A beneficiation and enrichment method for low-grade copper, sulfur, and phosphorus in coarse sand tailings

By classifying, sorting, and combining processes in coarse sand tailings, and employing hydraulic flotation machines and flotation columns, the problem of efficient recovery of low-grade copper, sulfur, and phosphorus in coarse sand tailings has been solved, achieving efficient utilization of valuable minerals and economical and efficient mineral processing and enrichment.

CN118698718BActive Publication Date: 2026-11-10KUNMING UNIV OF SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410877277.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2026-11-10
Estimated Expiration
2044-07-02

AI Technical Summary

Technical Problem

Existing technologies are insufficient for the efficient and economical recovery of low-grade copper, sulfur, and phosphorus from coarse sand tailings, leading to resource waste and environmental hazards. Traditional flotation equipment and processes are costly and ineffective.

Method used

Using coarse particle flotation equipment, hydraulic flotation machine and flotation column, combined with the "coarse and fine classification - copper and sulfur classification and mixed flotation - copper and sulfur coarse concentrate merging and regrinding - copper and sulfur separation - coarse phosphorus hydraulic flotation - iron removal from high iron phosphorus concentrate", coarse sand tailings are classified and separated. Copper and sulfur are floated first, then phosphorus is floated and then iron is removed, so as to achieve efficient recovery of valuable minerals.

Benefits of technology

It achieves efficient beneficiation and enrichment of low-grade copper, sulfur and phosphorus in coarse sand tailings, reduces costs, improves recovery rate and product grade, avoids the adverse effects of over-grinding, and has the characteristics of strong process targeting and economic efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118698718B_ABST
    Figure CN118698718B_ABST
Patent Text Reader

Abstract

This invention discloses a method for beneficiation and enrichment of low-grade copper, sulfur, and phosphorus in coarse sand tailings, belonging to the field of mineral processing engineering technology. The method involves: classifying the coarse sand tailings into coarse and fine particles; performing copper-sulfur co-flotation on the coarse and fine particles using hydraulic flotation machines and flotation columns, respectively; obtaining frothy copper-sulfur rough concentrates I and II through roughing and scavenging; combining copper-sulfur rough concentrates I and II for regrinding and reagent removal; and employing a sulfur-suppressing copper flotation process, sequentially performing copper roughing, scavenging, and cleaning, and sulfur roughing, scavenging, and cleaning to obtain copper concentrate and sulfur concentrate, respectively; performing phosphorus separation on the tailings after copper-sulfur co-flotation using a hydraulic flotation machine, performing flotation roughing, scavenging, and cleaning to obtain iron-containing phosphorus concentrate; and using strong magnetic roughing, scavenging, and cleaning to remove iron from the iron-containing phosphorus concentrate to obtain qualified phosphorus concentrate. This invention utilizes unique processes and equipment to achieve efficient beneficiation and enrichment of low-grade copper, sulfur, and phosphorus in coarse sand tailings, resulting in significant comprehensive utilization effects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a beneficiation and enrichment method for low-grade copper, sulfur, and phosphorus in coarse sand tailings, belonging to the field of mineral processing engineering. Background Technology

[0002] my country possesses relatively abundant iron ore resources, but the average iron grade is low, with most being low-grade associated minerals with fine particle size, making beneficiation difficult. Due to uneven development of beneficiation technology, a large amount of valuable elements such as phosphorus, sulfur, and copper remain in the coarse sand tailings after iron ore beneficiation. For coarse sand tailings, due to their low content of valuable components and coarse particle size, conventional flotation processes and equipment necessitate fine grinding followed by separation, resulting in high beneficiation costs and often failing to achieve economical and efficient recovery of low-grade phosphorus, sulfur, and copper. Currently, enterprises mostly use traditional flotation equipment such as mechanically stirred flotation cells, performing simple flotation recovery of low-grade phosphogypsum from coarse sand tailings. This yields high-iron phosphorus concentrate with excessive impurities, and the phosphorus recovery rate is low, resulting in a significant waste of valuable resources in the coarse sand tailings and posing certain environmental hazards. Therefore, the comprehensive recovery of low-grade phosphorus, sulfur, and copper from large quantities of such coarse sand tailings is an urgent problem to be solved for the efficient utilization of these resources.

[0003] Based on the analysis of the process mineralogical properties of coarse sand tailings, this invention proposes a targeted coarse sand classification and separation process, taking into account the characteristics of copper-sulfur coexistence with coarse particle size and high liberation degree of coarse phosphate rock. For coarse-grained copper-sulfur ore and apatite that cannot be separated by traditional flotation equipment, a hydraulic flotation machine is innovatively used, avoiding the high energy consumption and high cost caused by grinding. Simultaneously, a unique process combination has been developed: a combined process of "coarse sand tailings classification - copper-sulfur classification and mixed flotation - copper-sulfur coarse concentrate merging and regrinding - copper-sulfur separation - coarse phosphate hydraulic flotation - iron removal from high-iron phosphate concentrate". This solves the problem that existing single flotation processes and conventional flotation equipment cannot efficiently and economically recover coarse-grained minerals, achieving efficient beneficiation and enrichment of low-grade copper, sulfur, and phosphorus in coarse sand tailings. Summary of the Invention

[0004] This invention provides a beneficiation and enrichment method for low-grade copper, sulfur, and phosphorus in coarse sand tailings. The method involves pre-classifying the coarse sand tailings, then using coarse-grained and fine-grained separation equipment respectively. First, copper- and iron-containing sulfide ores are floated to obtain copper concentrate and sulfur concentrate. Next, phosphorus-containing apatite is floated using the coarse-grained separation equipment to obtain iron-containing phosphate concentrate. Finally, the iron-containing phosphate concentrate is purified by magnetic separation. This process sequentially enriches, separates, and recovers low-grade copper, sulfur, and phosphorus components from the coarse sand tailings. The method employs a reasonable process flow, is highly targeted and adaptable, and achieves good recovery of valuable components.

