A leaching and separation method for mixed rare earth concentrate
Through the surface modification and multi-stage leaching treatment of rare earth concentrate by plasma airflow, pollution and resource waste in the existing rare earth smelting process are solved, efficient separation and recycling of rare earth, phosphorus and fluorine elements are achieved, and the rare earth industry is promoted. green development.
Patent Information
- Application Number
- CN202411210144.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-30
AI Technical Summary
The existing rare earth smelting process has problems of three waste pollution and resource waste, and is not easy to produce on a large scale, which limits the green and sustainable development of the rare earth industry.
The mixed rare earth concentrate is surface modified by plasma gas flow, and the effective separation and resource recovery of rare earths, phosphorus and fluorine elements are achieved through ore phase conversion and multi-stage leaching treatment, reducing oxidation reactions and resource waste.
It has improved the comprehensive resource utilization rate of rare earth concentrate, reduced production costs, reduced pollutant emissions, and achieved green, healthy and sustainable development of the rare earth industry.
Smart Images

Figure CN118703807B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of rare earth ore dressing, and in particular relates to a leaching and separation method of a mixed rare earth concentrate. Background Art
[0002] The Bayan Obo Mine is a rare super-large deposit of iron, niobium, rare earths and other polymetallic associated minerals in the world. The Bayan Obo rare earth mine is mainly a mixed ore of fluorocarbon cerium ore and monazite. The main associated minerals are fluorite, iron minerals, apatite, etc. Due to the complex composition and structure of rare earth minerals, close mineral symbiosis and low ore grade, the smelting of rare earth minerals is difficult.
[0003] At present, the industrial smelting processes of Bayan Obo mixed rare earth concentrate mainly include concentrated sulfuric acid roasting method and caustic soda decomposition method. Concentrated sulfuric acid roasting method is the most important smelting process of Bayan Obo mixed rare earth ore. This process is to mix rare earth mixed concentrate with concentrated sulfuric acid in a rotary kiln for high-temperature roasting, and then obtain rare earth mixed solution through water leaching, and obtain rare earth products through a series of neutralization, precipitation and impurity removal. This process is simple and continuous, and the production cost is low. However, in this process, concentrated sulfuric acid is easily decomposed and wasted in the high-temperature roasting stage, and sulfur-containing and fluorine-containing tail gas is generated. Ammonia nitrogen wastewater is generated in the leaching, neutralization, precipitation and impurity removal stages. Phosphorus and thorium also exist in the leaching slag in the form of insoluble salts, resulting in resource waste and radioactive pollution. Problems such as pollution restrict the green and healthy development of the rare earth industry. The main process of caustic soda decomposition is liquid alkali normal pressure decomposition, in which rare earth mixed concentrate and sodium hydroxide are stirred and leached at high temperature in a reaction vessel. This process does not produce sulfur-containing and fluorine-containing tail gas, but the process has high requirements on the grade of rare earth mixed concentrate and requires a pre-impurity removal process, which leads to discontinuous process and is not easy for large-scale production. These problems limit the application of this process in industry.
[0004] In summary, the main processes in this field have factors such as three wastes pollution or are not easy for large-scale production, which restrict the green and sustainable development of the rare earth industry. Therefore, it is of great significance to explore a green, healthy and sustainable development of the Bayan Obo mixed rare earth ore smelting and separation process. Summary of the invention
[0005] In view of the above-mentioned deficiencies in the prior art, the present invention provides a leaching and separation method for a mixed rare earth concentrate.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0007] The present invention provides a leaching and separation method for a mixed rare earth concentrate, comprising:
[0008] The mixed rare earth concentrate is subjected to surface modification under the action of a plasma gas flow to obtain a surface-modified mixed rare earth concentrate;
[0009] Performing mineral phase transformation on the surface-modified mixed rare earth concentrate to transform the bastnaesite phase in the mixed rare earth concentrate into cerium fluoride oxide, thereby obtaining a mineral phase transformation product containing cerium fluoride oxide;
[0010] Acid leaching is performed on the mineral phase conversion product to obtain an acid leaching solution and an acid leaching residue; the acid leaching solution contains rare earth ions and fluoride ions, and the acid leaching residue contains monazite;
[0011] The acidic leaching residue is subjected to surface modification under the action of plasma gas flow to obtain surface-modified acidic leaching residue;
[0012] The surface-modified acidic leaching residue is subjected to alkaline leaching treatment to obtain alkaline leaching solution and alkaline leaching residue; the alkaline leaching solution contains phosphorus elements, and the alkaline leaching residue contains rare earth elements.
[0013] Optionally, the mixed rare earth concentrate is subjected to surface modification under the action of a plasma gas flow to obtain a surface-modified mixed rare earth concentrate, comprising:
[0014] The mixed rare earth concentrate is placed in a plasma cleaning device with a first preset atmosphere and a power of 100 to 300 W for 10 to 60 minutes to obtain a mixed rare earth concentrate with changed surface oxidation properties; the first preset atmosphere is a mixture of hydrogen and inert gas.
[0015] Optionally, the surface-modified mixed rare earth concentrate is subjected to mineral phase transformation, so that the bastnaesite phase in the mixed rare earth concentrate is transformed into cerium fluoride oxide to obtain a mineral phase transformation product containing cerium fluoride oxide, including:
[0016] The surface-modified mixed rare earth concentrate is subjected to fluidized roasting in an inert atmosphere to convert the fluorocarbon cerium ore phase in the mixed rare earth concentrate into cerium oxyfluoride, thereby obtaining a roasting product containing cerium oxyfluoride, and using the roasting product as a mineral phase conversion product.
[0017] Optionally, the surface-modified mixed rare earth concentrate is subjected to fluidized roasting in an inert atmosphere to convert the bastnaesite phase in the mixed rare earth concentrate into cerium oxyfluoride to obtain a roasting product containing cerium oxyfluoride, comprising:
[0018] After the surface-modified mixed rare earth concentrate is placed in a roasting furnace, an inert gas is continuously introduced into the bottom of the roasting furnace, and the inert gas is used as a fluidizing gas to keep the mixed rare earth concentrate in a fluidized state under an inert atmosphere;
[0019] The heating temperature of the roasting furnace is adjusted so that the mixed rare earth concentrate in a fluidized state is heated at a temperature of 450 to 750° C. for 20 to 120 minutes to complete the reaction of converting fluorocarbon cerium ore in the mixed rare earth concentrate into cerium fluoride oxide to obtain a roasting product.
