A tungsten-lanthanum alloy wire with dispersed lanthanum element and preparation method thereof

By using the mixing and segmented calcining process of lanthanum hydroxide, ammonium sulfate and tungsten powder in the preparation of tungsten alloy wire, the problems of uneven mixing of lanthanum element compounds and high calcining energy consumption are solved, and the uniform dispersion of lanthanum elements and the High tensile strength.

CN118639045BActive Publication Date: 2024-11-01CHONGYI ZHANGYUAN TUNGSTEN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411114961.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-01
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

In the existing preparation method for tungsten lanthanum alloy wire, the mixture of lanthanum element compounds is uneven, resulting in large fluctuations in the strength of the alloy wire, and the calcination energy consumption is high during mass production, and there is a problem of lanthanum element segregation.

Method used

The tungsten hydroxide and ammonium sulfate are mixed with tungsten powder, calcined in a mixed atmosphere of hydrogen and nitrogen, and processed in a sectional calcination process to generate ultrafine lanthanum oxide and press, sintering and rotary hammer to prepare tungsten lanthanum alloy wire with diffuse distribution of lanthanum elements.

Benefits of technology

The uniform dispersion of lanthanum elements is achieved, the tensile strength of the alloy wire is improved, the ratio of the extreme difference to the average value is less than 2%, and the energy consumption of calcination is reduced, and the segregation of lanthanum elements is avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118639045B_ABST
    Figure CN118639045B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of powder metallurgy, and specifically relates to a tungsten-lanthanum alloy wire with dispersed lanthanum element and a preparation method thereof. Lanthanum hydroxide is added as a lanthanum source, and tungsten powder is used as a solid "solvent" to disperse the lanthanum source, which not only provides the "solvent" required for dispersion but also avoids the pollution of other phases of "solvent", and at the same time avoids the problem of high energy consumption caused by calcination after mixing a large number of raw materials; at the same time, ammonium sulfate is added as a calcination dispersant, and hydrogen is fully utilized to coordinate the temperature to process the tungsten-lanthanum composite powder, so that lanthanum hydroxide generates ultrafine lanthanum oxide, and the lanthanum oxides are mutually dispersed to generate ultrafine dispersed lanthanum oxide, and obtain tungsten-lanthanum alloy wire with dispersed lanthanum element. The tensile strength of the tungsten-lanthanum alloy wire with dispersed lanthanum element of the present invention is ≥5650MPa, and the ratio of the extreme difference of strength to the average value is less than 2%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of powder metallurgy, and specifically relates to a tungsten-lanthanum alloy wire with dispersed lanthanum element and a preparation method thereof. Background Art

[0002] Tungsten-lanthanum alloy wire has high strength and toughness and has been widely recognized by the market. The differences in the preparation methods of tungsten-lanthanum alloy wire mainly focus on the different mixing methods of tungsten powder and lanthanum elements, which can be summarized as: liquid-liquid mixing, solid-liquid mixing, and solid-solid mixing. Among them, liquid-liquid mixing is to use soluble lanthanum salt and soluble tungsten salt to mix in liquid state to prepare tungsten-lanthanum mixed powder. This method has a long production process and is only suitable for enterprises with full-process production. Solid-liquid mixing is to use soluble lanthanum salt solution and solid tungsten source to mix, and then dry to prepare tungsten-lanthanum composite powder. This process has high requirements for solid-liquid ratio and drying method, and it is easy to cause lanthanum segregation; the current mainstream is to use lanthanum compounds and tungsten powder to mix "solid-solid" to obtain tungsten-lanthanum mixed powder. This method is suitable for mass production, but there is uneven mixing of lanthanum compounds, and they exist in the alloy in the form of large particles, forming a fracture source, which causes large fluctuations in the strength of the alloy wire. Summary of the invention

[0003] In order to solve the problems existing in the prior art, the main purpose of the present invention is to provide a tungsten-lanthanum alloy wire with dispersed lanthanum element and a preparation method thereof.