[0005] The technical solution adopted to achieve the purpose of this invention is as follows:

[0006] A beneficiation and enrichment method for low-grade copper, sulfur, and phosphorus in coarse sand tailings specifically includes the following steps:

[0007] (1) Classify the coarse sand tailings (-0.5mm): The coarse sand tailings are screened and classified into coarse and fine particles; the coarse particles are fed into mixing tank I to adjust the slurry to a certain slurry concentration, and xanthate reagents and No. 2 oil foaming agent are added; the fine particles are fed into mixing tank II to adjust the slurry to a certain slurry concentration, and xanthate reagents and No. 2 oil foaming agent are added.

[0008] (2) Copper-sulfur mixed flotation of coarse slurry after mixing tank I: a coarse particle flotation equipment hydraulic flotation machine is used to perform one roughing and one scavenging. The foam from the roughing and scavenging is combined to obtain copper-sulfur crude concentrate I.

[0009] (3) Copper-sulfur mixed flotation of fine-grained slurry after mixing tank II: using a fine-grained flotation equipment flotation column, one roughing and one scavenging are performed, and the foam from the roughing and scavenging is combined to obtain copper-sulfur crude concentrate II;

[0010] (4) After merging copper-sulfur crude concentrate I and copper-sulfur crude concentrate II, the mixture is regrinded and de-treated.

[0011] (5) After the regrinding slurry is adjusted to a certain slurry concentration, copper-sulfur flotation separation is carried out: the slurry concentration is adjusted to 30-35%, and copper-sulfur separation is carried out by the sulfur suppression and copper flotation process. The copper undergoes one roughing, one scavenging and three cleaning processes. The underflow of copper scavenging enters the sulfur roughing process, and the sulfur undergoes one roughing, two scavenging and two cleaning processes.

[0012] (6) Combine the underflows after copper-sulfur mixed flotation in steps (2) and (3) for phosphorus flotation: Use a coarse particle flotation equipment hydraulic flotation machine. First, use sulfuric acid to adjust the pH of the slurry to 6. Then, use oxidized paraffin soap, MOH, oleic acid, water glass and form a combination of reagents in a certain ratio. After one phosphorus roughing, one phosphorus scavenging and three phosphorus cleaning, iron-containing phosphorus concentrate is obtained. The underflow after phosphorus scavenging enters the tailings.

[0013] (7) Magnetic separation to remove iron from iron-containing phosphate concentrate: A high-gradient strong magnetic separation process with one roughing, one scavenging and one cleaning is adopted to further remove iron from the iron-containing phosphate concentrate obtained in step (5). The magnetic product of strong magnetic cleaning is iron impurity, which is incorporated into the tailings. The non-magnetic products of strong magnetic scavenging and cleaning are combined to obtain high-quality phosphate concentrate.

[0014] Preferably, in step (1) of the present invention, the coarse sand tailings are screened and classified into coarse particles (-0.5 to +0.1 mm) and fine particles (-0.1 mm); the coarse particles are fed into mixing tank I and slurry is adjusted to a slurry concentration of 30-40%, and the fine particles are fed into mixing tank II and slurry is adjusted to a slurry concentration of 30-35%.

[0015] Preferably, in step (2) of the present invention, the coarse particles in mixing tank I are slurried to a slurry concentration of 30-40%, the amount of xanthate added is 100-120 g / t, the xanthate is a mixture of ethyl sodium xanthate and butyl xanthate in a mass ratio of 1:1, and the amount of No. 2 oil foaming agent added is 40-60 g / t; the fine particles in mixing tank II are slurried to a slurry concentration of 30-35%, the amount of xanthate added is 80-100 g / t, the xanthate is a mixture of ethyl sodium xanthate and butyl xanthate in a mass ratio of 1:1, and the amount of No. 2 oil foaming agent added is 20-30 g / t.

[0016] Preferably, in step (3) of the present invention, when using a hydraulic flotation machine for flotation, the water flow rate is 8-10 L / min and the aeration rate is 0.3-0.5 m³ / min. 3 / min; No reagents are added during copper-sulfur roughing, and 50-60g / t of xanthate reagent and 20-30g / t of No. 2 oil frother are added during copper-sulfur scavenging; No reagents are added during copper-sulfur roughing using a flotation column in step (3), and 40-50g / t of xanthate reagent and 10-15g / t of No. 2 oil frother are added during copper-sulfur scavenging.

[0017] Preferably, in step (4) of the present invention, sodium sulfide 300-500 g / t, activated carbon 500-800 g / t and lime 1500-2500 g / t are added during the regrinding process, and the grinding fineness of the regrinding is -200 mesh 90-95%.

[0018] Preferably, in step (5) of the present invention, a fine particle flotation column is used. In the copper roughing process, Z-200 20-30 g / t, ethyl thiocyanate 10-20 g / t and No. 2 oil 10-20 g / t are added. In the copper scavenging process, lime 500-1000 g / t, Z-200 10-20 g / t, ethyl thiocyanate 5-10 g / t and No. 2 oil 10-20 g / t are added respectively. The foam from the copper roughing and copper scavenging processes is combined and enters the copper cleaning process. No reagents are added in copper cleaning I. In copper cleaning II, lime 200-300 g / t and Z-200 10-20 g / t are added. No reagents are added in copper cleaning III. The middlings in the copper cleaning process are returned to the previous operation. The foam in copper cleaning III is copper concentrate.

[0019] Preferably, in step (5) of the present invention, sulfur roughing is performed with 700-1000 g / t of sulfuric acid, 300-400 g / t of copper sulfate, 80-100 g / t of butyl xanthate and 20-30 g / t of No. 2 oil. Sulfur scavenging I is performed with 300-400 g / t of sulfuric acid, 150-200 g / t of copper sulfate, 40-50 g / t of butyl xanthate and 10-20 g / t of No. 2 oil. Sulfur scavenging II is performed with 100-200 g / t of sulfuric acid, 50-100 g / t of copper sulfate, 10-20 g / t of butyl xanthate and 10 g / t of No. 2 oil. The foam from sulfur roughing, sulfur scavenging I and sulfur scavenging II is combined and enters sulfur cleaning. No reagents are added during sulfur cleaning. The middlings produced by sulfur cleaning are returned to the previous operation in sequence. The foam from sulfur cleaning II is sulfur concentrate. The underflow from sulfur scavenging II enters phosphorus scavenging.

