A method for promoting calcium nitrate crystallization in nitric acid decomposition phosphate ore process
Patent Information
- Application Number
- CN202411125653.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-08-16
Smart Images

Figure CN118637656B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of phosphate rock decomposition by nitric acid method, and particularly relates to a method for promoting calcium nitrate crystallization in the process of phosphate rock decomposition by nitric acid. Background Art
[0002] Phosphate rock is the raw material for phosphoric acid production. It is a non-renewable mineral resource with the main component of Ca5F(PO4)3. There are two methods for producing phosphoric acid, thermal method and wet method. The thermal phosphoric acid production process mainly involves burning yellow phosphorus obtained by the electric heating method in excess air to produce phosphoric acid, which has the disadvantages of high production energy consumption and serious impact on the environment. The wet phosphoric acid production process mainly involves decomposing phosphate rock with various inorganic acids to produce phosphoric acid, and its main inorganic acids include sulfuric acid, hydrochloric acid, and nitric acid. Among them, the sulfuric acid method is the most commonly used method at present, accounting for more than 80% of the total phosphoric acid production. However, the raw material sulfur used in this method is as high as 68% dependent on foreign countries, resulting in high production costs for enterprises. In addition, the production of 1 ton of sulfuric acid will produce 5 tons of phosphogypsum as a by-product. The accumulation of phosphorus and fluorine impurities in the produced gypsum is extremely harmful to the environment, and there is no effective comprehensive utilization method.
[0003]
[0004] The process of using hydrochloric acid to activate phosphate rock to produce phosphoric acid and calcium chloride is called the hydrochloric acid method. The main components of the acid solution are phosphoric acid, calcium chloride and a small amount of impurity ions. Calcium chloride must be removed from the system to obtain relatively pure phosphoric acid. In the 1960s, Israeli mining companies developed the IMI method using n-butanol and isoamyl alcohol as extractants to separate phosphoric acid and calcium chloride from the acid solution. However, the extractants (n-butanol and isoamyl alcohol) used in this method are low-carbon alcohols and are slightly soluble in water. In the process of recovering and purifying phosphoric acid and dissolving the extractant in the residual calcium chloride brine, a large amount of heat is consumed. If the recovery is incomplete, it will not only cause great economic losses, but also cause major environmental pollution. In addition, the extractant has a low flash point and is volatile, which is a safety hazard that is difficult to handle properly during operation. The latest literature reports the use of low-solubility, high-boiling-point, high-flash-point, non-volatile ketones, sulfones, and phosphate extractants to replace the above-mentioned low-carbon alcohols. However, this still brings some new problems such as high phosphorus loss rate and difficulty in phase separation. In addition to the problems that are difficult to solve, such as the low added value of the by-product calcium chloride, the small market demand, and the serious corrosion of chloride ions to equipment, this method is rarely used in industry.
[0005]
[0006] The process of using nitric acid to decompose phosphate rock to produce phosphoric acid and calcium nitrate is called the nitric acid method. This method has the advantages of fast decomposition speed and no production of phosphogypsum. The nitric acid method is usually used directly to produce nitrophosphate fertilizer, and its product is a highly efficient compound fertilizer. The nitric acid method was first proposed by Russian scholars in 1908. Twenty years later, the Norwegian Oda Company proposed a method of separating calcium nitrate by freezing crystallization. In 1936, it was first industrialized by Norwegian Hydro. Later, due to raw material problems, the method was improved and ammonia and carbon dioxide were used to neutralize the frozen mother liquor. According to the different methods of removing calcium ions in the acid hydrolysis mother liquor, the nitric acid method can be mainly divided into carbonization method, mixed acid method and freezing method.
