Ultrafine hard alloy and preparation method thereof
Ultrafine WC powder and cobalt-rhenium boron ternary boride were prepared by liquid-liquid doping method and ball milling process. Combined with the rhenium effect during sintering, the problem of insufficient performance of traditional cemented carbide under high temperature and high stress was solved, and the performance of traditional cemented carbide was achieved. Preparation of ultrafine carbide with high hardness and high toughness.
Patent Information
- Application Number
- CN202411115072.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-14
AI Technical Summary
Traditional WC-Co carbides have insufficient high temperature strength, fatigue resistance and crack resistance during processing, and it is difficult to disperse evenly by directly adding rare earth elements or rare earth oxides during the preparation process, resulting in unstable performance.
Ultrafine WC powder is prepared by liquid-liquid doping method, and cobalt-rhenium boron ternary boride is prepared by hydrogen reduction and ball milling process. The grains are refined in combination with the rhenium effect during sintering to form a stable ultrafine cemented carbide.
The uniformity and high performance of ultrafine cemented carbides are achieved, with hardness HV20≥2000kg/mm2, cracking toughness Kic≥8.5MPa·m1/2, grain size≤0.25μm, and porosity in metallographic microstructure, which significantly improves The toughness and fatigue resistance of the material.
Smart Images

Figure CN118621174B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of powder metallurgy, and specifically relates to an ultrafine hard alloy and a preparation method thereof. Background Art
[0002] Cemented carbide is an alloy made by powder metallurgy with one or more refractory metal carbide powders as the main component and metal powder as a binder. Cemented carbide has a series of excellent properties and is widely used as a tool material for cutting steel, stainless steel, heat-resistant alloys, cast iron and other difficult-to-process materials. Traditional WC-Co cemented carbide has deficiencies in high-temperature strength, fatigue resistance and crack resistance during processing. In order to overcome these limitations, researchers are committed to developing high-performance ultrafine cemented carbide. The grain size of ultrafine cemented carbide is significantly reduced, resulting in higher hardness, strength and wear resistance. In addition, the ultrafine grain structure can also improve the toughness, fatigue resistance and fracture resistance of the material, so that it can still maintain excellent performance in harsh environments such as high temperature and high stress.
[0003] In the research of high-performance cemented carbide, the physical properties of cemented carbide are mostly strengthened by adding rare earth additives. A large number of experiments have shown that adding rare earth elements or rare earth oxides to traditional cemented carbide can not only strengthen the hard phase and the bonding phase, making the cemented carbide have higher strength, but also increase the proportion of plastic phase, purify the grain boundary and refine the grains to improve toughness. However, if rare earth elements or rare earth oxides are directly added during the preparation of cemented carbide, it is not conducive to dispersion, resulting in holes, poor strengthening effect and unstable performance. Summary of the invention
[0004] In order to solve the problems existing in the prior art, the main purpose of the present invention is to provide an ultrafine cemented carbide and a preparation method thereof.
[0005] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:
[0006] A method for preparing ultrafine cemented carbide comprises the following steps:
[0007] S1, dissolving ammonium metatungstate, vanadium oxalate and chromium acetate in deionized water, and then spray drying to obtain an ultrafine powder precursor;
[0008] S2, the ultrafine powder precursor is calcined and then reduced and carbonized by hydrogen, and then crushed and sieved to obtain ultrafine WC powder;
[0009] S3, dissolving cobalt acetate and ammonium perrhenate in water, drying and reducing with hydrogen to obtain a cobalt-rhenium mixed powder, ball-milling the cobalt-rhenium mixed powder and boron powder to obtain a mixed powder, calcining the mixed powder under argon protection to obtain a mixed powder, and crushing and sieving to obtain an ultrafine cobalt-rhenium-boron ternary boride;
[0010] S4. Mix the ultrafine WC powder and cobalt-rhenium-boron ternary boride and then ball-mill to obtain an ultrafine cemented carbide mixture, which is then pressed and sintered to obtain an ultrafine cemented carbide.
[0011] As a preferred embodiment of the method for preparing ultrafine cemented carbide described in the present invention, in the step S1, ammonium metatungstate, vanadium oxalate and chromium acetate are taken according to the mass ratio of WC:V:Cr in the ultrafine WC powder of (98.7~99.2):(0.3~0.5):(0.5~0.8).
[0012] As a preferred embodiment of the method for preparing ultrafine cemented carbide described in the present invention, in step S2, the calcination temperature is 590-610° C., and the calcination time is 1.5-2.5 h.