[0020] Preferably, in step (6) of the present invention, the flotation of phosphorus is carried out using a coarse particle flotation device, a hydraulic flotation machine, with a water flow rate of 10-12 L / min and an aeration rate of 0.4-0.6 m³ / min. 3 / min; In the phosphorus roughing process, 700-900 g / t of sulfuric acid and 300-400 g / t of combined reagents are added. The ratio of MOH, oleic acid, oxidized paraffin soap, and water glass in the combined reagents is 4:2:1:9. In the phosphorus scavenging process, 200-300 g / t of sulfuric acid and 100-150 g / t of combined reagents are added. The foam from the phosphorus roughing and scavenging processes is combined and enters the phosphorus cleaning process. No reagents are added to phosphorus cleaning I. In phosphorus cleaning II, 100 g / t of sulfuric acid and 50-100 g / t of combined reagents are added. No reagents are added to phosphorus cleaning III. The underflow (mid-ore) from phosphorus cleaning is sequentially returned to the previous operation without the addition of reagents. The foam from phosphorus cleaning III is iron-containing phosphorus concentrate. The underflow from phosphorus scavenging enters the tailings.

[0021] Preferably, in step (7) of the present invention, the coarse magnetic field strength is 0.6T to 0.7T, the sweep magnetic field strength is 0.8T to 0.9T, and the fine magnetic field strength is 0.5T.

[0022] In order to comprehensively recover the valuable components copper, sulfur and phosphorus, this invention proposes a combined process of "coarse sand tailings classification - copper-sulfur classification and flotation - copper-sulfur coarse concentrate merging and regrinding - copper-sulfur separation - coarse phosphorus hydraulic flotation - iron removal from high-iron phosphorus concentrate". First, the coarse sand tailings are pre-classified to obtain fine and coarse particles. The coarse particles are subjected to copper-sulfur mixed flotation using a coarse particle flotation hydraulic flotation machine, while the fine particles are subjected to copper-sulfur mixed flotation using a flotation column. This process enriches copper and pyrite minerals to obtain a copper-sulfur rough concentrate. The copper-sulfur rough concentrate is then regrinded and subjected to a copper-sulfur separation process to obtain copper concentrate and sulfur concentrate. The tailings after copper-sulfur mixed flotation are subjected to phosphorus flotation using a hydraulic flotation machine to obtain an iron-containing phosphorus concentrate. Finally, a high-gradient magnetic separation process is used to remove ferrosilicon and siderite from the iron-containing phosphorus concentrate, ultimately yielding a high-quality phosphorus concentrate. The beneficiation and enrichment method for low-grade copper, sulfur, and phosphorus in iron coarse sand tailings developed in this invention can achieve efficient utilization of valuable components in iron tailings and has a significant comprehensive recovery effect.

[0023] Beneficial effects of the present invention

[0024] (1) The coarse sand tailings have a relatively coarse overall particle size (-0.5 mm), characterized by coarse copper-sulfur coexistence and coarse embedded particles, coarse apatite particles with high individual liberation, a variety of valuable minerals but low grades, and high content of iron silicate and siderite. This invention first pre-classifies the coarse sand tailings into coarse and fine particles. Without grinding, the coarse particles (-0.5 to +0.1 mm) and fine particles (-0.1 mm) are separated using hydraulic flotation machines and flotation columns, respectively, achieving economical and efficient recovery of both coarse and fine valuable minerals. Compared with traditional mineral processing methods, this invention introduces a coarse particle flotation device, the hydraulic flotation machine, into the coarse sand tailings, avoiding the high costs associated with regrinding and reprocessing the tailings and the adverse effects of over-grinding on the recovery of valuable minerals.

[0025] (2) A combined process of “coarse and fine classification - copper-sulfur graded flotation - copper-sulfur coarse concentrate merging and regrinding - copper-sulfur separation - coarse phosphorus hydraulic flotation - iron removal from high-iron phosphorus concentrate” was proposed for coarse sand tailings, which realizes the efficient utilization of each valuable element. This feature is an important support for the realization of this technology.

[0026] (3) Based on the characteristics of valuable minerals in coarse sand tailings, this invention adopts a step-by-step separation process: copper and sulfur are separated first, followed by phosphorus and then iron removal. This process comprehensively recovers copper, sulfur, and phosphorus in sequence, featuring the advantages of prioritizing sulfur over oxygen, starting with easier minerals and proceeding to more difficult ones, simple reagent formulation, strong process targeting, and high economic efficiency. Conversely, if flotation is carried out in different sequences such as sulfur, phosphorus, phosphorus, or phosphorus, sulfur, and copper, it has significant disadvantages such as complex reagent formulation and process, high separation cost, and poor performance. Therefore, the separation sequence in this invention has outstanding beneficial effects. Attached Figure Description

[0027] Figure 1This is a process flow diagram of the present invention. Detailed Implementation

[0028] The present invention will be further described in detail below with reference to specific embodiments, but the scope of protection of the present invention is not limited to the content described.

[0029] The coarse sand tailings (-0.5mm) produced in North my country contain small amounts of chalcopyrite, pyrite, and apatite. The chalcopyrite and pyrite are mostly coarse-grained intergrowths and are liberated from the gangue minerals, while the apatite is mostly coarse-grained with good individual liberation. In addition, the tailings contain a certain amount of iron silicate, a small amount of siderite, and a very small amount of magnetite. The gangue mineral is mainly quartz. This section uses three relatively typical coarse sand tailings (No. 1 to No. 3) produced in North China as examples to implement the technology of the present invention. The indicators and beneficial effects obtained by the specific examples are shown in Table 1.

[0030] Example 1

[0031] This embodiment uses No. 1 coarse sand tailings (containing 0.13% copper, 1.50% sulfur, and 3.80% phosphorus pentoxide) as an example for illustration. The copper mineral, sulfur mineral, and phosphorus mineral are chalcopyrite, pyrite, and apatite, respectively. In addition, it contains a small amount of iron silicate, siderite, and a very small amount of magnetite. The gangue mineral is mainly quartz.

