Substrate for semiconductor device
By forming a characteristic Ni-P external electrode body on the substrate of the semiconductor device and controlling its magnetic parameters, the adverse magnetic effects on the semiconductor element when the inductance is high are solved, and the reliability and detection accuracy of the device are improved.
Patent Information
- Application Number
- CN202410307324.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-22
- Filing Date
- 2024-03-18
- Publication Date
- 2024-09-24
AI Technical Summary
In existing semiconductor devices, although the non-magnetic Ni-P formation of external electrodes can suppress the adverse effects of magnetism, it may still have adverse effects on semiconductor elements, especially the detection accuracy and malfunction of magnetic sensors, when the inductance is high. question.
By forming Ni-P in the main body of the external electrode on the substrate, its magnetic permeability, maximum magnetic flux density, residual magnetic flux density and coercive force are controlled within a specific range to ensure the magnetization and magnetic saturation of the external electrode under a magnetic field. Minimize the impact on semiconductor components.
It effectively suppresses the magnetic influence of external electrodes on semiconductor components, prevents malfunctions and deterioration of detection accuracy, reduces magnetic flux density during magnetic saturation, and reduces the influence of residual magnetism.
Smart Images

Figure CN118693052A
Abstract
Description
Technical Field
[0001] The present invention relates to a semiconductor device substrate having external electrodes formed on the substrate. Background Art
[0002] In the semiconductor device substrate of the present invention, the external electrode main body of the external electrode is formed of Ni-P, which is disclosed in Patent Document 1. The external electrode of the semiconductor device substrate of Patent Document 1 includes a third surface layer formed on the substrate, an external electrode main body formed on the surface of the third surface layer, and a fourth surface layer formed on the surface of the external electrode main body, and the external electrode main body of the external electrode is formed of non-magnetic Ni-P.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2021-145060 Summary of the invention
[0006] Problems to be solved by the invention
[0007] According to the semiconductor device of Patent Document 1, the external electrode main body of the external electrode is formed of non-magnetic Ni-P, so even if the semiconductor element mounted on the substrate is easily induced by magnetic force, it can be expected that the adverse effect of the magnetism on the semiconductor element can be suppressed to a minimum. However, in general, "non-magnetic body" is a general term for non-ferromagnetic substances, including paramagnetic bodies, diamagnetic bodies, antiferromagnetic bodies, etc. In view of this, according to the inductance of the semiconductor element mounted on the substrate, even if the external electrode main body is formed of "non-magnetic" as described above, its magnetism may cause a significant adverse effect on the semiconductor element.
[0008] The present invention is completed with the purpose of solving the above-mentioned problems possessed by conventional semiconductor device substrates, and its purpose is to, in a semiconductor device substrate in which the external electrode main body portion of the external electrode is formed of Ni-P, suppress the adverse effect of the magnetic force of the external electrode main body portion on the semiconductor element to a smaller extent even when the inductance of the semiconductor element is high.
[0009] Methods for solving problems
[0010] The present invention is directed to a semiconductor device substrate having an external electrode 3 connected to a semiconductor element 1 formed on the surface of a substrate 16. The external electrode 3 includes a third surface layer 7 formed on the surface of the substrate 16, an external electrode main body 9 formed on the surface of the third surface layer 7, and a fourth surface layer 13 formed on the surface of the external electrode main body 9. Furthermore, the external electrode main body 9 of the external electrode 3 is characterized in that it is formed of non-magnetic Ni-P, and the amplitude relative permeability of the Ni-P is less than 4.0.
[0011] The amplitude relative permeability of Ni—P is preferably 2.0 or more and 4.0 or less, and more preferably 2.3 or more and 3.1 or less.
[0012] The maximum magnetic flux density of Ni-P is less than 7.0 mT.
[0013] The maximum magnetic flux density of Ni—P is preferably 4.0 mT to 7.0 mT, and more preferably 4.7 mT to 6.2 mT.
[0014] The residual magnetic flux density of Ni-P is less than 0.10 mT.
