X-ray detector based on halide metal complex gel and preparation method thereof
By using halogenated metal complex gel material in X-ray detectors, the problems of poor stability and low sensitivity of traditional detector materials are solved, and a large-area X-ray detector with high responsiveness and stability are achieved.
Patent Information
- Application Number
- CN202411171015.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-26
AI Technical Summary
Traditional X-ray detector materials have problems such as poor stability, low sensitivity, slow response speed and insensitive to X-rays. It is difficult to prepare large-area, large-thickness materials and high cost.
Using gel materials based on halide metal complexes, the halide metal complex is mixed with the phosphorus-containing complex and the metal halide in a solvent to form a halide metal complex, annealing treatment forms a gel active layer, construct an X-ray detector, and adjust the gel active layer. Thickness to improve the thickness and stability of the detector.
An X-ray detector with high stability, large atomic number, high sensitivity and fast response is achieved, which reduces edge effects and interface tension, and improves the stability of material use and large-scale uniformity.
Smart Images

Figure CN118714860B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of X-ray detectors, and in particular relates to an X-ray detector based on a halide metal complex gel and a preparation method thereof. Background Art
[0002] X-ray detectors are widely used in medical diagnosis, security inspection, materials science and other fields. Traditional X-ray detectors have the advantages of high energy resolution, fast response speed and low noise level, but they also have problems such as small atomic number, insufficient X-ray absorption ability, low sensitivity and insensitivity to X-rays. Therefore, there is an urgent need to develop new X-ray detector materials that can overcome the shortcomings of traditional X-ray detector materials.
[0003] In order to improve the material's ability to absorb X-rays, X-ray detectors require a relatively thick active layer, but currently most of the materials used for X-ray detection are thin film materials. However, when preparing large-area and thick X-ray detection materials, there are problems such as difficulty and high cost. Metal halide gel is a gel system formed by metal halides (such as chloride, bromide, iodide, etc.) in an appropriate solvent, and stable metal halide gel materials as X-ray detector materials have the advantages of easy preparation, simple process, and adjustable thickness. Therefore, the new stable metal halide gel has a very broad application prospect in the fields of X-ray detection and so on.
[0004] However, existing X-ray detectors made of metal halide gels still have defects such as poor stability, low sensitivity, and slow response speed. Summary of the invention
[0005] In view of this, the present invention aims to provide an X-ray detector based on a halogenated metal complex gel and a preparation method thereof, aiming to solve at least one technical problem in the background technology.
[0006] The present invention is achieved in that:
[0007] The present invention provides an X-ray detector based on a halogenated metal complex gel, which comprises a substrate, a modification layer, a gel active layer and an electrode stacked in sequence from bottom to top;
[0008] The gelling material is coated on the surface of the substrate to form the modified layer;
[0009] The material of the gel active layer is a halogenated metal complex formed by mixing a phosphorus-containing complex and a metal halide in a solvent; the halogenated metal complex is annealed to form the gel active layer on the modified layer on the surface of the substrate;
[0010] The general structural formula of the phosphorus-containing complex is:
[0011] ;
[0012] The general structural formula of the halogenated metal complex is:
[0013] ;
[0014] Wherein, R1, R2, R3, R4 are all cycloalkyl, benzene ring or chain alkyl; R5 is chain hydrocarbon group; X is halogen; MX a is a metal halide, a is the valence number of metal M, and b is the molar ratio of the metal halide.
[0015] Furthermore, the cycloalkyl group is C3 cycloalkyl~C6 cycloalkyl; R5 is C3 chain hydrocarbon group~C6 chain hydrocarbon group.
[0016] Furthermore, the halogen is F, Cl or Br.
[0017] Furthermore, the solvent is any one of amide solvents, hydrazide solvents, alcohol solvents, ester solvents, sulfone solvents, sulfoxide solvents, ketone solvents, nitrile solvents, pyridine, and tetrahydrofuran.
