Preparation method and use of ionic copper / zinc catalyst
The ionic copper/zinc catalyst synthesized through a one-pot method solves the problem of uneven catalyst components and halogen-assisted catalysis, and achieves efficient catalysis of olefin epoxidation and carbon dioxide cycloaddition reaction without additional halogens, improving the environmental efficiency. Economic benefits and conversion rate of carbonate.
Patent Information
- Application Number
- CN202411088766.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-08-09
AI Technical Summary
Existing catalysts in the olefin epoxidation and carbon dioxide cycloaddition reactions have problems such as non-single catalyst components, the need for halogen cocatalysis and high production costs, which limits the economic benefits and types of cyclic carbonates.
An ionic copper/zinc catalyst is synthesized using a one-pot method. The [Cu2(L)]2[ZnCl4] catalyst is generated by reacting copper salts and zinc salts with salicylaldehyde and tetraethylenepentamine. It has dual active centers and synergistic catalysis. Alkene epoxidation and carbon dioxide cycloaddition reaction.
It achieves efficient catalysis of olefin epoxidation and carbon dioxide cycloaddition reaction without additional halogen cocatalyst, improves the high conversion rate and selectivity of cyclic carbonate, and reduces production costs.
Smart Images

Figure CN118619977B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalyst material preparation, and relates to a preparation method of an ionic copper / zinc catalyst and application thereof. Background Art
[0002] Among the many carbon dioxide conversion technologies, the reaction of CO2 and epoxides to synthesize cyclic carbonates is widely used. Based on this, a large number of research results on the synthesis of cyclic carbonates from CO2 and epoxides have been reported one after another, but most of the catalytic systems require the presence of halogen promoters ( Chem. Eng. J. 2023, 474, 15, 145918; Adv. Mater. 2022, 34, 44, 2206991). Importantly, the main raw material epoxide in the above synthesis of cyclic carbonates is relatively expensive, resulting in low economic benefits in actual production and limiting the entry of more types of cyclic carbonates into the chemical market. In order to improve economic benefits, considering that epoxides are mainly synthesized by epoxidation of olefins, the direct series synthesis of cyclic carbonates using cheap olefins as raw materials can effectively avoid the separation of intermediate epoxides and provide a safe, economical and green synthesis route. Therefore, if it is possible to directly synthesize cyclic carbonates from cheap raw material olefins upstream of epoxides through oxidation-cycloaddition reactions, it has important scientific significance and potential application value. In the current research process, most reactions use two catalysts to complete olefin epoxidation and cycloaddition reactions, and there are a series of problems in the reported research results, such as high reaction temperature, excessive reaction pressure, and the need for halogen co-catalysts ( Chem. Eng. J. 2022, 444, 15, 135478; J. CO2 Util. 2024, 82, 102760), therefore, the development of a single-component catalyst for olefin epoxidation and carbon dioxide cycloaddition without additional halogen co-catalysts has become a top priority in solving this problem.
[0003] In order to solve the above problems, based on the research of the existing literature "A preparation method and use of an ionic zinc catalyst" (application number: 2024102337672), according to the development concept of green chemistry, it is very necessary to design an environmentally friendly ionic copper / zinc efficient catalytic system for the epoxidation of olefins and the cycloaddition of carbon dioxide to form cyclic carbonates.
[0004] However, in the previous study of the existing document "A preparation method and use of an ionic zinc catalyst" (application number: 2024102337672), it was found that the ionic zinc catalyst can better realize the cycloaddition reaction of carbon dioxide without additional halogen conditions, but in the olefin epoxidation reaction, because this catalyst does not have an active center for catalyzing the olefin epoxidation reaction, this catalyst cannot catalyze the reaction. Further designing and synthesizing a single-component catalyst with dual active centers is the key to solving the problem of realizing olefin epoxidation and cycloaddition reactions without the addition of additional halogens. Based on this, the solution of this application is proposed. Summary of the invention
[0005] The purpose of the present invention is to provide a one-pot method for preparing an ionic copper / zinc catalyst single-component catalyst in view of the problems that the catalyst component is not single, halogen exists, and the production cost is high in the catalytic conversion reaction of olefin epoxidation and carbon dioxide cycloaddition, so as to play a synergistic catalytic role in the olefin epoxidation and carbon dioxide cycloaddition series reaction, so as to achieve the goal of being able to realize the olefin epoxidation and carbon dioxide cycloaddition series reaction under the action of a relatively low amount of the single-component catalyst and without an additional halogen promoter.