[0015] The residual magnetic flux density of Ni—P is preferably 0.04 mT to 0.10 mT, and more preferably 0.048 to 0.066 mT.
[0016] The coercive force of Ni—P is 23 A / m or less.
[0017] The coercive force of Ni—P is preferably 10 A / m or more and 23 A / m or less, and more preferably 11 A / m or more and 21 A / m or less.
[0018] Effects of the Invention
[0019] As in the present invention, if the amplitude relative permeability of Ni-P forming the external electrode main body 9 is 4.0 or less, even when a magnetic field is applied to the external electrode main body 9 due to external factors, the external electrode main body 9 can be prevented from being easily magnetized. As a result, it is possible to effectively prevent the external electrode main body 9 from being magnetized and the magnetic force generated from the external electrode main body 9 from reaching the semiconductor element 1 and causing the semiconductor element 1 to be adversely affected. More specifically, it is possible to effectively prevent the semiconductor element 1 from being adversely affected by the magnetic force generated from the external electrode main body 9, such as malfunction of the semiconductor element 1 with high inductance or deterioration of detection accuracy when the semiconductor element 1 is a magnetic sensor.
[0020] The amplitude relative permeability of Ni-P is preferably greater than 2.0 and less than 4.0. In addition, the amplitude relative permeability of Ni-P is more preferably greater than 2.3 and less than 3.1. Thus, even when a magnetic field is applied to the external electrode main body 9, it is possible to further prevent the external electrode main body 9 from being easily magnetized.
[0021] If the maximum magnetic flux density of Ni-P forming the external electrode main body 9 is 7.0 mT or less, even if the external electrode main body 9 is magnetized due to external factors, the magnetic flux density of the external electrode main body 9 at the time of magnetic saturation can be reduced. Therefore, even if the magnetic force generated by the external electrode main body 9 reaches the semiconductor element 1, the adverse effect on the semiconductor element 1 can be suppressed as small as possible.
[0022] The maximum magnetic flux density of Ni-P is preferably 4.0 mT or more and 7.0 mT or less. In addition, the maximum magnetic flux density of Ni-P is more preferably 4.7 mT or more and 6.2 mT or less. Thus, even when the external electrode main body 9 is magnetized, the magnetic flux density of the external electrode main body 9 when it is magnetically saturated can be made smaller.
[0023] The residual magnetic flux density of Ni—P forming the external electrode main body 9 is preferably less than 0.10 mT, thereby reducing the magnetic force remaining in the magnetized external electrode main body 9, thereby minimizing the adverse effects of the magnetic force from the external electrode main body 9 on the semiconductor element 1.
[0024] The residual magnetic flux density of Ni—P is preferably 0.04 mT to 0.10 mT. In addition, the residual magnetic flux density of Ni—P is more preferably 0.048 mT to 0.066 mT. Thus, the magnetic force remaining in the magnetized external electrode main body 9 can be further reduced.
[0025] The coercive force of Ni—P forming the external electrode main body 9 is preferably less than 23 A / m, thereby being able to eliminate the magnetic force remaining in the magnetized external electrode main body 9 with a smaller magnetic field, thereby also being able to minimize the adverse effects of the magnetic force from the external electrode main body 9 on the semiconductor element 1.
[0026] The coercive force of Ni-P is preferably 10 A / m or more and 23 A / m or less. In addition, the coercive force of Ni-P is more preferably 11 A / m or more and 21 A / m or less. Thus, the magnetic force remaining in the magnetized external electrode main body 9 can be eliminated with a smaller magnetic field. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1It is a longitudinal sectional front view of a semiconductor device in which a semiconductor element is mounted on a semiconductor device substrate according to an embodiment of the present invention.
[0028] Figure 2 This is a perspective view of the semiconductor device as viewed from the bottom side.
[0029] Figure 3 (a) to (f) are explanatory diagrams showing a manufacturing process of a semiconductor device substrate according to an embodiment of the present invention.
[0030] Figure 4 (a) to (d) are explanatory diagrams showing a manufacturing process of a semiconductor device according to an embodiment of the present invention.
