A test method for X-ray diffraction of polytetrafluoroethylene suspension resin
By calculating the particle size range, screening and molding treatment, the problem of insufficient stability in X-ray diffraction analysis of polytetrafluoroethylene resin is solved, and the stability of the X-ray diffraction pattern of polytetrafluoroethylene suspension resin is improved.
Patent Information
- Application Number
- CN202411157776.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-22
AI Technical Summary
In X-ray diffraction analysis, polytetrafluoroethylene resin has small particle size and high surface activity, resulting in fluctuations in agglomeration and diffraction particle size, affecting the stability of the analysis.
By calculating the particle size range of the sample to be tested, screening and molding it into a diaphragm, combining ultrasonic dispersion and circulating spraying treatment, ensuring that the particle size is distributed within a specific range and reducing the fluctuations in X-ray diffraction intensity.
The stability of the X-ray diffraction pattern of polytetrafluoroethylene suspension resin was significantly improved, and the average diffraction intensity fluctuated between 0.01% and 0.5%.
Smart Images

Figure CN118671114B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polytetrafluoroethylene resin analysis, and specifically relates to a polytetrafluoroethylene suspension resin X-ray diffraction testing method. Background Art
[0002] The structure of polymer materials is complex at multiple scales. Analyzing the microstructure of polymer materials at all levels and establishing the relationship between structure and performance are important goals and challenges in the field of polymer research. For crystalline polymers, the characterization and analysis of their crystal structure is crucial. X-ray diffraction is the most classic and commonly used method for analyzing polymer crystal structures.
[0003] Polytetrafluoroethylene is a polymer material with special properties. It occupies an extremely important position among new materials and is widely used in aerospace, electronics, metallurgy, medicine, semiconductors and other fields. However, there are many problems when using X-ray diffraction to analyze polytetrafluoroethylene resin.
[0004] X-ray diffraction requires that there are a sufficient number of crystal grains in the volume of the irradiated sample, and the sample particles are uniform, which is conducive to suppressing the preferred orientation caused by crystal habit; and in quantitative analysis, the effects of extinction and micro-absorption effects on diffraction intensity can be ignored. However, due to its small particle size and high surface activity, polytetrafluoroethylene resin is very easy to agglomerate and form larger agglomerates, which leads to obvious fluctuations in the number of diffracted crystal grains and the size of diffracted particles during the X-ray diffraction analysis, which in turn leads to large fluctuations in the X-ray diffraction intensity and poor stability, affecting the analysis of the microstructure of polytetrafluoroethylene resin. Summary of the invention
[0005] The object of the present invention is to provide a method for testing polytetrafluoroethylene suspension resin by X-ray diffraction in view of the problem that the existing X-ray diffraction testing method has insufficient stability, so that the X-ray diffraction spectrum of the polytetrafluoroethylene suspension resin has excellent stability.
[0006] The technical solution of the present invention is: a test method for polytetrafluoroethylene suspension resin X-ray diffraction, comprising the following steps:
[0007] (1) Calculate the particle size range required for the sample to be tested:
[0008] First, the median particle size D of the polytetrafluoroethylene suspension resin to be tested is analyzed and measured. 50 The median particle size D was determined by laser particle size analyzer. 50 . D 50 Represents the size at which the cumulative particle size distribution is 50%, which is most representative for polytetrafluoroethylene.
[0009] Then, the median particle size D 50The particle size range of the sample to be tested is calculated according to the following standard: median particle size D 50 Value × 80% ≤ Particle size of the sample to be tested ≤ Median particle size D 50 value × 120%, and 15%≤ ×100%≤35%.
[0010] As is known to all, X-ray diffraction is mainly detected by reflection, and the sample stage is a circular groove with a length of less than 2 cm. During detection, X-rays hit the sample, reflect to the detector, and the signal is received by the instrument. Based on this mechanism, the present invention has found that when the particle size range of the polytetrafluoroethylene suspension resin sample to be tested meets the above calculation standard, the fluctuation of the X-ray diffraction intensity is significantly reduced, thereby greatly improving the stability of the test method.
[0011] (2) Screening out the samples to be tested in the required particle size range:
[0012] First, add the polytetrafluoroethylene suspension resin to be tested into an organic solvent and perform ultrasonic dispersion to obtain a polytetrafluoroethylene suspension resin dispersion. Because PTFE particles are agglomerated particles, they are very easy to agglomerate, resulting in uneven sample particle size. This operation can avoid self-agglomeration of polytetrafluoroethylene resin particles.