[0004] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:

[0005] A method for preparing a tungsten-lanthanum alloy wire with dispersed lanthanum elements comprises the following steps:

[0006] S1, adding lanthanum hydroxide and ammonium sulfate to tungsten powder and mixing evenly to obtain tungsten-lanthanum mixed powder 1;

[0007] S2, calcining the tungsten-lanthanum mixed powder 1 in a mixed atmosphere of hydrogen and nitrogen to obtain a tungsten-lanthanum mixed powder 2;

[0008] S3, adding tungsten-lanthanum mixed powder 2 to tungsten powder to mix, to obtain tungsten-lanthanum mixed powder 3;

[0009] S4, pressing, sintering and hammering the tungsten-lanthanum mixed powder 3 to obtain a tungsten-lanthanum alloy wire with dispersed lanthanum elements.

[0010] As a preferred embodiment of the method for preparing a tungsten-lanthanum alloy wire with dispersed distribution of lanthanum element described in the present invention, wherein: in the step S1, the mass ratio of lanthanum hydroxide to ammonium sulfate is (15-20):1.

[0011] As a preferred embodiment of the method for preparing a tungsten-lanthanum alloy wire with dispersed distribution of lanthanum element described in the present invention, in the step S1, the proportion of lanthanum hydroxide in the tungsten-lanthanum mixed powder 1 is 10-15wt%.

[0012] As a preferred embodiment of the method for preparing a tungsten-lanthanum alloy wire with dispersed lanthanum element according to the present invention, in step S2, the calcination is performed by a staged calcination process:

[0013] Stage 1: The flow ratio of hydrogen to nitrogen is 1:(8-10), the temperature is raised to 200°C at 5-10°C / min, and kept at this temperature for 15-30min;

[0014] Stage 2: The flow ratio of hydrogen to nitrogen is 1:(4~5), the temperature is increased to 750~800℃ at 15~20℃ / min, and the temperature is kept for 120~180min.

[0015] As a preferred embodiment of the method for preparing a tungsten-lanthanum alloy wire with dispersed distribution of lanthanum element described in the present invention, in step S2, the tungsten-lanthanum mixed powder 2 is tungsten powder and lanthanum oxide.

[0016] As a preferred embodiment of the method for preparing a tungsten-lanthanum alloy wire with dispersed distribution of lanthanum element described in the present invention, in the step S3, the proportion of lanthanum oxide in the tungsten-lanthanum mixed powder 3 is 0.1-2.0wt%.

[0017] To solve the above technical problem, according to another aspect of the present invention, the present invention provides the following technical solution:

[0018] A tungsten-lanthanum alloy wire with dispersed lanthanum element is prepared by adopting the preparation method of the tungsten-lanthanum alloy wire with dispersed lanthanum element.

[0019] As a preferred embodiment of the tungsten-lanthanum alloy wire with dispersed lanthanum element described in the present invention, the tensile strength of the tungsten-lanthanum alloy wire with dispersed lanthanum element is ≥5650MPa, and the ratio of the extreme difference of strength to the average value is less than 2%.

[0020] The beneficial effects of the present invention are as follows:

[0021] The present invention proposes a tungsten-lanthanum alloy wire with dispersed lanthanum element and a preparation method thereof. Lanthanum hydroxide is added as a lanthanum source, and tungsten powder is used as a solid "solvent" to disperse the lanthanum source, which not only provides the "solvent" required for dispersion but also avoids the contamination of other phases of "solvent", and avoids the problem of high energy consumption caused by calcination after mixing a large number of raw materials; at the same time, ammonium sulfate is added as a calcination dispersant, and hydrogen is fully utilized to coordinate the temperature to process the tungsten-lanthanum composite powder, so that lanthanum hydroxide generates ultrafine lanthanum oxide, and the lanthanum oxides are mutually dispersed to generate ultrafine dispersed lanthanum oxide, and a tungsten-lanthanum alloy wire with dispersed lanthanum element is obtained. The tensile strength of the tungsten-lanthanum alloy wire with dispersed lanthanum element of the present invention is ≥5650MPa, and the ratio of the extreme difference to the average value of strength is less than 2%. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0023] Figure 1 This is a photo of the tungsten-lanthanum alloy wire prepared in Example 1 of the present invention.

