MIM process for flexible pulley of harmonic reducer

Through the metal powder injection molding process, the problems of high cost and low efficiency of traditional soft wheel processing are solved, and efficient, low cost and high-quality soft wheel production are achieved, which meets the long-term use requirements under alternating stress conditions and improves the Mechanical properties and fatigue resistance.

CN118663903BActive Publication Date: 2024-11-01GANNAN UNIV OF SCI & TECH +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411147038.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-01
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

The traditional soft wheel processing method has problems such as high cost, low efficiency, complex molding process and low dimensional accuracy, and it is difficult to meet the long-term use requirements under alternating stress conditions.

Method used

Using metal powder injection molding (MIM) technology, the integrated molding of the harmonic reducer soft wheel is achieved through the mixing, refining, granulation, injection molding, degreasing, sintering and solid solution treatment of alloy powder and binder. High-strength steel powder and optimized process parameters improve material density and mechanical properties.

Benefits of technology

It greatly improves molding efficiency, reduces production costs, reduces subsequent processing steps, improves material utilization and yield, ensures the mechanical properties and fatigue resistance of the flexible wheel when it is subjected to alternating stress for a long time, and meets the efficiency, greenness and high efficiency of modern manufacturing industry. The demand for sustainable production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118663903B_ABST
    Figure CN118663903B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of metal powder injection molding, and specifically to a MIM process for a harmonic reducer flexible wheel, comprising the following steps: mixing alloy powder with a binder and adding the mixture to a mixer for mixing, feeding the obtained feed into a granulator to prepare fixed particles, loading the mixture into an injection machine for heating and melting, injecting the mixture into a mold for molding, cooling and opening the mold to take out the obtained blank, degreasing the blank after catalytic degreasing with nitric acid, and rapidly cooling the obtained sintered part after solution treatment to obtain a harmonic reducer flexible wheel. The present invention adopts metal powder injection molding, mixing alloy powder with a binder for internal mixing, feeding granulation, injection molding, blank degreasing, atmosphere sintering, solution treatment, and rapid cooling to achieve integrated molding of a harmonic reducer flexible wheel. Compared with traditional metal cutting processes, the present invention can greatly improve molding efficiency, shorten processing cycle, reduce production costs, and meet the requirements of integrated molding of complex shapes, reduce subsequent processing steps, and improve material utilization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal powder injection molding, and in particular to a MIM process for a flexible wheel of a harmonic reducer. Background Art

[0002] Harmonic reducers are widely used in high-tech fields such as robotics, aerospace, and instrumentation due to their small size, light weight, and superior transmission performance. The flexspline is the core component. The flexspline structure is characterized by thin walls and large deformation during operation, so it has high requirements on toughness. The flexspline is the most complex component in the harmonic reducer and is also the component most prone to failure in the harmonic reducer.

[0003] Usually, the processing of flexible splines is divided into the processing of flexible spline blanks and the processing of flexible spline teeth. The flexible spline blanks are made by conventional processing methods such as precision turning, grinding, and drilling, while the processing of gear teeth relies on professional gear tools. However, small-modulus gear tools face the problems of high manufacturing costs and technical bottlenecks. Although some companies use high-precision slow-wire cutting technology to process flexible splines, this technology has very high requirements on the positioning accuracy of the tooling, which limits large-scale production.

[0004] In summary, the traditional flexible wheel processing method still has the problems of high processing cost, complex molding process and low dimensional accuracy. A low-cost and high-efficiency production process is urgently needed, and the gear is required to meet the working life requirements of the harmonic reducer flexible wheel under the operating conditions of alternating stress. In recent years, metal powder injection molding (MIM) has introduced modern plastic injection molding technology into the field of powder metallurgy to form a new type of powder metallurgy near-net shape molding technology, which has the advantages of high precision and low cost. Therefore, the present invention provides a MIM process for a harmonic reducer flexible wheel to solve the above problems. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, an object of the present invention is to provide a MIM process for a flexible spline of a harmonic reducer.