[0007]
[0008] Among them, the freezing method is widely used. This method is a method of precipitating calcium nitrate by reducing the solubility of calcium nitrate in the acid hydrolysis solution by cooling. This method does not require the addition of chemicals in the entire process and can effectively control the calcium-phosphorus ratio in the mother liquor, which is conducive to the subsequent processing and utilization of the acid hydrolysis solution. At present, the calcium removal rate of this method is about 75~80%, but if fine phosphates are to be further produced, the remaining calcium nitrate is a major obstacle. Although sulfuric acid can be used as a decalcifying agent to remove the calcium sulfate with a higher purity, the utilization of calcium sulfate is limited. If the by-product is too large, it is not conducive to the application of the technology. Therefore, a method is needed to strengthen the crystallization of calcium nitrate and minimize the by-product calcium sulfate.
[0009] The prior art discloses a nitrophosphate fertilizer and a preparation method thereof, wherein part of the calcium nitrate precipitate obtained in the calcium nitrate filtering process in the production process of frozen nitrophosphate fertilizer is subjected to secondary crystallization together with part of the calcium nitrate mother liquor after filtration, followed by a neutralization process. This method can improve the crystallization rate of calcium nitrate tetrahydrate in the production process of frozen nitrophosphate fertilizer, but can only utilize 1 / 2 to 2 / 3 of the total amount of frozen mother liquor, and the temperature of the secondary crystallization is -10 to -15°C (only -5°C in one stage), the overall crystallization rate of calcium nitrate is not much improved, the energy consumption is large, and the product is still a nitrophosphate fertilizer product with low added value. The prior art also discloses a freezing method nitrophosphate fertilizer production process with adjustable nitrogen-phosphorus ratio. Based on the existing freezing method nitrophosphate fertilizer production process, an acid solution concentration process is added after the acid insoluble precipitation separation process; a calcium nitrate screening process and a calcium nitrate dehydration process are added after the calcium nitrate filtration process; calcium nitrate particles with larger particle size after the calcium nitrate screening process are sent to the calcium nitrate conversion process, and calcium nitrate particles with smaller particles after the calcium nitrate screening process enter the calcium nitrate dehydration process, and after removing the crystal water, they return to the calcium nitrate freezing crystallization process as a seed and a dehydrating agent. The amount of dehydrating agent added in this method is 20-30 wt% of the calcium nitrate particles with smaller particles, which means that the amount of calcium nitrate added can only take away 0.8-1.2 molecules of crystal water equivalent to the calcium nitrate content, thereby reducing the solubility of calcium nitrate, and there is no significant improvement. And after improving the crystallization rate, the content of P2O5 in the best product is only 19%, and the product is a nitrophosphate fertilizer with low added value that can control the nitrogen-phosphorus ratio.
[0010] In the article "Discussion on the Methods of Using Freezing Method Nitrophosphate Fertilizer Process to Deal with Phosphate Ore Depletion", the feasibility of using low-grade phosphate ore to produce high-efficiency nitrophosphate fertilizer was discussed and analyzed. It was found that in order to reduce the calcium-phosphorus ratio in the mother liquor, appropriate phosphoric acid can be added to the mother liquor from which most of the calcium is removed by freezing method, so as to increase the amount of P2O5 in the solution and reduce the calcium-phosphorus ratio, so as to increase the water solubility of P2O5 in the finished product. This method adds phosphoric acid after the freezing crystallization is completed to reduce the calcium-phosphorus ratio, and the product is still a low-value-added nitrophosphate fertilizer.
