[0141] Example 1
[0142] 1. Preparation of conductive agent
[0143] (1) Different coaxial spinning solutions, namely the shell spinning solution and the core spinning solution, are placed in the micro-injection pumps of the core and shell of the coaxial spinning head respectively.
[0144] Shell spinning solution: LiNO 3 、Al(NO 3 ) 3 9H 2 O、Ti(OC 4 H 9 ) 4 , C 6 H 7 O 3 P was dissolved in DMF with acetic acid and PVP in a molar ratio of 1.4:0.4:1.6:3, wherein the solid content of the shell spinning solution was 15%, and stirring at room temperature for 10 h was required to obtain a uniform transparent solution.
[0145] Core spinning solution: PAN is dispersed in N,N-dimethylformamide solvent, wherein the solid content of the core spinning solution is 15%, and it needs to be stirred at room temperature for 10 h to obtain a uniform solution;
[0146] (2) The distance between the coaxial spinning head and the receiving plate was 15 cm, and the rotation speed of the drum receiver was 1500 rpm; the pushing speed of the core and shell microinjection pumps was 0.5 ml / h;
[0147] (3) coaxially electrospinning the obtained shell spinning solution and core spinning solution for 2 min to obtain the precursor of the desired coating material, wherein the coating material precursor nanowires of different lengths can be obtained by controlling the electrospinning time;
[0148] (4) After drying the obtained coating material precursor, it was first pre-oxidized at 250℃ for 2 h in an oxygen atmosphere, and then placed in a tube furnace in an argon atmosphere for high-temperature treatment at 600℃ for 10 h, where the heating rate was 5℃ / min. At high temperature, the thermal decomposition reaction of PAN in the inner core began, releasing a large amount of small molecular gas to form holes in the outer shell. The precursor in the shell layer formed a porous fast ion conductor LATP shell layer under high-temperature sintering. Finally, it was kept at 1200℃ for 2 hours to completely carbonize PAN, and a fast ion conductor coated carbon fiber material (LATP@C coating material) was obtained, marked as M1. Among them, the diameter of the inner core and the thickness of the shell of the LATP@C coating material and the ratio of the two, the specific surface area of the inner core and the shell, the porosity of the shell, and the aspect ratio of the conductive agent in fiber form are shown in Table 1.
[0149] 2. Preparation of batteries
[0150] Anisole was used as a solvent to add 90wt% Ni88 ternary positive electrode material, 9wt% LPSC, 1wt% LATP@C and 0.5wt% NBR and stirred for 12 hours to obtain a positive electrode slurry. The positive electrode slurry was coated on aluminum foil and dried to obtain a composite positive electrode sheet. The battery was assembled using LPSC as the solid electrolyte layer and Li / In as the negative electrode.
[0151] Example 2
[0152] The difference from Example 1 is that the solid content of the shell spinning solution is 20%, the pushing speed of the shell microinjection pump is 0.8 ml / h, and a suitable coaxial electrospinning needle is replaced, and the other operations remain unchanged. As a result, the core diameter and shell thickness of the LATP@C coating material are 20 nm and 200 nm, respectively, and the ratio between the two is 0.1:1; marked as M2.
[0153] Example 3
[0154] The difference from Example 1 is that the solid content of the core spinning solution is 10%, the pushing speed of the shell microinjection pump is 0.3 ml / h, and a suitable coaxial electrospinning needle is replaced, and the other operations remain unchanged. As a result, the core diameter and shell thickness of the LATP@C coating material are 50 nm and 500 nm, respectively, and the ratio of the two is 10:1; marked as M3.
[0155] Example 4
[0156] The difference from Example 1 is that the solid content of the core spinning solution is 5%, the solid content of the shell spinning solution is 25%, the pushing speed of the shell microinjection pump is 0.3 ml / h, the pushing speed of the core microinjection pump is 1 ml / h, and a suitable coaxial electrospinning needle is replaced. The other operations remain unchanged. Thus, the core diameter and shell thickness of the LATP@C coating material are 50 nm and 750 nm, respectively, and the ratio between the two is 0.07:1; marked as M4.