[0006] A MIM process for a harmonic reducer flexible wheel includes the following steps:

[0007] S1: uniformly mix the alloy powder and the binder, add them into an internal mixer, mix them at 100-150°C for 2-4h, set the melt index range to 1200-1500g / min, and obtain feed;

[0008] S2: feeding the mixed feed into a granulator to prepare fixed particles of uniform size that are convenient for injection molding;

[0009] S3: loading the pellets into the barrel of an injection machine, heating and melting them, injecting the molten feed into a mold under high pressure to form the pellets, and opening the mold to take them out after cooling to obtain a high-strength steel alloy blank;

[0010] S4: using 98% nitric acid to catalytically degrease at 500±5°C to remove the organic binder in the blank to obtain a degreased blank;

[0011] S5: Sintering in an argon protective atmosphere, the sintering temperature is controlled at 1150-1350℃, and the duration is 2-3h, ensuring that the sintering density is greater than 7.6g / cm 3 , the shrinkage ratio is controlled within the range of 1.165±0.003 to obtain a sintered part;

[0012] S6: The sintered alloy is heated to 1035-1045°C, kept at this temperature for 1-2 hours to complete the solution treatment, and then rapidly cooled with a cooling medium to obtain a harmonic reducer flexible wheel.

[0013] Furthermore, the alloy powder has a yield strength of ≥1800 MPa, an elongation of ≥8%, and a surface Rockwell hardness of ≥40 HRC.

[0014] Furthermore, the alloy powder is prepared by using high-strength steel powder.

[0015] Furthermore, the high-strength steel powder includes, by mass percentage, 0.15-0.3% carbon, 12-20% chromium, 1-3% molybdenum, 1-5% nickel, 1-2% tungsten, 0.3-0.5% niobium, 0.3-0.5% titanium, and the remainder is iron and other trace elements.

[0016] Furthermore, the alloy powder preparation method is: adding high-strength steel powder into a ball mill for ball milling, with a ball-to-material ratio of 5-15:1 by mass, a ball milling vacuum degree of less than 50 kPa, a ball milling speed of 300-1500 r / min, a ball milling time of 3-10 h, and a ball milling temperature of less than 80°C.

[0017] Furthermore, the binder is a wax-based binder, a polymer binder and a functional additive.

[0018] Furthermore, the amount of the binder accounts for 6-15% of the total mass of the feed.

[0019] Furthermore, the adhesive component includes 30-50% wax-based material, 10-30% polyvinyl alcohol, 5-20% polyacrylate, 5-10% plasticizer, 3-5% cross-linking agent, 0.5-2% lubricant and 3-5% other additives.

[0020] Furthermore, the solution treatment is carried out in an argon protective atmosphere with a gas pressure of 5-100 kPa.

[0021] Furthermore, the cooling medium is nitrogen, argon or a mixture of nitrogen and argon, and the cooling rate is greater than 50°C / min.

[0022] The present invention has the following beneficial effects: 1. The present invention adopts metal powder injection molding (MIM) and utilizes alloy powder injection molding to produce a flexible wheel. The alloy powder is mixed with a binder and kneaded, the feed is granulated, injection molded, the blank is degreased, and then atmosphere sintered, solution treated, and rapidly cooled to achieve integrated molding of the harmonic reducer flexible wheel. Compared with traditional metal cutting processes, the molding efficiency can be greatly improved, the processing cycle can be shortened, the production cost can be reduced, and the integrated molding of complex shapes can be met, the subsequent processing steps can be reduced, and the material utilization rate can be improved.

[0023] 2. The present invention adopts high-strength steel powder as alloy powder raw material, which can improve the density and uniformity of the material, and optimize the fluidity of the feed so that the mold can be filled more fully during the injection molding process, thereby reducing defects and improving the yield rate. At the same time, the process controls the oxygen content of the powder and reduces oxide inclusions, which can ensure the toughness of the flexible wheel while improving the mechanical properties and fatigue resistance of the material, ensuring that the flexible wheel can still meet its life requirements in a working environment that is subjected to alternating stress for a long time.