[0011] It can be seen that in the current freezing method nitrophosphate fertilizer production process, although most of the calcium nitrate (about 75-80%) in the acid solution is separated in the form of Ca(NO3)2·4H2O crystals after the freezing crystallization and calcium nitrate separation process, the mother liquor still contains a certain amount of calcium nitrate, magnesium nitrate, iron nitrate, and aluminum nitrate. In the mother liquor ammonia neutralization process, the presence of excessive calcium elements will lead to the formation of monocalcium phosphate and dicalcium phosphate in the neutralization process, which will further affect the change of the slurry viscosity value, especially when it coexists with impurities such as magnesium and fluorine. The impact is even greater, and the viscosity of the neutralized slurry rises sharply, which brings great difficulties to the neutralization operation, hinders the diffusion of ammonia under stirring, and the smooth flow of slurry in the channels and pipes of the equipment system, and even reaches the point where it cannot be operated, causing the system to be forced to stop, bringing huge economic losses to the factory. In addition, the excessive presence of calcium will cause some P2O5 to combine with calcium to form insoluble phosphates (tricalcium phosphate and calcium fluorophosphate) during the neutralization process, causing some soluble phosphorus products to degenerate into insoluble phosphates, thereby affecting the water solubility of phosphorus in the final product and the utilization rate of phosphorus in the process. At the same time, the degraded phosphorus is difficult to be absorbed by plants, resulting in a certain amount of resource waste. Summary of the invention
[0012] In view of the above-mentioned prior art, the present invention provides a method for promoting the crystallization of calcium nitrate in the process of nitric acid decomposition of phosphate rock, which solves the problem that the calcium nitrate freezing crystallization rate in the existing nitric acid decomposition of phosphate rock technology is low and is not suitable for subsequent industrial technology development.
[0013] In order to achieve the above object, the technical solution adopted by the present invention is: to provide a method for promoting the crystallization of calcium nitrate in the process of nitric acid decomposition of phosphate ore, comprising the following steps:
[0014] S1: Phosphate ore is hydrolyzed with nitric acid, followed by solid-liquid separation to obtain acid-insoluble matter and acid hydrolyzate;
[0015] S2: evaporating and concentrating the acid hydrolyzate until the phosphorus concentration is 20-30 wt.% in terms of H3PO4 to obtain a concentrated solution;
[0016] S3: adding concentrated phosphoric acid to the concentrated solution until the phosphorus concentration is 30-35 wt.% in terms of H3PO4, followed by freezing and crystallization, and separation to obtain a crystallization mother liquor and calcium nitrate precipitate;
[0017] The freezing crystallization process is: crystallization temperature is -5~-15 ℃, and crystallization time is 3~6 h.
[0018] The beneficial effects of the present invention are as follows: the method provided by the present invention uses concentrated phosphoric acid as an additive, which is added to a freezing crystallization process. During concentration, the phosphorus concentration is not directly concentrated to 30-35 wt.% in terms of H3PO4, but concentrated phosphoric acid is added to reduce the salt content in the system, reduce the viscosity of the concentrated solution, utilize high-concentration phosphoric acid to reduce the solubility of calcium nitrate tetrahydrate in a nitric acid-phosphoric acid-water system, thereby increasing the precipitation rate of calcium nitrate, and reduce the calcium ion content in the freezing crystallization mother liquor during freeze decalcification, thereby reducing the amount of sulfuric acid used in the subsequent deep decalcification process, reducing the by-product calcium sulfate, and reducing the calcium ion content brought into the freezing mother liquor from the source.
[0019] Based on the above technical solution, the present invention can also be improved as follows.
[0020] Furthermore, the concentration of nitric acid is 60-65 wt %.
[0021] Further, the nitric acid used in S1 is prepared by the following steps:
[0022] The calcium nitrate precipitate obtained by S3 is subjected to high-temperature decomposition, and the gas generated by the decomposition is reacted with water to obtain the product.
[0023] Furthermore, the temperature of the high temperature decomposition is 560~600 °C.
[0024] The beneficial effect of adopting further technical solutions is that the obtained nitric acid can be recycled, which greatly improves the economic efficiency of the technology. At the same time, the by-product calcium oxide obtained has high value and a wide range of utilization methods, which is conducive to the promotion and application of the technology.
[0025] Furthermore, the concentration of concentrated phosphoric acid is 65-85 wt %.
[0026] Further, concentrated phosphoric acid is prepared by the following steps:
[0027] The crystallization mother liquor is mixed with sulfuric acid for reaction, filtered, and the filtrate is concentrated to a phosphoric acid content of 65-85wt%.