[0020] Optionally, the inert gas continuously introduced into the bottom of the roasting furnace has a gas flow rate of 300 to 1000 mL / min.
[0021] Optionally, the mineral phase conversion product is subjected to acid leaching treatment to obtain acid leaching solution and acid leaching residue, including:
[0022] The mineral phase conversion product is added to the hydrochloric acid leaching solution, and stirred for 20 to 120 min at a temperature of 60 to 100° C., an ultrasonic power of 300 to 600 W, and a stirring speed of 200 to 600 r / min to obtain an acidic leaching solution and acidic leaching residue.
[0023] Optionally, the liquid-to-solid ratio of the hydrochloric acid leaching solution and the mineral phase conversion product is 4 to 20:1; the hydrochloric acid leaching solution includes a hydrochloric acid solution with a concentration of 1 to 10 mol / L and a leaching aid with a concentration of 0.1 to 0.5 mol / L; the leaching aid is aluminum chloride or boric acid.
[0024] Optionally, the acidic leaching residue is subjected to surface modification under the action of a plasma gas flow to obtain surface-modified acidic leaching residue, comprising:
[0025] The acidic leaching residue is placed in a plasma cleaning device with a second preset atmosphere and a power of 100 to 300 W for 10 to 60 minutes to obtain acidic leaching residue with changed surface oxidation properties; the second preset atmosphere includes a mixture of hydrogen and inert gas.
[0026] Optionally, the surface-modified acidic leached residue is subjected to alkaline leaching treatment to obtain alkaline leaching solution and alkaline leached residue, comprising:
[0027] The surface-modified acidic leaching residue is added with a sodium hydroxide solution, and reacted for 60 to 360 min at a temperature of 120 to 200° C. and a pressure of 0.1 to 5 MPa at a stirring speed of 200 to 600 r / min to obtain an alkaline leaching solution and alkaline leaching residue; wherein the alkali-ore ratio of the sodium hydroxide solution and the acidic leaching residue is 1 to 7:1, and the liquid-solid ratio is 1 to 10:1.
[0028] Optionally, it also includes:
[0029] A hydrochloric acid solution with a concentration of 1 to 10 mol / L is added to the alkaline leaching residue to dissolve the alkaline leaching residue to obtain an acidic solution containing rare earth elements.
[0030] The present invention provides a leaching and separation method for a mixed rare earth concentrate, wherein the surface of the mixed rare earth concentrate is modified under the action of a plasma gas flow, so that the generation of CeO2 is reduced during the mineral phase transformation process of the surface-modified mixed rare earth concentrate, so that the fluorocarbon cerium ore in the mixed rare earth concentrate can be directionally transformed into cerium fluoride oxide, thereby making the mineral phase transformation product have a higher rare earth leaching rate; then, the surface of the acidic leaching slag obtained by acid leaching the mineral phase transformation product is modified under the action of a plasma gas flow, so that the surface-modified During the alkaline leaching treatment of the acidic leaching residue, the occurrence of oxidation reaction can be reduced, so that the obtained alkaline leaching residue contains no or a small amount of tetravalent cerium ions; finally, by performing alkaline leaching treatment on the surface-modified acidic leaching residue, an alkaline leaching solution containing phosphorus and an alkaline leaching residue containing rare earth elements can be obtained; it can be seen that the present invention can effectively separate the rare earth elements, phosphorus elements and fluorine elements in the mixed rare earth concentrate, realize the comprehensive recovery of resources such as fluorite and apatite associated with the mixed rare earth concentrate, and improve the comprehensive resource utilization rate of the mixed rare earth concentrate.
[0031] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained by the structures particularly pointed out in the written description and the accompanying drawings.
[0032] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 The present invention is a flowchart of a method for leaching and separating a mixed rare earth concentrate according to an exemplary embodiment of the present invention. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0035] The present invention provides a leaching and separation method for a mixed rare earth concentrate, comprising the following steps:
[0036] Step 100: subjecting the mixed rare earth concentrate to surface modification under the action of plasma gas flow to obtain a surface-modified mixed rare earth concentrate;
[0037] Step 200: performing mineral phase conversion on the surface-modified mixed rare earth concentrate to convert the bastnaesite phase in the mixed rare earth concentrate into cerium fluoride oxide, thereby obtaining a mineral phase conversion product containing cerium fluoride oxide;
[0038] Step 300: performing acid leaching treatment on the mineral phase conversion product to obtain an acid leaching solution and an acid leaching residue; the acid leaching solution contains rare earth ions and fluoride ions, and the acid leaching residue contains monazite;
[0039] Step 400: subjecting the acidic leaching residue to surface modification under the action of a plasma gas flow to obtain surface-modified acidic leaching residue;
[0040] Step 500: performing alkaline leaching treatment on the surface-modified acidic leaching residue to obtain alkaline leaching solution and alkaline leaching residue; the alkaline leaching solution contains phosphorus, and the alkaline leaching residue contains rare earth elements.
[0041] It should be noted that the mixed rare earth concentrate can be the Bayan Obo mixed rare earth ore, the REO grade of the mixed rare earth concentrate is 50% to 67%, and the main rare earth minerals included are fluorocarbon cerium ore and monazite; the F grade of the mixed rare earth concentrate is 4% to 10%, and the main fluorine-containing minerals included are fluorocarbon cerium ore, fluorite, and apatite; the P grade of the mixed rare earth concentrate is 4% to 10%, and the main phosphorus-containing minerals included are monazite and apatite.
[0042] Here, in step 100, the mixed rare earth concentrate is subjected to the action of a plasma gas flow, so that the plasma gas flow collides with the surface of the mixed rare earth concentrate, causing the chemical bonds of the molecules on the surface of the mixed rare earth concentrate to break and recombine, thereby generating a new chemical structure and changing the oxidation performance of the surface of the mixed rare earth concentrate, so that the surface-modified mixed rare earth concentrate is oxidized as little as possible during the mineral phase transformation process in step 200, thereby converting the fluorocarbon cerium ore phase in the mixed rare earth concentrate into fluorocerium oxide that is more easily treated by acid leaching.