[0013] Then, a sieve is selected based on the particle size range calculated in step (1), and the obtained polytetrafluoroethylene suspension resin dispersion is screened using the selected sieve, and an organic solvent is used for circulating spraying during the screening. The lower limit of the aperture size corresponding to the mesh number of the sieve is 80%-95% of the median particle size D50, and the upper limit is 105%-120% of the median particle size D50.
[0014] Finally, the sieved polytetrafluoroethylene suspension resin is dried to obtain a sample to be tested.
[0015] (3) Molding: Weigh the sample to be tested obtained in step (2) and add it into a mold. Use a press to mold the sample to be tested at a pressure of 2-30 MPa to obtain a diaphragm to be tested.
[0016] The present invention has found that the molding pressure also has a certain influence on the diffraction intensity, and molding within the pressure range can ensure the stability of the X-ray diffraction results.
[0017] (4) Testing: The film obtained in step (3) is tested using an X-ray diffractometer. The fluctuation of the average diffraction intensity of the obtained X-ray diffraction pattern is between 0.01% and 0.5%.
[0018] In the present invention, the X-ray diffraction test method for polytetrafluoroethylene suspension resin, in which the particle size range of the sample to be tested in step (1) is: median particle size D50 Value × 90% ≤ Particle size of the sample to be tested ≤ Median particle size D 50 value × 110%, and 16%≤ ×100%≤20%.
[0019] In the present invention, in the X-ray diffraction testing method for polytetrafluoroethylene suspension resin, the organic solvent in step (2) is one or more of methanol, ethanol or isopropanol.
[0020] In the present invention, in the X-ray diffraction test method for polytetrafluoroethylene suspension resin, the ultrasonic dispersion time in step (2) is at least 60 minutes.
[0021] In the present invention, in the test method for polytetrafluoroethylene suspension resin by X-ray diffraction, the sieve selected in step (2) is a nickel mesh precision sieve.
[0022] In the present invention, in the X-ray diffraction test method for polytetrafluoroethylene suspension resin, the spraying flow rate in step (2) is 1-5 L / min, and the spraying time is at least 20 minutes.
[0023] In the present invention, in the X-ray diffraction test method for polytetrafluoroethylene suspension resin, the drying temperature in step (2) is 60-100° C. and the drying time is at least 6 hours.
[0024] In the present invention, in the X-ray diffraction testing method for polytetrafluoroethylene suspension resin, the mold in step (3) is cylindrical and has a diameter of 1.5-2.0 cm.
[0025] Furthermore, in the test method for polytetrafluoroethylene suspension resin X-ray diffraction, in step (3), 0.5-2 g of the sample to be tested obtained in step (2) is weighed and added into the mold.
[0026] The beneficial effects of the present invention are as follows: the testing method for polytetrafluoroethylene suspension resin X-ray diffraction of the present invention first calculates the particle size range that the polytetrafluoroethylene suspension resin sample to be tested needs to meet according to the standard; then the tested samples that meet the requirements are screened according to the particle size range; and finally, the tested samples are molded into flat membranes and tested on a machine.
[0027] The test method has excellent stability when using X-ray diffraction to test polytetrafluoroethylene suspension resin, and the measured X-ray diffraction spectrum has good stability, and the fluctuation of the average diffraction intensity is 0.01%-0.5%. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The XRD diffraction patterns are obtained from five tests in Example 1 (the X-axis of each data test result is increased by 2°).
[0029] Figure 2 The XRD diffraction patterns of the five tests in Comparative Example 1 (the X-axis of each data test result is increased by 2°). DETAILED DESCRIPTION
[0030] The present invention will be further described below in conjunction with specific embodiments.
[0031] 1. PTFE resins DF-16A and DF-106 were purchased from Shandong Dongyue Polymer Materials Co., Ltd.
[0032] 2. The average particle size of DF-16A is 20-30μm; the average particle size of DF-106 is 200-250μm.
[0033] 3. Average particle size test: refer to the standards "GB / T 19077-2016 Particle size analysis laser diffraction method" and "GB / T29022-2021 Particle size analysis dynamic light scattering method".