[0032] A beneficiation and enrichment method for low-grade copper, sulfur, and phosphorus in coarse sand tailings specifically includes the following steps:

[0033] (1) The coarse sand tailings are screened and classified into coarse particles (-0.5 to +0.1 mm) and fine particles (-0.1 mm): the coarse particles are fed into mixing tank I and adjusted to a slurry concentration of 30%, and the fine particles are fed into mixing tank II and adjusted to a slurry concentration of 30%. The amount of xanthate added in mixing tank I is 100 g / t, and the xanthate is a mixture of ethyl sodium xanthate and butyl xanthate in a mass ratio of 1:1. The amount of No. 2 oil frother added is 40 g / t. The amount of xanthate added in mixing tank II is 80 g / t, and the xanthate is a mixture of ethyl sodium xanthate and butyl xanthate in a mass ratio of 1:1. The amount of No. 2 oil frother added is 20 g / t.

[0034] (2) Copper-sulfur co-flotation of the slurry after conditioning:

[0035] ① Copper-sulfur co-flotation of the coarse-grained slurry after conditioning in mixing tank I: A coarse-grained flotation device—a hydraulic flotation machine—was used for one roughing and one scavenging stage. The water flow rate in the hydraulic flotation machine was 8 L / min, and the aeration rate was 0.3 m³ / min. 3 / min; No reagents are added during the copper-sulfur roughing process, and 50g / t of xanthate reagent and 20g / t of No. 2 oil frother are added during the copper-sulfur scavenging process.

[0036] ② Copper-sulfur co-flotation of fine-grained slurry after mixing in tank II: one roughing and one scavenging are carried out using a fine-grained flotation equipment - flotation column. No reagents are added during the copper-sulfur roughing, and 40g / t of xanthate reagent and 10g / t of No. 2 oil frother are added during the copper-sulfur scavenging.

[0037] (3) After merging copper-sulfur crude concentrate I and II, regrinding and de-refining are carried out: 300g / t of sodium sulfide, 500g / t of activated carbon and 1500g / t of lime are added during the regrinding process. The regrinding fineness is -200 mesh, accounting for 90%.

[0038] (4) After the regrinding and de-removing slurry is adjusted to a certain slurry concentration, copper-sulfur flotation separation is carried out: the slurry concentration is adjusted to 30%, a fine particle flotation equipment flotation column is used, and the copper-sulfur separation is carried out by the sulfur suppression and copper flotation process. The copper undergoes one roughing, one scavenging and three cleaning processes. The underflow of the copper scavenging enters the sulfur roughing process, and the sulfur undergoes one roughing, two scavenging and two cleaning processes.

[0039] In the copper roughing process, 20 g / t of Z-200, 10 g / t of ethyl nitrogen, and 10 g / t of No. 2 oil are added. In the copper scavenging process, 500 g / t of lime, 10 g / t of Z-200, 5 g / t of ethyl nitrogen, and 10 g / t of No. 2 oil are added respectively. The foam from the copper roughing and copper scavenging processes is combined and enters the copper cleaning process. No reagents are added in copper cleaning I. In copper cleaning II, 200 g / t of lime and 10 g / t of Z-200 are added. No reagents are added in copper cleaning III. The middlings in the copper cleaning process are returned to the previous operation. The foam in copper cleaning III is copper concentrate.

[0040] In the sulfur roughing process, 700 g / t of sulfuric acid, 300 g / t of copper sulfate, 80 g / t of butyl xanthate, and 20 g / t of No. 2 oil are added. In sulfur scavenging I, 300 g / t of sulfuric acid, 150 g / t of copper sulfate, 40 g / t of butyl xanthate, and 10 g / t of No. 2 oil are added. In sulfur scavenging II, 100 g / t of sulfuric acid, 50 g / t of copper sulfate, 10 g / t of butyl xanthate, and 10 g / t of No. 2 oil are added. The foam from the sulfur roughing, sulfur scavenging I, and sulfur scavenging II processes is combined and enters the sulfur cleaning process. No reagents are added during the sulfur cleaning process. The middlings produced by the sulfur cleaning process are returned to the previous operation in sequence. The foam from sulfur cleaning II is the sulfur concentrate. The underflow from sulfur scavenging II enters the phosphorus scavenging process.

[0041] (5) Flotation of phosphorus in the undercurrent of copper-sulfur mixed flotation scavenging II:

[0042] A coarse-particle flotation device, a hydraulic flotation machine, is used, employing a primary phosphorus roughing, a primary phosphorus scavenging, and a secondary phosphorus cleaning process. The water flow rate of the hydraulic flotation machine is 10 L / min, and the aeration rate is 0.4 m³ / min. 3 / min; MOH, oleic acid, oxidized paraffin soap and water glass are mixed in a mass ratio of 4:2:1:9 to form a combined reagent; 700g / t of sulfuric acid and 300g / t of combined reagent are added to the phosphorus roughing process, and 300g / t of sulfuric acid and 150g / t of combined reagent are added to the phosphorus scavenging process. The foam from the phosphorus roughing and scavenging processes is combined and enters the phosphorus cleaning process. No reagent is added to phosphorus cleaning I. 100g / t of sulfuric acid and 50g / t of combined reagent are added to phosphorus cleaning II. No reagent is added to phosphorus cleaning III. The underflow (mid-ore) from phosphorus cleaning is returned to the previous operation in sequence without adding reagent. The foam from phosphorus cleaning III is iron-containing phosphorus concentrate. The underflow from phosphorus scavenging enters the tailings.

[0043] (6) Magnetic separation to remove iron from iron-bearing phosphate concentrate obtained by flotation: A high gradient magnetic separation process with one roughing, one scavenging and one cleaning is adopted. The magnetic field strength of the roughing is 0.6T and the magnetic field strength of the scavenging is 0.8T. The magnetic products of the roughing and scavenging are combined into the cleaning process. The magnetic field strength of the cleaning process is 0.5T. The magnetic products of the cleaning process are iron impurities, which are incorporated into the tailings. The non-magnetic products of the cleaning process are combined with the tailings of the scavenging process to obtain phosphate concentrate.

[0044] The indicators and beneficial effects obtained by implementing the above-described technical steps of the present invention in Example 1 are shown in Table 1.

[0045] Example 2

[0046] The No. 2 coarse sand tailings sample contains 0.15% copper, 1.80% sulfur, and 4.50% phosphorus pentoxide. The copper, sulfur, and phosphorus minerals are chalcopyrite, pyrite, and apatite, respectively. In addition, it contains small amounts of iron silicate, siderite, and a very small amount of magnetite. The gangue mineral is mainly quartz.