[0043] In step 200, the surface-modified mixed rare earth concentrate is subjected to a mineral phase transformation, so that the fluorocarbon cerium ore phase in the mixed rare earth concentrate is transformed into cerium oxyfluoride which is more susceptible to acid leaching reaction, and then the mineral phase transformation product containing cerium oxyfluoride is subjected to the acid leaching treatment of step 300, and the acidic leaching solution containing rare earth ions and fluoride ions generated contains cerium rare earth elements.
[0044] Because the acidic leaching residue obtained in step 300 includes trivalent cerium ions, and the trivalent cerium ions are easily oxidized during the alkaline leaching process, therefore, before the acidic leaching residue is subjected to alkaline leaching treatment, step 400 is performed, that is, surface modification of the acidic leaching residue is performed by using a plasma gas flow, so that the surface-modified acidic leaching residue is oxidized as little as possible during the alkaline leaching treatment process, so that the alkaline leaching residue in step 500 does not contain or contains a small amount of tetravalent cerium ions.
[0045] In this embodiment, the surface of the mixed rare earth concentrate is modified under the action of plasma gas flow, so that the generation of CeO2 is reduced in the process of mineral phase transformation of the surface-modified mixed rare earth concentrate, so that the fluorocarbon cerium ore in the mixed rare earth concentrate can be directionally transformed into cerium fluoride oxide, and then the mineral phase transformation product has a higher rare earth leaching rate; then, the acid leaching slag obtained by acid leaching treatment of the mineral phase transformation product is surface-modified under the action of plasma gas flow, so that the surface-modified acid leaching slag can be leached in alkali water. During the alkaline leaching treatment, the occurrence of oxidation reaction can be reduced, so that the obtained alkaline leaching residue contains no or a small amount of tetravalent cerium ions; finally, by performing alkaline leaching treatment on the surface-modified acidic leaching residue, an alkaline leaching solution containing phosphorus and an alkaline leaching residue containing rare earth elements can be obtained; it can be seen that the present invention can effectively separate the rare earth elements, phosphorus elements and fluorine elements in the mixed rare earth concentrate, realize the comprehensive recovery of resources such as fluorite and apatite associated with the mixed rare earth concentrate, and improve the comprehensive resource utilization rate of the mixed rare earth concentrate.
[0046] In some possible embodiments, the mixed rare earth concentrate is subjected to surface modification under the action of a plasma gas flow to obtain a surface-modified mixed rare earth concentrate, which may include: placing the mixed rare earth concentrate in a plasma cleaning apparatus having an atmosphere of a first preset atmosphere and a power of 100 to 300 W for treatment for 10 to 60 minutes to obtain a mixed rare earth concentrate with changed surface oxidation properties; the first preset atmosphere is a mixture of hydrogen and an inert gas.
[0047] Here, the inert gas in the first preset atmosphere may be one or more of nitrogen, helium, and argon; and the plasma cleaning apparatus may enable the first preset atmosphere to generate a hydrogen ion flow.
[0048] In this embodiment, by using a mixture of hydrogen and inert gas as the first preset atmosphere, the plasma cleaner can generate a hydrogen plasma flow, so that the molecular chemical bonds on the surface of the mixed rare earth concentrate are broken and reorganized under the action of the hydrogen plasma flow, generating a new chemical structure, and completing the change of the oxidation performance of the surface of the mixed rare earth concentrate, so that the surface-modified mixed rare earth concentrate is oxidized as little as possible during the mineral phase transformation process in step 200.
[0049] In some possible embodiments, a surface-modified mixed rare earth concentrate is subjected to a mineral phase transformation, so that the fluorocarbon cerium ore phase in the mixed rare earth concentrate is transformed into cerium fluoride oxide, and a mineral phase transformation product containing cerium fluoride oxide is obtained. This may include: fluidizing the surface-modified mixed rare earth concentrate in an inert atmosphere to transform the fluorocarbon cerium ore phase in the mixed rare earth concentrate into cerium fluoride oxide, and obtaining a roasting product containing cerium fluoride oxide, and using the roasting product as a mineral phase transformation product.
[0050] In this embodiment, by fluidizing and roasting the surface-modified mixed rare earth concentrate in an inert gas atmosphere, it is possible to prevent the bastnaesite in the mixed rare earth concentrate from reacting with oxygen in the air to generate CeO2, thereby causing the bastnaesite (REFCO3) in the mixed rare earth concentrate to be directionally converted into cerium oxyfluoride (REOF) that is more easily acid leached, so that the acidic leachate in step 300 contains more cerium ions.
[0051] In some possible embodiments, the surface-modified mixed rare earth concentrate is subjected to fluidized roasting in an inert atmosphere to convert the bastnaesite phase in the mixed rare earth concentrate into cerium oxyfluoride to obtain a roasting product containing cerium oxyfluoride, which may include the following steps:
[0052] Step 201: After the surface-modified mixed rare earth concentrate is placed in a roasting furnace, an inert gas is continuously introduced into the bottom of the roasting furnace, and the inert gas is used as a fluidizing gas to keep the mixed rare earth concentrate in a fluidized state under an inert atmosphere;
[0053] Step 202: Adjust the heating temperature of the roasting furnace so that the mixed rare earth concentrate in a fluidized state is heated at a temperature of 450-750° C. for 20-120 min to complete the reaction of converting bastnaesite in the mixed rare earth concentrate into cerium fluoride oxide to obtain a roasting product.
[0054] Here, the roasting furnace may be a vertical tube type roasting furnace.
[0055] In step 201, by continuously introducing inert gas into the bottom of the roasting furnace and using the inert gas as fluidizing gas, it is possible to ensure that the mixed rare earth concentrate maintains a good fluidized state under an inert atmosphere.