[0024] Figure 2 This is a photo of the tungsten-lanthanum alloy wire prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0025] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] According to one aspect of the present invention, the present invention provides the following technical solution:

[0027] A method for preparing a tungsten-lanthanum alloy wire with dispersed lanthanum elements comprises the following steps:

[0028] S1, adding lanthanum hydroxide and ammonium sulfate to tungsten powder and mixing evenly to obtain tungsten-lanthanum mixed powder 1;

[0029] S2, calcining the tungsten-lanthanum mixed powder 1 in a mixed atmosphere of hydrogen and nitrogen to obtain a tungsten-lanthanum mixed powder 2;

[0030] S3, adding tungsten-lanthanum mixed powder 2 to tungsten powder to mix, to obtain tungsten-lanthanum mixed powder 3;

[0031] S4, pressing, sintering and hammering the tungsten-lanthanum mixed powder 3 to obtain a tungsten-lanthanum alloy wire with dispersed lanthanum elements.

[0032] Preferably, in step S1, the mass ratio of lanthanum hydroxide to ammonium sulfate is (15-20): 1. Specifically, the mass ratio of lanthanum hydroxide to ammonium sulfate can be, for example, any one of 15: 1, 16: 1, 17: 1, 18: 1, 19: 1, 20: 1 or a range between any two thereof. The addition of ammonium sulfate makes the lanthanum oxide obtained by the conversion of lanthanum hydroxide finer, and the addition of ammonium sulfate makes the ultrafine lanthanum oxide more dispersed to avoid agglomeration.

[0033] Preferably, in step S1, the proportion of lanthanum hydroxide in the tungsten-lanthanum mixed powder 1 is 10-15wt%. Specifically, the proportion of lanthanum hydroxide in the tungsten-lanthanum mixed powder 1 can be, for example, any one of 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, or any range between two thereof.

[0034] Preferably, in step S2, the calcination is performed by a staged calcination process:

[0035] Stage 1: The flow ratio of hydrogen to nitrogen is 1:(8-10), the temperature is raised to 200°C at 5-10°C / min, and the temperature is kept for 15-30min; hydrogen can purify tungsten powder, and the high nitrogen atmosphere can reduce the decomposition of ammonium sulfate; specifically, the flow ratio of hydrogen to nitrogen can be, for example, any one of 1:8, 1:8.5, 1:9, 1:9.5, 1:10, or any range between two thereof;

[0036] Stage 2: The flow ratio of hydrogen to nitrogen is 1:(4~5), the temperature is raised to 750~800℃ at 15~20℃ / min, and the temperature is kept for 120~180min; the flow ratio of hydrogen to nitrogen can be, for example, any one of 1:4, 1:4.5, 1:5 or any range between the two; hydrogen can prevent tungsten powder from reacting with other oxidizing substances, and the addition of nitrogen increases the flow rate and speeds up the removal of impurities, but using only hydrogen may produce excessive water vapor.

[0037] Preferably, in step S2, the tungsten-lanthanum mixed powder 2 is tungsten powder and lanthanum oxide.

[0038] Preferably, in step S2, the proportion of lanthanum oxide in the tungsten-lanthanum mixed powder 3 is 0.1-2.0wt%. The proportion of lanthanum oxide in the tungsten-lanthanum mixed powder 3 can be, for example, any one of 0.1wt%, 0.2wt%, 0.5wt%, 1.0wt%, 1.5wt%, 2.0wt% or any range between two thereof.

[0039] To solve the above technical problem, according to another aspect of the present invention, the present invention provides the following technical solution:

[0040] A tungsten-lanthanum alloy wire with dispersed lanthanum element is prepared by the above-mentioned preparation method of tungsten-lanthanum alloy wire with dispersed lanthanum element. The tensile strength of the tungsten-lanthanum alloy wire with dispersed lanthanum element is ≥5650MPa, and the ratio of the extreme difference of strength to the average value is less than 2%.

