Ceramic glaze, handicraft ceramic and preparation method thereof
Ceramic glaze is prepared by using matrix raw materials such as sodium feldspar and potassium feldspar in handicraft ceramics, based on the combination of whisker regulators and nano-silica modifiers, which solves the problems of ceramic mechanical strength and anti-fouling properties. , realizes the high-efficiency alkali corrosion resistance and flexural strength of ceramic products.
Patent Information
- Application Number
- CN202411140686.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-20
AI Technical Summary
The mechanical strength and fracture performance of existing handicraft ceramics are difficult to coordinately improve, and the anti-fouling performance is poor, which limits the efficiency of the product.
Sodium feldspar, potassium feldspar, calcium talc, borax and lithium carbonate as matrix raw materials, add whisker adjustment-based effectors and nanosilicon dioxide modifiers, combined with calcium feldspar, calcium borate and zirconium oxide modifiers , ceramic glaze of zinc oxide and mica was prepared by wet ball milling and sintering treatment to prepare handicraft ceramics with enhanced fracture performance, mechanical flexural strength and alkali mist resistance.
It significantly improves the fracture toughness, flexural strength and anti-fouling properties of handicraft ceramics, optimizes the overall alkali-corrosion stability of the product, enhances the bonding strength between the glaze layer and the blank, and improves the product's use efficiency.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ceramics, and in particular to a ceramic glaze, handicraft ceramics and a preparation method thereof. Background Art
[0002] Ceramics is a general term for pottery and porcelain. Common ceramic materials include clay, alumina, kaolin, etc. Ceramic materials are generally hard but less plastic. In addition to being used in tableware and decoration, ceramics also play an important role in the development of science and technology. Ceramic raw materials are made by quenching clay, a large amount of resources originally available on the earth.
[0003] The existing handicraft ceramics have poor mechanical strength and poor product fracture performance. The mechanical strength and fracture performance of the products are difficult to improve in a coordinated manner, which limits the use efficiency of the products. The poor anti-fouling performance of ceramics further limits the use efficiency of the products. Summary of the invention
[0004] In view of the defects of the prior art, the object of the present invention is to provide a ceramic glaze, handicraft ceramics and a preparation method thereof to solve the problems raised in the above background technology.
[0005] The present invention solves the technical problem by adopting the following technical solution:
[0006] The invention provides a ceramic glaze, comprising the following raw materials in parts by weight: 10-15 parts of calcium feldspar, 4-7 parts of calcium borate, 4-6 parts of zirconium oxide regulator, 2-5 parts of zinc oxide, 3-5 parts of quartz and 4-7 parts of muscovite.
[0007] The present invention also provides a method for preparing handicraft ceramics, comprising the following steps:
[0008] Step 1: Preparation of green body:
[0009] (1) First, weigh the raw materials according to weight: 35-45 parts of sodium feldspar, 20-30 parts of potassium feldspar, 10-15 parts of calcined talc, 8-14 parts of whisker-based conditioning agent, 8-12 parts of borax, 6-9 parts of nano-silicon dioxide modifier, and 4-7 parts of lithium carbonate;
[0010] (2) The raw materials weighed above are fed into a ball mill for wet ball milling for 25 to 30 hours, passed through a 200-mesh sieve, and then pressed in a molding machine at a pressing pressure of 70 to 75 MPa to obtain a green body;
[0011] Step 2: Preparation of ceramic glaze:
[0012] Wet-mill 10-15 parts of calcium feldspar, 4-7 parts of calcium borate, 4-6 parts of zirconium oxide regulator, 2-5 parts of zinc oxide, 3-5 parts of quartz and 4-7 parts of muscovite for 2 hours to obtain a ceramic glaze;
[0013] Step 3: Apply ceramic glaze to the surface of the body with a glaze amount of 300-400g / m 2 , glazing is completed, and the ceramic body is obtained after drying;
[0014] Step 4: the ceramic body is sintered for improvement, the sintering temperature is 1250-1270°C, the sintering time is 3-5 hours, and after the sintering is completed, the ceramic body is air-cooled to room temperature to obtain a handicraft ceramic.
[0015] Preferably, the preparation method of the whisker-based effector is:
[0016] S1: Preparation of graphene effect liquid:
[0017] S11: irradiating the graphene flakes with protons for 5-10 minutes at an irradiation power of 350-400 W, and obtaining irradiated graphene flakes after the irradiation is completed;
[0018] S12: ultrasonically mixing the irradiated graphene flakes and the lanthanum nitrate solution in a weight ratio of 2:5, and then finishing the ultrasonication to obtain lanthanum-doped graphene flakes;
[0019] S13: 4-6 parts of lanthanum-doped flake graphene, 2-5 parts of 5% by mass sodium lignin sulfonate solution, 1-3 parts of chitosan solution and 2-4 parts of carboxymethyl cellulose are mixed and milled thoroughly at a ball milling speed of 1500 r / min for 2 h to obtain a graphene effect solution;
[0020] S2: mixing the silicon carbide whiskers in a sufficient amount of a phosphate buffer solution having a pH value of 5.0 to obtain a whisker dispersion;
[0021] S3: The whisker dispersion and the graphene effect liquid are mixed and stirred in a weight ratio of 5:3. After the stirring is completed, the mixture is washed with water and dried to obtain an effect agent based on whisker adjustment.