[0024] 3. The present invention adopts MIM process to directly form parts with complex geometric shapes and fine features, such as the gear tooth structure of the flexible wheel, which reduces the subsequent processing steps and reduces the dimensional accuracy problem caused by the cumulative error of multiple processing.

[0025] 4. The present invention can solve the problems of high processing cost, low efficiency and insufficient material performance of flexible wheels in the prior art, and realize efficient, low-cost and high-quality flexible wheel production. The process can improve the comprehensive performance of the flexible wheel, including toughness and extend service life. At the same time, it also meets the needs of modern manufacturing industry for efficient, green and sustainable production models.

[0026] 5. The flexible wheel of the present invention adopts a powder injection processing method, which can improve processing efficiency and facilitate the control of processing and production accuracy by adjusting equipment production equipment parameters. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The figure is a flow chart of the MIM process of the flexible pulley of the harmonic reducer adopted in the embodiment of the present invention.

[0028] Figure 2 This is a schematic diagram of the structure of the harmonic reducer used in an embodiment of the present invention.

[0029] Figure 3 The figure is a schematic diagram of the flexible wheel structure of the harmonic reducer adopted in the embodiment of the present invention.

[0030] Among them, 1-steel wheel, 2-flexible wheel, 3-wave generator. DETAILED DESCRIPTION

[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] The main structure of the harmonic reducer referred to in the following embodiments is as follows: Figure 2 and Figure 3 As shown, it is composed of a rigid wheel, a flexible wheel and a wave generator. The transmission principle of the harmonic reducer is to rotate the elliptical wave generator to make the flexible wheel produce controllable elastic deformation and generate a moving deformation wave. This waveform meshes with the rigid wheel teeth. Due to the elastic deformation of the flexible wheel, the transmission purpose is achieved.

[0033] Example 1: A MIM process for a harmonic reducer flexspline, such as Figure 1 As shown, the following steps are included:

[0034] S1: uniformly mix the alloy powder and the binder, add them into an internal mixer, mix them at 120°C for 2h, set the melt index range to 1350g / min, and obtain the feed;

[0035] S2: feeding the mixed feed into a granulator to prepare fixed particles of uniform size that are convenient for injection molding;

[0036] S3: loading the pellets into the barrel of an injection machine, heating and melting them, injecting the molten feed into a mold under high pressure to form the pellets, and opening the mold to take them out after cooling to obtain a high-strength steel alloy blank;

[0037] S4: using 98% nitric acid to perform catalytic degreasing at 500°C to remove the organic binder in the blank to obtain a degreased blank;

[0038] S5: Sintering in an argon protective atmosphere, the sintering temperature is controlled at 1250℃, and the duration is 2.5h, ensuring that the sintering density is greater than 7.6g / cm 3 , the shrinkage ratio is controlled within the range of 1.165±0.003 to obtain a sintered part;

[0039] S6: The sintered alloy is heated to 1040°C, kept warm for 1.5 hours, and solution treated in an argon protective atmosphere with a gas pressure of 50 kPa. Then, argon is used for rapid cooling at a cooling rate of 80°C / min to obtain a harmonic reducer flexible wheel.

[0040] The alloy powder is prepared from high-strength steel powder, which includes, by mass percentage, 0.25% carbon, 15% chromium, 2% molybdenum, 3% nickel, 1.5% tungsten, 0.4% niobium, 0.4% titanium, and the remainder is iron and other trace elements.

[0041] The preparation method of the alloy powder is as follows: adding high-strength steel powder into a ball mill for ball milling, with a ball-to-material ratio of 10:1 by mass, a ball milling vacuum of 45 kPa, a ball milling speed of 1000 r / min, a ball milling time of 5 h, and a ball milling temperature of 75°C, ensuring that the yield strength of the alloy powder is ≥1800 MPa, the elongation is ≥8%, and the surface Rockwell hardness is ≥40 HRC.