[0031] Description of Reference Numerals
[0032] 3: external electrode, 7: third surface layer, 9: external electrode main body, 13: fourth surface layer, 16: substrate. DETAILED DESCRIPTION
[0033] (Implementation Method)
[0034] Figures 1 to 4 The present invention shows a semiconductor device substrate and a manufacturing process thereof, and a semiconductor device having a semiconductor element 1 mounted on the semiconductor device substrate. Figure 1 As shown, the semiconductor device is composed of a semiconductor element 1 that induces magnetic force (susceptible to the influence of magnetic field), a mounting pad 2 and six external electrodes 3 exposed on the mounting surface S of the semiconductor device, and a lead 4 that electrically connects the semiconductor element 1 to the external electrodes 3, which are sealed inside an insulating resin (sealing material) 5, and is used as a unit electronic component (semiconductor device) for surface mounting. The mounting pad 2 is arranged in the center of the mounting surface S of the semiconductor device, and the external electrodes 3 are arranged in a straight line every three in a state of sandwiching the mounting pad 2 in the middle. The semiconductor device is formed into a flat rectangular parallelepiped.
[0035] like Figure 1As shown, the mounting pad 2 and the external electrode 3 respectively include a first surface layer 6 and a third surface layer 7 exposed on the mounting surface S of the semiconductor device, a mounting pad main body 8 continuous with the first surface layer 6, an external electrode main body 9 continuous with the third surface layer 7, a second surface layer 12 and a fourth surface layer 13 covering the surfaces of the two main bodies 8 and 9. The mounting pad main body 8 and the external electrode main body 9 are respectively formed of non-magnetic Ni-P, and each surface layer 6, 7, 12, 13 is respectively formed of a single layer or a layer composed of two or more metals (precious metals) stacked by any one of non-magnetic metals (precious metals) such as gold, silver, palladium, and tin. In this embodiment, the first surface layer 6 and the third surface layer 7 exposed on the mounting surface S are formed of gold, and the second surface layer 12 and the fourth surface layer 13 covering the surfaces of the two main bodies 8 and 9 are formed of silver.
[0036] The semiconductor device is formed by a process of forming a semiconductor device substrate and a process of mounting a semiconductor element 1 on the semiconductor device substrate. The semiconductor device substrate is formed by the following processes: a resist patterning process of forming a pattern resist 21 on the surface of the substrate 16, a first metal layer forming process of forming a first surface layer 6 and a third surface layer 7 on the surface of the substrate 16 using the pattern resist 21 formed in the resist patterning process, a main body forming process of forming a mounting pad main body 8 and an external electrode main body 9 on the surface of the first surface layer 6 and the third surface layer 7, and a second metal layer forming process of forming a second surface layer 12 and a fourth surface layer 13 on the surface of the mounting pad main body 8 and the external electrode main body 9. After that, the semiconductor device is completed by a mounting process of the semiconductor element 1, a bonding process using the lead 4, a resin sealing process, a substrate peeling process, and a cutting process. Below, an overview of the manufacturing process of the semiconductor device substrate and the semiconductor device is described.
[0037] like Figure 3 As shown in (a), in the resist patterning process, a photosensitive film resist is laminated on the surface of a substrate 16 formed of a conductive metal plate to form a resist layer 17, a pattern film 18 is made to be in close contact with the surface of the resist layer 17, and ultraviolet light is irradiated from an ultraviolet light lamp 19 for exposure. At this time, the ultraviolet light is irradiated to the resist layer 17 facing the light-transmitting hole 20 formed in the pattern film 18, so that the exposed resist layer 17 is cured. The unexposed portion of the resist layer 17 shielded by the pattern film 18 is dissolved and removed by development, as shown in FIG. Figure 3 As shown in (b), only the exposed portions remain on the substrate 16, and a pattern resist 21 having through holes for forming the mounting pads 2 and the external electrodes 3 is formed between the exposed portions.