[0047] A beneficiation and enrichment method for low-grade copper, sulfur, and phosphorus in coarse sand tailings specifically includes the following steps:

[0048] (1) The coarse sand tailings are screened and classified into coarse particles (-0.5 to +0.1 mm) and fine particles (-0.1 mm); the coarse particles are fed into mixing tank I and slurry is adjusted to a slurry concentration of 35%, and the fine particles are fed into mixing tank II and slurry is adjusted to a slurry concentration of 30%; the amount of xanthate added in mixing tank I is 110 g / t, the xanthate is a mixture of ethyl sodium xanthate and butyl xanthate in a mass ratio of 1:1, and the amount of No. 2 oil frother added is 50 g / t; the amount of xanthate added in mixing tank II is 90 g / t, the xanthate is a mixture of ethyl sodium xanthate and butyl xanthate in a mass ratio of 1:1, and the amount of No. 2 oil frother added is 30 g / t.

[0049] (2) Copper-sulfur co-flotation of the slurry after conditioning:

[0050] ① Copper-sulfur co-flotation of the coarse-grained slurry after conditioning in mixing tank I: A hydraulic flotation machine was used for one roughing and one scavenging stage. The water flow rate in the hydraulic flotation machine was 9 L / min, and the aeration rate was 0.4 m³ / min. 3 / min; No reagents are added during the copper-sulfur roughing process, and 55g / t of xanthate reagent and 25g / t of No. 2 oil frother are added during the copper-sulfur scavenging process.

[0051] ② Copper-sulfur co-flotation of fine-grained slurry after mixing in tank II: one roughing and one scavenging are carried out using a fine-grained flotation equipment - flotation column. No reagents are added during the copper-sulfur roughing, and 45g / t of xanthate reagent and 15g / t of No. 2 oil frother are added during the copper-sulfur scavenging.

[0052] (3) After merging copper-sulfur crude concentrate I and II, regrinding and de-refining are carried out: 400g / t of sodium sulfide, 650g / t of activated carbon and 2000g / t of lime are added during the regrinding process. The regrinding fineness is -200 mesh, accounting for 95%.

[0053] (3) De-processing and regrinding of copper-sulfur crude concentrate: 400 g / t of sodium sulfide, 700 g / t of activated carbon and 2000 g / t of lime are added during the regrinding process. The fineness of the regrinding is -200 mesh, accounting for 93%.

[0054] (4) After the regrinding and de-removing slurry is adjusted to a certain slurry concentration, copper-sulfur flotation separation is carried out: the slurry concentration is adjusted to 35%, a fine particle flotation equipment flotation column is used, and the copper-sulfur separation is carried out by the sulfur suppression and copper flotation process. The copper undergoes one roughing, one scavenging and three cleaning processes respectively. The underflow of copper scavenging enters the sulfur roughing process, and the sulfur undergoes one roughing, two scavenging and two cleaning processes.

[0055] In the copper roughing process, 25 g / t of Z-200, 15 g / t of ethyl thiocyanate, and 15 g / t of No. 2 oil are added. In the copper scavenging process, 800 g / t of lime, 15 g / t of Z-200, 10 g / t of ethyl thiocyanate, and 15 g / t of No. 2 oil are added respectively. The foam from the copper roughing and copper scavenging processes is combined and enters the copper cleaning process. No reagents are added in copper cleaning I. In copper cleaning II, 250 g / t of lime and 15 g / t of Z-200 are added. No reagents are added in copper cleaning III. The middlings in the copper cleaning process are returned to the previous operation. The foam in copper cleaning III is copper concentrate.

[0056] In the sulfur roughing process, 850 g / t of sulfuric acid, 350 g / t of copper sulfate, 90 g / t of butyl xanthate, and 25 g / t of No. 2 oil are added. In sulfur scavenging I, 350 g / t of sulfuric acid, 200 g / t of copper sulfate, 45 g / t of butyl xanthate, and 15 g / t of No. 2 oil are added. In sulfur scavenging II, 150 g / t of sulfuric acid, 100 g / t of copper sulfate, 15 g / t of butyl xanthate, and 10 g / t of No. 2 oil are added. The foam from the sulfur roughing, sulfur scavenging I, and sulfur scavenging II processes is combined and enters the sulfur cleaning process. No reagents are added during the sulfur cleaning process. The middlings produced by the sulfur cleaning process are returned to the previous operation in sequence. The foam from sulfur cleaning II is the sulfur concentrate. The underflow from sulfur scavenging II enters the phosphorus scavenging process.

[0057] (5) Flotation of phosphorus in the undercurrent of copper-sulfur mixed flotation scavenging II:

[0058] A coarse-particle flotation device, a hydraulic flotation machine, is used, employing a primary phosphorus roughing, a primary phosphorus scavenging, and a secondary phosphorus cleaning process. The water flow rate of the hydraulic flotation machine is 11 L / min, and the aeration rate is 0.5 m³ / min. 3 / min; MOH, oleic acid, oxidized paraffin soap and water glass are mixed in a mass ratio of 4:2:1:9 to form a combined reagent; one phosphorus roughing, one phosphorus scavenging and three phosphorus cleaning are adopted; 800g / t of sulfuric acid and 350g / t of combined reagent are added in the phosphorus roughing, 300g / t of sulfuric acid and 150g / t of combined reagent are added in the phosphorus scavenging, the foam from the phosphorus roughing and phosphorus scavenging are combined into the phosphorus cleaning, no reagent is added in phosphorus cleaning I, 100g / t of sulfuric acid and 50g / t of combined reagent are added in phosphorus cleaning II, no reagent is added in phosphorus cleaning III, the underflow (mid-ore) of phosphorus cleaning is returned to the previous operation in sequence without adding reagents, the foam of phosphorus cleaning III is iron-containing phosphorus concentrate, and the underflow of phosphorus scavenging is sent to the tailings.