[0028] Further, the concentration of sulfuric acid is 98%, and the volume ratio of sulfuric acid to the crystallization mother liquor is 1:10.
[0029] Further, the nitric acid used in S1 is prepared by the following steps:
[0030] The steam generated when the filtrate is concentrated is collected and condensed into liquid to obtain the product.
[0031] The beneficial effects of the present invention are that the obtained nitric acid and phosphoric acid can be recycled, thereby improving the economic efficiency of the technology, being conducive to the popularization and application of the technology, and having excellent industrial prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a process flow chart of calcium nitrate crystallization of the present invention;
[0033] Among them, 1. acid hydrolysis, 2. filtration, 3. concentration, 4. frozen crystallization, 5. concentration, 6. filtration, 7. decalcification, 8. filtration, 9. pyrolysis, 10. hydration, 11. nitric acid, 12. phosphate rock, 13. acid insoluble matter, 14. concentrated phosphoric acid, 15. concentrated phosphoric acid, 16. calcium sulfate, 17. sulfuric acid, 18. nitrogen oxides, and 19. calcium oxide. DETAILED DESCRIPTION
[0034] The specific implementation modes of the present invention are described in detail below with reference to the embodiments.
[0035] Example 1
[0036] A method for promoting the crystallization of calcium nitrate in the process of nitric acid decomposition of phosphate rock, the process flow is as follows Figure 1 As shown, the following steps are included:
[0037] S1: Add 62 wt% nitric acid to the phosphate rock for acid hydrolysis (the amount of nitric acid used is 110% of the mass of the phosphate rock), and then separate the solid and liquid to obtain acid insoluble matter and acid hydrolysis solution; the nitric acid used is prepared by the following steps:
[0038] The calcium nitrate precipitate obtained by subsequent separation is subjected to high temperature decomposition at 580°C to obtain calcium oxide and nitrogen dioxide, and the nitrogen dioxide is reacted with water to obtain nitric acid;
[0039] The acid solution is composed of:
[0040] H3PO410.07wt%, N 9.69wt%, CaO 10.68wt%, Fe2O30.43wt%, Al2O30.68wt%, MgO0.21wt%, F 0.53wt%, SiO20.15wt%;
[0041] S2: evaporating and concentrating the acid hydrolyzate until the phosphorus concentration is 20 wt.% in terms of H3PO4 to obtain a concentrated solution;
[0042] S3: Add 85 wt% concentrated phosphoric acid to the concentrated solution until the phosphorus concentration is 30 wt.% in terms of H3PO4, and then freeze and crystallize at -10 °C for 5 h. After the crystallization is completed, separate the crystallization mother liquor and calcium nitrate precipitate; the concentrated phosphoric acid used is prepared by the following steps:
[0043] The obtained crystallization mother liquor is mixed with sulfuric acid for reaction, filtered, and the liquid is evaporated and concentrated to obtain phosphoric acid, which is used in step S3. The gas during evaporation and concentration is condensed to obtain nitric acid, which is then used in step S1.
[0044] Example 2
[0045] The freezing crystallization temperature in S3 of Example 1 was adjusted to -5°C, and the remaining operations were the same as in Example 1.
[0046] Example 3
[0047] The freezing crystallization temperature in S3 of Example 1 was adjusted to -15°C, and the remaining operations were the same as in Example 1.
