A method for preparing ammonium paratungstate using wolframite concentrate

Through high-temperature roasting and acid leaching, combined with ammonia dissolution and evaporation crystallization processes, the problems of potassium element exceeding the standard and wastewater discharge in the preparation of ammonium paratungstenate in black tungsten concentrate are solved, and a low-cost and low-pollution production process is achieved, which is in line with the National standards.

CN118637662BActive Publication Date: 2024-11-08CHONGYI ZHANGYUAN TUNGSTEN
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411114870.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-08
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

In the existing tungsten smelting process, there are problems of high-salt wastewater discharge and potassium element exceeding the standard in the preparation of ammonium paratungstate in black tungsten concentrate, resulting in high production costs and serious environmental pollution.

Method used

After high-temperature roasting of black tungsten concentrate, wet grinding and acid leaching are carried out. Through ammonia dissolution, purification and decomposition and evaporation crystallization processes, ammonium paratungstate products with a potassium content of 1~10mg/kg are prepared.

Benefits of technology

It effectively reduces wastewater discharge, reduces waste slag production, realizes effective removal of potassium, complies with the national zero-level standard, and eliminates roasting additives, improving resource utilization and production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention belongs to the technical field of tungsten smelting, and specifically relates to a method for preparing ammonium paratungstate by using wolframite concentrate, wherein the wolframite concentrate is directly activated by high-temperature roasting, and after roasting, potassium is converted into potassium oxide and potassium sulfate which are easy to be leached, and then ball milling is performed, and the wolframite concentrate is leached by acid to prepare solid tungstic acid, and the tungstic acid can be prepared into an ammonium paratungstate product which meets the national zero-grade standard through the steps of washing, ammonia dissolution, purification and impurity removal of ammonium tungstate solution, evaporation and crystallization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of tungsten smelting, and specifically relates to a method for preparing ammonium paratungstate by using wolframite concentrate. Background Art

[0002] In the tungsten smelting process, wolframite concentrate is mainly decomposed by sodium hydroxide. The obtained sodium tungstate solution is filtered and diluted, and then P, As, Si and cationic impurities are removed by strong alkaline anion exchange. The saturated resin loaded with tungsten is desorbed, transformed and enriched with NH4Cl and NH4OH to obtain a pure high-concentration (NH4)2WO4 solution, which is then evaporated and crystallized to produce ammonium paratungstate products after deep Mo removal. The ion exchange process is widely used in the tungsten industry because of its stable process, adaptability to various complex mines and high tungsten recovery rate. However, since 2016, alkali decomposition of tungsten smelting slag has been listed as hazardous waste. It is stipulated that alkali decomposition of tungsten smelting slag must be harmlessly treated, and there are more alkali decomposition slags in wolframite concentrate, which will inevitably increase the smelting cost of tungsten smelting enterprises. The harmless treatment of black tungsten alkali boiled slag is generally to leach the alkali boiled slag with hydrochloric acid, and then separate and recover other valuable metals such as Fe, Mn, Ta, Nb in the acid decomposition solution by neutralization precipitation, extraction and other methods. At the same time, the technology of preparing ammonium paratungstate by ion exchange process from wolframite concentrate is limited by the ion exchange principle and process. + and Cl -There is no closed-loop circulation and no economically feasible precipitation or membrane separation method. Therefore, 80~100m³ of high-salt wastewater will be discharged for every ton of ammonium paratungstate product produced. How to treat wolframite concentrate with low cost, low pollution and low wastewater is the technical development direction of the current tungsten industry and has very important practical significance. Many experts in the industry have proposed to use hydrochloric acid to decompose wolframite concentrate to prepare solid tungstic acid and waste acid liquid, and then obtain ammonium tungstate solution after tungstic acid is dissolved in ammonia, and then obtain pure ammonium tungstate solution after impurity removal, and finally prepare ammonium paratungstate product after evaporation and crystallization. Although this process has the advantages of short process flow, less wastewater generation, less waste residue, and low production cost, the K element in the final ammonium paratungstate product exceeds the standard. Therefore, how to effectively remove the K element becomes the key technical problem of this process. The Chinese patent with the announcement number CN115679127B proposes to roast tungsten concentrate in an atmosphere containing acidic gas to obtain roasted clinker, and then the roasted clinker is leached with hydrochloric acid to remove impurities, and then successively subjected to ammonia dissolution, fine impurity removal and evaporation crystallization to obtain qualified APT products. The Chinese patent application with the publication number CN114956181A proposes to roast scheelite with waste acid, and then leached with water to remove potassium. The scheelite acid after leaching is decomposed to obtain crude tungstic acid, and the crude tungstic acid is subjected to ammonia dissolution-purification and impurity removal-evaporation crystallization process to obtain a national standard zero-grade ammonium paratungstate product. Although the above methods realize the short-process smelting of tungsten concentrate, since the auxiliary agents used in the roasting process are all acidic reagents, there are problems such as severe equipment corrosion, difficulty in treating roasting tail gas, and greater environmental pollution during the roasting process. Summary of the invention