[0013] As a preferred embodiment of the method for preparing ultrafine cemented carbide described in the present invention, in step S2, the hydrogen flow rate is 3-5 L / min, the carbonization temperature is 1200-1300° C., and the carbonization time is 2-4 h.
[0014] As a preferred embodiment of the method for preparing ultrafine cemented carbide described in the present invention, wherein: in the step S3, the mass ratio of rhenium to cobalt in ammonium perrhenate and cobalt acetate is (1-2):100.
[0015] As a preferred embodiment of the method for preparing ultrafine cemented carbide described in the present invention, in step S3, the reduction temperature is 480-520° C. and the reduction time is 1-2 hours.
[0016] As a preferred embodiment of the method for preparing ultrafine cemented carbide described in the present invention, wherein: in step S3, the molar ratio of the cobalt-rhenium mixed powder to the boron powder is (3-6):1.
[0017] As a preferred embodiment of the method for preparing ultrafine cemented carbide described in the present invention, wherein: in the step S3, the ball-to-material ratio is (5-8):1, the ball milling speed is 280-320 r / min, and the ball milling time is 7-9 h.
[0018] As a preferred embodiment of the method for preparing ultrafine cemented carbide described in the present invention, in step S3, the calcination temperature is 1050-1150° C. and the calcination time is 1-2 hours.
[0019] As a preferred embodiment of the method for preparing ultrafine cemented carbide according to the present invention, in step S4, the mass ratio of ultrafine WC powder to cobalt-rhenium-boron ternary boride is (90-94):(6-10).
[0020] As a preferred embodiment of the method for preparing ultrafine cemented carbide described in the present invention, wherein: in the step S4, the ball-to-material ratio is (8-12):1, the ball milling speed is 280-320 r / min, and the ball milling time is 10-15 h.
[0021] As a preferred embodiment of the method for preparing ultrafine cemented carbide according to the present invention, in said step S4, the sintering temperature is 1400-1420° C., and the sintering time is 0.5-1.5 h.
[0022] To solve the above technical problem, according to another aspect of the present invention, the present invention provides the following technical solution:
[0023] An ultrafine cemented carbide is prepared by adopting the above-mentioned method for preparing the ultrafine cemented carbide.
[0024] As a preferred embodiment of the ultrafine cemented carbide of the present invention, the hardness of the ultrafine cemented carbide HV20 ≥ 2000 kg / mm 2 , crack toughness Kic ≥ 8.5MPa·m 1 / 2 , grain size ≤ 0.25μm, and the porosity in the metallographic microstructure of ultrafine cemented carbide is A02B00.
[0025] The beneficial effects of the present invention are as follows:
[0026] The present invention proposes an ultrafine cemented carbide and a preparation method thereof. Ultrafine WC powder is prepared by liquid-liquid doping, so that the inhibitor is evenly distributed in the ultrafine WC powder, and then the binder is added to prepare cobalt-rhenium-boron ternary boride, and the grains are further refined by the rhenium effect that occurs during sintering. Stable ultrafine-grained cemented carbide is obtained by dual strengthening of the hard phase and the binder phase; the ultrafine cemented carbide is uniform, has no inclusions, and has no voids, and its hardness HV20 ≥ 2000kg / mm 2 , crack toughness Kic ≥ 8.5MPa·m 1 / 2 The average grain size is ≤0.25μm, and the porosity in the metallographic microstructure is A02B00. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0028] Figure 1 This is a photo of the ultrafine cemented carbide prepared in Example 1 of the present invention.
[0029] Figure 2 This is a photograph of the cemented carbide prepared in Comparative Example 2.
[0030] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0031] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] According to one aspect of the present invention, the present invention provides the following technical solution:
[0033] A method for preparing ultrafine cemented carbide comprises the following steps:
[0034] S1, dissolving ammonium metatungstate, vanadium oxalate and chromium acetate in deionized water, and then spray drying to obtain an ultrafine powder precursor;
[0035] S2, the ultrafine powder precursor is calcined and then reduced and carbonized by hydrogen, and then crushed and sieved to obtain ultrafine WC powder;
[0036] S3, dissolving cobalt acetate and ammonium perrhenate in water, drying and reducing with hydrogen to obtain a cobalt-rhenium mixed powder, ball-milling the cobalt-rhenium mixed powder and boron powder to obtain a mixed powder, calcining the mixed powder under argon protection to obtain a mixed powder, and crushing and sieving to obtain an ultrafine cobalt-rhenium-boron ternary boride;
[0037] S4. Mix the ultrafine WC powder and cobalt-rhenium-boron ternary boride and then ball-mill to obtain an ultrafine cemented carbide mixture, which is then pressed and sintered to obtain an ultrafine cemented carbide.