[0056] In this embodiment, by continuously introducing inert gas as fluidizing gas from the bottom of the roasting furnace, it is possible to prevent oxygen in the air from contacting the mixed rare earth concentrate, thereby preventing oxidation of the fluorocarbon cerium in the mixed rare earth concentrate. Since the fluidizing gas formed by the inert gas can keep the mixed rare earth concentrate in a fluidized state, the mixed rare earth concentrate in step 202 can be roasted in a fluidized state, so as to improve the reaction efficiency of converting the fluorocarbon cerium ore in the mixed rare earth concentrate into cerium fluoride oxide, and at the same time, the ore conversion rate of the fluorocarbon cerium can be improved.
[0057] In some possible embodiments, the inert gas continuously introduced into the bottom of the roasting furnace has a gas flow rate of 300-1000 mL / min.
[0058] Here, the gas flow rate of the inert gas may be, but is not limited to, 300, 350, 400, 450, 500, 550, 600, 650, 700, 750, 800, 850, 900, 950, and 1000 mL / min.
[0059] In some possible embodiments, the mineral phase conversion product is subjected to acid leaching treatment to obtain an acidic leachate and an acidic leaching residue, which can include: adding the mineral phase conversion product to a hydrochloric acid leachate, and stirring the mixture for 20 to 120 min at a temperature of 60 to 100° C. and an ultrasonic power of 300 to 600 W, at a stirring speed of 200 to 600 r / min, to obtain an acidic leachate and an acidic leaching residue.
[0060] Here, by applying an ultrasonic external field, that is, an ultrasonic power of 300 to 600 W, during the acid leaching process of the mineral phase transformation product, the cavitation effect of the ultrasonic wave can be used to break through the constraints of some conventional reactions, and the shear force provided by the ultrasonic wave can also be used to remove the passivation film on the surface of the mineral phase transformation product, so as to achieve the effect of enhanced leaching of the mineral phase transformation product.
[0061] In this embodiment, when the mineral phase conversion product is added to the hydrochloric acid leaching solution for acid leaching treatment, an ultrasonic power of 300 to 600 W is applied to make the acid leaching reaction of the mineral phase conversion product more thorough, thereby achieving full recovery of the rare earth elements in the mineral phase conversion product.
[0062] In some possible embodiments, the liquid-to-solid ratio of the hydrochloric acid leachate and the mineral phase conversion product is 4 to 20:1; the hydrochloric acid leachate includes a hydrochloric acid solution with a concentration of 1 to 10 mol / L and a leaching aid with a concentration of 0.1 to 0.5 mol / L; the leaching aid is aluminum chloride or boric acid.
[0063] Here, when the ore phase conversion product is subjected to acid leaching treatment, the hydrochloric acid leaching solution is selected as a mixture of hydrochloric acid solution and a leaching aid, so that the leaching aid can complex fluoride ions, reduce the formation of CeF3 precipitation, and improve the rare earth leaching rate of the mixed rare earth concentrate.
[0064] In some possible embodiments, the surface modification of the acidic leaching slag is completed under the action of a plasma gas flow to obtain the surface-modified acidic leaching slag, which may include: placing the acidic leaching slag in a plasma cleaning apparatus having a second preset atmosphere and a power of 100 to 300 W for 10 to 60 min to obtain the acidic leaching slag with changed surface oxidation properties; the second preset atmosphere includes a mixture of hydrogen and an inert gas.
[0065] Here, the inert gas in the second preset atmosphere may be one or more of nitrogen, helium, and argon; and the plasma cleaning apparatus may enable the second preset atmosphere to generate a hydrogen ion flow.
[0066] In this embodiment, by using a mixture of hydrogen and inert gas as the second preset atmosphere, the plasma cleaner can generate a hydrogen plasma flow, so that the molecular chemical bonds on the surface of the acidic leached slag are broken and reorganized under the action of the hydrogen plasma flow, generating a new chemical structure, and completing the change of the oxidation performance of the surface of the acidic leached slag, so that the surface-modified acidic leached slag is oxidized as little as possible during the alkaline leaching treatment process in step 400.
[0067] In some possible embodiments, the surface-modified acidic leaching residue is subjected to alkaline leaching treatment to obtain alkaline leachate and alkaline leaching residue, which may include: adding the surface-modified acidic leaching residue to a sodium hydroxide solution, and reacting for 60 to 360 min at a temperature of 120 to 200° C. and a pressure of 0.1 to 5 MPa, at a stirring speed of 200 to 600 r / min, to obtain an alkaline leachate and an alkaline leaching residue; wherein the alkali-ore ratio of the sodium hydroxide solution and the acidic leaching residue is 1 to 7:1, and the liquid-solid ratio is 1 to 10:1.
[0068] It should be noted that when the surface-modified acidic leaching residue is subjected to alkaline leaching treatment, an inert gas is filled into the reactor so that the acidic leaching residue can complete the leaching treatment in an environment protected by the inert gas.
[0069] Here, in order to prevent the trivalent cerium ions contained in the surface-modified acidic leaching residue from being oxidized during the alkaline leaching treatment, an inert gas is used for pressurized leaching during the alkaline leaching treatment, so that the surface-modified acidic leaching residue is easier to be treated with alkaline leaching, and the trivalent cerium ions can be protected from oxidation.
[0070] In this embodiment, when the surface-modified acidic leaching residue is subjected to alkaline leaching treatment, the reaction is carried out under a pressure of 0.1 to 5 MPa, so that the alkaline leaching reaction of the acidic leaching residue can be carried out more thoroughly and the reaction efficiency of the alkaline leaching of the acidic leaching residue can be improved.
[0071] In some possible embodiments, the leaching separation of the mixed rare earth concentrate further includes: adding a hydrochloric acid solution with a concentration of 1 to 10 mol / L to the alkaline leaching residue to dissolve the alkaline leaching residue to obtain an acidic solution containing rare earth elements.
[0072] In this embodiment, a hydrochloric acid solution with a temperature of 50 to 70° C. is added to the alkaline leaching residue, so that the hydrochloric acid solution dissolves the alkaline leaching residue, and the rare earth elements in the leaching residue are dissolved in the hydrochloric acid solution, thereby obtaining an acidic solution containing rare earth elements that is convenient for recovering the rare earth elements, thereby reducing the waste of resources and the discharge of wastewater in the recovery process of the rare earth elements.