[0034] 4. Laser particle size analyzer: Model HORIBA-LA-960; Dandong Better-2600LD.
[0035] 5. X-ray diffractometer: Shimadzu XRD-6100, Japan.
[0036] Example 1
[0037] The test method of X-ray diffraction of polytetrafluoroethylene suspension resin comprises the following specific steps:
[0038] (1) Calculate the particle size range required for the sample to be tested:
[0039] First, the median particle size D of the polytetrafluoroethylene suspension resin DF-16A to be tested was measured by laser particle size analyzer. 50 is 25μm.
[0040] Then, the median particle size D 50 As the reference particle size, calculate the particle size range of the sample to be tested according to the following standards:
[0041] The maximum particle size of the sample DF-16A to be tested = 25×108% = 27μm; the minimum particle size of the sample DF-16A to be tested = 25×92% = 23μm.
[0042] in, = ×100%=16%.
[0043] (2) Screening out the samples to be tested in the required particle size range:
[0044] First, 50 g of the polytetrafluoroethylene suspension resin to be tested was added to the organic solvent methanol and ultrasonically dispersed for 80 minutes to obtain a polytetrafluoroethylene suspension resin dispersion.
[0045] Then, a nickel mesh precision sieve is selected based on the particle size range calculated in step (1), wherein the mesh number of the top sieve is 560 mesh and the mesh number of the bottom sieve is 650 mesh. The obtained polytetrafluoroethylene suspension resin dispersion is electrically screened using the selected nickel mesh precision sieve, and the organic solvent methanol is used for circulating spraying during the screening, with a spraying flow rate of 3 L / min and a spraying time of 40 min.
[0046] Finally, the polytetrafluoroethylene suspension resin on the 650-mesh sieve was placed in an oven at 80° C. and dried for 10 h to obtain a sample to be tested.
[0047] (3) Molding: Weigh 1 g of the sample to be tested obtained in step (2) and add it to a cylindrical mold with a diameter of 2.0 cm. Use a press to mold the sample to be tested at a pressure of 15 MPa to obtain a membrane to be tested.
[0048] (4) Testing: The film obtained in step (3) is tested using an X-ray diffractometer.
[0049] Step (3) and step (4) were repeated 5 times, i.e., the test was performed 5 times. The diffraction intensity, average diffraction intensity and fluctuation of the diffraction intensity of each test data obtained 5 times are summarized in Table 1.
[0050] Example 2
[0051] The test method of X-ray diffraction of polytetrafluoroethylene suspension resin comprises the following specific steps:
[0052] (1) Calculate the particle size range required for the sample to be tested:
[0053] First, the median particle size D of the polytetrafluoroethylene suspension resin DF-106 to be tested was measured by laser particle size analyzer. 50 It is 230μm.
[0054] Then, the median particle size D 50 As the reference particle size, calculate the particle size range of the sample to be tested according to the following standards:
[0055] The maximum particle size of the sample DF-106 to be tested = 230×108.7%=250μm; the minimum particle size of the sample DF-106 to be tested = 230×91.3%=210μm.
[0056] in, = ×100%=17.4%.
[0057] (2) Screening out the samples to be tested in the required particle size range:
[0058] First, 50 g of the polytetrafluoroethylene suspension resin to be tested was added to the organic solvent ethanol and ultrasonically dispersed for 70 minutes to obtain a polytetrafluoroethylene suspension resin dispersion.
[0059] Then, a nickel mesh precision sieve is selected based on the particle size range calculated in step (1), wherein the mesh number of the top sieve is 60 mesh and the mesh number of the bottom sieve is 70 mesh. The obtained polytetrafluoroethylene suspension resin dispersion is electrically screened using the selected nickel mesh precision sieve, and the organic solvent ethanol is used for circulating spraying at a spraying flow rate of 2 L / min and a spraying time of 30 min.
[0060] Finally, the polytetrafluoroethylene suspension resin on the 70-mesh sieve was placed in an oven at 90° C. and dried for 10 h to obtain a sample to be tested.
[0061] (3) Molding: Weigh 1 g of the sample to be tested obtained in step (2) and add it to a cylindrical mold with a diameter of 2.0 cm. Use a press to mold the sample to be tested at a pressure of 2 MPa to obtain a membrane to be tested.
[0062] (4) Testing: The film obtained in step (3) is tested using an X-ray diffractometer.