[0042] The binder components include 45% wax-based material (paraffin), 20% polyvinyl alcohol, 15% polyacrylate, 7.5% plasticizer (environmentally friendly dioctyl phthalate), 4% cross-linking agent (N,N'-methylenebisacrylamide), 1.5% lubricant (zinc stearate) and 3% other additives (antioxidant and antistatic agent in a mass ratio of 1:1). The amount of binder accounts for 10% of the total feed mass.

[0043] Embodiment 2: A MIM process for a harmonic reducer flexible wheel, such as Figure 1 As shown, the following steps are included:

[0044] S1: uniformly mix the alloy powder and the binder, add them into an internal mixer, mix them at 100°C for 3h, and set the melt index range to 1250g / min to obtain feed;

[0045] S2: feeding the mixed feed into a granulator to prepare fixed particles of uniform size that are convenient for injection molding;

[0046] S3: loading the pellets into the barrel of an injection machine, heating and melting them, injecting the molten feed into a mold under high pressure to form the pellets, and opening the mold to take them out after cooling to obtain a high-strength steel alloy blank;

[0047] S4: using 98% nitric acid to catalytically degrease at 545°C to remove the organic binder in the blank to obtain a degreased blank;

[0048] S5: Sintering in an argon protective atmosphere, the sintering temperature is controlled at 1150°C, and the duration is 3 hours, ensuring that the sintering density is greater than 7.6g / cm 3 , the shrinkage ratio is controlled within the range of 1.165±0.003 to obtain a sintered part;

[0049] S6: The sintered alloy is heated to 1035°C, kept at this temperature for 2 hours, and solution treated in an argon protective atmosphere with a gas pressure of 80 kPa. Then, nitrogen is used for rapid cooling at a cooling rate of 60°C / min to obtain a harmonic reducer flexible wheel.

[0050] The alloy powder is prepared from high-strength steel powder, which includes, by mass percentage, 0.2% carbon, 13% chromium, 1.5% molybdenum, 2% nickel, 1.2% tungsten, 0.3% niobium, 0.3% titanium, and the remainder is iron and other trace elements.

[0051] The preparation method of the alloy powder is as follows: adding high-strength steel powder into a ball mill for ball milling, with a ball-to-material ratio of 12:1 by mass, a ball milling vacuum of 45 kPa, a ball milling speed of 800 r / min, a ball milling time of 3 h, and a ball milling temperature of 75°C, ensuring that the yield strength of the alloy powder is ≥1800 MPa, the elongation is ≥8%, and the surface Rockwell hardness is ≥40 HRC.

[0052] The binder components include 50% wax-based material (paraffin), 15% polyvinyl alcohol, 12% polyacrylate, 8.5% plasticizer (environmentally friendly dioctyl phthalate), 3% cross-linking agent (N,N'-methylenebisacrylamide), 1.2% lubricant (zinc stearate) and 4% other additives (antioxidant and antistatic agent in a mass ratio of 1:1). The amount of binder accounts for 12% of the total feed mass.

[0053] Embodiment 3: A MIM process for a harmonic reducer flexible wheel, such as Figure 1 As shown, the following steps are included:

[0054] S1: uniformly mix the alloy powder and the binder, add them into an internal mixer, mix them at 140°C for 2.5h, and set the melt index range to 1450g / min to obtain feed;

[0055] S2: feeding the mixed feed into a granulator to prepare fixed particles of uniform size that are convenient for injection molding;

[0056] S3: loading the pellets into the barrel of an injection machine, heating and melting them, injecting the molten feed into a mold under high pressure to form the pellets, and opening the mold to take them out after cooling to obtain a high-strength steel alloy blank;

[0057] S4: using 98% nitric acid to catalytically degrease at 505°C to remove the organic binder in the blank to obtain a degreased blank;

[0058] S5: Sintering in an argon protective atmosphere, the sintering temperature is controlled at 1350℃, and the duration is 2h, ensuring that the sintering density is greater than 7.6g / cm 3 , the shrinkage ratio is controlled within the range of 1.165±0.003 to obtain a sintered part;

[0059] S6: The sintered alloy is heated to 1045°C, kept warm for 1 hour, and solution treated in an argon protective atmosphere with a gas pressure of 100 kPa. Then, argon is used for rapid cooling at a cooling rate of 100°C / min to obtain a harmonic reducer flexible wheel.