[0018] Furthermore, in practical applications, the molar ratio of the metal halide to the phosphorus-containing complex, that is, the value of b, is controlled according to the valence state of the metal M in the metal halide; when the metal M is divalent, b=2; when the metal M is trivalent, b=1.2~1.4; when the metal M is monovalent, b=2~4; when the metal M is tetravalent, b=1~1.2.
[0019] The present invention provides a method for preparing the above-mentioned X-ray detector based on the halide metal complex gel, comprising the following steps:
[0020] The phosphorus-containing complex is mixed with a metal halide, and then fully dissolved in a solvent to prepare a gel precursor solution;
[0021] Applying a liquid gelling material on a substrate to form a finishing layer after drying;
[0022] A gel precursor solution is dripped onto the surface of the modified layer of the substrate to cover the modified layer, and a gel active layer is obtained after annealing;
[0023] Conductive electrodes are arranged on the surface of the gel active layer to produce an X-ray detector.
[0024] Furthermore, the general structural formula of the phosphorus-containing complex is:
[0025] ;
[0026] Wherein, R1, R2, R3, and R4 are all cycloalkyl, benzene ring, or chain alkyl; R5 is a chain hydrocarbon group; X is a halogen;
[0027] The metal halide is MX a , a is the valence number of the metal M, and X is the same halogen as in the phosphorus-containing complex.
[0028] Furthermore, the annealing treatment is performed at a temperature of 100° C. to 120° C. and for a time of 9 h to 11 h.
[0029] Furthermore, the cycloalkyl group is C3 cycloalkyl~C6 cycloalkyl; R5 is C3 chain hydrocarbon group~C6 chain hydrocarbon group.
[0030] Furthermore, the molar ratio of the metal halide to the phosphorus-containing complex is b; when the metal M in the metal halide is divalent, b=2; when the metal M is trivalent, b=1.2-1.4; when the metal M is monovalent, b=2-4; when the metal M is tetravalent, b=1-1.2.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] (1) The phosphorus-containing complex of the present invention can be combined with different metal halide cations to form a series of stable halide metal complex gel materials, which can still maintain their original properties under unconventional environments (such as high temperatures); the X-ray detector prepared based on the gel has many advantages such as high stability, large atomic number, high sensitivity, fast response to X-rays, and adjustable thickness.
[0033] (2) The present invention can adjust the thickness of the gel active layer, thereby changing the thickness of the X-ray detector.
[0034] (3) The thickness of the X-ray detector of the present invention can be adjusted by changing the thickness of the gel active layer. Increasing the thickness of the X-ray detector can reduce the edge effect and interfacial tension, which is beneficial to the expanded manufacturing of the X-ray detector. In addition, the increase in thickness can promote the uniformity of the large-scale gel active layer.
[0035] (4) The X-ray detector of the present invention uses the halide metal complex gel as the active layer and has strong stability in use; it can maintain long-term stability in actual use environments such as dark state and light state. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is a schematic diagram of the structure of the X-ray detector made by the present invention;
[0037] Figure 2 This is a physical picture of the gel active layer formed in Example 1 of the present invention;
[0038] Figure 3 is a thermogravimetric diagram of the gel active layer formed in Example 1 of the present invention at 100°C;
[0039] Figure 4 This is a physical picture of the gel active layer formed in Example 2 of the present invention;
[0040] Figure 5 is a thermogravimetric diagram of the gel active layer formed in Example 2 of the present invention at 100°C;
[0041] Figure 6 is a schematic diagram of the crystal molecular structure of the lead iodide complex formed in Example 3 of the present invention;
[0042] Figure 7 This is a physical picture of the gel active layer formed in Example 3 of the present invention;
[0043] Figure 8 This is a current density-time response diagram of the X-ray detector prepared in Example 1 of the present invention under different bias voltages and different dose rate X-rays;
[0044] Fig. 9 This is a current density-time response diagram of the X-ray detector prepared in Example 2 of the present invention under different bias voltages and different dose rate X-rays;
[0045] Fig.10 This is a current density-time response diagram of the X-ray detector prepared in Example 3 of the present invention under different bias voltages and different dose rate X-rays;
[0046] Fig.11 is a data relationship diagram of dose rate-current density of the X-ray detector manufactured in Example 1 of the present invention under different bias voltages;
[0047] Fig.12 is a data relationship diagram of dose rate-current density of the X-ray detector manufactured in Example 2 of the present invention under different bias voltages;
[0048] Fig.13 is a data relationship diagram of dose rate-current density of the X-ray detector manufactured in Example 3 of the present invention under different bias voltages;
[0049] Fig.14 is a dark current drift diagram of the X-ray detector prepared in Example 1 of the present invention in a dark state;
[0050] Fig.15 is a dark current drift diagram of the X-ray detector prepared in Example 2 of the present invention in a dark state;
[0051] Fig.16 This is a dark current drift diagram of the X-ray detector prepared in Example 3 of the present invention in a dark state. DETAILED DESCRIPTION
[0052] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific implementation cases described herein are only used to explain the present invention and are not used to limit the present invention.