[0048] Example 4
[0049] A method for promoting the crystallization of calcium nitrate in the process of nitric acid decomposition of phosphate rock, the process flow is as follows Figure 1 As shown, the following steps are included:
[0050] S1: Add 60 wt% nitric acid to the phosphate rock for acid hydrolysis (the amount of nitric acid used is 110% of the mass of the phosphate rock), and then separate the solid and liquid to obtain acid insoluble matter and acid hydrolysis solution; the nitric acid used is prepared by the following steps:
[0051] The calcium nitrate precipitate obtained by subsequent separation is subjected to high temperature decomposition at 600°C to obtain calcium oxide and nitrogen dioxide, and the nitrogen dioxide is reacted with water to obtain nitric acid;
[0052] The acid solution is composed of:
[0053] H3PO410.07wt%, N 9.69wt%, CaO 10.68wt%, Fe2O30.43wt%, Al2O30.68wt%, MgO0.21wt%, F 0.53wt%, SiO20.15wt%;
[0054] S2: evaporating and concentrating the acid hydrolyzate to a phosphorus concentration of 30 wt.% in terms of H3PO4 to obtain a concentrated solution;
[0055] S3: Add 65 wt% concentrated phosphoric acid to the concentrated solution until the phosphorus concentration is 35 wt.% in terms of H3PO4, and then freeze and crystallize at -10 °C for 3 h. After the crystallization is completed, separate the crystallization mother liquor and calcium nitrate precipitate; the concentrated phosphoric acid used is prepared by the following steps:
[0056] The obtained crystallization mother liquor is mixed with sulfuric acid for reaction, filtered, and the liquid is evaporated and concentrated to obtain phosphoric acid, which is used in step S3. The gas during evaporation and concentration is condensed to obtain nitric acid, which is then used in step S1.
[0057] Example 5
[0058] The freezing crystallization temperature in S3 of Example 4 was adjusted to -5°C, and the remaining operations were the same as in Example 4.
[0059] Example 6
[0060] The freezing crystallization temperature in S3 of Example 4 was adjusted to -15°C, and the remaining operations were the same as in Example 4.
[0061] Comparative Example 1
[0062] A method for crystallizing calcium nitrate, comprising the following steps:
[0063] S1: Add 65 wt% nitric acid to the phosphate rock for acid hydrolysis (the amount of nitric acid used is 110% of the mass of the phosphate rock), and then separate the solid and liquid to obtain acid insoluble matter and acid hydrolysis solution; the nitric acid used is prepared by the following steps:
[0064] The calcium nitrate precipitate obtained by subsequent separation is subjected to high temperature decomposition at 560°C to obtain calcium oxide and nitrogen dioxide, and the nitrogen dioxide is reacted with water to obtain nitric acid;
[0065] The acid solution is composed of:
[0066] H3PO410.07wt%, N 9.69wt%, CaO 10.68wt%, Fe2O30.43wt%, Al2O30.68wt%, MgO0.21wt%, F 0.53wt%, SiO20.15wt%;
[0067] S2: evaporating and concentrating the acid hydrolyzate until the phosphorus concentration is 20 wt.% in terms of H3PO4 to obtain a concentrated solution;
[0068] S3: Freeze the concentrated solution at -10 °C for crystallization for 6 h. After the crystallization is completed, separate the crystallization mother liquor and calcium nitrate precipitate.
[0069] In this comparative example, the obtained crystallization mother liquor is mixed with sulfuric acid for reaction, filtered, and the liquid is evaporated and concentrated to obtain phosphoric acid. The gas during evaporation and concentration is condensed to obtain nitric acid, and the obtained nitric acid is reused in step S1.
[0070] Comparative Example 2
[0071] The freezing crystallization temperature in S3 of Comparative Example 1 was adjusted to -5°C, and the remaining operations were the same as those of Comparative Example 1.
[0072] Comparative Example 3
[0073] The freezing crystallization temperature in S3 of Comparative Example 1 was adjusted to -15°C, and the remaining operations were the same as those of Comparative Example 1.
[0074] Experimental example
[0075] Crystallization rate experiment: The calcium ion content of the mother liquor of Examples 1 to 6 and Comparative Examples 1 to 3 before and after freezing was measured by inductively coupled plasma emission spectrometry (ICP), and the difference divided by the original value was the crystallization rate. The results are shown in Table 1.