[0073] The following is a detailed description of the leaching and separation method of a mixed rare earth concentrate provided by the present invention through examples. It should be noted that the methods, reagents and materials described in the following examples, unless otherwise specified, can all be obtained from commercial channels; the test methods, unless otherwise specified, are all conventional methods.
[0074] Example 1
[0075] The present embodiment provides a leaching and separation method of a mixed rare earth concentrate, comprising the following steps:
[0076] (1) A mixed rare earth concentrate with a REO grade of 58.22%, a F grade of 6.11%, and a P grade of 5.30% was placed in a plasma cleaning apparatus with a hydrogen-argon atmosphere and a power of 240 W for 20 min to obtain a mixed rare earth concentrate with changed surface oxidation properties;
[0077] (2) After the surface-modified mixed rare earth concentrate is placed in a roaster, 400 mL / min of nitrogen is continuously introduced into the bottom of the roaster to keep the mixed rare earth concentrate in a fluidized state under the nitrogen atmosphere, and the mixed rare earth concentrate in the roaster is fluidized roasted at a temperature of 650°C for 60 min to obtain a mineral phase conversion product containing cerium oxide with fluoride;
[0078] (3) adding hydrochloric acid leachate to the mineral phase transformation product so that the liquid-to-solid ratio of the hydrochloric acid leachate to the mineral phase transformation product is 10:1, setting the stirring speed to 600 r / min, setting the ultrasonic power to 300 W, and stirring at a temperature of 75° C. for 20 min to obtain a hydrochloric acid leaching mixture including an acidic leachate containing rare earth and fluorine elements and a leach residue containing monazite; wherein the hydrochloric acid leachate includes a hydrochloric acid solution with a concentration of 4 mol / L and an AlCl3 solution with a concentration of 0.3 mol / L;
[0079] (4) placing the acid leaching residue in a plasma cleaning apparatus with a hydrogen-argon atmosphere and a power of 240 W for 20 minutes to obtain surface-modified acid leaching residue;
[0080] (5) adding sodium hydroxide solution to the surface-modified acidic leaching residue to make the alkali-ore ratio between the alkaline leaching solution and the secondary activation product be 5:1 and the liquid-solid ratio be 5:1, and applying a pressure of 0.5 MPa at a temperature of 160°C and a stirring speed of 600 r / min for 120 min to obtain an alkaline leaching solution containing phosphorus elements and an alkaline leaching residue containing rare earth elements; wherein the alkaline leaching solution containing phosphorus elements can be treated to recover the alkaline solution;
[0081] (6) Adding a hydrochloric acid solution with a concentration of 2 mol / L to the alkaline leaching residue, stirring the alkaline leaching residue until it is dissolved, thereby obtaining an acidic solution containing rare earth elements.
[0082] In this embodiment, the total leaching rate of the rare earth element-containing leaching solution (the rare earth element-containing leaching solution includes the acidic leaching solution containing rare earth and fluorine elements in step (3) and the acidic solution containing rare earth elements in step (6)) is 98.01%, wherein the leaching rate of fluorine element in the acidic leaching solution containing rare earth and fluorine elements in step (3) is 97.82%, and the leaching rate of phosphorus element in the alkaline leaching solution containing phosphorus element in step (5) is 98.58%.
[0083] Example 2
[0084] The present embodiment provides a leaching and separation method of a mixed rare earth concentrate, comprising the following steps:
[0085] (1) A mixed rare earth concentrate with a REO grade of 58.22%, a F grade of 6.11%, and a P grade of 5.30% was placed in a plasma cleaning apparatus with a hydrogen-argon atmosphere and a power of 240 W for 20 min to obtain a mixed rare earth concentrate with changed surface oxidation properties;
[0086] (2) After the surface-modified mixed rare earth concentrate is placed in a roaster, 400 mL / min of nitrogen is continuously introduced into the bottom of the roaster to keep the mixed rare earth concentrate in a fluidized state under the nitrogen atmosphere, and the mixed rare earth concentrate in the roaster is fluidized roasted at a temperature of 550°C for 60 min to obtain a mineral phase conversion product containing cerium oxide with fluoride;
[0087] (3) adding hydrochloric acid leachate to the mineral phase transformation product so that the liquid-to-solid ratio of the hydrochloric acid leachate to the mineral phase transformation product is 10:1, setting the stirring speed to 600 r / min, setting the ultrasonic power to 300 W, and stirring at a temperature of 75° C. for 20 min to obtain a hydrochloric acid leaching mixture including an acidic leachate containing rare earth and fluorine elements and a leach residue containing monazite; wherein the hydrochloric acid leachate includes a hydrochloric acid solution with a concentration of 4 mol / L and an AlCl3 solution with a concentration of 0.3 mol / L;
[0088] (4) placing the acid leaching residue in a plasma cleaning apparatus with a hydrogen-argon atmosphere and a power of 240 W for 20 minutes to obtain surface-modified acid leaching residue;
[0089] (5) adding sodium hydroxide solution to the surface-modified acidic leaching residue to make the alkali-ore ratio between the alkaline leaching solution and the secondary activation product be 5:1 and the liquid-solid ratio be 5:1, and applying a pressure of 0.5 MPa at a temperature of 160°C and a stirring speed of 600 r / min for 120 min to obtain an alkaline leaching solution containing phosphorus elements and an alkaline leaching residue containing rare earth elements; wherein the alkaline leaching solution containing phosphorus elements can be treated to recover the alkaline solution;
[0090] (6) Adding a hydrochloric acid solution with a concentration of 2 mol / L to the alkaline leaching residue, stirring the alkaline leaching residue until it is dissolved, thereby obtaining an acidic solution containing rare earth elements.
[0091] In this embodiment, the total leaching rate of the rare earth element-containing leaching solution (the rare earth element-containing leaching solution includes the acidic leaching solution containing rare earth and fluorine elements in step (3) and the acidic solution containing rare earth elements in step (6)) is 95.32%, wherein the leaching rate of fluorine element in the acidic leaching solution containing rare earth and fluorine elements in step (3) is 93.82%, and the leaching rate of phosphorus element in the alkaline leaching solution containing phosphorus element in step (5) is 97.58%.