[0038] like Figure 3As shown in (c), in the first metal layer forming process, the substrate 16 that has been subjected to pre-plating treatment (degreasing, acid immersion, oxide film removal, activation, chemical etching, electrolytic treatment, strike plating, etc.) is immersed in an electroforming tank, and gold is electroformed (plated) on the substrate 16 previously exposed to the pattern resist 21 to form the first surface layer 6 and the third surface layer 7. At this time, the thickness of the first surface layer 6 and the third surface layer 7 is preferably 0.04 μm or more and 1.0 μm or less, and the present embodiment adjusts the electroforming (plating) time in a manner of 0.1 μm. If the thickness of the first surface layer 6 and the third surface layer 7 is less than 0.04 μm, the solder wettability is poor when the semiconductor device is installed. In addition, the adhesion between the Ni-P layer (mounting pad main body 8 and external electrode main body 9) and the substrate 16 becomes too strong, and it may be difficult to peel off and remove the substrate 16. In addition, if the thickness of the first surface layer 6 and the third surface layer 7 exceeds 1.0 μm, there is a possibility that the solder joint strength of the mounted semiconductor device may deteriorate.
[0039] In the subsequent main body forming process, Figure 3 As shown in (d), the substrate 16 is immersed in the electroforming tank again, and the surface side of the surface layers 6 and 7 is subjected to Ni-P electroplating treatment to form the mounting pad main body 8 and the external electrode main body 9. At this time, by adjusting the electroforming (plating) treatment time, the overhangs 10 and 11 can be formed on the upper part of the mounting pad main body 8 (mounting pad 2) and the external electrode main body 9 (external electrode 3). The overhangs 10 and 11 are formed by electroforming (plating) each main body 8 and 9 exceeding the thickness of the resist layer 17 in the main body forming process, and the peripheral edge portion (front end portion) of the overhangs 10 and 11 extends to the side of the previously solidified resist layer 17. It should be noted that when the Ni-P layer is directly formed on the surface of the substrate 16 without forming the first surface layer 6 and the third surface layer 7, the Ni-P layer is firmly adhered to the substrate 16, so it is difficult to peel off and remove the substrate 16.
[0040] The surface roughness (arithmetic mean roughness Ra) of the mounting pad body 8 of the mounting pad 2 and the external electrode body 9 of the external electrode 3 formed of the Ni-P layer is 0.2 to 0.3 μm, and the second surface layer 12 and the fourth surface layer 13 formed on the surface of each body 8, 9 are formed thin, so that the surface state of each surface layer 12, 13 is presented in imitation of the surface of each body 8, 9. By the way, as the surface roughness of the second surface layer 12 and the fourth surface layer 13 becomes smaller (smooth), the mounting property of the semiconductor element 1 relative to the mounting pad 2 becomes better, but the adhesion with the resin 5 becomes worse. On the contrary, as the surface roughness becomes larger (coarser), the adhesion with the resin 5 becomes better, but the bonding property when the electrode of the semiconductor element 1 is electrically connected to the external electrode 3 becomes worse. It should be noted that when the mounting pad body and the external electrode body are formed of Ni, the surface roughness (arithmetic mean roughness Ra) of each surface layer is 0.3 to 0.5 μm, and the surface of the mounting pad 2 and the external electrode 3 formed by the Ni-P layer is slightly smoother.
[0041] In the subsequent second metal layer forming process, as Figure 3 As shown in (e), silver is electroformed (plated) on the surface of each main body 8, 9 to form a second surface layer 12 and a fourth surface layer 13. At this time, the thickness of each surface layer 12, 13 is preferably more than 1.5μm and less than 6.0μm. In the present embodiment, the electroforming (plating) time is adjusted to 2μm. If the thickness of each surface layer 12, 13 is less than 1.5μm, the bonding property deteriorates. If the thickness of each surface layer 12, 13 exceeds 6.0μm, there is a disadvantage of increased cost. It should be noted that, when each surface layer 12, 13 is difficult to be closely formed with the surface of each main body 8, 9, it is preferred that before the electroforming (plating) of each surface layer 12, 13, the surface of each main body 8, 9 is pre-plated to improve the close adhesion of each surface layer 12, 13 to each main body 8, 9. The mounting pad body 8 and the external electrode body 9 preferably make the total thickness T1 of the mounting pad 2 and the external electrode 3 within the range of 20 to 100 μm. In the present embodiment, the total thickness T1 of the mounting pad 2 and the external electrode 3 is formed to be 40 μm. If the thickness of the second surface layer 12 and the fourth surface layer 13 is thin, the influence on the magnetic sensor (semiconductor element 1) is reduced. However, depending on the characteristics of the semiconductor element 1, the thickness and area of each surface layer 12, 13, the degree of influence on the magnetic sensor (semiconductor element 1) may also change.