[0006] The design ideas of the present invention are as follows:
[0007] The copper salt, zinc salt and organic ligand were synthesized in situ in a one-pot method to construct an ionic copper / zinc complex, which synergistically catalyzed olefin epoxidation and carbon dioxide cycloaddition at multiple active sites during the reaction process.
[0008] The ionic multi-site catalyst was synthesized by reacting copper salt, zinc salt with salicylaldehyde and tetraethylenepentamine in the presence of methanol. The copper catalytic site in the catalyst reacted with [ZnCl4] 2- Active sites play a synergistic catalytic role in the catalytic process of olefin epoxidation and carbon dioxide cycloaddition;
[0009] An ionic multi-site single-component catalyst with a clear structure is applied to the cycloaddition reaction of olefin epoxidation and carbon dioxide to achieve the goal of obtaining cyclic carbonates with high carbon dioxide conversion rate and high selectivity.
[0010] The crystal structure information of the above catalyst is obtained by the following method: the crystal of the ionic multi-site single-component catalyst is synthesized by conventional solvothermal method. The specific technical scheme is as follows:
[0011] In a clean round-bottom flask, add a certain amount of salicylaldehyde, tetraethylenepentamine and MeOH (10mL) in sequence, then add copper salt and zinc chloride under reflux stirring, and stir for another 2 hours. After the reaction is completed, filter while hot, and let the filtrate stand at room temperature for volatilization to obtain [Cu2(L)]2[ZnCl4] (L is the product of the condensation of tetraethylenepentamine and salicylaldehyde) catalyst.
[0012] The preferred solution is to sequentially add salicylaldehyde (0.50-2.5mmol) and tetraethylenepentamine (0.17-0.85mmol) and MeOH (10mL) into a clean round-bottom flask, stir at 60-100°C for 2-6h, then add copper perchlorate hexahydrate (0.33-1.65mmol) and zinc chloride (0.11-0.55mmol), stir for another 2h, then filter while hot, and let the filtrate stand at room temperature for 2-4 weeks to evaporate. [Cu2(L)]2[ZnCl4] (L is the product of the condensation of tetraethylenepentamine and salicylaldehyde) is obtained with a yield of about 30-50%.
[0013] The product was characterized by single crystal X-ray diffraction and powder X-ray diffraction to obtain accurate information about the crystal structure. The specific results are as follows:
[0014] The molecular formula of the crystal is [Cu2(L)]2[ZnCl4], and its asymmetric unit contains two [Cu2(L)] + cation and a [ZnCl4] 2- Anion. The binuclear Cu unit is located at the center of the cationic structural framework. Due to the flexibility of the ligand and the presence of multiple coordination sites, two different coordination modes are observed for the Cu atom. One of the Cu atoms is coordinated by two N atoms (from the imine group and the imidazolidine ring) and three O atoms (from three phenoxy groups), forming a distorted trigonal bipyramidal geometry. The other Cu atom adopts an octahedral coordination mode, with two N atoms from the amino and imine groups and two O atoms from the phenoxy groups occupying the equatorial positions. In addition, one N atom and one hydroxyl oxygen atom of the imidazolidine group of the ligand are located at the axial positions of the octahedron. The length of the Cu-N / O bond ranges from 1.977-2.308 Å. In addition, the two Cu atoms are bridged by two phenolic oxygen atoms to form a quaternary binuclear unit with a square planar geometry. The anion part has [ZnCl4] 2- Unit, where Zn 2+ The ion consists of four Cl - Ion coordination forms a tetrahedral geometric structure. The two are combined together by the electrostatic attraction between anions and cations. Structural analysis revealed that this type of catalyst contains two active centers, one of which is [Cu2(L)] + Active site, one is [ZnCl4] 2-Anion active sites, both contribute to olefin epoxidation and carbon dioxide cycloaddition reactions respectively, playing a synergistic catalytic role.