[0053] X-ray detectors based on halide metal complex gels, the structure of which is Figure 1 As shown, it includes a substrate 1, a modification layer 2, a gel active layer 3 and an electrode 4 stacked in sequence from bottom to top; wherein the modification layer 2 is formed by coating a gelling material on the surface of the substrate 1; the material of the gel active layer 3 adopts a halogenated metal complex formed by mixing a phosphorus-containing complex with a metal halide in a solvent; the halogenated metal complex is a gel, and the gel is annealed to form the gel active layer 3 on the modification layer 2 on the surface of the substrate 1; the electrode 4 is arranged on the surface of the gel active layer 3, and can be obtained by pasting or evaporation deposition.
[0054] The substrate 1 adopts an X-ray detector substrate permitted in the art, such as quartz glass, indium tin oxide glass, fluorine-doped tin oxide glass, PCB circuit board, flexible FPC, thin film transistor array as a substrate. In the following embodiments, quartz glass, indium tin oxide glass, etc. are used as examples, but are not limited to these substrate materials, and other substrate materials not listed are also applicable.
[0055] The material of the modification layer 2 is a gelling material permitted in the art, including but not limited to polymethyl methacrylate, poly(9-vinyl carbazole), polyacrylic acid, polyvinyl pyrrolidone, organic silica gel, epoxy resin, anaerobic glue, hot melt adhesive, pressure sensitive adhesive, latex. In the following embodiments, polyvinyl pyrrolidone and poly(9-vinyl carbazole) are used as examples, but are not limited to these gelling materials. Other gelling materials not listed are also applicable.
[0056] The halogenated metal complex in the gel active layer 3 can be purchased from the market or synthesized by itself, and its general structural formula is:
[0057] ;
[0058] Wherein, R1, R2, R3, and R4 are all C3 cycloalkyl to C6 cycloalkyl, benzene ring or C3 chain alkyl to C6 chain alkyl; R1 to R4 are groups that form ligands with P, and they adopt any C3 to C6 cyclic, saturated carbon chain, unsaturated carbon chain straight chain or branched chain structure. In the following embodiments, cyclohexane is used as an example, but it is not limited to this material, and other groups not listed are also applicable;
[0059] R5 is a chain hydrocarbon group; it adopts any saturated carbon chain of C3~C6, unsaturated carbon chain straight chain or branched chain structure, and the following embodiments are illustrated by propane group, but it is not limited to this material, and other chain hydrocarbon groups not listed are also applicable;
[0060] X is a halogen, such as F or Cl or Br;
[0061] MX a is a metal halide, a is the valence number of the metal M, b is the molar ratio of the metal halide, specifically refers to the ratio of the metal halide to the phosphorus-containing complex, and the value of b is related to the valence of the metal; when the metal M is divalent, b=2; when the metal M is trivalent, b=1.2-1.4; when the metal M is monovalent, b=2-4; when the metal M is tetravalent, b=1-1.2; in practical applications, the value of b is controlled according to the valence of the metal M in the metal halide;
[0062] Metal M can be any metal element permitted in the art, such as Pb 2+ 、Bi 3+ , Fe 3+ , Fe 2+ 、Co 2+ 、In 3+ 、In + , K + , Cs + , Rb + 、Te 4+ ,Ge 2+ , Ca 2+ , Ba 2+ , Sr 2+ , Hg 2+ 、Cd 2+ , Pt 2+ 、Zn 2+ , Sb 3+ Sn 2+ Sn 4+ , Mn 2+ , Cu 2+ , Cu + ,La 3 + 、Eu 2+ 、Eu 3+ , Tb 3+ In the following examples, Pb 2+ , Sb 3+ 、Co 2+ The above are examples, but are not limited to these materials, and other metals not listed are also applicable.