[0038] The present invention prepares ultrafine WC powder by liquid-liquid doping, so that the inhibitor is evenly distributed in the ultrafine WC powder, and then the adhesive is added to prepare cobalt-rhenium-boron ternary boride, and the grains are further refined by the rhenium effect that occurs during sintering. Stable ultrafine-grained cemented carbide is obtained by dual strengthening of hard phase and adhesive phase; the influence of impurities can be reduced by dissolving cobalt-rhenium salt in water and mixing and calcining, and pure cobalt-rhenium mixed powder can be obtained. In this method, rhenium can be evenly dispersed in cobalt, so that its strengthening effect is better, and ultrafine cobalt-rhenium-boron ternary boride is obtained by ball milling and mixing and calcining with an appropriate amount of boron powder; rhenium can improve the high-temperature creep resistance of cemented carbide, refine grains, and improve toughness, and boron can improve hardness. By using cobalt-rhenium-boron ternary boride as an adhesive, an ultrafine cemented carbide with high hardness, good toughness, and good red hardness is obtained.
[0039] Preferably, in step S1, ammonium metatungstate, vanadium oxalate and chromium acetate are taken according to the mass ratio of WC:V:Cr in the ultrafine WC powder of (98.7-99.2):(0.3-0.5):(0.5-0.8).
[0040] Preferably, in step S2, the calcination temperature is 590-610° C., and the calcination time is 1.5-2.5 h.
[0041] Preferably, in step S2, the hydrogen flow rate is 3-5 L / min, the carbonization temperature is 1200-1300° C., and the carbonization time is 2-4 h.
[0042] Preferably, in step S3, the mass ratio of rhenium to cobalt in ammonium perrhenate and cobalt acetate is (1-2):100.
[0043] Preferably, in step S3, the reduction temperature is 480-520° C., and the reduction time is 1-2 h.
[0044] Preferably, in step S3, the molar ratio of the cobalt-rhenium mixed powder to the boron powder is (3-6):1.
[0045] Preferably, in step S3, the ball-to-material ratio is (5-8):1, the ball milling speed is 280-320 r / min, and the ball milling time is 7-9 h.
[0046] Preferably, in step S3, the calcination temperature is 1050-1150° C., and the calcination time is 1-2 hours.
[0047] Preferably, in step S4, the mass ratio of the ultrafine WC powder to the cobalt-rhenium-boron ternary boride is (90-94):(6-10).
[0048] Preferably, in step S4, the ball-to-material ratio is (8-12):1, the ball milling speed is 280-320 r / min, and the ball milling time is 10-15 h.
[0049] Preferably, in step S4, the sintering temperature is 1400-1420° C., and the sintering time is 0.5-1.5 h.
[0050] According to another aspect of the present invention, the present invention provides the following technical solution:
[0051] An ultrafine cemented carbide is prepared by the above-mentioned method for preparing ultrafine cemented carbide, wherein the hardness of the ultrafine cemented carbide is HV20≥2000kg / mm 2 , crack toughness Kic ≥ 8.5MPa·m 1 / 2 The average grain size is ≤0.25μm, and the porosity in the metallographic microstructure of ultrafine cemented carbide is A02B00.
[0052] The technical solution of the present invention is further described below in conjunction with specific embodiments.
[0053] Example 1
[0054] A method for preparing ultrafine cemented carbide comprises the following steps:
[0055] S1, dissolving ammonium metatungstate, vanadium oxalate and chromium acetate in deionized water, and then spray drying to obtain an ultrafine powder precursor; taking ammonium metatungstate, vanadium oxalate and chromium acetate according to the mass ratio of WC:V:Cr in the ultrafine WC powder of 98.9:0.3:0.8;
[0056] S2. The ultrafine powder precursor is calcined and then reduced and carbonized by hydrogen, and then crushed and sieved to obtain ultrafine WC powder; the calcination temperature is 600°C, the calcination time is 2.0h, the hydrogen flow rate is 3L / min, the carbonization temperature is 1200°C, and the carbonization time is 2h.