[0015] The present invention mainly synthesizes an ionic copper / zinc single-component catalyst for olefin epoxidation and carbon dioxide cycloaddition, and has applied it to olefin epoxidation and carbon dioxide cycloaddition reactions. This type of catalyst can realize a series reaction of olefin epoxidation and carbon dioxide cycloaddition, and the preparation method of this type of catalyst has a simple reaction process.
[0016] The present invention has the following beneficial effects:
[0017] 1. The preparation method is simple, and the catalysts have a clear molecular structure, which is conducive to studying the mechanism of catalytic reactions.
[0018] 2. The catalyst has [Cu2(L)] + Active site, [ZnCl4] 2- Anion active sites, both contribute to olefin epoxidation and carbon dioxide cycloaddition reactions respectively. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 Schematic diagram of the crystal structure of the compound [Cu2(L)]2[ZnCl4];
[0020] Figure 2 This is the RXRD characterization diagram of the compound [Cu2(L)]2[ZnCl4]. DETAILED DESCRIPTION
[0021] In order to demonstrate the essential features and significant improvements of the present invention, the following examples are used to further illustrate the implementation methods and effects.
[0022] Example 1: Preparation of compound [Cu2(L)]2[ZnCl4]
[0023] In a clean round-bottom flask, salicylaldehyde (0.50 mmol) and tetraethylenepentamine (0.17 mmol) were mixed with MeOH (10 mL) at 80 °C. o Reflux and stir at 4 °C for 4 h, then add copper perchlorate hexahydrate (0.33 mmol) and zinc chloride (0.11 mmol), continue the reaction for 2 h, filter while hot, and let the resulting solution stand at room temperature for 4 weeks. Green crystals [Cu2(L)]2[ZnCl4] were obtained with a yield of 40%.
[0024] Example 2: Preparation of compound [Cu2(L)]2[ZnCl4]
[0025] In a clean round-bottom flask, salicylaldehyde (2.50 mmol) and tetraethylenepentamine (0.85 mmol) were mixed with MeOH (10 mL) at 90 °C. o Reflux and stir at 40 °C for 6 h, then add copper perchlorate hexahydrate (1.65 mmol) and zinc chloride (0.55 mmol), continue the reaction for 2 h, filter while hot, and let the resulting solution stand at room temperature for 4 weeks. Green crystals [Cu2(L)]2[ZnCl4] were obtained with a yield of 50%.
[0026] Example 3: Preparation of compound [Cu2(L)]2[ZnCl4]
[0027] In a clean round-bottom flask, salicylaldehyde (2.50 mmol) and tetraethylenepentamine (0.85 mmol) were mixed with MeOH (10 mL) at 60 o Reflux and stir at 40 °C for 5 h, then add copper perchlorate hexahydrate (1.65 mmol) and zinc chloride (0.44 mmol), continue the reaction for 2 h, filter while hot, and let the resulting solution stand at room temperature for 3 weeks. Green crystals [Cu2(L)]2[ZnCl4] were obtained with a yield of 37%.
[0028] Example 4: Preparation of compound [Cu2(L)]2[ZnCl4]
[0029] In a clean round-bottom flask, salicylaldehyde (2.00 mmol) and tetraethylenepentamine (0.85 mmol) were mixed with MeOH (10 mL) at 100 °C. o Reflux and stir at 40 °C for 2 h, then add copper perchlorate hexahydrate (1.32 mmol) and zinc chloride (0.55 mmol), continue the reaction for 2 h, filter while hot, and let the resulting solution stand at room temperature for 4 weeks. Green crystals [Cu2(L)]2[ZnCl4] were obtained with a yield of 43%.