[0063] Repeat steps (3) and (4) for 5 times, i.e., test 5 times. The diffraction intensity, average diffraction intensity and fluctuation of diffraction intensity of each test data obtained 5 times are summarized in 1.
[0064] Example 3
[0065] The test method of X-ray diffraction of polytetrafluoroethylene suspension resin comprises the following specific steps:
[0066] (1) Calculate the particle size range required for the sample to be tested:
[0067] First, the median particle size D of the polytetrafluoroethylene suspension resin DF-106 to be tested was measured by laser particle size analyzer. 50 is 230μm.
[0068] Then, the median particle size D 50 As the reference particle size, calculate the particle size range of the sample to be tested according to the following standards:
[0069] The maximum particle size of the sample DF-106 to be tested = 230 × 117.4% = 270 μm; the minimum particle size of the sample DF-106 to be tested = 230 × 82.6% = 190 μm.
[0070] in, = ×100%=34.8%.
[0071] (2) Screening out the samples to be tested in the required particle size range:
[0072] First, 50 g of the polytetrafluoroethylene suspension resin to be tested was added to an organic solvent, isopropanol, and ultrasonic dispersion was performed for 70 minutes to obtain a polytetrafluoroethylene suspension resin dispersion.
[0073] Then, a nickel mesh precision sieve is selected based on the particle size range calculated in step (1), wherein the mesh number of the top sieve is 56 mesh and the mesh number of the bottom sieve is 78 mesh. The obtained polytetrafluoroethylene suspension resin dispersion is electrically screened using the selected nickel mesh precision sieve, and the organic solvent isopropanol is used for circulating spraying during the screening, with a spraying flow rate of 2 L / min and a spraying time of 30 min.
[0074] Finally, the polytetrafluoroethylene suspension resin on the 78-mesh sieve was placed in an oven at 90° C. and dried for 10 h to obtain a sample to be tested.
[0075] (3) Molding: Weigh 1 g of the sample to be tested obtained in step (2) and add it to a cylindrical mold with a diameter of 2.0 cm. Use a press to mold the sample to be tested at a pressure of 30 MPa to obtain a membrane to be tested.
[0076] (4) Testing: Perform an X-ray diffractometer test on the film obtained in step (3).
[0077] Step (3) and step (4) were repeated 5 times, i.e., the test was performed 5 times. The diffraction intensity, average diffraction intensity and fluctuation of the diffraction intensity of each test data obtained 5 times are summarized in Table 1.
[0078] Comparative Example 1
[0079] The difference between this comparative example and Example 1 is that the required particle size range of the sample to be tested is not calculated according to the standard and the sample to be tested with the required particle size range is not screened out, but 1g of DF-16A resin is weighed and directly molded and tested. The details are as follows:
[0080] (1) Molding: Weigh 1 g of DF-16A resin and add it to a cylindrical mold with a diameter of 2.0 cm. Use a press to mold the sample to be tested at a pressure of 15 MPa to obtain a diaphragm to be tested.
[0081] (2) Testing: The film obtained in step (1) is tested using an X-ray diffractometer.
[0082] Step (1) and step (2) were repeated 5 times, i.e., the test was performed 5 times. The diffraction intensity, average diffraction intensity and fluctuation of diffraction intensity of each test data obtained 5 times are summarized in Table 1.
[0083] Comparative Example 2
[0084] The difference between this comparative example and Example 2 is that the required particle size range of the sample to be tested is not calculated according to the standard and the sample to be tested with the required particle size range is not screened out, but 1g of DF-106 resin is weighed and directly molded and tested. The details are as follows:
[0085] (1) Molding: Weigh 1 g of DF-106 resin and add it to a cylindrical mold with a diameter of 2.0 cm. Use a press to mold the sample to be tested at a pressure of 2 MPa to obtain a diaphragm to be tested.
[0086] (2) Testing: Perform an X-ray diffractometer test on the film obtained in step (1).
[0087] Step (1) and step (2) were repeated 5 times, i.e., the test was performed 5 times. The diffraction intensity, average diffraction intensity and fluctuation of diffraction intensity of each test data obtained 5 times are summarized in Table 1.
[0088] Comparative Example 3
[0089] The difference between this comparative example and Example 1 is that the particle size range of the sample to be tested is calculated according to the following standard: the maximum particle size of the sample to be tested DF-16A = 25×160% = 40 μm; the minimum particle size of the sample to be tested DF-16A = 25×60% = 15 μm.