[0057] S3. Dissolve cobalt acetate and ammonium perrhenate in water, dry and reduce with hydrogen to obtain a cobalt-rhenium mixed powder, ball-mill the cobalt-rhenium mixed powder and boron powder to obtain a mixed powder, calcine the mixed powder under argon protection to obtain a mixed powder, and crush and sieve to obtain an ultrafine cobalt-rhenium-boron ternary boride; the mass ratio of rhenium to cobalt in ammonium perrhenate and cobalt acetate is 1.5:100; the reduction temperature is 500°C, the reduction time is 1.5h, the molar ratio of cobalt-rhenium mixed powder to boron powder is 6:1; the ball-to-material ratio is 5:1, the ball milling speed is 300r / min, and the ball milling time is 8h; the calcination temperature is 1100°C, and the calcination time is 1h.
[0058] S4. Mix the ultrafine WC powder and cobalt-rhenium-boron ternary boride and then ball-mill them. The mass ratio of the ultrafine WC powder and the cobalt-rhenium-boron ternary boride is 90:10, the ball-to-material ratio is 10:1, the ball-milling speed is 300 r / min, and the ball-milling time is 12 h. An ultrafine cemented carbide mixture is obtained. The mixture is then pressed and sintered. The sintering temperature is 1410°C and the sintering time is 1.0 h. Ultrafine cemented carbide is obtained.
[0059] The photo of the ultrafine cemented carbide prepared in this example is shown in Figure 1 As shown, it can be seen that the ultrafine cemented carbide prepared in this embodiment is uniform, has no inclusions, and has no voids, and its hardness HV20 is 2011kg / mm 2 , crack toughness Kic is 9.0MPa·m 1 / 2 The average grain size is 0.25μm, and the porosity in the metallographic microstructure of ultrafine cemented carbide is A02B00.
[0060] Example 2
[0061] A method for preparing ultrafine cemented carbide comprises the following steps:
[0062] S1. Dissolve ammonium metatungstate, vanadium oxalate and chromium acetate in deionized water, and then spray dry to obtain an ultrafine powder precursor; according to the mass ratio of WC:V:Cr in the ultrafine WC powder of 99.0:0.5:0.5, take ammonium metatungstate, vanadium oxalate and chromium acetate;
[0063] S2. The ultrafine powder precursor is calcined and then reduced and carbonized by hydrogen, and then crushed and sieved to obtain ultrafine WC powder; the calcination temperature is 600°C, the calcination time is 2.0h, the hydrogen flow rate is 5L / min, the carbonization temperature is 1300°C, and the carbonization time is 2h.
[0064] S3. Dissolve cobalt acetate and ammonium perrhenate in water, dry and reduce with hydrogen to obtain a cobalt-rhenium mixed powder, ball-mill the cobalt-rhenium mixed powder and boron powder to obtain a mixed powder, calcine the mixed powder under argon protection to obtain a mixed powder, and crush and sieve to obtain an ultrafine cobalt-rhenium-boron ternary boride; the mass ratio of rhenium to cobalt in ammonium perrhenate and cobalt acetate is 1.5:100; the reduction temperature is 500°C, the reduction time is 1.5h, and the molar ratio of the cobalt-rhenium mixed powder to the boron powder is 5:1; the ball-to-material ratio is 8:1, the ball milling speed is 300r / min, and the ball milling time is 8h; the calcination temperature is 1100°C, and the calcination time is 1h.
[0065] S4. Mix the ultrafine WC powder and cobalt-rhenium-boron ternary boride and then ball-mill them. The mass ratio of the ultrafine WC powder and the cobalt-rhenium-boron ternary boride is 94:6, the ball-to-material ratio is 10:1, the ball-milling speed is 300 r / min, and the ball-milling time is 12 h. An ultrafine cemented carbide mixture is obtained. The mixture is then pressed and sintered. The sintering temperature is 1410°C and the sintering time is 1.0 h. Ultrafine cemented carbide is obtained.
[0066] The ultrafine cemented carbide prepared in this embodiment is uniform, has no inclusions, and has no voids. Its hardness HV20 is 2030kg / mm 2 , crack toughness Kic is 8.6MPa·m 1 / 2 The average grain size is 0.23μm, and the porosity in the metallographic microstructure of ultrafine cemented carbide is A02B00.
[0067] Comparative Example 1
[0068] The difference from Example 1 is that steps S1-S2 are not performed and ordinary WC powder is used.