[0059] (6) Magnetic separation to remove iron from iron-bearing phosphate concentrate obtained by flotation: A high gradient strong magnetic separation process with one roughing, one scavenging and one cleaning is adopted. The magnetic field strength of the roughing is 0.65T and the magnetic field strength of the scavenging is 0.85T. The magnetic products of the roughing and scavenging are combined into the cleaning process. The magnetic field strength of the cleaning process is 0.5T. The magnetic products of the cleaning process are iron impurities and are incorporated into the tailings. The non-magnetic products of the cleaning process are combined with the tailings of the scavenging process to obtain phosphate concentrate.

[0060] The indicators and beneficial effects obtained by implementing the above-described technical steps of the present invention in Example 2 are shown in Table 1.

[0061] Example 3

[0062] The No. 3 coarse sand tailings sample contains 0.18% copper, 2.10% sulfur, and 5.10% phosphorus pentoxide. The copper, sulfur, and phosphorus minerals are chalcopyrite, pyrite, and apatite, respectively. In addition, it contains small amounts of iron silicate, siderite, and a very small amount of magnetite. The gangue mineral is mainly quartz.

[0063] A beneficiation and enrichment method for low-grade copper, sulfur, and phosphorus in coarse sand tailings specifically includes the following steps:

[0064] (1) The coarse sand tailings are screened and classified into coarse particles (-0.5 to +0.1 mm) and fine particles (-0.1 mm); the coarse particles are fed into mixing tank I and slurry is adjusted to a slurry concentration of 40%, and the fine particles are fed into mixing tank II and slurry is adjusted to a slurry concentration of 30%; the amount of xanthate added in mixing tank I is 120 g / t, the xanthate is a mixture of ethyl sodium xanthate and butyl xanthate in a mass ratio of 1:1, and the amount of No. 2 oil frother added is 60 g / t; the amount of xanthate added in mixing tank II is 100 g / t, the xanthate is a mixture of ethyl sodium xanthate and butyl xanthate in a mass ratio of 1:1, and the amount of No. 2 oil frother added is 40 g / t.

[0065] (2) Copper-sulfur co-flotation of the slurry after conditioning:

[0066] ① Copper-sulfur co-flotation of the coarse-grained slurry after conditioning in mixing tank I: A hydraulic flotation machine is used for one roughing and one scavenging stage. The water flow rate in the hydraulic flotation machine is 10 L / min, and the aeration rate is 0.5 m³ / min. 3 / min; No reagents are added during the copper-sulfur roughing process, and 60g / t of xanthate reagent and 30g / t of No. 2 oil frother are added during the copper-sulfur scavenging process.

[0067] ② Copper-sulfur co-flotation of fine-grained slurry after mixing in tank II: one roughing and one scavenging are carried out using a fine-grained flotation equipment - flotation column. No reagents are added during the copper-sulfur roughing, and 50g / t of xanthate reagent and 15g / t of No. 2 oil frother are added during the copper-sulfur scavenging.

[0068] (3) After merging copper-sulfur crude concentrate I and II, regrinding and de-refining are carried out: 500g / t of sodium sulfide, 800g / t of activated carbon and 2500g / t of lime are added during the regrinding process. The regrinding fineness is -200 mesh, accounting for 95%.

[0069] (4) After the regrinding and de-removing slurry is adjusted to a certain slurry concentration, copper-sulfur flotation separation is carried out: the slurry concentration is adjusted to 35%, a fine particle flotation equipment flotation column is used, and the copper-sulfur separation is carried out by the sulfur suppression and copper flotation process. The copper undergoes one roughing, one scavenging and three cleaning processes respectively. The underflow of copper scavenging enters the sulfur roughing process, and the sulfur undergoes one roughing, two scavenging and two cleaning processes.

[0070] In the copper roughing process, 30 g / t of Z-200, 20 g / t of ethyl thiocyanate, and 20 g / t of No. 2 oil are added. In the copper scavenging process, 1000 g / t of lime, 20 g / t of Z-200, 10 g / t of ethyl thiocyanate, and 20 g / t of No. 2 oil are added respectively. The foam from the copper roughing and copper scavenging processes is combined and enters the copper cleaning process. No reagents are added in copper cleaning I. In copper cleaning II, 300 g / t of lime and 20 g / t of Z-200 are added. No reagents are added in copper cleaning III. The middlings in the copper cleaning process are returned to the previous operation. The foam in copper cleaning III is copper concentrate.

[0071] In the sulfur roughing process, 1000 g / t of sulfuric acid, 400 g / t of copper sulfate, 100 g / t of butyl xanthate, and 30 g / t of No. 2 oil are added. In sulfur scavenging I, 400 g / t of sulfuric acid, 200 g / t of copper sulfate, 50 g / t of butyl xanthate, and 20 g / t of No. 2 oil are added. In sulfur scavenging II, 200 g / t of sulfuric acid, 100 g / t of copper sulfate, 20 g / t of butyl xanthate, and 10 g / t of No. 2 oil are added. The foam from the sulfur roughing, sulfur scavenging I, and sulfur scavenging II processes is combined and enters the sulfur cleaning process. No reagents are added during the sulfur cleaning process. The middlings produced by the sulfur cleaning process are returned to the previous operation in sequence. The foam from sulfur cleaning II is the sulfur concentrate. The underflow from sulfur scavenging II enters the phosphorus scavenging process.

[0072] (5) Flotation of phosphorus in the undercurrent of copper-sulfur mixed flotation scavenging II:

[0073] A coarse-particle flotation device, a hydraulic flotation machine, is used, employing a primary phosphorus roughing, a primary phosphorus scavenging, and a secondary phosphorus cleaning process. The water flow rate of the hydraulic flotation machine is 12 L / min, and the aeration rate is 0.6 m³ / min. 3 / min; MOH, oleic acid, oxidized paraffin soap and water glass are mixed in a mass ratio of 4:2:1:9 to form a combined reagent; one phosphorus roughing, one phosphorus scavenging and three phosphorus cleaning are adopted; 900g / t of sulfuric acid and 400g / t of combined reagent are added in the phosphorus roughing, 250g / t of sulfuric acid and 100g / t of combined reagent are added in the phosphorus scavenging, the foam from the phosphorus roughing and phosphorus scavenging are combined and enter the phosphorus cleaning. No reagent is added in phosphorus cleaning I, 100g / t of sulfuric acid and 100g / t of combined reagent are added in phosphorus cleaning II, no reagent is added in phosphorus cleaning III, the underflow (mid-ore) of phosphorus cleaning is returned to the previous operation in sequence without adding reagent during the process, the foam of phosphorus cleaning III is iron-containing phosphorus concentrate, and the underflow of phosphorus scavenging enters the tailings.