[0022] Preferably, the ultrasonic power of the ultrasonic mixing treatment is 350-400W, and the ultrasonic time is 20-30min; the stirring temperature of the mixed stirring treatment is 50-55°C, the stirring speed is 550-650r / min, and the stirring is 20-30min.
[0023] Preferably, the mass fraction of the lanthanum nitrate solution is 2-5%; the mass fraction of the chitosan solution is 3-6%.
[0024] Preferably, the preparation method of the nano-silicon dioxide modifier is:
[0025] S101: firstly heat the nano-silicon dioxide to 150-160°C at a rate of 1-3°C / min, keep the temperature for 5-10 minutes, then heat the nano-silicon dioxide to 275-285°C at a rate of 2-5°C / min, keep the temperature for 2-5 minutes, and finally air-cool to room temperature;
[0026] S102: adding 1-3 parts of yttrium oxide and 2-5 parts of nano-bentonite to 4-7 parts of 6% by mass sodium dodecylbenzene sulfonate solution, and then adding 2-4 parts of silane coupling agent KH560 and 0.5-0.7 parts of stearic acid and mixing well to obtain a modified solution;
[0027] S103: The nano-silicon dioxide treated in S101 and the modified liquid obtained in S102 are stirred and modified in a weight ratio of 3:7. After the modification is completed, the nano-silicon dioxide modifier is obtained by washing with water, filtering and drying.
[0028] Preferably, the stirring speed of the stirring modification treatment is 550-750 r / min, and the stirring time is 40-50 min.
[0029] Preferably, the preparation method of the zirconium oxide regulator is:
[0030] 2-5 parts of aluminum silicate fiber, 1-3 parts of citric acid, 4-7 parts of 5% by mass sodium alginate solution and 2-5 parts of silane coupling agent KH550 are fully mixed to obtain an aluminum silicate fiber solution;
[0031] The zirconium oxide is preheated at 55-65°C for 10-15 minutes, then added into a sufficient amount of aluminum silicate fiber solution and immersed in ultrasonic treatment. After the immersion is completed, the fiber is washed with water, filtered and dried to obtain a zirconium oxide regulator.
[0032] Preferably, the ultrasonic power of the immersion ultrasonic treatment is 350-400 W, and the ultrasonic time is 20-30 min.
[0033] The invention also provides a handicraft ceramic, which is prepared by the handicraft ceramic preparation method.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] 1. The handicraft ceramic of the present invention adopts a body glazed with ceramic glaze, and then undergoes sintering improvement treatment to obtain a ceramic product. The body adopts sodium feldspar, potassium feldspar, burned talc, borax and lithium carbonate as matrix raw materials, and by adding a whisker-based effect agent and a nano-silicon dioxide modifier, the two are coordinated and synergistic, thereby enhancing the fracture performance and mechanical flexural strength performance of the product, and optimizing the alkali mist resistance stability of the product. At the same time, the glaze obtained by mutually mixing calcium feldspar, calcium borate, zirconium oxide regulator, zinc oxide, quartz and white mica is coordinated and coordinated to enhance the anti-fouling performance of the product, and the overall alkali corrosion resistance stability of the prepared craft ceramic is remarkable;
[0036] 2. The whisker-adjusted active agent uses flake graphene to be first proton-irradiated to optimize the active performance of flake graphene, and then mixed and improved with a lanthanum nitrate solution to optimize the active performance of graphene, and then fully obtains a graphene active liquid by mixing and ball-milling a sodium lignin sulfonate solution, a chitosan solution, and a carboxymethyl cellulose. The raw materials in the graphene active liquid are coordinated with graphene, and the raw materials are coordinated and coordinated to enhance the performance together, and silicon carbide whiskers are dispersed in a sufficient amount of a phosphate buffer solution with a pH value of 5.0, and a whisker dispersion is used to coordinate with the graphene active liquid, and the whisker-like structure is coordinated with the flake graphene distribution system to coordinate and improve the fracture performance and mechanical strength performance of the system;
[0037] 3. Nano-silicon dioxide modifier: Nano-silicon dioxide is used for segmented thermal improvement to optimize its activity, and then yttrium oxide, nano-bentonite, 6% sodium dodecylbenzene sulfonate solution by mass, silane coupling agent KH560, and stearic acid are fully blended to obtain a modified liquid. Nano-bentonite is used as a layer structure and interspersed in the system. The raw materials in the modified liquid are then deployed, and the modified liquid is coordinated with nano-silicon dioxide with a high specific surface area to improve the interface of the system raw materials, enhance the bonding strength between the glaze layer and the body, improve the overall performance stability of the product, and enhance the synergistic effect of the nano-silicon dioxide modifier and the whisker-based effect agent, further enhance the coordination of system performance, and improve the alkali fog resistance stability of the system;
[0038] 4. Zirconium oxide regulator: Zirconium oxide is preheated at 55-65°C for 10-15 minutes, and then mixed with aluminum silicate fiber, citric acid, 5% by mass sodium alginate solution and silane coupling agent KH550 to obtain aluminum silicate fiber liquid. The raw materials in the aluminum silicate fiber liquid are blended with each other, and the aluminum silicate fiber is interspersed with the reinforced zirconium oxide to obtain the zirconium oxide regulator, which further optimizes the glaze layer and improves the anti-fouling stability of the layer. At the same time, it cooperates with the green body to enhance the performance stability of the system, and the performance of the product is further improved. DETAILED DESCRIPTION
[0039] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0040] A ceramic glaze of the present embodiment includes the following raw materials in parts by weight: 10-15 parts of calcium feldspar, 4-7 parts of calcium borate, 4-6 parts of zirconium oxide regulator, 2-5 parts of zinc oxide, 3-5 parts of quartz and 4-7 parts of muscovite.