[0003] In order to solve the problems existing in the prior art, the main purpose of the present invention is to provide a method for preparing ammonium paratungstate using wolframite concentrate.

[0004] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:

[0005] A method for preparing ammonium paratungstate using wolframite concentrate comprises the following steps:

[0006] S1. Place the wolframite concentrate in a high-temperature tubular furnace and roast it with air;

[0007] S2, placing the roasted wolframite concentrate in a ball mill for wet grinding to obtain ore slurry;

[0008] S3, adding acid to the ore pulp for acid leaching, and then filtering and washing to obtain tungstic acid;

[0009] S4. After tungstic acid is subjected to ammonia dissolution-purification and impurity removal-evaporation crystallization process, ammonium paratungstate is obtained, and the potassium element in the ammonium paratungstate is 1~10mg / kg.

[0010] As a preferred embodiment of the method for preparing ammonium paratungstate from wolframite concentrate described in the present invention, wherein: in the step S1, the roasting temperature is 1100-1300°C, and the roasting time is 0.5-2.0h.

[0011] As a preferred embodiment of the method for preparing ammonium paratungstate using wolframite concentrate described in the present invention, wherein: in the step S1, the air flow rate is 20-100 L / h.

[0012] As a preferred embodiment of the method for preparing ammonium paratungstate using wolframite concentrate described in the present invention, in the step S2, 40-50wt% of water based on the mass of the roasted wolframite concentrate is added for wet grinding.

[0013] As a preferred embodiment of the method for preparing ammonium paratungstate using wolframite concentrate described in the present invention, wherein: in the step S2, the wet grinding time is 4 to 8 hours.

[0014] As a preferred embodiment of the method for preparing ammonium paratungstate using wolframite concentrate described in the present invention, in step S3, the acid is hydrochloric acid or sulfuric acid, the concentration of hydrochloric acid is 31wt%, and the concentration of sulfuric acid is 15wt%.

[0015] As a preferred embodiment of the method for preparing ammonium paratungstate using wolframite concentrate described in the present invention, wherein: in the step S3, the liquid-to-solid ratio after adding the acid is (2-3):1.

[0016] As a preferred embodiment of the method for preparing ammonium paratungstate using wolframite concentrate described in the present invention, wherein: in the step S3, the acid leaching temperature is 60-90° C., and the acid leaching time is 2-3 hours.

[0017] The beneficial effects of the present invention are as follows:

[0018] The invention provides a method for preparing ammonium paratungstate by using wolframite concentrate, wherein the wolframite concentrate is directly activated by high-temperature roasting, after which potassium is converted into potassium oxide and potassium sulfate which are easily leached, and then ball milling is performed, and the wolframite concentrate is leached by acid to prepare solid tungstic acid, and the tungstic acid is washed, dissolved in ammonia, purified and impurity-removed by ammonium tungstate solution, evaporated and crystallized to prepare an ammonium paratungstate product that meets the national zero-grade standard (the national standard GBT10116-2007 zero-grade product requires that the potassium content in the ammonium paratungstate product is less than or equal to 10 mg / kg). DETAILED DESCRIPTION