[0042] By removing the resist layer 17 remaining in the green body of the semiconductor device substrate obtained through the second metal layer forming step, Figure 3As shown in (f), a semiconductor device substrate having a mounting pad 2 and an external electrode 3 formed on a substrate 16 can be obtained. The hardness of each of the plurality of main body portions 8 and 9 in the above-mentioned semiconductor device substrate was measured, and the Vickers hardness of the mounting pad main body portion 8 and the external electrode main body portion 9 was 400HV to 600HV. In addition, a shear strength test of the mounting pad 2 and the external electrode 3 was performed on the semiconductor device substrate in a state where the resist layer 17 was removed, and the degree of closeness between the mounting pad 2 and the external electrode 3 and the substrate 16 was confirmed. In the shear strength test, on the basis of fixing the substrate 16, a shearing tool was attached to the peripheral side of the mounting pad 2 and the external electrode 3, and a force parallel to the substrate 16 was applied to the shearing tool, and the load when the mounting pad 2 and the external electrode 3 fell off from the substrate 16 was measured. The target value of the shear strength in the semiconductor device substrate of this embodiment is 100 to 500g, and the average load of the measured results is 297g. The average load of shear strength in the conventional semiconductor device substrate in which the mounting pad body and the external electrode body are formed of Ni is 324 g, so it is possible to exert substantially the same shear strength. It should be noted that if the adhesion strength between the mounting pad 2 and the external electrode 3 and the substrate 16 is small, the mounting pad 2 and the external electrode 3 may fall off from the substrate 16 when the semiconductor element 1 is mounted, when the bonding process is performed, when the resin sealing process is performed, etc. In addition, if the adhesion strength between the mounting pad 2 and the external electrode 3 and the substrate 16 is too large, it is difficult to peel off and remove the substrate 16.
[0043] In the step of mounting the semiconductor element 1 on the semiconductor device substrate obtained as described above, Figure 4 As shown in (a), a bonding material (solder, paste, tape, die attach film, etc.) is sandwiched on the mounting pad 2 to fix the semiconductor element 1, as shown in FIG. Figure 4 As shown in (b), the electrodes on the upper surface of the semiconductor element 1 are connected to the external electrodes 3 by using leads 4 made of fine wires such as gold or copper. Once the semiconductor element 1 and the external electrodes 3 are electrically connected and the bonding process is completed, the process is transferred to the resin sealing process. In the resin sealing process, the surface side of the substrate 16 is mounted on a molding die that serves as an upper mold, so that the substrate 16 serves as a lower mold, and a thermosetting epoxy resin is injected into the molding die and heated to cure. At this time, as shown in FIG. Figure 4 As shown in (c), on the substrate 16, a combination of a mounting pad 2 and a plurality of external electrodes 3 constituting a semiconductor device is sealed together while being arranged in a plurality, resulting in a state where a plurality of semiconductor devices are connected.
[0044] Then, if Figure 4As shown in (d), by removing the substrate 16, the back side of the mounting pad 2 (first surface layer 6) and the external electrode 3 (third surface layer 7) is exposed at the bottom (mounting surface S) of each semiconductor device. When removing the substrate 16, for example, a method of physically peeling off (peeling off) the substrate 16 from the semiconductor device side is used. By using a stainless steel material with excellent strength and peelability as the substrate 16, the substrate 16 can be peeled off from the semiconductor device side and quickly peeled off. In addition, in the case where the substrate 16 is other metal materials (such as copper materials), as a method for removing the substrate 16, a method of immersing the substrate 16 in an etching solution to dissolve it can also be used. Then, by performing a cutting process (cutting process), a semiconductor device can be obtained.