[0030] Example 5: Preparation of compound [Cu2(L)]2[ZnCl4]
[0031] In a clean round-bottom flask, salicylaldehyde (2.50 mmol) and tetraethylenepentamine (0.68 mmol) were mixed with MeOH (10 mL) at 80 °C. o Reflux and stir at 4 °C for 4 h, then add copper perchlorate hexahydrate (1.32 mmol) and zinc chloride (0.44 mmol), continue the reaction for 2 h, filter while hot, and let the resulting solution stand at room temperature for 4 weeks. Green crystals [Cu2(L)]2[ZnCl4] were obtained with a yield of 45%.
[0032] Example 6: Preparation of compound [Cu2(L)]2[ZnCl4]
[0033] In a clean round-bottom flask, salicylaldehyde (2.00 mmol) and tetraethylenepentamine (0.85 mmol) were mixed with MeOH (10 mL) at 80 °C. o Reflux and stir at 40 °C for 6 h, then add copper perchlorate hexahydrate (1.65 mmol) and zinc chloride (0.44 mmol), continue the reaction for 2 h, filter while hot, and let the resulting solution stand at room temperature for 2 weeks. Green crystals [Cu2(L)]2[ZnCl4] were obtained with a yield of 38%.
[0034] Example 7: Preparation of compound [Cu2(L)]2[ZnCl4]
[0035] In a clean round-bottom flask, salicylaldehyde (2.50 mmol) and tetraethylenepentamine (0.68 mmol) were mixed with MeOH (10 mL) at 100 °C. o Reflux and stir at 40 °C for 5 h, then add copper perchlorate hexahydrate (1.65 mmol) and zinc chloride (0.55 mmol), continue the reaction for 2 h, filter while hot, and let the resulting solution stand at room temperature for 4 weeks. Green crystals [Cu2(L)]2[ZnCl4] were obtained with a yield of 30%.
[0036] Example 8: Preparation of compound [Cu2(L)]2[ZnCl4]
[0037] In a clean round-bottom flask, salicylaldehyde (2.50 mmol) and tetraethylenepentamine (0.85 mmol) were mixed with MeOH (10 mL) at 70 °C. o Reflux and stir at 40 °C for 5 h, then add copper perchlorate hexahydrate (1.65 mmol) and zinc chloride (0.55 mmol), continue the reaction for 2 h, filter while hot, and let the resulting solution stand at room temperature for 3 weeks. Green crystals [Cu2(L)]2[ZnCl4] were obtained with a yield of 47%.
[0038] Example 9: Preparation of compound [Cu2(L)]2[ZnCl4]
[0039] In a clean round-bottom flask, salicylaldehyde (2.50 mmol) and tetraethylenepentamine (0.85 mmol) were mixed with MeOH (10 mL) at 70 °C. oC, reflux and stir for 5 h, then add copper chloride (1.60 mmol) and zinc chloride (0.55 mmol), continue the reaction for 2 h, filter while hot, and let the resulting solution stand at room temperature for 3 weeks. Green crystals [Cu2(L)]2[ZnCl4] were obtained with a yield of 39%.
[0040] Example 10: Preparation of compound [Cu2(L)]2[ZnCl4]
[0041] In a clean round-bottom flask, salicylaldehyde (2.50 mmol) and tetraethylenepentamine (0.85 mmol) were mixed with MeOH (10 mL) at 70 °C. o Reflux and stir at 40 °C for 5 h, then add copper acetate (1.60 mmol) and zinc chloride (0.55 mmol), continue the reaction for 2 h, filter while hot, and let the resulting solution stand at room temperature for 3 weeks. Green crystals [Cu2(L)]2[ZnCl4] were obtained with a yield of 31%.
[0042] Example 11: Preparation of compound [Cu2(L)]2[ZnCl4]
[0043] In a clean round-bottom flask, salicylaldehyde (2.50 mmol) and tetraethylenepentamine (0.85 mmol) were mixed with MeOH (10 mL) at 70 °C. o Reflux and stir at 40 °C for 5 h, then add copper chloride (1.65 mmol) and zinc acetate (0.55 mmol), continue the reaction for 2 h, filter while hot, and let the resulting solution stand at room temperature for 3 weeks. Green crystals [Cu2(L)]2[ZnCl4] were obtained with a yield of 39%.