[0090] The test method of X-ray diffraction of polytetrafluoroethylene suspension resin comprises the following specific steps:
[0091] (1) Calculate the particle size range required for the sample to be tested:
[0092] First, the median particle size D of the polytetrafluoroethylene suspension resin DF-16A to be tested was measured by laser particle size analyzer. 50 is 25μm.
[0093] Then, the median particle size D 50 As the reference particle size, calculate the particle size range of the sample to be tested according to the following standards:
[0094] The maximum particle size of the sample DF-16A to be tested = 25×160% = 40μm; the minimum particle size of the sample DF-16A to be tested = 25×60% = 15μm.
[0095] in, = ×100%=100%.
[0096] (2) Screening out the samples to be tested in the required particle size range:
[0097] First, 50 g of the polytetrafluoroethylene suspension resin to be tested was added to the organic solvent methanol and ultrasonically dispersed for 80 minutes to obtain a polytetrafluoroethylene suspension resin dispersion.
[0098] Then, a nickel mesh precision sieve is selected based on the particle size range calculated in step (1), wherein the mesh number of the top sieve is 380 mesh and the mesh number of the bottom sieve is 1000 mesh. The obtained polytetrafluoroethylene suspension resin dispersion is electrically screened using the selected nickel mesh precision sieve, and the organic solvent methanol is used for circulating spraying at a spraying flow rate of 3 L / min and a spraying time of 40 min.
[0099] Finally, the polytetrafluoroethylene suspension resin on the 1000-mesh sieve was placed in an oven at 80° C. for drying for 10 h to obtain a sample to be tested.
[0100] (3) Molding: Weigh 1 g of the sample to be tested obtained in step (2) and add it to a cylindrical mold with a diameter of 2.0 cm. Use a press to mold the sample to be tested at a pressure of 15 MPa to obtain a membrane to be tested.
[0101] (4) Testing: The film obtained in step (3) is tested using an X-ray diffractometer.
[0102] Step (3) and step (4) were repeated 5 times, i.e., the test was performed 5 times. The diffraction intensity, average diffraction intensity and fluctuation of the diffraction intensity of each test data obtained 5 times are summarized in Table 1.
[0103] Comparative Example 4
[0104] The difference between this comparative example and Example 2 is that the particle size range of the sample to be tested is calculated according to the following standard: the maximum particle size of the sample to be tested DF-106 = 230 × 130.4% = 300 μm; the minimum particle size of the sample to be tested DF-106 = 230 × 69.6% = 160 μm.
[0105] The test method of X-ray diffraction of polytetrafluoroethylene suspension resin comprises the following specific steps:
[0106] (1) Calculate the particle size range required for the sample to be tested:
[0107] First, the median particle size D of the polytetrafluoroethylene suspension resin DF-106 to be tested was measured by laser particle size analyzer. 50 is 230μm.
[0108] Then, the median particle size D 50As the reference particle size, calculate the particle size range of the sample to be tested according to the following standards:
[0109] The maximum particle size of the sample DF-106 to be tested = 230 × 130.4% = 300 μm; the minimum particle size of the sample DF-106 to be tested = 230 × 69.6% = 160 μm.
[0110] in, = ×100%=60.8%.
[0111] (2) Screening out the samples to be tested in the required particle size range:
[0112] First, 50 g of the polytetrafluoroethylene suspension resin to be tested was added to the organic solvent ethanol and ultrasonically dispersed for 70 minutes to obtain a polytetrafluoroethylene suspension resin dispersion.
[0113] Then, a nickel mesh precision sieve is selected based on the particle size range calculated in step (1), wherein the mesh number of the top sieve is 50 mesh and the mesh number of the bottom sieve is 90 mesh. The obtained polytetrafluoroethylene suspension resin dispersion is electrically screened using the selected nickel mesh precision sieve, and the organic solvent ethanol is used for circulating spraying at a spraying flow rate of 2 L / min and a spraying time of 30 min.
[0114] Finally, the polytetrafluoroethylene suspension resin on the 90-mesh sieve was placed in an oven at 90° C. and dried for 10 h to obtain a sample to be tested.