[0092] Example 3
[0093] The present embodiment provides a leaching and separation method of a mixed rare earth concentrate, comprising the following steps:
[0094] (1) A mixed rare earth concentrate with a REO grade of 58.22%, a F grade of 6.11%, and a P grade of 5.30% was placed in a plasma cleaning apparatus with a hydrogen-argon atmosphere and a power of 240 W for 20 min to obtain a mixed rare earth concentrate with changed surface oxidation properties;
[0095] (2) After the surface-modified mixed rare earth concentrate is placed in a roaster, 400 mL / min of nitrogen is continuously introduced into the bottom of the roaster to keep the mixed rare earth concentrate in a fluidized state under the nitrogen atmosphere, and the mixed rare earth concentrate in the roaster is fluidized roasted at a temperature of 650°C for 60 min to obtain a mineral phase conversion product containing cerium oxide with fluoride;
[0096] (3) adding hydrochloric acid leachate to the mineral phase transformation product so that the liquid-solid ratio of the hydrochloric acid leachate to the mineral phase transformation product is 10:1, setting the stirring speed to 600 r / min, setting the ultrasonic power to 300 W, stirring at a temperature of 90° C. for 20 min, and obtaining a hydrochloric acid leaching mixture including an acidic leachate containing rare earth and fluorine elements and a leach residue containing monazite; wherein the hydrochloric acid leachate includes a hydrochloric acid solution with a concentration of 4 mol / L and an AlCl3 solution with a concentration of 0.3 mol / L;
[0097] (4) placing the acid leaching residue in a plasma cleaning apparatus with a hydrogen-argon atmosphere and a power of 240 W for 20 minutes to obtain surface-modified acid leaching residue;
[0098] (5) adding sodium hydroxide solution to the surface-modified acidic leaching residue to make the alkali-ore ratio between the alkaline leaching solution and the secondary activation product be 5:1 and the liquid-solid ratio be 5:1, and applying a pressure of 0.5 MPa at a temperature of 160°C and a stirring speed of 600 r / min for 120 min to obtain an alkaline leaching solution containing phosphorus elements and an alkaline leaching residue containing rare earth elements; wherein the alkaline leaching solution containing phosphorus elements can be treated to recover the alkaline solution;
[0099] (6) Adding a hydrochloric acid solution with a concentration of 2 mol / L to the alkaline leaching residue, stirring the alkaline leaching residue until it is dissolved, thereby obtaining an acidic solution containing rare earth elements.
[0100] In this embodiment, the total leaching rate of the rare earth element-containing leaching solution (the rare earth element-containing leaching solution includes the acidic leaching solution containing rare earth and fluorine elements in step (3) and the acidic solution containing rare earth elements in step (6)) is 96.28%, wherein the leaching rate of fluorine element in the acidic leaching solution containing rare earth and fluorine elements in step (3) is 94.36%, and the leaching rate of phosphorus element in the alkaline leaching solution containing phosphorus element in step (5) is 99.19%.
[0101] Example 4
[0102] The present embodiment provides a leaching and separation method of a mixed rare earth concentrate, comprising the following steps:
[0103] (1) A mixed rare earth concentrate with a REO grade of 58.22%, a F grade of 6.11%, and a P grade of 5.30% was placed in a plasma cleaning apparatus with a hydrogen-argon atmosphere and a power of 240 W for 20 min to obtain a mixed rare earth concentrate with changed surface oxidation properties;
[0104] (2) After the surface-modified mixed rare earth concentrate is placed in a roaster, 400 mL / min of nitrogen is continuously introduced into the bottom of the roaster to keep the mixed rare earth concentrate in a fluidized state under the nitrogen atmosphere, and the mixed rare earth concentrate in the roaster is fluidized roasted at a temperature of 650°C for 60 min to obtain a mineral phase conversion product containing cerium oxide with fluoride;
[0105] (3) adding hydrochloric acid leachate to the mineral phase transformation product so that the liquid-to-solid ratio of the hydrochloric acid leachate to the mineral phase transformation product is 10:1, setting the stirring speed to 600 r / min, setting the ultrasonic power to 300 W, and stirring at a temperature of 75° C. for 20 min to obtain a hydrochloric acid leaching mixture including an acidic leachate containing rare earth and fluorine elements and a leach residue containing monazite; wherein the hydrochloric acid leachate includes a hydrochloric acid solution with a concentration of 4 mol / L and an AlCl3 solution with a concentration of 0.3 mol / L;
[0106] (4) placing the acid leaching residue in a plasma cleaning apparatus with a hydrogen-argon atmosphere and a power of 240 W for 20 minutes to obtain surface-modified acid leaching residue;
[0107] (5) adding sodium hydroxide solution to the surface-modified acidic leaching residue to make the alkali-ore ratio between the alkaline leaching solution and the secondary activation product be 5:1 and the liquid-solid ratio be 5:1, and applying a pressure of 1 MPa at a temperature of 180°C and a stirring speed of 600 r / min for 120 min to obtain an alkaline leaching solution containing phosphorus elements and an alkaline leaching residue containing rare earth elements; wherein the alkaline leaching solution containing phosphorus elements can be treated to recover the alkaline solution;
[0108] (6) Adding a hydrochloric acid solution with a concentration of 2 mol / L to the alkaline leaching residue, stirring the alkaline leaching residue until it is dissolved, thereby obtaining an acidic solution containing rare earth elements.
[0109] In this embodiment, the total leaching rate of the rare earth element-containing leaching solution (the rare earth element-containing leaching solution includes the acidic leaching solution containing rare earth and fluorine elements in step (3) and the acidic solution containing rare earth elements in step (6)) is 98.68%, wherein the leaching rate of fluorine element in the acidic leaching solution containing rare earth and fluorine elements in step (3) is 98.82%, and the leaching rate of phosphorus element in the alkaline leaching solution containing phosphorus element in step (5) is 99.37%.