[0157] Example 5
[0158] The difference from Example 1 is that the solid content of the core spinning solution is 25%, the solid content of the shell spinning solution is 10%, the pushing speed of the shell microinjection pump is 0.8 ml / h, the pushing speed of the core microinjection pump is 0.2 ml / h, and the appropriate coaxial electrospinning needle is replaced. The other operations remain unchanged. As a result, the core diameter and shell thickness of the LATP@C coating material are 750 nm and 50 nm, respectively, and the ratio between the two is 15:1; marked as M5.
[0159] Example 6
[0160] The difference from Example 1 is that the high temperature treatment is carried out at 600°C for 6 hours in a tube furnace with an argon atmosphere, the heating rate is 8°C / min, and the other operations remain unchanged. Thus, the porosity of the shell layer is 50%; it is marked as M6.
[0161] Example 7
[0162] The difference from Example 1 is that the high temperature treatment is carried out at 700°C for 8 hours in a tube furnace with an argon atmosphere, the heating rate is 3°C / min, and the other operations remain unchanged. Thus, the porosity of the shell layer is 80%; it is marked as M7.
[0163] Example 8
[0164] The difference from Example 1 is that the high temperature treatment is carried out at 500°C for 4 hours in a tube furnace with an argon atmosphere, the heating rate is 10°C / min, and the other operations remain unchanged. Thus, the porosity of the shell layer is 40%; it is marked as M8.
[0165] Example 9
[0166] The difference from Example 1 is that the high temperature treatment is carried out at 800°C for 10 hours in a tube furnace with an argon atmosphere, the heating rate is 2°C / min, the holding time is 10 hours, and the other operations remain unchanged. Thus, the porosity of the shell layer is 90%; it is marked as M9.
[0167] Example 10
[0168] The difference from Example 1 is that the spinning time is adjusted to 4 hours, and the other operations remain unchanged. Thus, the aspect ratio of the obtained LATP@C coating material is 150, which is marked as M10.
[0169] Embodiment 11
[0170] The difference from Example 1 is that the spinning time is adjusted to 1 hour, and the other operations remain unchanged. Thus, the aspect ratio of the obtained LATP@C coated material is 30; it is marked as M11.
[0171] Example 12
[0172] The difference from Example 1 is that in step 2, the amount of LPSC added is 7 wt % and the amount of LATP@C added is 3 wt %.
[0173] Example 13
[0174] The difference from Example 1 is that in step 2, the amount of LPSC added is 5 wt % and the amount of LATP@C added is 5 wt %.
[0175] Embodiment 14
[0176] The difference from Example 1 is that in step 2, the amount of LPSC added is 9.5wt% and the amount of LATP@C added is 0.5wt%.
[0177] Comparative Example 1
[0178] The difference from Example 1 is that the shell spinning solution is replaced by the core spinning solution, and the other steps remain unchanged. Thus, a carbon-coated carbon fiber material (C@C coated material) is obtained; it is marked as DM1.
[0179] Comparative Example 2
[0180] The difference from Example 1 is that the core spinning solution is replaced by the shell spinning solution, and the other steps remain unchanged. Thus, a fiber material of LATP coated with LATP (LATP@LATP coated material) is obtained, which is marked as DM2.
[0181] Comparative Example 3
[0182] The difference from Example 1 is that the shell spinning solution: 1 mol of Al(NO 3 ) 3 9H 2 O and PVP were dissolved in DMF, wherein the solid content of the shell spinning solution was 17%, and it was necessary to stir at room temperature for more than 8 hours to obtain a uniform transparent solution, and the other steps remained unchanged. 2 O 3 Coated carbon fiber material (Al 2 O 3 @C coating material); marked as DM3.