[0019] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0020] The present invention proposes a method for preparing ammonium paratungstate using wolframite concentrate, which has the following advantages:

[0021] (1) The researchers of the present invention analyzed the components in wolframite concentrate and found that potassium in wolframite concentrate generally exists in the form of potassium mica and potassium feldspar; wolframite concentrate, potassium mica and potassium feldspar are all single crystal minerals, and wolframite concentrate mainly contains tungsten, iron, manganese, calcium, sulfur, silicon and other elements; after roasting, potassium is converted into easily leached potassium oxide and potassium sulfate. Therefore, the present invention converts wolframite concentrate into easily leached potassium oxide and potassium sulfate through aerobic roasting. At the same time, there are elements such as iron, manganese, calcium, silicon and other elements in the ore, so there is no need to add slag-making agent, and while eliminating roasting aids, there is no need to grind the ore before roasting.

[0022] (2) The wolframite concentrate is roasted in an aerobic environment, and the sulfide ores in the ore, such as ferrous sulfide and copper sulfide, are also oxidized, so that the oxidized sulfide ores can also be leached out during the acid leaching process, and the obtained tungsten acid is purer with less ammonia slag. At the same time, the sulfur dioxide gas produced can also be used as a roasting aid to continue to activate metal elements such as potassium in the ore.

[0023] (3) The acid leaching solution of the wolframite concentrate in the present invention can be further used to extract other valuable metals such as Fe, Mn, Ta, Nb, etc. by alkali neutralization or extraction, and the amount of waste slag generated is small, and the resource utilization rate is high.

[0024] According to one aspect of the present invention, the present invention provides the following technical solution:

[0025] A method for preparing ammonium paratungstate using wolframite concentrate comprises the following steps:

[0026] S1. Place the wolframite concentrate in a high-temperature tubular furnace and roast it with air;

[0027] S2, placing the roasted wolframite concentrate in a ball mill for wet grinding to obtain ore slurry;

[0028] S3, adding acid to the ore pulp for acid leaching, and then filtering and washing to obtain tungstic acid;

[0029] S4. After tungstic acid is subjected to ammonia dissolution-purification and impurity removal-evaporation crystallization process, ammonium paratungstate is obtained, and the potassium element in the ammonium paratungstate is 1~10mg / kg.

[0030] Preferably, in step S1, the calcination temperature is 1100-1300°C, and the calcination time is 0.5-2.0h. Specifically, the calcination temperature can be, for example, any one of 1100°C, 1150°C, 1200°C, 1250°C, 1300°C, or any range between two thereof.

[0031] Preferably, in step S1, the air flow rate is 20-100 L / h. Specifically, the air flow rate can be, for example, any one of 20 L / h, 30 L / h, 40 L / h, 50 L / h, 60 L / h, 70 L / h, 80 L / h, 90 L / h, 100 L / h, or a range between any two thereof.

[0032] Preferably, in step S2, 40-50 wt% of water based on the mass of the roasted wolframite concentrate is added for wet grinding.

[0033] Preferably, in step S2, the wet grinding time is 4 to 8 hours.

[0034] Preferably, in step S3, the acid is hydrochloric acid or sulfuric acid, the concentration of hydrochloric acid is 31wt%, and the concentration of sulfuric acid is 15wt%.

[0035] Preferably, in step S3, the liquid-solid ratio after adding the acid is (2-3): 1. Specifically, the liquid-solid ratio after adding the acid can be, for example, any one of 2: 1, 2.5: 1, 3: 1, or a range between any two of them.

[0036] Preferably, in step S3, the acid leaching temperature is 60-90°C, and the acid leaching time is 2-3 hours. Specifically, the acid leaching temperature can be, for example, any one of 60°C, 70°C, 80°C, 90°C, or a range between any two thereof.