[0041] A method for preparing a handicraft ceramic in this embodiment includes the following steps:
[0042] Step 1: Preparation of green body:
[0043] (1) First, weigh the raw materials according to weight: 35-45 parts of sodium feldspar, 20-30 parts of potassium feldspar, 10-15 parts of calcined talc, 8-14 parts of whisker-based conditioning agent, 8-12 parts of borax, 6-9 parts of nano-silicon dioxide modifier, and 4-7 parts of lithium carbonate;
[0044] (2) The raw materials weighed above are fed into a ball mill for wet ball milling for 25 to 30 hours, passed through a 200-mesh sieve, and then pressed in a molding machine at a pressing pressure of 70 to 75 MPa to obtain a green body;
[0045] Step 2: Preparation of ceramic glaze:
[0046] Wet-mill 10-15 parts of calcium feldspar, 4-7 parts of calcium borate, 4-6 parts of zirconium oxide regulator, 2-5 parts of zinc oxide, 3-5 parts of quartz and 4-7 parts of muscovite for 2 hours to obtain a ceramic glaze;
[0047] Step 3: Apply ceramic glaze to the surface of the body with a glaze amount of 300-400g / m 2 , glazing is completed, and the ceramic body is obtained after drying;
[0048] Step 4: the ceramic body is sintered for improvement, the sintering temperature is 1250-1270°C, the sintering time is 3-5 hours, and after the sintering is completed, the ceramic body is air-cooled to room temperature to obtain a handicraft ceramic.
[0049] The preparation method of the whisker-regulated active agent of this embodiment is as follows:
[0050] S1: Preparation of graphene effect liquid:
[0051] S11: irradiating the graphene flakes with protons for 5-10 minutes at an irradiation power of 350-400 W, and obtaining irradiated graphene flakes after the irradiation is completed;
[0052] S12: ultrasonically mixing the irradiated graphene flakes and the lanthanum nitrate solution in a weight ratio of 2:5, and then finishing the ultrasonication to obtain lanthanum-doped graphene flakes;
[0053] S13: 4-6 parts of lanthanum-doped flake graphene, 2-5 parts of 5% by mass sodium lignin sulfonate solution, 1-3 parts of chitosan solution and 2-4 parts of carboxymethyl cellulose are mixed and milled thoroughly at a ball milling speed of 1500 r / min for 2 h to obtain a graphene effect solution;
[0054] S2: mixing the silicon carbide whiskers in a sufficient amount of a phosphate buffer solution having a pH value of 5.0 to obtain a whisker dispersion;
[0055] S3: The whisker dispersion and the graphene effect liquid are mixed and stirred in a weight ratio of 5:3. After the stirring is completed, the mixture is washed with water and dried to obtain an effect agent based on whisker adjustment.
[0056] The ultrasonic power of the ultrasonic mixing treatment in this embodiment is 350~400W, and the ultrasonic time is 20~30min; the stirring temperature of the mixing and stirring treatment is 50~55°C, the stirring speed is 550~650r / min, and the stirring is 20~30min.
[0057] The mass fraction of the lanthanum nitrate solution in this embodiment is 2-5%; the mass fraction of the chitosan solution is 3-6%.
[0058] The preparation method of the nano silicon dioxide modifier of this embodiment is:
[0059] S101: firstly heat the nano-silicon dioxide to 150-160°C at a rate of 1-3°C / min, keep the temperature for 5-10 minutes, then heat the nano-silicon dioxide to 275-285°C at a rate of 2-5°C / min, keep the temperature for 2-5 minutes, and finally air-cool to room temperature;
[0060] S102: adding 1-3 parts of yttrium oxide and 2-5 parts of nano-bentonite to 4-7 parts of 6% by mass sodium dodecylbenzene sulfonate solution, and then adding 2-4 parts of silane coupling agent KH560 and 0.5-0.7 parts of stearic acid and mixing well to obtain a modified solution;
[0061] S103: The nano-silicon dioxide treated in S101 and the modified liquid obtained in S102 are stirred and modified in a weight ratio of 3:7. After the modification is completed, the nano-silicon dioxide modifier is obtained by washing with water, filtering and drying.
[0062] The stirring speed of the stirring modification treatment in this embodiment is 550-750 r / min, and the stirring time is 40-50 min.
[0063] The preparation method of the zirconium oxide regulator of this embodiment is:
[0064] 2-5 parts of aluminum silicate fiber, 1-3 parts of citric acid, 4-7 parts of 5% by mass sodium alginate solution and 2-5 parts of silane coupling agent KH550 are fully mixed to obtain an aluminum silicate fiber solution;
[0065] The zirconium oxide is preheated at 55-65°C for 10-15 minutes, then added into a sufficient amount of aluminum silicate fiber solution and immersed in ultrasonic treatment. After the immersion is completed, the fiber is washed with water, filtered and dried to obtain a zirconium oxide regulator.