[0063] The solvent is any solvent that can dissolve the corresponding halogenated metal complex, such as any one of amide solvents, hydrazide solvents, alcohol solvents, ester solvents, sulfone solvents, sulfoxide solvents, ketone solvents, nitrile solvents, pyridine, and tetrahydrofuran. In the following embodiments, N,N-dimethylformamide DMF is used as an example, but it is not limited to this material. Other solvents not listed are also applicable.
[0064] The electrode 4 is made of a conductive electrode material permitted in the art, including but not limited to gold, silver, platinum, copper, aluminum, indium tin oxide, fluorine-doped tin oxide, carbon-based, conductive polymer and other electrode materials. In the following embodiments, gold and copper electrodes are selected as examples, but are not limited to these materials. Other conductive electrode materials not listed are also applicable.
[0065] The preparation method of the X-ray detector based on the halide metal complex gel comprises the following steps:
[0066] S1. Mix the phosphorus-containing complex with the metal halide, and then fully dissolve them in a solvent to obtain a gel precursor solution. The phosphorus-containing complex has the structural formula: ;
[0067] S2, coating the liquid gelling material on the substrate, and forming a modified layer after drying;
[0068] S3, dripping the gel precursor solution on the surface of the modified layer of the substrate to cover the modified layer, and obtaining the gel active layer after annealing treatment, the annealing temperature is 100°C~120°C, and the time is 9h~11h;
[0069] S4. Disposing a conductive electrode on the surface of the gel active layer to obtain an X-ray detector.
[0070] Example 1
[0071] The X-ray detector based on the halide metal complex gel comprises the following steps:
[0072] S1. Synthesis of gel precursor solution of antimony iodide complex
[0073] (1) Dissolve 2 mmol of 1,3-bis(dicyclohexylphosphino)propane bis(tetrafluoroborate) in 30 ml of acetonitrile solution, then dissolve 4 mmol of potassium iodide in 30 ml of deionized water, mix the two thoroughly, and stir in an oil bath at 30°C for 6 hours;
[0074] (2) After the reaction is completed, there is a white precipitate at the bottom. Remove the white precipitate at the bottom by suction filtration, take the clarified solution and perform water bath rotary evaporation. After all the acetonitrile and deionized water are removed by rotary evaporation, add 60 ml of a mixed solvent of ether and isopropanol (the volume of ether: the volume of isopropanol = 3:1), and place it in an ultrasonic cleaner for ultrasonic cleaning for 5 minutes.
[0075] (3) A white precipitate is generated during the ultrasonic process. After the ultrasonic process is completed, the mixed solvent of ether and isopropanol is removed by filtration, and then the mixed solvent of ether and isopropanol is repeatedly added for washing three times and then filtered. The powder obtained after filtration is placed in a vacuum drying oven and dried for 3 hours at a drying temperature of 45°C. The obtained white precipitate is a clean and high-purity phosphorus-containing complex with a molar mass of 692.2 g / mol.