[0041] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0042] Example 1

[0043] A method for preparing a tungsten-lanthanum alloy wire with dispersed lanthanum elements comprises the following steps:

[0044] S1. Add lanthanum hydroxide and ammonium sulfate to tungsten powder and mix evenly to obtain tungsten-lanthanum mixed powder 1; the mass ratio of lanthanum hydroxide to ammonium sulfate is 15:1; the proportion of lanthanum hydroxide in the tungsten-lanthanum mixed powder 1 is 10wt%;

[0045] S2, calcining the tungsten-lanthanum mixed powder 1 in a mixed atmosphere of hydrogen and nitrogen to obtain a tungsten-lanthanum mixed powder 2; the calcination adopts a staged calcination process: stage 1: the flow ratio of hydrogen and nitrogen is 1:8, the temperature is increased to 200°C at 5°C / min, and the temperature is kept for 15 minutes; stage 2: the flow ratio of hydrogen and nitrogen is 1:4, the temperature is increased to 750°C at 15°C / min, and the temperature is kept for 120 minutes;

[0046] S3, adding tungsten-lanthanum mixed powder 2 to tungsten powder to obtain tungsten-lanthanum mixed powder 3, wherein the proportion of lanthanum oxide in the tungsten-lanthanum mixed powder 3 is 0.65wt%;

[0047] S4, pressing, sintering and hammering the tungsten-lanthanum mixed powder 3 to obtain a tungsten-lanthanum alloy wire with dispersed lanthanum elements.

[0048] The lanthanum element is evenly dispersed in the tungsten-lanthanum alloy wire prepared in this embodiment. After the cross-section is ground and polished, no obvious lanthanum oxide agglomerates (such as Figure 1 The prepared tungsten-lanthanum alloy wire was subjected to 11 strength tests, with an average tensile strength of 5723 MPa, a range of 92 MPa, and a ratio of the range to the average of 1.60%.

[0049] Example 2

[0050] A method for preparing a tungsten-lanthanum alloy wire with dispersed lanthanum elements comprises the following steps:

[0051] S1. Add lanthanum hydroxide and ammonium sulfate to tungsten powder and mix evenly to obtain tungsten-lanthanum mixed powder 1; the mass ratio of lanthanum hydroxide to ammonium sulfate is 17.5:1; the proportion of lanthanum hydroxide in the tungsten-lanthanum mixed powder 1 is 12.5wt%;

[0052] S2, calcining the tungsten-lanthanum mixed powder 1 in a mixed atmosphere of hydrogen and nitrogen to obtain a tungsten-lanthanum mixed powder 2; the calcination adopts a staged calcination process: stage 1: the flow ratio of hydrogen and nitrogen is 1:9, the temperature is increased to 200°C at 7.5°C / min, and the temperature is kept for 20 minutes; stage 2: the flow ratio of hydrogen and nitrogen is 1:5, the temperature is increased to 780°C at 17°C / min, and the temperature is kept for 150 minutes;

[0053] S3, adding tungsten-lanthanum mixed powder 2 to tungsten powder to obtain tungsten-lanthanum mixed powder 3, wherein the proportion of lanthanum oxide in the tungsten-lanthanum mixed powder 3 is 0.1wt%;

[0054] S4, pressing, sintering and hammering the tungsten-lanthanum mixed powder 3 to obtain a tungsten-lanthanum alloy wire with dispersed lanthanum elements.

[0055] The lanthanum element in the tungsten-lanthanum alloy wire prepared in this embodiment is evenly dispersed. After the cross section is ground and polished, no obvious lanthanum oxide agglomerates can be observed under a 200X metallographic microscope. The prepared tungsten-lanthanum alloy wire was subjected to 11 strength tests, and the average tensile strength was 5690MPa, the range was 104MPa, and the ratio of the range to the average was 1.83%.