[0066] The ultrasonic power of the immersion ultrasonic treatment in this embodiment is 350-400 W, and the ultrasonic time is 20-30 min.
[0067] A handicraft ceramic of the present embodiment is prepared by the handicraft ceramic preparation method.
[0068] Example 1: A ceramic glaze comprises the following raw materials in parts by weight: 10 parts of calcium feldspar, 4 parts of calcium borate, 4 parts of zirconium oxide regulator, 2 parts of zinc oxide, 3 parts of quartz and 4 parts of muscovite.
[0069] A method for preparing handicraft ceramics comprises the following steps:
[0070] Step 1: Preparation of green body:
[0071] (1) First, weigh the raw materials according to weight: 35 parts of sodium feldspar, 20 parts of potassium feldspar, 10 parts of calcined talc, 8 parts of whisker-based conditioning agent, 8 parts of borax, 6 parts of nano-silicon dioxide modifier, and 4 parts of lithium carbonate;
[0072] (2) The raw materials weighed above were fed into a ball mill for wet ball milling for 25 hours, passed through a 200-mesh sieve, and then pressed in a molding machine at a pressing pressure of 70 MPa to obtain a green body;
[0073] Step 2: Preparation of ceramic glaze:
[0074] 10 parts of calcium feldspar, 4 parts of calcium borate, 4 parts of zirconium oxide regulator, 2 parts of zinc oxide, 3 parts of quartz and 4 parts of muscovite were wet-milled for 2 hours to obtain a ceramic glaze;
[0075] Step 3: Apply ceramic glaze to the surface of the body with a glaze amount of 300g / m 2 , glazing is completed, and the ceramic body is obtained after drying;
[0076] Step 4: the ceramic body is sintered for improvement, the sintering temperature is 1250°C, the sintering time is 3 hours, and after the sintering is completed, the ceramic body is air-cooled to room temperature to obtain a handicraft ceramic.
[0077] The preparation method of the whisker-regulated active agent of this embodiment is as follows:
[0078] S1: Preparation of graphene effect liquid:
[0079] S11: irradiating the graphene flakes with protons for 5 minutes at an irradiation power of 350 W, and then obtaining irradiated graphene flakes after the irradiation is completed;
[0080] S12: ultrasonically mixing the irradiated graphene flakes and the lanthanum nitrate solution in a weight ratio of 2:5, and then finishing the ultrasonication to obtain lanthanum-doped graphene flakes;
[0081] S13: 4 parts of lanthanum-doped flake graphene, 2 parts of 5% by mass sodium lignin sulfonate solution, 1 part of chitosan solution and 2 parts of carboxymethyl cellulose are mixed and milled thoroughly at a ball milling speed of 1500 r / min for 2 h to obtain a graphene effect solution;
[0082] S2: mixing the silicon carbide whiskers in a sufficient amount of a phosphate buffer solution having a pH value of 5.0 to obtain a whisker dispersion;
[0083] S3: The whisker dispersion and the graphene effect liquid are mixed and stirred in a weight ratio of 5:3. After the stirring is completed, the mixture is washed with water and dried to obtain an effect agent based on whisker adjustment.
[0084] The ultrasonic power of the ultrasonic mixing treatment in this embodiment is 350W, and the ultrasonic time is 20min; the stirring temperature of the mixing and stirring treatment is 50°C, the stirring speed is 550r / min, and the stirring is 20min.
[0085] The mass fraction of the lanthanum nitrate solution in this embodiment is 2%; the mass fraction of the chitosan solution is 3%.
[0086] The preparation method of the nano silicon dioxide modifier of this embodiment is:
[0087] S101: The nano-silicon dioxide is first heated to 150°C at a rate of 1°C / min, kept at this temperature for 5 minutes, then heated to 275°C at a rate of 2°C / min, kept at this temperature for 2 minutes, and finally air-cooled to room temperature;
[0088] S102: adding 1 part of yttrium oxide and 2 parts of nano-bentonite to 4 parts of 6% by mass sodium dodecylbenzene sulfonate solution, and then adding 2 parts of silane coupling agent KH560 and 0.5 parts of stearic acid and mixing thoroughly to obtain a modified solution;
[0089] S103: The nano-silicon dioxide treated in S101 and the modified liquid obtained in S102 are stirred and modified in a weight ratio of 3:7. After the modification is completed, the nano-silicon dioxide modifier is obtained by washing with water, filtering and drying.
[0090] The stirring speed of the stirring modification treatment in this embodiment is 550 r / min, and the stirring time is 40 min.
[0091] The preparation method of the zirconium oxide regulator of this embodiment is:
[0092] 2 parts of aluminum silicate fiber, 1 part of citric acid, 4 parts of 5% by mass sodium alginate solution and 2 parts of silane coupling agent KH550 were fully mixed to obtain an aluminum silicate fiber solution;
[0093] The zirconium oxide is preheated at 55° C. for 10 minutes, then added into a sufficient amount of aluminum silicate fiber solution and immersed in ultrasonic treatment. After the immersion is completed, the fiber is washed with water, filtered and dried to obtain a zirconium oxide regulator.
[0094] The ultrasonic power of the immersion ultrasonic treatment in this embodiment is 350 W, and the ultrasonic time is 20 min.