[0183] Test Case
[0184] 1. Ionic conductivity test
[0185] The solid electrolyte layer, indium foil, and lithium copper foil are assembled at the upper and lower ends of the composite positive electrode layer in order, and are cold pressed into shape using a sheet press with a molding pressure of 300 MPa. After tightening the bolts, a solid-state mold battery is obtained (this step is performed in an inert atmosphere). Then a CA test is performed, and the applied voltage is divided by the measured steady-state current to obtain the composite positive electrode resistance. Finally, the formula is used: Calculate the ionic conductivity of the composite positive electrode, where d is the thickness of the composite positive electrode, A is the effective conductive area of the composite positive electrode, and R I is the composite positive electrode impedance value.
[0186] 2. Electronic conductivity test
[0187] Assemble the carbon-coated aluminum foil at the upper and lower ends of the composite positive electrode layer in order, and use a sheet press to cold-press it into shape with a molding pressure of 300 MPa. After tightening the bolts, a solid-state mold battery is obtained (this step is performed in an inert atmosphere). Then perform a CA test, and divide the applied voltage by the measured steady-state current to obtain the composite positive electrode resistance. Finally, the formula: Calculate the electronic conductivity of the composite positive electrode, where d is the thickness of the composite positive electrode, A is the effective conduction area of the composite positive electrode, and R E is the composite positive electrode impedance value.
[0188] 3. Battery performance test
[0189] First, 100 mg of LPSC electrolyte was pre-pressed at 150 MPa using a PEEK mold, and then indium foil, lithium copper foil, composite cathode layer, and carbon-coated aluminum foil were assembled at the upper and lower ends of the electrolyte layer in order, and then cold-pressed using a tablet press with a molding pressure of 300 MPa. After tightening the bolts, a solid-state mold battery was obtained (this step was performed in an inert atmosphere). Then, 0.1C, 0.5C charge and discharge rates and 0.33C cycle tests were performed.
[0190] 4. Test method for core-shell thickness
[0191] The core-shell thickness of the composite cathode modified filler can be mainly tested by scanning electron microscopy (SEM) and transmission electron microscopy (TEM). The prepared composite cathode modified filler is characterized by SEM and TEM, and the fast ion shell and the conductive carbon core layer are distinguished by morphological differences and combined with energy dispersive spectrometer (EDS), and the core-shell thickness of the composite cathode modified filler is obtained.
[0192] The results are shown in Table 2. Compared with Comparative Examples 1-3, the electronic and ionic conductivity, rate performance and cycle performance of the batteries prepared in Examples 1-14 are more excellent overall. In Comparative Example 1, no fast ion conductor is added. Although the conductive carbon fiber in the inner core is in direct contact with the positive electrode material, which will improve the electronic conductivity, the ion transfer conductivity is low due to the lack of fast ion conductors. In addition, there is a high chemical reaction activity between the conductive carbon fiber and the sulfide electrolyte, and interfacial reactions are prone to occur. The electron transfer between the conductive carbon fiber and the sulfide electrolyte will aggravate the reaction, thereby reducing the cycle performance and rate performance of the battery.
[0193] In Comparative Example 2, since no conductive carbon fiber is added, the electron transport performance is poor, thereby reducing the cycle performance and rate performance of the battery.
[0194] In Comparative Example 3, Al 2 O 3 The coated carbon fiber has poorer ionic and electronic conductivity, cycle performance and rate performance than the fast ion conductor coating effect of the embodiment.
[0195] Table 1
[0196]
[0197] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.
Claims
1. A solid-state battery, characterized in that: include: A positive electrode sheet, a sulfide electrolyte layer and a negative electrode sheet, wherein the sulfide electrolyte layer is located between the positive electrode sheet and the negative electrode sheet; The positive electrode plate comprises: a positive electrode active material layer, wherein the positive electrode active material layer comprises: a positive electrode active material and a conductive agent; and / or, The negative electrode plate comprises: a negative electrode active material layer, and the negative electrode active material layer comprises: a negative electrode active material and a conductive agent, in, The conductive agent comprises: a core, the core comprising a conductive carbon material; A shell layer covers at least a portion of the surface of the core, and the shell layer includes a fast ion conductor.