[0045] As described above, in the semiconductor device of the above-mentioned embodiment, since the mounting pad body 8 of the mounting pad 2 and the external electrode body 9 of the external electrode 3 are respectively formed of non-magnetic Ni-P, the structure of the mounting pad body 8 and the external electrode body 9 can be simplified compared with the conventional semiconductor device in which a non-magnetic Ni-P layer is formed on the surface layer by chemical plating, a Cu layer having an overhanging portion is formed on the Ni-P layer, and a thin Au layer is further formed on the Cu layer. In addition, since the mounting pad body 8 and the external electrode body 9 are formed entirely of non-magnetic Ni-P, the induced magnetism of both (the mounting pad body 8 and the external electrode body 9) can be eliminated (non-magnetized), so even in the case of configuring a semiconductor device (such as a magnetic sensor) having a semiconductor element 1 having an induced magnetic force, the influence of magnetism can be prevented, which can contribute to the improvement of the reliability of the semiconductor device.
[0046] Since the mounting pad main body 8 of the mounting pad 2 and the external electrode main body 9 of the external electrode 3 are respectively formed by Ni-P electroplating layers, the number of plating steps for forming the mounting pad 2 and the external electrode 3 can be reduced compared to previous semiconductor devices, and the semiconductor device can be provided correspondingly more cheaply.
[0047] The Vickers hardness of the mounting pad body 8 of the mounting pad 2 and the external electrode body 9 of the external electrode 3 is preferably 400 to 600 HV. By forming the Vickers hardness of the mounting pad body 8 and the external electrode body 9 within the range of 400 to 600 HV, the strength (rigidity) of the mounting pad 2 and the external electrode 3 can be ensured, and even when the thickness of the mounting pad 2 and the external electrode 3 is formed thinner than in the past, the mounting pad 2 and the external electrode 3 can be prevented from falling off. The total thickness T1 of each of the mounting pad 2 and the external electrode 3 is preferably 20 to 100 μm. If the total thickness T1 of each of the mounting pad 2 and the external electrode 3 is less than 20 μm, the contact area with the resin 5 is small, and the mounting pad 2 and the external electrode 3 may fall off in the completed semiconductor device when the substrate 16 is physically peeled off. If the total thickness T1 of each of the mounting pad 2 and the external electrode 3 exceeds 100 μm, it takes time to form the mounting pad 2 and the external electrode 3, and the productivity (cost) is deteriorated.
[0048] (About magnetic analysis)
[0049] The magnetic properties of the external electrode main body 9 of the external electrode 3 of the above-described embodiment were measured. The measuring device, measuring conditions, etc. are as follows.
[0050] Device: BH analyzer
[0051] Model: SY-8219 (manufactured by Iwasaki Telecom Co., Ltd.)
[0052] Measurement conditions: Empty toroidal core SY-513, Ni-P powder and Ni powder as a comparative example (filling rate 17-19%) were analyzed.
[0053] Number of turns: primary turns (excitation) 100 turns, secondary turns (detection) 100 turns
[0054] Maximum magnetic field: 1630A / m (applied magnetic field)
[0055] Measuring frequency: 50Hz (0.05kHz)
[0056] Waveform: Sine wave (AC power wavelength)
[0057] Under the above conditions, the maximum magnetic flux density, residual magnetic flux density, coercive force and amplitude relative permeability of Ni-P were measured. Specifically, two types of Ni-P (referred to as "Ni-P (A)", "Ni-P (B)") and a material obtained by heating Ni-P (A) at 150°C (referred to as "Ni-P (A2)") were measured. In addition, as a comparative example, Ni was measured in the same manner. The results are shown in Table 1.