[0095] A handicraft ceramic is prepared by the handicraft ceramic preparation method.
[0096] Example 2: A ceramic glaze comprises the following raw materials in parts by weight: 15 parts of calcium feldspar, 7 parts of calcium borate, 6 parts of zirconium oxide regulator, 5 parts of zinc oxide, 5 parts of quartz and 7 parts of muscovite.
[0097] A method for preparing handicraft ceramics comprises the following steps:
[0098] Step 1: Preparation of green body:
[0099] (1) First, weigh the raw materials according to weight: 45 parts of sodium feldspar, 30 parts of potassium feldspar, 15 parts of calcined talc, 14 parts of whisker-based conditioning agent, 12 parts of borax, 9 parts of nano-silicon dioxide modifier, and 7 parts of lithium carbonate;
[0100] (2) The raw materials weighed above were fed into a ball mill for wet ball milling for 30 hours, passed through a 200-mesh sieve, and then pressed in a molding machine at a pressing pressure of 75 MPa to obtain a green body;
[0101] Step 2: Preparation of ceramic glaze:
[0102] 15 parts of calcium feldspar, 7 parts of calcium borate, 6 parts of zirconium oxide regulator, 5 parts of zinc oxide, 5 parts of quartz and 7 parts of muscovite were wet-milled for 2 hours to obtain a ceramic glaze;
[0103] Step 3: Apply ceramic glaze to the surface of the body with a glaze amount of 400g / m 2 , glazing is completed, and the ceramic body is obtained after drying;
[0104] Step 4: the ceramic body is sintered again for improvement, the sintering temperature is 1270°C, the sintering time is 5 hours, and after the sintering is completed, it is air-cooled to room temperature to obtain a handicraft ceramic.
[0105] The preparation method of the whisker-regulated active agent of this embodiment is as follows:
[0106] S1: Preparation of graphene effect liquid:
[0107] S11: irradiating the graphene flakes with protons for 10 min at an irradiation power of 400 W, and then obtaining irradiated graphene flakes after the irradiation is completed;
[0108] S12: ultrasonically mixing the irradiated graphene flakes and the lanthanum nitrate solution in a weight ratio of 2:5, and then finishing the ultrasonication to obtain lanthanum-doped graphene flakes;
[0109] S13: 6 parts of lanthanum-doped flake graphene, 5 parts of 5% by mass sodium lignin sulfonate solution, 3 parts of chitosan solution and 4 parts of carboxymethyl cellulose are mixed and milled thoroughly at a ball milling speed of 1500 r / min for 2 h to obtain a graphene effect solution;
[0110] S2: mixing the silicon carbide whiskers in a sufficient amount of a phosphate buffer solution having a pH value of 5.0 to obtain a whisker dispersion;
[0111] S3: The whisker dispersion and the graphene effect liquid are mixed and stirred in a weight ratio of 5:3. After the stirring is completed, the mixture is washed with water and dried to obtain an effect agent based on whisker adjustment.
[0112] The ultrasonic power of the ultrasonic mixing treatment in this embodiment is 400W, and the ultrasonic time is 30min; the stirring temperature of the mixing and stirring treatment is 55°C, the stirring speed is 650r / min, and the stirring is 30min.
[0113] The mass fraction of the lanthanum nitrate solution in this embodiment is 5%; the mass fraction of the chitosan solution is 6%.
[0114] The preparation method of the nano silicon dioxide modifier of this embodiment is:
[0115] S101: The nano-silicon dioxide is first heated to 160°C at a rate of 3°C / min, kept at this temperature for 10 minutes, then heated to 285°C at a rate of 5°C / min, kept at this temperature for 5 minutes, and finally air-cooled to room temperature;
[0116] S102: adding 3 parts of yttrium oxide and 5 parts of nano-bentonite to 7 parts of 6% by mass sodium dodecylbenzene sulfonate solution, and then adding 4 parts of silane coupling agent KH5600 and 7 parts of stearic acid and mixing thoroughly to obtain a modified solution;
[0117] S103: The nano-silicon dioxide treated in S101 and the modified liquid obtained in S102 are stirred and modified in a weight ratio of 3:7. After the modification is completed, the nano-silicon dioxide modifier is obtained by washing with water, filtering and drying.
[0118] The stirring speed of the stirring modification treatment in this embodiment is 750 r / min, and the stirring is 50 min.
[0119] The preparation method of the zirconium oxide regulator of this embodiment is:
[0120] 5 parts of aluminum silicate fiber, 3 parts of citric acid, 7 parts of 5% by mass sodium alginate solution and 5 parts of silane coupling agent KH550 were fully mixed to obtain an aluminum silicate fiber solution;
[0121] The zirconium oxide is preheated at 65° C. for 15 minutes, then added into a sufficient amount of aluminum silicate fiber solution and immersed in ultrasonic treatment. After the immersion is completed, the solution is washed with water, filtered and dried to obtain a zirconium oxide regulator.
[0122] The ultrasonic power of the immersion ultrasonic treatment in this embodiment is 400 W, and the ultrasonic time is 30 min.
[0123] A handicraft ceramic is prepared by the handicraft ceramic preparation method.