[0069] The ultrafine cemented carbide prepared in this comparative example has coarse grains and coarse inclusions, and has low performance. Its hardness HV20 is 1998kg / mm 2 , crack toughness Kic is 7.8MPa·m 1 / 2The average grain size is 0.36μm. In the metallographic microstructure of ultrafine cemented carbide, the porosity is A02B00, and there are many 2~5μm inclusions.
[0070] Comparative Example 2
[0071] The difference from Example 1 is that ordinary WC powder is ball-milled with cobalt powder, rhenium powder and boron powder in the same proportion as in Example 1, with a ball-to-material ratio of 10:1, and the ball milling is carried out for 12 hours to obtain a cemented carbide mixture, which is then pressed and sintered at a sintering temperature of 1410°C and a sintering time of 1.0 hour to obtain ultrafine cemented carbide.
[0072] The photo of the ultrafine cemented carbide prepared in this comparative example is shown in Figure 2 As shown, it can be seen that the ultrafine cemented carbide prepared in this comparative example has more pores and more coarse inclusions, and its hardness HV20 is 1897kg / mm 2 , crack toughness Kic is 7.3MPa·m 1 / 2 The average grain size is 0.48μm. In the metallographic microstructure of ultrafine cemented carbide, the porosity is A06B02, with many 2~5μm inclusions and individual 6~8μm inclusions.
[0073] Comparative Example 3
[0074] The difference from Example 1 is that the ultrafine WC powder obtained in step S2 is ball-milled with cobalt powder, rhenium powder and boron powder in the same proportion as in Example 1, with a ball-to-material ratio of 10:1, and the ball milling is performed for 12 hours to obtain a cemented carbide mixture, which is then pressed and sintered at a sintering temperature of 1410°C and a sintering time of 1.0 hour to obtain an ultrafine cemented carbide.
[0075] The hard alloy prepared in this comparative example has pores and its hardness HV20 is 1985kg / mm 2 , crack toughness Kic is 7.5MPa·m 1 / 2 The average grain size is 0.30μm, and the porosity in the metallographic microstructure of ultrafine cemented carbide is A04B02.
[0076] Comparative Example 4
[0077] The difference from Example 1 is that the ultrafine WC powder obtained in step S2 is ball-milled with cobalt powder and rhenium powder in the same proportion as in Example 1, with a ball-to-material ratio of 10:1, and the ball milling is performed for 12 hours to obtain a cemented carbide mixture, which is then pressed and sintered at a sintering temperature of 1410°C and a sintering time of 1.0 hour to obtain an ultrafine cemented carbide.
[0078] The hard alloy prepared in this comparative example has more pores and lower performance. Its hardness HV20 is 1905kg / mm 2 , crack toughness Kic is 7.6MPa·m1 / 2 The average grain size is 0.33μm, and the porosity in the metallographic microstructure of ultrafine cemented carbide is A04B00.
[0079] Comparative Example 5
[0080] The difference from Example 1 is that no boron powder is added in step S3.
[0081] The ultrafine cemented carbide prepared in this comparative example has low hardness, pores and inclusions, and its hardness HV20 is 1968kg / mm 2 , crack toughness Kic is 7.0MPa·m 1 / 2 The average grain size is 0.42μm. In the metallographic microstructure of ultrafine cemented carbide, the porosity is A04B02, and some are 2~4μm coarse.
[0082] Comparative Example 6
[0083] The difference from Example 1 is that the ultrafine WC powder obtained in step S2 is ball-milled with cobalt powder and boron powder in the same proportion as in Example 1, with a ball-to-material ratio of 10:1, and the ball milling is performed for 12 hours to obtain a cemented carbide mixture, which is then pressed and sintered at a sintering temperature of 1410°C and a sintering time of 1.0 hour to obtain an ultrafine cemented carbide.
[0084] The ultrafine cemented carbide prepared in this comparative example has coarser grains and lower hardness. Its hardness HV20 is 1929kg / mm 2 , crack toughness Kic is 7.1MPa·m 1 / 2 The average grain size is 0.35μm, and the porosity in the metallographic microstructure of ultrafine cemented carbide is A02B00.
[0085] Comparative Example 7
[0086] The difference from Example 1 is that the ultrafine WC powder and cobalt powder obtained in step S2 are ball-milled in the same ratio as in Example 1, with a ball-to-material ratio of 10:1, and the ball milling is performed for 12 hours to obtain a cemented carbide mixture, which is then pressed and sintered at a sintering temperature of 1410°C and a sintering time of 1.0 hour to obtain an ultrafine cemented carbide.