[0060] The alloy powder is prepared from high-strength steel powder, which includes, by mass percentage, 0.3% carbon, 18% chromium, 2.5% molybdenum, 4% nickel, 2% tungsten, 0.5% niobium, 0.5% titanium, and the remainder is iron and other trace elements.

[0061] The alloy powder preparation method is as follows: adding high-strength steel powder into a ball mill for ball milling, with a ball-to-material ratio of 15:1 by mass, a ball milling vacuum of 45 kPa, a ball milling speed of 1200 r / min, a ball milling time of 4 hours, and a ball milling temperature of 75°C, ensuring that the yield strength of the alloy powder is ≥1800 MPa, the elongation is ≥8%, and the surface Rockwell hardness is ≥40 HRC.

[0062] The binder components include 37% wax-based materials (paraffin), 25% polyvinyl alcohol, 18% polyacrylate, 5% plasticizer (environmentally friendly dioctyl phthalate), 5% cross-linking agent (N,N'-methylenebisacrylamide), 2% lubricant (zinc stearate) and 5% other additives (antioxidant and antistatic agent in a mass ratio of 1:1). The amount of binder accounts for 8% of the total feed mass.

[0063] Comparative example: The traditional machining process of the flexible wheel of the harmonic reducer includes the following steps:

[0064] S1: Cutting bar material (medium carbon alloy steel substrate, SNCM439) for blanking;

[0065] S2: heating the bar to 950°C and forging and shaping the bar through a forging die;

[0066] S3: normalizing the forged and shaped flexspline blank at a temperature of 920°C for 3 hours, and then air-cooling the flexspline blank to room temperature with the furnace;

[0067] S4: Rough turning the flexspline blank by CNC lathe, leaving 1.5mm machining allowance on one side;

[0068] S5: quenching and tempering treatment of the flexible wheel, quenching temperature 860℃, tempering temperature 540℃;

[0069] S6: Use the CNC lathe again for semi-finishing machining, leaving a machining allowance of 0.1mm on one side;

[0070] S7: stress relief treatment, temperature 220℃, keep warm for 12 hours;

[0071] S8: Use a surface grinder to grind the end face of the flexible wheel boss, and then use a composite grinder to grind the inner hole and outer circle to the final size of the drawing, ensuring that the concentricity is within 0.003mm;

[0072] S9: stress relief treatment, temperature 220℃, keep warm for 12 hours;

[0073] S10: Use CNC lathe for finishing, turning all the outer circles and end faces of the flexible wheel into place;

[0074] S11: stress relief treatment, temperature 220℃, heat preservation for 12 hours;

[0075] S12: Use gear hobbing machine to process the flexible wheel teeth to the requirements of the drawing.

[0076] Test example: testing the hardness, yield point and tensile strength of the flexible pulley of the harmonic reducer of Examples 1 to 3 and the comparative example;

[0077] Hardness test: The Rockwell hardness test method (HRC scale) is used to evaluate the hardness of the surface of the harmonic reducer flexspline to understand the material's ability to resist local plastic deformation.

[0078] Yield strength test: Through tensile testing, the stress value when the material begins to produce obvious plastic deformation, that is, the yield point, is measured in megapascals (MPa), so as to evaluate the initial resistance of the material when bearing load.

[0079] Tensile strength test: Also in the tensile test, the maximum stress value that the material can withstand before breaking is recorded, that is, the tensile strength, which is measured in megapascals (MPa) and reflects the maximum load-bearing capacity of the material.

[0080] Table 1 Hardness, yield point, tensile strength test results

[0081] Example 1 Example 2 Example 3 Comparative Example Hardness (HRC) 55.8 56.5 55.5 38.6 Yield point (MPa) 392 401 386 315 Tensile strength (MPa) 596 591 602 519

[0082] As shown in Table 1, Example 1: hardness 55.8HRC, yield point 392MPa, tensile strength 596MPa;

[0083] Example 2: hardness 56.5HRC, yield point 401MPa, tensile strength 591MPa;

[0084] Example 3: hardness 55.5HRC, yield point 386MPa, tensile strength 602MPa;

[0085] Comparative example: hardness 38.6HRC, yield point 315MPa, tensile strength 519MPa;

[0086] In summary, the flexible wheel of the harmonic reducer manufactured by the MIM process of the present invention has good wear resistance, deformation resistance and fatigue resistance, and meets the needs of industry use.