[0076] (4) taking 0.1 mmol of the phosphorus-containing complex and 0.13 mmol of antimony iodide, and fully dissolving the two in 200 μL of N,N-dimethylformamide to obtain a gel precursor solution, i.e., the antimony iodide complex dissolved in N,N-dimethylformamide;
[0077] The structural formula of antimony iodide complex is:
[0078] ;
[0079] S2. Preparation of modified layer
[0080] Polyvinyl pyrrolidone was dissolved in acetone to form a 20 mg / mL gel solution, and 20 μL of the gel solution was spin-coated on a quartz glass substrate on a gel coater at a speed of 3000 rpm for 30 seconds. After spin coating, the substrate was pre-treated on a 60°C hot plate for 5 minutes, and a modified layer with a thickness of about 20 nm was formed after drying.
[0081] S3. Preparation of gel active layer
[0082] 125 μL of gel precursor solution was dripped onto the surface of the substrate containing the modified layer, and the modified layer was covered, and then placed on a 110°C hot plate for annealing for 10 hours to obtain a stable halide metal complex gel, thereby forming a gel active layer with a thickness of about 210 μm. Figure 2 As shown;
[0083] S4. Preparation of electrodes
[0084] Two 1mm thick plastic bags were pressed and pasted on the surface of the gel active layer. 2 By using a conductive copper electrode, an X-ray detector based on halide metal complex gel can be produced.
[0085] The halogenated metal complex gel prepared in step S3 was subjected to a thermal weight loss test. 10 mg of the gel was placed in a crucible and heated to a target temperature of 100°C at a rate of 10°C / min. The temperature was then maintained. The weight of the gel at different times was measured and compared with the initial weight to measure the thermal weight loss. The thermal weight loss graph is shown in FIG. Figure 3 As shown, from Figure 3 It can be seen that the weight loss in the thermal gravimetric test under continuous heating at 100°C for more than 180 minutes does not exceed 0.8%, indicating that the gel sample still has excellent stability under extreme conditions.
[0086] Example 2
[0087] The X-ray detector based on the halide metal complex gel comprises the following steps:
[0088] S1. Synthesis of gel precursor solution of cobalt bromide complex
[0089] (1) Dissolve 2 mmol of 1,3-bis(dicyclohexylphosphino)propane bis(tetrafluoroborate) in 30 ml of acetonitrile solution, then dissolve 4 mmol of potassium bromide in 30 ml of deionized water, mix the two thoroughly, and stir in an oil bath at 30°C for 6 hours;
[0090] (2) After the reaction is completed, there is a white precipitate at the bottom. Remove the white precipitate at the bottom by suction filtration, take the clarified solution and perform water bath rotary evaporation to remove all acetonitrile and deionized water, then add 45 ml of ethyl acetate and place it in an ultrasonic cleaner for ultrasonic cleaning for 10 minutes;
[0091] (3) A white precipitate is generated during the ultrasonic process. After the ultrasonic process is completed, the ethyl acetate is removed by filtration. The mixture is repeatedly washed with ethyl acetate twice and then filtered. The powder obtained after filtration is placed in a vacuum drying oven at 45°C and dried for 3 hours. The obtained white precipitate is a clean and high-purity phosphorus-containing complex with a molar mass of 598.2 g / mol.
[0092] (4) taking 0.1 mmol of the phosphorus-containing complex and 0.2 mmol of anhydrous cobalt bromide, and fully dissolving the two in 200 μL of N,N-dimethylformamide to obtain a gel precursor solution, i.e., the cobalt bromide complex dissolved in N,N-dimethylformamide;
[0093] The structural formula of cobalt bromide complex is:
[0094] ;
[0095] S2. Preparation of modified layer
[0096] Poly(9-vinylcarbazole) was dissolved in methanol to form a 40 mg / mL gel solution, and 20 μL of the gel solution was spin-coated on an indium tin oxide glass substrate on a gel coater at a speed of 3000 rpm for 30 s. After spin coating, the substrate was pretreated on a 75°C hot plate for 10 min, and a modified layer with a thickness of about 20 nm was formed after drying.