[0110] Comparative Example 1
[0111] This comparative example provides a leaching and separation method for a mixed rare earth concentrate, comprising the following steps:
[0112] (1) After the mixed rare earth concentrate is placed in a roaster, 400 mL / min of nitrogen is continuously introduced into the bottom of the roaster to keep the mixed rare earth concentrate in a fluidized state under the nitrogen atmosphere, and the mixed rare earth concentrate in the roaster is fluidized roasted at a temperature of 650°C for 60 min to obtain a mineral phase conversion product containing cerium oxyfluoride;
[0113] (2) adding hydrochloric acid leachate to the mineral phase transformation product so that the liquid-to-solid ratio of the hydrochloric acid leachate to the mineral phase transformation product is 10:1, setting the stirring speed to 600 r / min, setting the ultrasonic power to 300 W, and stirring at a temperature of 75° C. for 20 min to obtain a hydrochloric acid leaching mixture including an acidic leachate containing rare earth and fluorine elements and a leach residue containing monazite; wherein the hydrochloric acid leachate includes a hydrochloric acid solution with a concentration of 4 mol / L and an AlCl3 solution with a concentration of 0.3 mol / L;
[0114] (3) adding sodium hydroxide solution to the acidic leaching residue so that the alkali-ore ratio between the alkaline leaching solution and the secondary activation product is 5:1 and the liquid-solid ratio is 5:1, and applying a pressure of 0.5 MPa at a temperature of 160°C and a stirring speed of 600 r / min for 120 min to obtain an alkaline leaching solution containing phosphorus elements and an alkaline leaching residue containing rare earth elements; wherein the alkaline leaching solution containing phosphorus elements can be treated to recover the alkaline solution;
[0115] (4) Adding a hydrochloric acid solution with a concentration of 2 mol / L to the alkaline leaching residue, stirring the alkaline leaching residue until it is dissolved, thereby obtaining an acidic solution containing rare earth elements.
[0116] The total leaching rate of the rare earth element-containing leaching solution finally obtained in this comparative example (the rare earth element-containing leaching solution includes the acidic leaching solution containing rare earth and fluorine elements in step (2) and the acidic solution containing rare earth elements in step (4)) is 94.55%, wherein the leaching rate of fluorine element in the acidic leaching solution containing rare earth and fluorine elements in step (2) is 92.49%, and the leaching rate of phosphorus element in the alkaline leaching solution containing phosphorus element in step (3) is 97.63%.
[0117] Comparative Example 2
[0118] A leaching and separation method for a mixed rare earth concentrate comprises the following steps:
[0119] (1) A mixed rare earth concentrate with a REO grade of 58.22%, a F grade of 6.11%, and a P grade of 5.30% was placed in a plasma cleaning apparatus with a hydrogen-argon atmosphere and a power of 240 W for 20 min to obtain a mixed rare earth concentrate with changed surface oxidation properties;
[0120] (2) After the surface-modified mixed rare earth concentrate is placed in a roaster, 400 mL / min of nitrogen is continuously introduced into the bottom of the roaster to keep the mixed rare earth concentrate in a fluidized state under the nitrogen atmosphere, and the mixed rare earth concentrate in the roaster is fluidized roasted at a temperature of 650°C for 60 min to obtain a mineral phase conversion product containing cerium oxide with fluoride;
[0121] (3) adding hydrochloric acid leachate to the mineral phase transformation product so that the liquid-to-solid ratio of the hydrochloric acid leachate to the mineral phase transformation product is 10:1, setting the stirring speed to 600 r / min, stirring at a temperature of 75°C for 20 min, and obtaining a hydrochloric acid leaching mixture including an acidic leachate containing rare earth and fluorine elements and a leach residue containing monazite; wherein the hydrochloric acid leachate is a hydrochloric acid solution with a concentration of 4 mol / L;
[0122] (4) placing the acid leaching residue in a plasma cleaning apparatus with a hydrogen-argon atmosphere and a power of 240 W for 20 minutes to obtain surface-modified acid leaching residue;
[0123] (5) adding sodium hydroxide solution to the surface-modified acidic leaching residue to make the alkali-ore ratio between the alkaline leaching solution and the secondary activation product be 5:1 and the liquid-solid ratio be 5:1, and applying a pressure of 0.5 MPa at a temperature of 160°C and a stirring speed of 600 r / min for 120 min to obtain an alkaline leaching solution containing phosphorus elements and an alkaline leaching residue containing rare earth elements; wherein the alkaline leaching solution containing phosphorus elements can be treated to recover the alkaline solution;
[0124] (6) Adding a hydrochloric acid solution with a concentration of 2 mol / L to the alkaline leaching residue, stirring the alkaline leaching residue until it is dissolved, thereby obtaining an acidic solution containing rare earth elements.
[0125] The total leaching rate of the rare earth element-containing leaching solution finally obtained in this comparative example (the rare earth element-containing leaching solution includes the acidic leaching solution containing rare earth and fluorine elements in step (3) and the acidic solution containing rare earth elements in step (6)) is 95.38%, wherein the leaching rate of fluorine element in the acidic leaching solution containing rare earth and fluorine elements in step (3) is 51.42%, and the leaching rate of phosphorus element in the alkaline leaching solution containing phosphorus element in step (5) is 96.37%.
[0126] It can be seen from the above-mentioned embodiments and comparative examples that the present invention adopts the method of surface modification of the mixed rare earth concentrate by subjecting the mixed rare earth concentrate to the action of plasma gas flow, so that the generation of CeO2 can be reduced in the process of mineral phase transformation of the surface-modified mixed rare earth concentrate, and then the fluorocarbon cerium ore in the mixed rare earth concentrate can be directionally phase-converted into cerium fluoride oxide, so that the mineral phase transformation product obtained by roasting has a higher rare earth leaching rate; at the same time, the acid leaching slag obtained by acid leaching treatment of the mineral phase transformation product is surface-modified by the action of plasma gas flow, so that the oxidation reaction of the surface-modified acid leaching slag is reduced in the process of alkaline leaching treatment, so that the alkaline leaching slag obtained does not contain or contains a small amount of tetravalent cerium ions, thereby realizing the effective separation of rare earth elements, phosphorus elements and fluorine elements in the mixed rare earth concentrate, and can also improve the leaching rate of rare earth elements, phosphorus elements and fluorine elements in the mixed rare earth concentrate. In addition, by adding a leaching aid to complex fluoride ions during the acid leaching process, the generation of CeF3 can be reduced, the rare earth leaching rate and the recovery rate of fluorine element can be improved. In addition, during the acid leaching process, an ultrasonic external field is applied to make the reaction more thorough, further improving the recovery rate of rare earth elements.