[0115] (3) Molding: Weigh 1 g of the sample to be tested obtained in step (2) and add it to a cylindrical mold with a diameter of 2.0 cm. Use a press to mold the sample to be tested at a pressure of 2 MPa to obtain a membrane to be tested.
[0116] (4) Testing: The film obtained in step (3) is tested using an X-ray diffractometer.
[0117] Step (3) and step (4) were repeated 5 times, i.e., the test was performed 5 times. The diffraction intensity, average diffraction intensity and fluctuation of the diffraction intensity of each test data obtained 5 times are summarized in Table 1.
[0118] Comparative Example 5
[0119] The difference between this comparative example and Example 2 is that the organic solvent used is n-propanol.
[0120] Comparative Example 6
[0121] The difference between this comparative example and Example 2 is that the molding pressure in step (3) is 1 MPa.
[0122] Comparative Example 7
[0123] The difference between this comparative example and Example 2 is that the molding pressure in step (3) is 35 MPa.
[0124] Table 1 X-ray diffraction test results of each embodiment and each comparative example
[0125]
[0126] It can be seen from Table 1 that the method of the present invention has excellent stability when using X-ray diffraction to test polytetrafluoroethylene resin.
Claims
1. A test method for X-ray diffraction of polytetrafluoroethylene suspension resin, characterized in that: The following steps are involved: (1) Calculate the particle size range required for the sample to be tested: First, the median particle size D of the polytetrafluoroethylene suspension resin to be tested is analyzed and measured. 50 ; Then, the median particle size D 50 The particle size range of the sample to be tested is calculated according to the following standard: median particle size D 50 Value × 80% ≤ Particle size of the sample to be tested ≤ Median particle size D 50 value × 120%, and 15%≤ ×100%≤35%; (2) Screening out the samples to be tested in the required particle size range: Firstly, the polytetrafluoroethylene suspension resin to be tested is added into an organic solvent and ultrasonically dispersed to obtain a polytetrafluoroethylene suspension resin dispersion liquid; Then, a sieve is selected based on the particle size range calculated in step (1), and the obtained polytetrafluoroethylene suspension resin dispersion is sieved using the selected sieve, and an organic solvent is used for circulating spraying during the sieving process; Finally, the sieved polytetrafluoroethylene suspension resin is dried to obtain a sample to be tested; (3) Molding: Weigh the sample to be tested obtained in step (2) and add it into a mold. Use a press to mold the sample to be tested at a pressure of 2-30 MPa to obtain a membrane to be tested; (4) Testing: The film obtained in step (3) is tested using an X-ray diffractometer. The fluctuation of the average diffraction intensity of the obtained X-ray diffraction pattern is between 0.01% and 0.5%.
2. The method for testing polytetrafluoroethylene suspension resin by X-ray diffraction according to claim 1, characterized in that: The particle size range of the sample to be tested in step (1) is: median particle size D 50 Value × 90% ≤ Particle size of the sample to be tested ≤ Median particle size D 50 value × 110%, and 16%≤ ×100%≤20%.
3. The method for testing polytetrafluoroethylene suspension resin by X-ray diffraction according to claim 1, characterized in that: The organic solvent in step (2) is one or more of methanol, ethanol or isopropanol.
4. The method for testing polytetrafluoroethylene suspension resin by X-ray diffraction according to claim 1, characterized in that: The ultrasonic dispersion time in step (2) is at least 60 minutes.
5. The method for testing polytetrafluoroethylene suspension resin by X-ray diffraction according to claim 1, characterized in that: The sieve selected in step (2) is a nickel mesh precision sieve.
6. The method for testing polytetrafluoroethylene suspension resin by X-ray diffraction according to claim 1, characterized in that: The spraying flow rate in step (2) is 1-5 L / min, and the spraying time is at least 20 min.
7. The method for testing polytetrafluoroethylene suspension resin by X-ray diffraction according to claim 1, characterized in that: The drying temperature in step (2) is 60-100° C. and the drying time is at least 6 hours.
8. The method for testing polytetrafluoroethylene suspension resin by X-ray diffraction according to claim 1, characterized in that: In step (3), the mold is cylindrical and has a diameter of 1.5-2.0 cm.
9. The method for testing polytetrafluoroethylene suspension resin by X-ray diffraction according to claim 8, characterized in that: In the step (3), 0.5-2 g of the sample to be tested obtained in the step (2) is weighed and added into the mold.