[0124] Example 3: A ceramic glaze comprises the following raw materials in parts by weight: 12.5 parts of calcium feldspar, 5.5 parts of calcium borate, 5 parts of zirconium oxide regulator, 3.5 parts of zinc oxide, 4 parts of quartz and 5.5 parts of muscovite.
[0125] A method for preparing handicraft ceramics comprises the following steps:
[0126] Step 1: Preparation of green body:
[0127] (1) First, weigh the raw materials according to weight: 40 parts of sodium feldspar, 25 parts of potassium feldspar, 12.5 parts of calcined talc, 11 parts of whisker-based conditioning agent, 10 parts of borax, 7.5 parts of nano-silicon dioxide modifier, and 5.5 parts of lithium carbonate;
[0128] (2) The raw materials weighed above were fed into a ball mill for wet ball milling for 27.5 hours, passed through a 200-mesh sieve, and then pressed in a molding machine at a pressing pressure of 72.5 MPa to obtain a green body;
[0129] Step 2: Preparation of ceramic glaze:
[0130] 12.5 parts of calcium feldspar, 5.5 parts of calcium borate, 5 parts of zirconium oxide regulator, 3.5 parts of zinc oxide, 4 parts of quartz and 5.5 parts of muscovite were wet-milled for 2 hours to obtain a ceramic glaze;
[0131] Step 3: Apply ceramic glaze to the surface of the body with a glaze amount of 350g / m 2 , glazing is completed, and the ceramic body is obtained after drying;
[0132] Step 4: the ceramic body is sintered for improvement, the sintering temperature is 1260°C, the sintering time is 4 hours, and after the sintering is completed, it is air-cooled to room temperature to obtain a handicraft ceramic.
[0133] The preparation method of the whisker-regulated active agent of this embodiment is as follows:
[0134] S1: Preparation of graphene effect liquid:
[0135] S11: irradiating the graphene flakes with protons for 7.5 min at an irradiation power of 370 W, and then obtaining irradiated graphene flakes after the irradiation is completed;
[0136] S12: ultrasonically mixing the irradiated graphene flakes and the lanthanum nitrate solution in a weight ratio of 2:5, and then finishing the ultrasonication to obtain lanthanum-doped graphene flakes;
[0137] S13: 5 parts of lanthanum-doped flake graphene, 3.5 parts of 5% sodium lignin sulfonate solution, 2 parts of chitosan solution and 3 parts of carboxymethyl cellulose are mixed and milled thoroughly at a ball milling speed of 1500 r / min for 2 h to obtain a graphene effect solution;
[0138] S2: mixing the silicon carbide whiskers in a sufficient amount of a phosphate buffer solution having a pH value of 5.0 to obtain a whisker dispersion;
[0139] S3: The whisker dispersion and the graphene effect liquid are mixed and stirred in a weight ratio of 5:3. After the stirring is completed, the mixture is washed with water and dried to obtain an effect agent based on whisker adjustment.
[0140] The ultrasonic power of the ultrasonic mixing treatment in this embodiment is 370W, and the ultrasonic time is 25min; the stirring temperature of the mixing and stirring treatment is 52.5°C, the stirring speed is 600r / min, and the stirring is for 25min.
[0141] The mass fraction of the lanthanum nitrate solution in this embodiment is 3.5%; the mass fraction of the chitosan solution is 4.5%.
[0142] The preparation method of the nano silicon dioxide modifier of this embodiment is:
[0143] S101: The nano-silicon dioxide was first heated to 155°C at a rate of 2°C / min, kept at that temperature for 7.5min, then heated to 280°C at a rate of 3.5°C / min, kept at that temperature for 3.5min, and finally air-cooled to room temperature;
[0144] S102: adding 2 parts of yttrium oxide and 3.5 parts of nano-bentonite to 5.5 parts of 6% sodium dodecylbenzene sulfonate solution, and then adding 3 parts of silane coupling agent KH560 and 0.6 parts of stearic acid and mixing well to obtain a modified solution;
[0145] S103: The nano-silicon dioxide treated in S101 and the modified liquid obtained in S102 are stirred and modified in a weight ratio of 3:7. After the modification is completed, the nano-silicon dioxide modifier is obtained by washing with water, filtering and drying.
[0146] The stirring speed of the stirring modification treatment in this embodiment is 600 r / min, and the stirring time is 45 min.
[0147] The preparation method of the zirconium oxide regulator of this embodiment is:
[0148] 3.5 parts of aluminum silicate fiber, 2 parts of citric acid, 5.5 parts of 5% by mass sodium alginate solution and 3.5 parts of silane coupling agent KH550 were fully mixed to obtain an aluminum silicate fiber solution;
[0149] The zirconium oxide is preheated at 60° C. for 12.5 minutes, then added into a sufficient amount of aluminum silicate fiber solution and immersed in ultrasonic treatment. After the immersion is completed, the solution is washed with water, filtered and dried to obtain a zirconium oxide regulator.
[0150] The ultrasonic power of the immersion ultrasonic treatment in this embodiment is 370 W, and the ultrasonic time is 25 min.
[0151] A handicraft ceramic is prepared by the handicraft ceramic preparation method.
[0152] Comparative Example 1:
[0153] The difference from Example 3 is that no whisker-based conditioning agent is added.
[0154] Comparative Example 2:
[0155] The difference from Example 3 is that graphene-based liquid treatment is not used in the preparation of the whisker-based agent.