[0087] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical ideas disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A MIM process for a harmonic reducer flexible wheel, characterized in that: The specific steps include: S1: uniformly mix the alloy powder and the binder, add them into an internal mixer, mix them at 100-150°C for 2-4h, set the melt index range to 1200-1500g / min, and obtain feed; S2: feeding the mixed feed into a granulator to prepare fixed particles of uniform size that are convenient for injection molding; S3: loading the pellets into the barrel of the injection machine, heating and melting them, injecting the molten feed into the mold under high pressure to form them, and opening the mold to take them out after cooling to obtain a high-strength steel alloy blank; S4: using 98% nitric acid to catalytically degrease at 500±5°C to remove the organic binder in the blank to obtain a degreased blank; S5: Sintering in an argon protective atmosphere, the sintering temperature is controlled at 1150-1350℃, and the duration is 2-3h, ensuring that the sintering density is greater than 7.6g / cm 3 , the shrinkage ratio is controlled within the range of 1.165±0.003 to obtain a sintered part; S6: The sintered alloy is heated to 1035-1045°C, kept at this temperature for 1-2 hours to complete the solution treatment, and then rapidly cooled with a cooling medium to obtain a harmonic reducer flexible wheel.

2. The MIM process of a harmonic reducer flexspline according to claim 1 is characterized in that: The alloy powder has a yield strength of ≥1800 MPa, an elongation of ≥8%, and a surface Rockwell hardness of ≥40 HRC.

3. The MIM process of a harmonic reducer flexspline according to claim 1 is characterized in that: The alloy powder is prepared by adopting high-strength steel powder.

4. The MIM process of a harmonic reducer flexspline according to claim 3 is characterized in that: The high-strength steel powder includes, by mass percentage, 0.15-0.3% carbon, 12-20% chromium, 1-3% molybdenum, 1-5% nickel, 1-2% tungsten, 0.3-0.5% niobium, 0.3-0.5% titanium, and the remainder is iron and other trace elements.

5. The MIM process of a harmonic reducer flexspline according to claim 3 is characterized in that: The alloy powder preparation method comprises: adding high-strength steel powder into a ball mill for ball milling, wherein the ball-to-material ratio is 5-15:1 by mass, the ball milling vacuum is less than 50 kPa, the ball milling speed is 300-1500 r / min, the ball milling time is 3-10 h, and the ball milling temperature is less than 80° C.

6. The MIM process of a harmonic reducer flexspline according to claim 1 is characterized in that: The binder is a wax-based binder, a polymer binder and a functional additive.

7. The MIM process of a harmonic reducer flexspline according to claim 6, characterized in that: The amount of the binder is 6-15% of the total mass of the feed.

8. The MIM process of a harmonic reducer flexspline according to claim 7, characterized in that: The adhesive component includes 30-50% wax-based material, 10-30% polyvinyl alcohol, 5-20% polyacrylate, 5-10% plasticizer, 3-5% cross-linking agent, 0.5-2% lubricant and 3-5% other additives, and the other additives are antioxidant and antistatic agent, and the mass ratio of antioxidant to antistatic agent is 1:

1.

9. The MIM process of a harmonic reducer flexspline according to claim 1, characterized in that: The solution treatment is carried out in an argon protective atmosphere with a gas pressure of 5-100 kPa.

10. The MIM process of a harmonic reducer flexspline according to claim 1, characterized in that: The cooling medium is nitrogen, argon or a mixture of nitrogen and argon, and the cooling rate is greater than 50°C / min.

Citation Information

Cited By

  • Material for harmonic reducer flexible gear and blank machining method