[0044] Example 12: Preparation of compound [Cu2(L)]2[ZnCl4]
[0045] In a clean round-bottom flask, salicylaldehyde (2.50 mmol) and tetraethylenepentamine (0.85 mmol) were mixed with MeOH (10 mL) at 70 °C. o Reflux and stir at 40 °C for 5 h, then add copper chloride (1.65 mmol) and zinc sulfate (0.55 mmol), continue the reaction for 2 h, filter while hot, and let the resulting solution stand at room temperature for 3 weeks. Green crystals [Cu2(L)]2[ZnCl4] were obtained with a yield of 36%.
[0046] Table 1. Crystallographic data of compound [Cu2(L)]2[ZnCl4]
[0047]
[0048] Embodiment 13:
[0049] Application of ionic copper / zinc single-component catalysts to olefin epoxidation and carbon dioxide cycloaddition reactions:
[0050] In a 20 mL high pressure organic synthesis parallel reaction tube, a polytetrafluoroethylene magnetic stirrer was placed. At room temperature, 5 mmol of styrene, 5.5 mmol of TBHP, and a catalyst [Cu2(L)]2[ZnCl4] (0.5 mol%) were added. 2 mL of acetonitrile was heated at 100 degrees Celsius for 4 h, cooled to room temperature, and analyzed by GC / GC-MS.
[0051] In a 20 mL high pressure organic synthesis parallel reaction tube, epoxy compound (5 mmol) and catalyst [Cu2(L)]2[ZnCl4] (0.5 mol%) were added in sequence; the reaction tube was placed in a high pressure organic synthesis parallel reactor, and the reaction device was sealed; the pressure was increased to 2 MPa with CO2; at 100 o C for 4 h with vigorous stirring. After cooling to room temperature, the mixture was extracted with acetonitrile (10 mL) and analyzed by GC / GC-MS / NMR.
[0052] As shown below, the results of the catalyst [Cu2(L)]2[ZnCl4] on olefin epoxidation and carbon dioxide cycloaddition are as follows:
[0053]
[0054] The above results show that [Cu2(L)]2[ZnCl4] exhibits high catalytic activity in the epoxidation reaction of synthetic olefins. Under the condition of tert-butyl hydroperoxide as an oxidant, it can effectively catalyze the conversion of styrene to generate epoxystyrene compounds, and the yield can reach 83% within 4 hours. The catalyst is filtered, and then in the second step of the catalytic reaction, this catalyst can synthesize cyclic carbonate products under halogen-free and solvent-free conditions, and the yield can reach 96%. The results show that this dual-active center single-component catalyst can realize the reaction of synthesizing the final product cyclic carbonate from olefins without additional halogen-free catalysts, highlighting the ability of green catalytic carbon dioxide conversion, and solving the scientific problem that ionic zinc catalysts cannot catalyze olefin epoxidation and cycloaddition reactions in previous studies.
Claims
1. A method for preparing an ionic copper / zinc catalyst, characterized in that: The method comprises the following steps: adding salicylaldehyde, tetraethylenepentamine and a solvent to a container in sequence, stirring at 60-100°C for 2-6 hours, wherein the solvent is methanol, and then adding copper salt and zinc chloride, wherein the copper salt is one of hexahydrate copper perchlorate, copper chloride or copper acetate, wherein the molar ratio of salicylaldehyde: tetraethylenepentamine: copper salt: zinc chloride is 0.50-2.5: 0.17-0.85: 0.33-1.65: 0.11-0.55, stirring for another 2 hours, and then filtering while hot, and allowing the filtrate to stand at room temperature for 2-4 weeks for volatilization to obtain [Cu2(L)]2[ZnCl4], wherein L is a product of condensation of tetraethylenepentamine and salicylaldehyde, and the structural formula is as follows: 。 2. Use of the ionic copper / zinc catalyst obtained by the preparation method as claimed in claim 1 in catalyzing the epoxidation of olefins and the cycloaddition reaction of carbon dioxide.
Citation Information
Patent Citations
Preparation method and application of heterogeneous Schiff base catalyst
CN109675634A
Preparation method and application of ionic zinc catalyst
CN118165014A