[0156] Comparative Example 3:
[0157] The difference from Example 3 is that no lanthanum-doped flaky graphene is added to the graphene effect solution.
[0158] Comparative Example 4:
[0159] The difference from Example 3 is that the lanthanum-doped flake graphene is replaced by flake graphene.
[0160] Comparative Example 5:
[0161] The difference from Example 3 is that no chitosan solution and carboxymethyl cellulose are added to the graphene effect solution.
[0162] Comparative Example 6:
[0163] The difference from Example 3 is that no nano silicon dioxide modifier is added.
[0164] Comparative Example 7:
[0165] The difference from Example 3 is that S101 treatment was not used in the preparation of the nano-silica modifier.
[0166] Comparative Example 8:
[0167] The difference from Example 3 is that no modifying liquid treatment is used in the preparation of the nano-silicon dioxide modifier.
[0168] Comparative Example 9:
[0169] The difference from Example 3 is that no yttrium oxide or nano-bentonite is added to the modified liquid.
[0170] Comparative Example 10:
[0171] The difference from Example 3 is that no silane coupling agent KH560 and stearic acid are added to the modified liquid.
[0172] Comparative Example 11:
[0173] The difference from Example 3 is that no zirconium oxide regulator is added.
[0174] The products of Examples 1 to 3 and Comparative Examples 1 to 11 were subjected to conventional performance tests, and the test results are shown in Table 1.
[0175] Table 1: Test results of conventional performance of products of Examples 1 to 3 and Comparative Examples 1 to 11:
[0176]
[0177] The product was placed in a 2% humidity environment for 12 hours, and then placed in a 2% sodium hydroxide alkaline mist for 12 hours to test its alkali resistance stability. The test results are shown in Table 2.
[0178] Table 2: Test results of alkali resistance stability of products of Examples 1 to 3 and Comparative Examples 1 to 11:
[0179]
[0180] From Table 1 and Table 2, we can see that:
[0181] The product of Example 3 has excellent flexural strength and fracture toughness, and the antifouling effect of the product is remarkable. The flexural strength, fracture toughness and antifouling performance can be improved in a coordinated manner. In addition, the product has excellent performance stability under alkaline corrosion conditions.
[0182] The product does not contain whisker-based activators, nano-silica modifiers, or zirconium oxide modifiers. The fracture toughness, flexural strength, and antifouling properties of the product are difficult to coordinate and improve, and the alkali resistance of the product deteriorates significantly. The product performance effect is most obvious when whisker-based activators, nano-silica modifiers, and zirconium oxide modifiers are coordinated and deployed to enhance their synergy.
[0183] In the preparation of the whisker-adjusting agent, the graphene-adjusting liquid treatment was not used, the lanthanum-doped flake graphene was not added to the graphene-adjusting liquid, the lanthanum-doped flake graphene was replaced by flake graphene, and the chitosan solution and carboxymethyl cellulose were not added to the graphene-adjusting liquid. The performance of the product showed a trend of deterioration. Only the whisker-adjusting agent obtained by the method of the present invention had the most significant performance effect. The effects of other methods were not as obvious as those of the present invention.
[0184] When S101 treatment is not used in the preparation of the nano-silica modifier, the modifying liquid treatment is not used in the preparation of the nano-silica modifier, yttrium oxide and nano-bentonite are not added to the modifying liquid, and silane coupling agent KH560 and stearic acid are not added to the modifying liquid, the performance of the product tends to deteriorate. Only the nano-silica modifier modified with the modifying liquid obtained by the method of the present invention has the most significant performance effect.
[0185] The present invention further explores the product performance through the preparation of zirconium oxide regulator.
[0186] Experimental Example 1:
[0187] The only difference from Example 3 is that no zirconium oxide is added in the preparation of the zirconium oxide regulator.
[0188] Experimental Example 2:
[0189] The only difference from Example 3 is that no aluminum silicate fiber liquid is added in the preparation of the zirconium oxide regulator.
[0190] Experimental Example 3:
[0191] The only difference from Example 3 is that no aluminum silicate fiber is added to the aluminum silicate fiber liquid.
[0192] Experimental Example 4:
[0193] The only difference from Example 3 is that no silane coupling agent KH550 and citric acid are added to the aluminum silicate fiber liquid.
[0194] Taking the above-mentioned alkaline corrosion test conditions as the test object, the effect of zirconium oxide regulator on the performance of the product was tested. The test results are shown in Table 3.
[0195] Table 3: Product performance test results of Experimental Examples 1 to 4:
[0196]
[0197] As can be seen from Table 3, when zirconium oxide was not added in the preparation of the zirconium oxide regulator, the performance of the product changed. In the preparation of the zirconium oxide regulator, the performance deterioration was the most obvious, followed by the fact that no aluminum silicate fiber liquid was added. At the same time, no aluminum silicate fiber was added to the aluminum silicate fiber liquid, and no silane coupling agent KH550 and citric acid were added to the aluminum silicate fiber liquid. The performance of the product showed a trend of deterioration. The zirconium oxide regulators obtained by different methods showed a trend of deterioration to varying degrees. The zirconium oxide regulator obtained by combining the specific aluminum silicate fiber liquid of the present invention with zirconium oxide had the most significant product performance effect.