[0127] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A leaching and separation method for mixed rare earth concentrate, characterized in that: include: subjecting the mixed rare earth concentrate to surface modification under the action of a plasma gas flow to obtain a surface-modified mixed rare earth concentrate; Performing mineral phase transformation on the surface-modified mixed rare earth concentrate to transform the bastnaesite phase in the mixed rare earth concentrate into cerium fluoride oxide, thereby obtaining a mineral phase transformation product containing cerium fluoride oxide; The mineral phase conversion product is subjected to acid leaching treatment to obtain an acid leaching solution and an acid leaching residue; the acid leaching solution contains rare earth ions and fluoride ions, and the acid leaching residue contains monazite; wherein, during the acid leaching treatment of the mineral phase conversion product, an ultrasonic external field is applied; and during the acid leaching treatment, a leaching aid is added; The acidic leaching residue is subjected to surface modification under the action of a plasma gas flow to obtain surface-modified acidic leaching residue; The surface-modified acidic leaching residue is subjected to alkaline leaching treatment to obtain alkaline leaching solution and alkaline leaching residue; the alkaline leaching solution contains phosphorus, and the alkaline leaching residue contains rare earth elements.
2. The leaching and separation method of mixed rare earth concentrate according to claim 1, characterized in that: The method of subjecting the mixed rare earth concentrate to the action of a plasma gas flow to complete the surface modification of the mixed rare earth concentrate to obtain a surface-modified mixed rare earth concentrate comprises: The mixed rare earth concentrate is placed in a plasma cleaning device with a first preset atmosphere and a power of 100 to 300 W for 10 to 60 minutes to obtain a mixed rare earth concentrate with changed surface oxidation properties; the first preset atmosphere is a mixture of hydrogen and inert gas.
3. The leaching and separation method of mixed rare earth concentrate according to claim 1, characterized in that: The method of performing mineral phase transformation on the surface-modified mixed rare earth concentrate to transform the bastnaesite phase in the mixed rare earth concentrate into cerium fluoride oxide to obtain a mineral phase transformation product containing cerium fluoride oxide comprises: The surface-modified mixed rare earth concentrate is subjected to fluidized roasting in an inert atmosphere to convert the bastnaesite phase in the mixed rare earth concentrate into cerium fluoride oxide, thereby obtaining a roasting product containing cerium fluoride oxide, and the roasting product is used as the mineral phase conversion product.
4. The leaching and separation method of the mixed rare earth concentrate according to claim 3, characterized in that: The surface-modified mixed rare earth concentrate is subjected to fluidized roasting in an inert atmosphere to convert the bastnaesite phase in the mixed rare earth concentrate into cerium oxyfluoride to obtain a roasting product containing cerium oxyfluoride, comprising: After the surface-modified mixed rare earth concentrate is placed in a roasting furnace, an inert gas is continuously introduced into the bottom of the roasting furnace, and the inert gas is used as a fluidizing gas to keep the mixed rare earth concentrate in a fluidized state under an inert atmosphere; The heating temperature of the roasting furnace is adjusted so that the mixed rare earth concentrate in a fluidized state is heated at a temperature of 450 to 750° C. for 20 to 120 minutes to complete the reaction of converting bastnaesite in the mixed rare earth concentrate into cerium fluoride oxide to obtain the roasting product.
5. The leaching and separation method of mixed rare earth concentrate according to claim 4, characterized in that: The inert gas continuously introduced into the bottom of the calcining furnace has a gas flow rate of 300 to 1000 mL / min.
6. The leaching and separation method of mixed rare earth concentrate according to claim 1, characterized in that: The acid leaching treatment of the mineral phase conversion product to obtain acid leaching solution and acid leaching residue comprises: The mineral phase conversion product is added to the hydrochloric acid leaching solution, and stirred for 20 to 120 min at a temperature of 60 to 100° C., an ultrasonic power of 300 to 600 W, and a stirring speed of 200 to 600 r / min to obtain the acidic leaching solution and acidic leaching residue.
7. The leaching and separation method of mixed rare earth concentrate according to claim 6, characterized in that: The liquid-to-solid ratio of the hydrochloric acid leaching solution and the mineral phase conversion product is 4-20:1; the hydrochloric acid leaching solution comprises a hydrochloric acid solution with a concentration of 1-10 mol / L and a leaching aid with a concentration of 0.1-0.5 mol / L; the leaching aid is aluminum chloride or boric acid.
8. The leaching and separation method of mixed rare earth concentrate according to claim 1, characterized in that: The acidic leaching residue is subjected to surface modification under the action of a plasma gas flow to obtain surface-modified acidic leaching residue, comprising: The acidic leaching residue is placed in a plasma cleaning device with a second preset atmosphere and a power of 100 to 300 W for 10 to 60 minutes to obtain acidic leaching residue with changed surface oxidation properties; the second preset atmosphere includes a mixture of hydrogen and inert gas.
9. The leaching and separation method of mixed rare earth concentrate according to claim 1, characterized in that: The alkaline leaching treatment is performed on the surface-modified acidic leaching residue to obtain an alkaline leaching solution and alkaline leaching residue, comprising: The surface-modified acidic leaching residue is added with a sodium hydroxide solution, and reacted for 60 to 360 min at a temperature of 120 to 200° C. and a pressure of 0.1 to 5 MPa at a stirring speed of 200 to 600 r / min to obtain the alkaline leaching solution and alkaline leaching residue; wherein the alkali-ore ratio of the sodium hydroxide solution and the acidic leaching residue is 1 to 7:1, and the liquid-solid ratio is 1 to 10:
1.
10. The leaching and separation method of mixed rare earth concentrate according to any one of claims 1 to 9, characterized in that: Also includes: A hydrochloric acid solution with a concentration of 1 to 10 mol / L is added to the alkaline leaching residue to dissolve the alkaline leaching residue to obtain an acidic solution containing rare earth elements.