[0074] (6) Magnetic separation to remove iron from iron-bearing phosphate concentrate obtained by flotation: A high gradient strong magnetic separation process with one roughing, one scavenging and one cleaning is adopted. The magnetic field strength of the roughing is 0.7T and the magnetic field strength of the scavenging is 0.9T. The magnetic products of the roughing and scavenging are combined into the cleaning process. The magnetic field strength of the cleaning process is 0.5T. The magnetic products of the cleaning process are iron impurities, which are incorporated into the tailings. The non-magnetic products of the cleaning process are combined with the tailings of the scavenging process to obtain phosphate concentrate.

[0075] Table 1 shows the indicators and beneficial effects obtained using the method of the present invention for Examples 1-3.

[0076]

[0077] As shown in Table 1, for the three implementation examples of coarse sand tailings, when the coarse sand tailings contain 0.13-0.18% Cu, 2.10-2.51% S, and 3.80-5.10% P2O5, copper concentrate, sulfur concentrate, and phosphorus concentrate with high grades and recovery rates were obtained. Specifically, the Cu grade of the copper concentrate was 16.28-21.10%, and the Cu recovery rate was 70.11-71.49%; the S grade of the sulfur concentrate was 40.77-43.23%, and the S recovery rate was 70.55-71.39%; and the P2O5 grade of the phosphorus concentrate was 32.48-33.66%, and the P2O5 recovery rate was 75.12-76.88%. This invention achieves efficient and comprehensive recovery of low-grade copper, sulfur, and phosphorus from coarse sand tailings.

[0078] Analysis revealed that the three implementation examples employed the combined process flow and reagent system of the present invention, namely, "coarse and fine classification - copper-sulfur graded flotation - copper-sulfur coarse concentrate merging and regrinding - copper-sulfur separation - coarse phosphorus hydraulic flotation - iron removal from high-iron phosphorus concentrate". Because this combined process adopts a step-by-step separation process, prioritizing easier processes and sulfur over oxygen (i.e., selecting copper and sulfur first, then phosphorus, and finally removing iron), the process is highly targeted. Furthermore, the application of the coarse particle flotation equipment—the hydraulic flotation machine—avoids the grinding costs associated with re-selecting large quantities of coarse sand tailings, and achieves good flotation enrichment and separation indicators, demonstrating significant economic and efficient results.

[0079] Experiments revealed that, using conventional flotation processes (first, all coarse sand tailings are finely ground to a fineness of -0.074 mm, accounting for 85% to 95%, to fully liberate the sulfur and copper minerals, and then flotation cells are used to select the sulfur-phosphorus-copper or phosphorus-sulfur-copper priority flotation process to obtain the corresponding concentrate products), after adjusting the order of the flotation process steps for coarse sand tailings, the overall grade and recovery rate of the obtained copper concentrate, sulfur concentrate, and phosphorus concentrate were lower than the results in Table 1. Analysis revealed that when using the conventional process described above to finely grind all the coarse sand tailings for flotation enrichment and separation, the over-grinding of already liberated apatite and the resulting mud formation of a large amount of gangue components are highly detrimental to the flotation enrichment of apatite, leading to low flotation indices for the phosphate concentrate. Furthermore, the mud-formed phosphate minerals and gangue components after fine grinding are difficult to effectively suppress, further worsening the flotation indices for sulfur and copper minerals, resulting in high impurity content and unsatisfactory flotation indices in both copper and sulfur concentrates. Comparative experiments further demonstrate that the process flow in this invention is innovative and unique, and has significant beneficial effects.

[0080] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the described embodiments are only some embodiments of this invention, and not all embodiments. In the absence of conflict, the embodiments and features in the embodiments of this application can be combined with each other. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.

Claims

1. A method for beneficiation and enrichment of low-grade copper, sulfur, and phosphorus in coarse sand tailings, characterized in that, Specifically, the steps include the following: (1) Classify the coarse sand tailings (-0.5mm): The coarse sand tailings are screened and classified into coarse and fine particles; the coarse particles are fed into mixing tank I to adjust the slurry to a certain slurry concentration, and xanthate reagents and No. 2 oil foaming agent are added; the fine particles are fed into mixing tank II to adjust the slurry to a certain slurry concentration, and xanthate reagents and No. 2 oil foaming agent are added. (2) Copper-sulfur mixed flotation of coarse slurry after mixing tank I: a coarse particle flotation equipment hydraulic flotation machine is used to perform one roughing and one scavenging. The foam from the roughing and scavenging is combined to obtain copper-sulfur crude concentrate I. (3) Copper-sulfur mixed flotation of fine-grained slurry after mixing tank II: using a fine-grained flotation equipment flotation column, one roughing and one scavenging are performed, and the foam from the roughing and scavenging is combined to obtain copper-sulfur crude concentrate II; (4) After merging copper-sulfur crude concentrates I and II, the concentrates were regrinded and de-treated. (5) After the regrinding and de-removing slurry is adjusted to a certain slurry concentration, copper-sulfur flotation separation is carried out: the slurry concentration is adjusted to 30-35%, and copper-sulfur separation is carried out by the sulfur suppression and copper flotation process. The copper undergoes one roughing, one scavenging and three cleaning processes respectively. The underflow of copper scavenging enters the sulfur roughing process, and the sulfur undergoes one roughing, two scavenging and two cleaning processes. (6) Combine the underflows after copper-sulfur mixed flotation in steps (2) and (3) for phosphorus flotation: use a coarse particle flotation equipment hydraulic flotation machine, first adjust the pH of the slurry to 6 with sulfuric acid, then use oxidized paraffin soap, MOH, oleic acid, water glass in a certain ratio to form a combined reagent, and obtain iron-containing phosphorus concentrate after one phosphorus roughing, one phosphorus scavenging and three phosphorus cleaning. The underflow after phosphorus scavenging enters the tailings. (7) Magnetic separation to remove iron from iron-containing phosphate concentrate: A high-gradient strong magnetic separation process with one roughing, one scavenging and one cleaning is adopted to further remove iron from the iron-containing phosphate concentrate obtained in step (5). The magnetic product of strong magnetic cleaning is iron impurity, which is incorporated into the tailings. The non-magnetic products of strong magnetic scavenging and cleaning are combined to obtain high-quality phosphate concentrate.