[0056] Example 3

[0057] A method for preparing a tungsten-lanthanum alloy wire with dispersed lanthanum elements comprises the following steps:

[0058] S1. Add lanthanum hydroxide and ammonium sulfate to tungsten powder and mix evenly to obtain tungsten-lanthanum mixed powder 1; the mass ratio of lanthanum hydroxide to ammonium sulfate is 20:1; the proportion of lanthanum hydroxide in the tungsten-lanthanum mixed powder 1 is 15wt%;

[0059] S2, calcining the tungsten-lanthanum mixed powder 1 in a mixed atmosphere of hydrogen and nitrogen to obtain a tungsten-lanthanum mixed powder 2; the calcination adopts a staged calcination process: stage 1: the flow ratio of hydrogen and nitrogen is 1:10, the temperature is increased to 200°C at 10°C / min, and the temperature is kept for 30 minutes; stage 2: the flow ratio of hydrogen and nitrogen is 1:5, the temperature is increased to 800°C at 20°C / min, and the temperature is kept for 180 minutes;

[0060] S3, adding tungsten-lanthanum mixed powder 2 to tungsten powder to obtain tungsten-lanthanum mixed powder 3, wherein the proportion of lanthanum oxide in the tungsten-lanthanum mixed powder 3 is 2.0wt%;

[0061] S4, pressing, sintering and hammering the tungsten-lanthanum mixed powder 3 to obtain a tungsten-lanthanum alloy wire with dispersed lanthanum elements.

[0062] The lanthanum element in the tungsten-lanthanum alloy wire prepared in this embodiment is evenly dispersed. After the cross section is ground and polished, no obvious lanthanum oxide agglomerates can be observed under a 200X metallographic microscope. The prepared tungsten-lanthanum alloy wire was subjected to 11 strength tests, and the average tensile strength was 5819 MPa, the range was 106 MPa, and the ratio of the range to the average was 1.82%.

[0063] Comparative Example 1

[0064] The difference from Example 1 is that steps S1-S2 are not performed, and step S3 adopts a traditional solid-solid mixing method to mix lanthanum oxide and tungsten powder, and the proportion of lanthanum oxide is consistent with that in Example 1.

[0065] The lanthanum element in the tungsten-lanthanum alloy wire prepared in this comparative example is unevenly dispersed. After the cross section is polished, obvious lanthanum oxide agglomerates (such as Figure 2 The prepared tungsten-lanthanum alloy wire was subjected to 11 strength tests, with an average tensile strength of 5310 MPa, a range of 415 MPa, and a ratio of the range to the average of 7.80%.

[0066] Comparative Example 2

[0067] The difference from Example 1 is that ammonium sulfate is not added in step S1.

[0068] The lanthanum element in the tungsten-lanthanum alloy wire prepared in this comparative example is unevenly dispersed. After the cross section is ground and polished, obvious lanthanum oxide agglomerates can be observed under a 200X metallographic microscope. The prepared tungsten-lanthanum alloy wire was subjected to 11 strength tests, with an average tensile strength of 5418MPa, a range of 362MPa, and a ratio of the range to the average of 6.68%.

[0069] Comparative Example 3

[0070] The difference from Example 1 is that the calcination atmosphere in step S2 is hydrogen.

[0071] The lanthanum element is evenly dispersed in the tungsten-lanthanum alloy wire prepared in this comparative example. After cross-section grinding and polishing, a small amount of lanthanum oxide agglomerates can be observed in a 200X metallographic microscope. The prepared tungsten-lanthanum alloy wire was subjected to 11 strength tests, and the average tensile strength was 4961 MPa, the range was 256 MPa, and the ratio of the range to the average was 5.16%.

[0072] Comparative Example 4

[0073] The difference from Example 1 is that the step S2 does not use a staged calcination process, and the calcination process is: the flow ratio of hydrogen to nitrogen is 1:4, and the temperature is increased from room temperature to 750° C. at 15° C. / min and kept at this temperature for 120 min.