[0058] [Table 1]
[0059]
[0060] According to the comparison of the measurement results of the magnetic properties of the three samples of Ni-P mentioned above and the measurement results of the magnetic properties of Ni, it can be known that the amplitude relative permeability of Ni-P of the external electrode body 9 of the external electrode 3 is preferably less than 4.0. It can be known that the maximum magnetic flux density of Ni-P is preferably less than 7.0mT. It can be known that the residual magnetic flux density of Ni-P is preferably less than 0.10mT. It can be known that the coercive force of Ni-P is preferably less than 23A / m. It should be noted that the resistance value of each of the above-mentioned Ni-P and the resistance value of Ni were measured, and the result was that each Ni-P was higher than Ni (Ni-P>Ni).
[0061] The amplitude relative permeability of Ni-P is preferably 2.0 or more and 4.0 or less, more preferably 2.3 or more and 3.1 or less. The maximum magnetic flux density of Ni-P is preferably 4.0 mT or more and 7.0 mT or less, more preferably 4.7 mT or more and 6.2 mT or less. The residual magnetic flux density of Ni-P is preferably 0.04 mT or more and 0.10 mT or less, more preferably 0.048 mT or more and 0.066 mT or less. The coercive force of Ni-P is preferably 10 A / m or more and 23 A / m or less, more preferably 11 A / m or more and 21 A / m or less.
[0062] In addition to the above-mentioned embodiments, the mounting pad 2 can be formed in a state where other metal layers consisting of one or more layers are sandwiched between the mounting pad body 8 and the first surface layer 6 and / or between the mounting pad body 8 and the second surface layer 12. Similarly, the external electrode 3 can be formed in a state where other metal layers consisting of one or more layers are sandwiched between the external electrode body 9 and the third surface layer 7 and / or between the external electrode body 9 and the fourth surface layer 13. In addition, the mounting pad 2 and the external electrode 3 can also be in a form where either or both of the surface layers 6, 7 exposed on the mounting surface S of the semiconductor device and the surface layers 12, 13 covering the surfaces of the main bodies 8, 9 are omitted. Each surface layer 6, 7, 12, 13 can also be composed of a layer composed of an alloy mainly composed of gold, silver, palladium, tin, etc. The semiconductor device substrate of the present invention can also be applied to a semiconductor device that does not have a mounting pad 2. In this case, the semiconductor element is mounted on the substrate (wire bonding connection) or mounted on the external electrode 3 (flip chip connection).
[0063] The semiconductor device substrate of the present invention can contribute to Goal 9 (laying the foundation for industrial and technological innovation) and Goal 12 (responsible consumption and production) of the Sustainable Development Goals (SDGs) advocated by the United Nations.
Claims
1. A semiconductor device substrate, wherein an external electrode (3) connected to a semiconductor element (1) is formed on a surface of the substrate (16), characterized in that: The external electrode (3) comprises a third surface layer (7) formed on the surface of a substrate (16), an external electrode main body (9) formed on the surface of the third surface layer (7), and a fourth surface layer (13) formed on the surface of the external electrode main body (9). The external electrode main body (9) of the external electrode (3) is formed of non-magnetic Ni-P. The amplitude relative permeability of Ni—P is 4.0 or less.
2. The semiconductor device substrate according to claim 1, wherein The amplitude relative permeability of Ni—P is 2.0 or more and 4.0 or less.
3. The semiconductor device substrate according to claim 1, wherein The maximum magnetic flux density of Ni-P is less than 7.0 mT.
4. The semiconductor device substrate according to claim 3, wherein: The maximum magnetic flux density of Ni—P is 4.0 mT or more and 7.0 mT or less.
5. The semiconductor device substrate according to claim 3, wherein: The residual magnetic flux density of Ni-P is less than 0.10 mT.
6. The semiconductor device substrate according to claim 5, wherein: The residual magnetic flux density of Ni—P is 0.04 mT or more and 0.10 mT or less.
7. The semiconductor device substrate according to claim 5, wherein: The coercive force of Ni—P is 23 A / m or less.
8. The semiconductor device substrate according to claim 7, wherein The coercive force of Ni—P is 10 A / m or more and 23 A / m or less.