[0198] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
[0199] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A method for preparing handicraft ceramics, wherein the ceramic glaze used comprises the following raw materials in parts by weight: 10 to 15 parts of calcium feldspar, 4 to 7 parts of calcium borate, 4 to 6 parts of zirconium oxide regulator, 2 to 5 parts of zinc oxide, 3 to 5 parts of quartz and 4 to 7 parts of muscovite, characterized in that: The following steps are involved: Step 1: Preparation of green body: (1) First, weigh the raw materials according to weight: 35-45 parts of sodium feldspar, 20-30 parts of potassium feldspar, 10-15 parts of calcined talc, 8-14 parts of whisker-based conditioning agent, 8-12 parts of borax, 6-9 parts of nano-silicon dioxide modifier, and 4-7 parts of lithium carbonate; (2) The raw materials weighed above are fed into a ball mill for wet ball milling for 25 to 30 hours, passed through a 200-mesh sieve, and then pressed in a molding machine at a pressing pressure of 70 to 75 MPa to obtain a green body; Step 2: Preparation of ceramic glaze: Wet-mill 10-15 parts of calcium feldspar, 4-7 parts of calcium borate, 4-6 parts of zirconium oxide regulator, 2-5 parts of zinc oxide, 3-5 parts of quartz and 4-7 parts of muscovite for 2 hours to obtain a ceramic glaze; Step 3: Apply ceramic glaze to the surface of the body with a glaze amount of 300-400g / m 2 , glazing is completed, and the ceramic body is obtained after drying; Step 4: the ceramic body is sintered and improved, the sintering temperature is 1250-1270°C, the sintering time is 3-5 hours, and after the sintering is completed, the ceramic body is air-cooled to room temperature to obtain a handicraft ceramic. The preparation method of the whisker-based effector is as follows: S1: Preparation of graphene effect liquid: S11: irradiating the graphene flakes with protons for 5-10 minutes at an irradiation power of 350-400 W, and obtaining irradiated graphene flakes after the irradiation is completed; S12: ultrasonically mixing the irradiated graphene flakes and the lanthanum nitrate solution in a weight ratio of 2:5, and then finishing the ultrasonication to obtain lanthanum-doped graphene flakes; S13: 4-6 parts of lanthanum-doped flake graphene, 2-5 parts of 5% by mass sodium lignin sulfonate solution, 1-3 parts of chitosan solution and 2-4 parts of carboxymethyl cellulose are mixed and milled thoroughly at a ball milling speed of 1500 r / min for 2 h to obtain a graphene effect solution; S2: mixing the silicon carbide whiskers in a sufficient amount of a phosphate buffer solution having a pH value of 5.0 to obtain a whisker dispersion; S3: mixing the whisker dispersion and the graphene effect liquid in a weight ratio of 5:3, and after the stirring is completed, washing with water and drying to obtain an effect agent based on whisker adjustment; The preparation method of the nano silicon dioxide modifier is: S101: firstly heat the nano-silicon dioxide to 150-160°C at a rate of 1-3°C / min, keep the temperature for 5-10 minutes, then heat the nano-silicon dioxide to 275-285°C at a rate of 2-5°C / min, keep the temperature for 2-5 minutes, and finally air-cool to room temperature; S102: adding 1-3 parts of yttrium oxide and 2-5 parts of nano-bentonite to 4-7 parts of 6% by mass sodium dodecylbenzene sulfonate solution, and then adding 2-4 parts of silane coupling agent KH560 and 0.5-0.7 parts of stearic acid and mixing well to obtain a modified solution; S103: The nano-silicon dioxide treated in S101 and the modified liquid obtained in S102 are stirred and modified in a weight ratio of 3:
7. After the modification is completed, the nano-silicon dioxide is washed, filtered and dried to obtain a nano-silicon dioxide modifier. The preparation method of the zirconium oxide regulator is: 2-5 parts of aluminum silicate fiber, 1-3 parts of citric acid, 4-7 parts of 5% by mass sodium alginate solution and 2-5 parts of silane coupling agent KH550 are fully mixed to obtain an aluminum silicate fiber solution; The zirconium oxide is preheated at 55-65°C for 10-15 minutes, then added into a sufficient amount of aluminum silicate fiber solution and immersed in ultrasonic treatment. After the immersion is completed, the fiber is washed with water, filtered and dried to obtain a zirconium oxide regulator.
2. The method for preparing handicraft ceramics according to claim 1, characterized in that: The ultrasonic power of the ultrasonic mixing treatment is 350-400W, and the ultrasonic time is 20-30min; the stirring temperature of the mixed stirring treatment is 50-55°C, the stirring speed is 550-650r / min, and the stirring is 20-30min.
3. The method for preparing handicraft ceramics according to claim 1, characterized in that: The mass fraction of the lanthanum nitrate solution is 2-5%; the mass fraction of the chitosan solution is 3-6%.
4. The method for preparing handicraft ceramics according to claim 1, characterized in that: The stirring speed of the stirring modification treatment is 550-750 r / min, and the stirring time is 40-50 min.
5. The method for preparing handicraft ceramics according to claim 1, characterized in that: The ultrasonic power of the immersion ultrasonic treatment is 350-400W, and the ultrasonic time is 20-30min.
6. A handicraft ceramic prepared by the preparation method of the handicraft ceramic according to any one of claims 1 to 5.