[0074] The lanthanum element in the tungsten-lanthanum alloy wire prepared in this comparative example is unevenly dispersed. After the cross section is ground and polished, a large number of lanthanum oxide agglomerates can be observed under a 200X metallographic microscope. The prepared tungsten-lanthanum alloy wire is subjected to 11 strength tests, and the average tensile strength is 5206 MPa, the range is 239 MPa, and the ratio of the range to the average value is 4.59%.

[0075] It can be seen from the above embodiments and comparative examples that the present invention disperses the lanthanum source by adding lanthanum hydroxide and using tungsten powder as a solid "solvent", which not only provides the "solvent" required for dispersion but also avoids the contamination of other phases of "solvent", and at the same time avoids the problem of high energy consumption caused by calcination after mixing a large number of raw materials; at the same time, ammonium sulfate is added as a calcination dispersant, and hydrogen is fully utilized to coordinate the temperature to process the tungsten-lanthanum composite powder, so that lanthanum hydroxide generates ultrafine lanthanum oxide and lanthanum oxides are mutually dispersed to generate ultrafine dispersed lanthanum oxide, and obtain tungsten-lanthanum alloy wire with dispersed distribution of lanthanum elements. The tensile strength of the tungsten-lanthanum alloy wire with dispersed distribution of lanthanum elements in the present invention is ≥5650MPa, and the ratio of the extreme difference in strength to the average value is less than 2%.

[0076] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A method for preparing a tungsten-lanthanum alloy wire with dispersed lanthanum element, characterized in that: The steps include: S1, adding lanthanum hydroxide and ammonium sulfate to tungsten powder and mixing evenly to obtain tungsten-lanthanum mixed powder 1; S2, calcining the tungsten-lanthanum mixed powder 1 in a mixed atmosphere of hydrogen and nitrogen to obtain a tungsten-lanthanum mixed powder 2; the calcination adopts a staged calcination process: stage 1: the flow ratio of hydrogen and nitrogen is 1: (8-10), the temperature is increased to 200°C at 5-10°C / min, and the temperature is kept for 15-30min; stage 2: the flow ratio of hydrogen and nitrogen is 1: (4-5), the temperature is increased to 750-800°C at 15-20°C / min, and the temperature is kept for 120-180min; S3, adding tungsten-lanthanum mixed powder 2 to tungsten powder to mix, to obtain tungsten-lanthanum mixed powder 3; S4, pressing, sintering and hammering the tungsten-lanthanum mixed powder 3 to obtain a tungsten-lanthanum alloy wire with dispersed lanthanum elements.

2. The method for preparing the tungsten-lanthanum alloy wire with dispersed distribution of lanthanum element according to claim 1, characterized in that: In step S1, the mass ratio of lanthanum hydroxide to ammonium sulfate is (15-20):

1.

3. The method for preparing the tungsten-lanthanum alloy wire with dispersed distribution of lanthanum element according to claim 1, characterized in that: In the step S1, the proportion of lanthanum hydroxide in the tungsten-lanthanum mixed powder 1 is 10-15wt%.

4. The method for preparing the tungsten-lanthanum alloy wire with dispersed distribution of lanthanum element according to claim 1, characterized in that: In step S2, the tungsten-lanthanum mixed powder 2 is tungsten powder and lanthanum oxide.

5. The method for preparing the tungsten-lanthanum alloy wire with dispersed distribution of lanthanum element according to claim 1, characterized in that: In the step S3, the proportion of lanthanum oxide in the tungsten-lanthanum mixed powder 3 is 0.1-2.0 wt%.

6. A tungsten-lanthanum alloy wire with dispersed lanthanum element, characterized in that: The tungsten-lanthanum alloy wire is prepared by the method for preparing the tungsten-lanthanum alloy wire with dispersed distribution of lanthanum element as described in any one of claims 1 to 5.

7. The tungsten-lanthanum alloy wire with dispersed lanthanum element according to claim 6, characterized in that: The tensile strength of the tungsten-lanthanum alloy wire with dispersed lanthanum element is ≥5650MPa, and the ratio of the extreme difference to the average value of the strength is less than 2%.