2. The solid-state battery according to claim 1, characterized in that: The fast ion conductor includes at least one of lithium aluminum titanium phosphate, lithium lanthanum titanium oxide and lithium lanthanum zirconium oxide.
3. The solid-state battery according to claim 1, characterized in that: The fast ion conductor includes Li 1+x Al x Ti 2-x (PO4)3, 0≤x≤0.
5.
4. The solid-state battery according to claim 1, characterized in that: The conductive carbon material includes at least one of carbon nanotubes, carbon fibers, carbon black and graphene.
5. The solid-state battery according to claim 1, characterized in that: The conductive agent satisfies at least one of the following conditions: The ratio of the diameter of the core to the thickness of the shell is (0.1-10):1; The diameter of the core is 0.5 nm to 0.5 μm; The thickness of the shell layer is 0.5 nm to 0.5 μm; The specific surface area of the core is 10 m 2 / g~500 m 2 / g; The specific surface area of the shell is 10 m 2 / g ~500 m 2 / g; The shell layer has a porous structure, and the porosity of the shell layer is 50% to 80%; The conductive agent is in a fibrous shape with an aspect ratio of (30-150):
1.
6. The solid-state battery according to claim 1, characterized in that: The conductive agent satisfies at least one of the following conditions: The ratio of the diameter of the inner core to the thickness of the shell is (1-3):1; The diameter of the core is 50 nm to 200 nm; The thickness of the shell layer is 100 nm to 200 nm; The specific surface area of the core is 10 m 2 / g~100 m 2 / g; The specific surface area of the shell is 50 m 2 / g ~200 m 2 / g; The shell layer has a porous structure, and the porosity of the shell layer is 50% to 80%; The conductive agent is in a fibrous shape with an aspect ratio of (30-70):
1.
7. The solid-state battery according to any one of claims 1 to 6, characterized in that: The preparation method of the conductive agent comprises: The inner core spinning solution and the shell layer spinning solution are subjected to coaxial electrospinning to obtain a precursor; The precursor is subjected to a heat treatment to obtain the conductive agent.
8. The solid-state battery according to claim 7, characterized in that: The method comprises at least one of the following conditions: The shell spinning solution comprises: lithium salt, aluminum salt, titanium salt, phosphonate, complexing agent, binder and organic solvent; The solid content of the core spinning solution is 5% to 25% by mass; The core spinning solution includes polyacrylonitrile and an organic solvent; The solid content of the shell spinning solution is 5% to 25% by mass; The injection speed of the core spinning solution is 0.2 ml / h ~1 ml / h; The injection speed of the shell spinning solution is 0.3 ml / h to 0.8 ml / h; The coaxial electrospinning treatment time is 5 min to 15 min.
9. The solid-state battery according to claim 7, characterized in that: The heating treatment comprises: subjecting the precursor to a first heating treatment, a second heating treatment and a third heating treatment in sequence; The heating treatment satisfies at least one of the following conditions: The temperature of the first heating treatment is 200°C to 300°C, and the time is 0.5 h to 4 h; The second heating treatment is performed at a temperature of 650°C to 900°C and for a time of 6 h to 12 h; The temperature of the third heat treatment is 1000° C. to 1500° C., and the time is 1 h to 4 h; The heating rate of heating to the second heating treatment temperature after the first heating treatment is 5°C / min-10°C / min.
10. The solid-state battery according to claim 1, characterized in that: The positive electrode active material includes lithium iron phosphate or nickel-cobalt-manganese ternary positive electrode material; and / or, the positive electrode active material layer further comprises a sulfide electrolyte; And / or, the mass of the conductive agent accounts for 0.5% to 7% of the mass of the positive electrode active material layer.
11. The solid-state battery according to claim 1, characterized in that: The mass of the conductive agent accounts for 0.5% to 1% of the mass of the positive electrode active material layer.
12. An electrical equipment, characterized in that: include: A solid-state battery according to any one of claims 1 to 11.
Citation Information
Cited By
Conductive agent for solid-state lithium battery and preparation method of conductive agent
CN122455774A