[0087] The ultrafine cemented carbide prepared in this comparative example has coarse grains and low performance. Its hardness HV20 is 1889kg / mm 2 , crack toughness Kic is 7.0MPa·m 1 / 2 The average grain size is 0.44μm. In the metallographic microstructure of ultrafine cemented carbide, the porosity is A02B00, with most of the 2~4μm inclusions.
[0088] It can be seen from the above examples and comparative examples that the present invention prepares ultrafine WC powder by liquid-liquid doping, so that the inhibitor is evenly distributed in the ultrafine WC powder, and then combined with the binder to prepare cobalt-rhenium-boron ternary boride, the grains are further refined by the rhenium effect that occurs during sintering. Through the dual strengthening of the hard phase and the binder phase, a stable ultrafine-grained cemented carbide is obtained; the ultrafine cemented carbide is uniform, has no inclusions, and has no voids, and its hardness HV20 ≥ 2000kg / mm 2 , crack toughness Kic ≥ 8.5MPa·m 1 / 2 The average grain size is ≤0.25μm, and the porosity in the metallographic microstructure is A02B00.
[0089] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A method for preparing ultrafine cemented carbide, characterized in that: The steps include: S1. Dissolve ammonium metatungstate, vanadium oxalate and chromium acetate in deionized water, and then spray dry to obtain an ultrafine powder precursor; according to the mass ratio of WC:V:Cr in the ultrafine WC powder (98.7~99.2):(0.3~0.5):(0.5~0.8), take ammonium metatungstate, vanadium oxalate and chromium acetate; S2, the ultrafine powder precursor is calcined and then reduced and carbonized by hydrogen, and then crushed and sieved to obtain ultrafine WC powder; S3, dissolving cobalt acetate and ammonium perrhenate in water, drying and reducing with hydrogen to obtain a cobalt-rhenium mixed powder, ball-milling the cobalt-rhenium mixed powder and boron powder to obtain a mixed powder, calcining the mixed powder under argon protection to obtain a mixed powder, crushing and sieving to obtain ultrafine cobalt-rhenium-boron ternary boride; the mass ratio of rhenium to cobalt in ammonium perrhenate and cobalt acetate is (1-2):100; the molar ratio of the cobalt-rhenium mixed powder to the boron powder is (3-6):1; S4. The ultrafine WC powder and the cobalt-rhenium-boron ternary boride are mixed and ball-milled, wherein the mass ratio of the ultrafine WC powder and the cobalt-rhenium-boron ternary boride is (90-94):(6-10), to obtain an ultrafine cemented carbide mixture, which is then pressed and sintered to obtain an ultrafine cemented carbide, wherein the grain size of the ultrafine cemented carbide is ≤0.25 μm.
2. The method for preparing ultrafine cemented carbide according to claim 1, characterized in that: In the step S2, the calcination temperature is 590-610°C, and the calcination time is 1.5-2.5 hours; the hydrogen flow rate is 3-5 L / min, the carbonization temperature is 1200-1300°C, and the carbonization time is 2-4 hours.
3. The method for preparing ultrafine cemented carbide according to claim 1, characterized in that: In step S3, the reduction temperature is 480-520° C., and the reduction time is 1-2 hours; the calcination temperature is 1050-1150° C., and the calcination time is 1-2 hours.
4. The method for preparing ultrafine cemented carbide according to claim 1, characterized in that: In step S3, the ball-to-material ratio is (5-8):1, the ball milling speed is 280-320 r / min, and the ball milling time is 7-9 h.
5. The method for preparing ultrafine cemented carbide according to claim 1, characterized in that: In the step S4, the ball-to-material ratio is (8-12):1, the ball milling speed is 280-320 r / min, and the ball milling time is 10-15 h; the sintering temperature is 1400-1420° C., and the sintering time is 0.5-1.5 h.
6. An ultrafine cemented carbide, characterized in that: The ultrafine cemented carbide is prepared by the preparation method of any one of claims 1 to 5.
7. The ultrafine cemented carbide according to claim 6, characterized in that: The hardness of the ultrafine cemented carbide is HV20≥2000kg / mm 2 , crack toughness Kic ≥ 8.5MPa·m 1 / 2 , grain size ≤ 0.25μm, and the porosity in the metallographic microstructure of ultrafine cemented carbide is A02B00.