[0037] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0038] The composition of the wolframite concentrate processed in each embodiment and comparative example is shown in the following table:

[0039] Example 1

[0040] A method for preparing ammonium paratungstate using wolframite concentrate comprises the following steps:

[0041] S1. Take 500g of wolframite concentrate and place it in a high-temperature tubular furnace for air roasting. The roasting temperature of the tubular furnace is set to 1200°C, the air flow rate is controlled at 40L / h, and the roasting time is 1.0h;

[0042] S2, placing the roasted wolframite concentrate in a ball mill, adding 200 mL of water and wet grinding for 6 h, and filtering to obtain a pulp;

[0043] S3, adding 1000mL of 31wt% hydrochloric acid to the slurry for acid leaching, the acid leaching temperature is 90°C and the acid leaching time is 2h, and then filtering and washing to obtain tungstic acid;

[0044] S4. After tungstic acid is subjected to ammonia dissolution-purification and impurity removal-evaporation crystallization process, ammonium paratungstate is obtained. After testing, the potassium element in the ammonium paratungstate is 2 mg / kg. Example 2

[0045] A method for preparing ammonium paratungstate using wolframite concentrate comprises the following steps:

[0046] S1. Take 500g of wolframite concentrate and place it in a high-temperature tubular furnace for air roasting. The roasting temperature of the tubular furnace is set to 1100°C, the air flow rate is controlled at 40L / h, and the roasting time is 0.5h;

[0047] S2, placing the roasted wolframite concentrate in a ball mill, adding 200 mL of water and wet grinding for 6 h, and filtering to obtain a pulp;

[0048] S3, adding 1000mL of 31wt% hydrochloric acid to the slurry for acid leaching, the acid leaching temperature is 90°C and the acid leaching time is 2h, and then filtering and washing to obtain tungstic acid;

[0049] S4. After tungstic acid is subjected to ammonia dissolution-purification and impurity removal-evaporation crystallization process, ammonium paratungstate is obtained. After testing, the potassium element in the ammonium paratungstate is 5 mg / kg. Example 3

[0050] A method for preparing ammonium paratungstate using wolframite concentrate comprises the following steps:

[0051] S1. Take 500g of wolframite concentrate and place it in a high-temperature tubular furnace for air roasting. The roasting temperature of the tubular furnace is set to 1300°C, the air flow rate is controlled at 40L / h, and the roasting time is 1.0h;

[0052] S2, placing the roasted wolframite concentrate in a ball mill, adding 200 mL of water and wet grinding for 6 h, and filtering to obtain a pulp;

[0053] S3, adding 1000mL of 15wt% sulfuric acid to the slurry for acid leaching, the acid leaching temperature is 90°C and the acid leaching time is 2h, and then filtering and washing to obtain tungstic acid;

[0054] S4. After tungstic acid is subjected to ammonia dissolution-purification and impurity removal-evaporation crystallization process, ammonium paratungstate is obtained. After testing, the potassium element in the ammonium paratungstate is 4 mg / kg. Example 4

[0055] A method for preparing ammonium paratungstate using wolframite concentrate comprises the following steps:

[0056] S1. Take 500g of wolframite concentrate and place it in a high-temperature tubular furnace for air roasting. The roasting temperature of the tubular furnace is set to 1200°C, the air flow rate is controlled at 100L / h, and the roasting time is 2.0h;

[0057] S2, placing the roasted wolframite concentrate in a ball mill, adding 250 mL of water and wet grinding for 8 hours, and filtering to obtain a pulp;

[0058] S3, adding 1000mL of 31wt% hydrochloric acid to the slurry for acid leaching, the acid leaching temperature is 80°C and the acid leaching time is 2h, and then filtering and washing to obtain tungstic acid;

[0059] S4. After tungstic acid is subjected to ammonia dissolution-purification and impurity removal-evaporation crystallization process, ammonium paratungstate is obtained. After testing, the potassium element in the ammonium paratungstate is 3 mg / kg. Example 5

[0060] A method for preparing ammonium paratungstate using wolframite concentrate comprises the following steps:

[0061] S1. Take 500g of wolframite concentrate and place it in a high-temperature tubular furnace for air roasting. The roasting temperature of the tubular furnace is set to 1100°C, the air flow rate is controlled at 100L / h, and the roasting time is 2.0h;

[0062] S2. Place the roasted wolframite concentrate in a ball mill, add 200 mL of water and wet grind for 4 h, and filter to obtain a pulp;

[0063] S3, add 1000mL of 31wt% hydrochloric acid to the slurry for acid leaching, the acid leaching temperature is 60°C and the acid leaching time is 3h, then filter and wash to obtain tungstic acid;

[0064] S4. After tungstic acid is subjected to ammonia dissolution-purification and impurity removal-evaporation crystallization process, ammonium paratungstate is obtained. After testing, the potassium element in the ammonium paratungstate is 8 mg / kg. Comparative Example 1

[0065] The difference from Example 1 is that the calcination temperature in step S1 is 850°C.

[0066] After testing, the potassium content in the ammonium paratungstate prepared in this comparative example is 46 mg / kg. Comparative Example 2

[0067] The difference from Example 1 is that 500 mL of 31 wt % hydrochloric acid is added for acid leaching in step S3.

[0068] After testing, the potassium content in the ammonium paratungstate prepared in this comparative example is 17 mg / kg. Comparative Example 3

[0069] The difference from Example 1 is that the calcination is performed without air in step S1.

[0070] After testing, the potassium content in the ammonium paratungstate prepared in this comparative example is 39 mg / kg.

[0071] It can be seen from the above embodiments and comparative examples that the present invention directly activates the wolframite concentrate by high-temperature roasting. After roasting, potassium is converted into potassium oxide and potassium sulfate that are easily leached. Then, the wolframite concentrate is ball-milled and acid-leached to obtain solid tungstic acid. The tungstic acid is washed, dissolved in ammonia, purified and impurity-removed by ammonium tungstate solution, evaporated and crystallized to prepare an ammonium paratungstate product that meets the national zero-grade standard (the national standard GBT10116-2007 zero-grade product requires that the potassium content in the ammonium paratungstate product is less than or equal to 10 mg / kg).

[0072] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A method for preparing ammonium paratungstate using wolframite concentrate, characterized in that: The steps include: S1. Place the wolframite concentrate in a high-temperature tubular furnace and roast it with air. The roasting temperature is 1100~1300℃ and the roasting time is 0.5~2.0h; S2, placing the roasted wolframite concentrate in a ball mill for wet grinding to obtain ore slurry; S3, adding acid to the slurry for acid leaching, the liquid-to-solid ratio after adding the acid is (2-3):1; then filtering and washing to obtain tungstic acid; S4. After tungstic acid is subjected to ammonia dissolution-purification and impurity removal-evaporation crystallization process, ammonium paratungstate is obtained, and the potassium element in the ammonium paratungstate is 1~10mg / kg.

2. The method for preparing ammonium paratungstate using wolframite concentrate according to claim 1, characterized in that: In step S1, the air flow rate is 20-100 L / h.

3. The method for preparing ammonium paratungstate using wolframite concentrate according to claim 1, characterized in that: In the step S2, 40-50 wt% of water based on the mass of the roasted wolframite concentrate is added for wet grinding.

4. The method for preparing ammonium paratungstate using wolframite concentrate according to claim 1, characterized in that: In step S2, the wet grinding time is 4 to 8 hours.

5. The method for preparing ammonium paratungstate using wolframite concentrate according to claim 1, characterized in that: In step S3, the acid is hydrochloric acid or sulfuric acid, the concentration of hydrochloric acid is 31wt%, and the concentration of sulfuric acid is 15wt%.

6. The method for preparing ammonium paratungstate using wolframite concentrate according to claim 1, characterized in that: In step S3, the acid leaching temperature is 60-90° C., and the acid leaching time is 2-3 hours.

Citation Information

Cited By

  • Method for preparing ammonium paratungstate from grinding waste

    CN120864559A

  • Process for the preparation of ammonium paratungstate from grinding waste

    CN120864559B