2. The beneficiation and enrichment method for low-grade copper, sulfur, and phosphorus in coarse sand tailings according to claim 1, characterized in that: In step (1), the coarse sand tailings are screened and classified into coarse particles (-0.5 to +0.1 mm) and fine particles (-0.1 mm); the coarse particles are fed into mixing tank I and slurry is adjusted to a slurry concentration of 30-40%, and the fine particles are fed into mixing tank II and slurry is adjusted to a slurry concentration of 30-35%. In step (1), the amount of xanthate agent added to mixing tank I is 100-120 g / t, and the xanthate agent is a mixture of ethyl sodium xanthate and butyl xanthate in a mass ratio of 1:

1. The amount of No. 2 oil foaming agent added is 40-60 g / t. In mixing tank II, the amount of xanthate agent added is 80-100 g / t, and the xanthate agent is a mixture of ethyl sodium xanthate and butyl xanthate in a mass ratio of 1:

1. The amount of No. 2 oil foaming agent added is 20-30 g / t.

3. The beneficiation and enrichment method for low-grade copper, sulfur, and phosphorus in coarse sand tailings according to claim 1, characterized in that: In step (2), when using a hydraulic flotation machine for flotation, the water flow rate is 8-10 L / min and the aeration rate is 0.3-0.5 m³ / min. 3 / min; no reagents are added during copper-sulfur roughing, and 50-60g / t of xanthate reagent and 20-30g / t of No. 2 oil frother are added during copper-sulfur scavenging.

4. The beneficiation and enrichment method for low-grade copper, sulfur, and phosphorus in coarse sand tailings according to claim 1, characterized in that: In step (3), no reagents are added when using a flotation column for copper-sulfur roughing. For copper-sulfur scavenging, 40-50 g / t of xanthate reagent and 10-15 g / t of No. 2 oil frother are added.

5. The beneficiation and enrichment method for low-grade copper, sulfur, and phosphorus in coarse sand tailings according to claim 1, characterized in that: In step (4), sodium sulfide 300-500 g / t, activated carbon 500-800 g / t and lime 1500-2500 g / t are added during the regrinding process. The regrinding fineness is -200 mesh, accounting for 90-95%.

6. The beneficiation and enrichment method for low-grade copper, sulfur, and phosphorus in coarse sand tailings according to claim 1, characterized in that: In step (5), a fine-particle flotation column is used. In the copper roughing process, Z-200 20-30 g / t, ethyl thiocyanate 10-20 g / t and No. 2 oil 10-20 g / t are added. In the copper scavenging process, lime 500-1000 g / t, Z-200 10-20 g / t, ethyl thiocyanate 5-10 g / t and No. 2 oil 10-20 g / t are added respectively. The foam from the copper roughing and copper scavenging processes is combined and enters the copper cleaning process. No reagents are added in copper cleaning I. In copper cleaning II, lime 200-300 g / t and Z-200 10-20 g / t are added. No reagents are added in copper cleaning III. The middlings in the copper cleaning process are returned to the previous operation. The foam in copper cleaning III is copper concentrate. In step (5), sulfur roughing is carried out with 700-1000 g / t of sulfuric acid, 300-400 g / t of copper sulfate, 80-100 g / t of butyl xanthate and 20-30 g / t of No. 2 oil. In sulfur scavenging I, sulfuric acid is carried out with 300-400 g / t of sulfuric acid, 150-200 g / t of copper sulfate, 40-50 g / t of butyl xanthate and 10-20 g / t of No. 2 oil. In sulfur scavenging II, sulfuric acid is carried out with 100-200 g / t of sulfuric acid, 50-100 g / t of copper sulfate, 10-20 g / t of butyl xanthate and 10 g / t of No. 2 oil. The foam from sulfur roughing, sulfur scavenging I and sulfur scavenging II is combined and enters sulfur cleaning. No reagents are added during sulfur cleaning. The middlings produced by sulfur cleaning are returned to the previous operation in sequence. The foam of sulfur cleaning II is sulfur concentrate. The underflow of sulfur scavenging II enters the tailings.

7. The beneficiation and enrichment method for low-grade copper, sulfur, and phosphorus in coarse sand tailings according to claim 1, characterized in that: In step (6), a coarse particle flotation device, a hydraulic flotation machine, is used, with a water flow rate of 10-12 L / min and an aeration rate of 0.4-0.6 m³ / min. 3 / min; In the phosphorus roughing process, add 700-900 g / t of sulfuric acid and 300-400 g / t of combined reagents. The mass ratio of MOH, oleic acid, oxidized paraffin soap, and water glass in the combined reagents is 4:2:1:

9. In the phosphorus scavenging process, add 200-300 g / t of sulfuric acid and 100-150 g / t of combined reagents. The foam from the phosphorus roughing and scavenging processes is combined and enters the phosphorus cleaning process. No reagents are added to phosphorus cleaning I. In phosphorus cleaning II, add 100 g / t of sulfuric acid and 50-100 g / t of combined reagents. No reagents are added to phosphorus cleaning III. The underflow from phosphorus cleaning is returned sequentially to the previous operation without adding reagents. The foam from phosphorus cleaning III is iron-containing phosphorus concentrate. The underflow from phosphorus scavenging enters the tailings.

8. The beneficiation and enrichment method for low-grade copper, sulfur, and phosphorus in coarse sand tailings according to claim 1, characterized in that: In step (7): the coarse selection magnetic field strength is 0.6T to 0.7T, the sweep selection magnetic field strength is 0.8T to 0.9T, and the fine selection magnetic field strength is 0.5T.

Citation Information

Patent Citations

  • Method for recycling copper minerals from copper and sulfur separating tailings

    CN111036391A

  • Beneficiation method for cascade enhanced flotation and efficient recovery of low-grade molybdenum-bismuth-sulfur polymetallic ore

    CN115780069A