[0076] Table 1 Crystallization rate statistics of Examples 1 to 6 and Comparative Examples 1 to 3
[0077]
[0078] In summary, increasing the phosphoric acid concentration in the concentrated solution can strengthen the crystallization of calcium nitrate and increase the crystallization rate of calcium nitrate frozen crystallization. At the same time, lowering the crystallization temperature can also increase the crystallization rate of calcium nitrate frozen crystallization.
[0079] Although the specific implementation of the present invention is described in detail in conjunction with the embodiments, it should not be understood as limiting the scope of protection of this patent. Within the scope described in the claims, various modifications and variations that can be made by those skilled in the art without creative work still fall within the scope of protection of this patent.
Claims
1. A method for promoting the crystallization of calcium nitrate in a nitric acid decomposition phosphate rock process, characterized in that: The following steps are involved: S1: Phosphate ore is hydrolyzed with nitric acid, followed by solid-liquid separation to obtain acid-insoluble matter and acid hydrolyzate; S2: evaporating and concentrating the acid hydrolyzate until the phosphorus concentration is 20-30 wt.% in terms of H3PO4 to obtain a concentrated solution; S3: adding concentrated phosphoric acid to the concentrated solution until the phosphorus concentration is 30-35 wt.% in terms of H3PO4, followed by freezing and crystallization, and separation to obtain a crystallization mother liquor and calcium nitrate precipitate; The freezing crystallization process is as follows: the crystallization temperature is -5 to -15 °C and the crystallization time is 3 to 6 h.
2. The method for promoting calcium nitrate crystallization in the process of nitric acid decomposition of phosphate rock according to claim 1, characterized in that: The nitric acid concentration is 60-65 wt %.
3. The method for promoting calcium nitrate crystallization in the process of nitric acid decomposition of phosphate rock according to claim 1, characterized in that: The nitric acid used in S1 is prepared by the following steps: The calcium nitrate precipitate obtained by S3 is subjected to high-temperature decomposition, and the gas generated by the decomposition is reacted with water to obtain the product.
4. The method for promoting calcium nitrate crystallization in the process of nitric acid decomposition of phosphate rock according to claim 3, characterized in that: The temperature of the high temperature decomposition is 560-600°C.
5. The method for promoting calcium nitrate crystallization in the process of nitric acid decomposition of phosphate rock according to claim 1, characterized in that: The concentration of the concentrated phosphoric acid is 65-85 wt %.
6. The method for promoting calcium nitrate crystallization in the process of nitric acid decomposition of phosphate rock according to claim 1, characterized in that: The concentrated phosphoric acid is prepared by the following steps: The crystallization mother liquor is mixed with sulfuric acid for reaction, filtered, and the filtrate is concentrated to a phosphoric acid content of 65-85 wt %.
7. The method for promoting calcium nitrate crystallization in the process of nitric acid decomposition of phosphate rock according to claim 6, characterized in that: The concentration of the sulfuric acid is 98%, and the volume ratio of the sulfuric acid to the crystallization mother liquor is 1:
10.
8. The method for promoting calcium nitrate crystallization in the process of nitric acid decomposition of phosphate rock according to claim 6, characterized in that: The nitric acid used in S1 is prepared by the following steps: The steam generated when the filtrate is concentrated is collected and condensed into liquid to obtain the product.
Citation Information
Patent Citations
Method for producing nitric phosphate fertilizer at low temperature under vacuum through concentrated crystallization and calcium removal as well asdevice
CN102584386A
Method for producing water-soluble calcium nitrate dihydrate and phosphoric acid by decomposing phosphorite through nitric acid
CN103073041A
Method for preparing compound fertilizer from phosphate ore acidolysis solution and compound fertilizer
CN109279939A
Technology for producing nitrophosphate fertilizer by freezing method with adjustable nitrogen-phosphorus ratio
CN114524684A
Method for preparing phosphoric acid and byproduct fertilizer by using nitrophosphate fertilizer freezing process
CN114572952A