[0097] S3. Preparation of gel active layer
[0098] 175 μL of gel precursor solution was dripped onto the surface of the substrate containing the modified layer, and the modified layer was covered, and then placed on a 120°C hot plate for annealing for 9 hours to obtain a stable halide metal complex gel, thereby forming a gel active layer with a thickness of about 330 μm. Figure 4 As shown;
[0099] S4. Preparation of electrodes
[0100] The indium tin oxide glass substrate was placed in a vacuum coating machine at 2×10 -4 Under a pressure of 1.3 Pa, a copper electrode with a thickness of 90 nm was deposited on the surface of the gel active layer by thermal evaporation through a mask, thereby producing an X-ray detector based on the halide metal complex gel.
[0101] The halogenated metal complex gel prepared in step S3 was subjected to a thermal weight loss test. 10 mg of the gel was placed in a crucible and heated to a target temperature of 100°C at a rate of 10°C / min. The temperature was then maintained. The weight of the gel at different times was measured and compared with the initial weight to measure the thermal weight loss. The thermal weight loss graph is shown in FIG. Figure 5 As shown, from Figure 5 It can be seen that the weight loss in the thermal gravimetric test under continuous heating at 100°C for more than 180 minutes does not exceed 2.6%, indicating that the gel sample still has excellent stability under extreme conditions.
[0102] Example 3
[0103] The X-ray detector based on the halide metal complex gel comprises the following steps:
[0104] S1. Synthesis of gel precursor solution of lead iodide complex
[0105] (1) Dissolve 2 mmol of 1,3-bis(dicyclohexylphosphino)propane bis(tetrafluoroborate) in 30 ml of acetonitrile solution, then dissolve 4 mmol of potassium iodide in 30 ml of deionized water, mix the two thoroughly, and stir in an oil bath at 30°C for 6 hours;
[0106] (2) After the reaction is completed, there is a white precipitate at the bottom. Remove the white precipitate at the bottom by suction filtration, take the clarified solution and perform water bath rotary evaporation. After all the acetonitrile and deionized water are removed by rotary evaporation, add 60 ml of a mixed solvent of ether and isopropanol (the volume of ether: the volume of isopropanol = 3:1), and place it in an ultrasonic cleaner for ultrasonic cleaning for 5 minutes.
[0107] (3) A white precipitate is generated during the ultrasonic process. After the ultrasonic process is completed, the mixed solvent of ether and isopropanol is removed by filtration, and then the mixed solvent of ether and isopropanol is repeatedly added for washing three times and then filtered. The powder obtained after filtration is placed in a vacuum drying oven and dried for 3 hours at a drying temperature of 45°C. The obtained white precipitate is a clean and high-purity phosphorus-containing complex with a molar mass of 692.2 g / mol.
[0108] (4) taking 0.1 mmol of the phosphorus-containing complex and 0.2 mmol of anhydrous lead iodide, and fully dissolving the two in 200 μL of N,N-dimethylformamide to obtain a gel precursor solution, i.e., the lead iodide complex dissolved in N,N-dimethylformamide;
[0109] The crystal molecular structure of lead iodide complex is as follows Figure 6 As shown, its structural formula is:
[0110] ;
[0111] S2. Preparation of modified layer
[0112] Polymethyl methacrylate is dissolved in toluene to form a 40 mg / mL gel solution, which is coated on a fluorine-doped tin oxide glass substrate to form a modified layer after drying;
[0113] S3. Preparation of gel active layer
[0114] 170 μL of gel precursor solution was dripped onto the surface of the substrate containing the modified layer, and the modified layer was covered, and then placed on a 100°C hot plate for annealing for 11 hours to obtain a stable halide metal complex gel, thereby forming a gel active layer with a thickness of about 320 μm. Figure 7 As shown;
[0115] S4. Preparation of electrodes
[0116] The fluorine-doped tin oxide glass was placed in a vacuum coater at 2 × 10 -4 Under a pressure of 2.3 Pa, a planar copper electrode is deposited on the surface of the gel active layer by thermal evaporation through a mask plate to produce an X-ray detector based on the halide metal complex gel.
[0117] Comparative Example 1
[0118] This comparative example is a commercially available Si-based direct X-ray detector, which is manufactured by Amptek, USA, and its model is XR-100SDD.
[0119] Comparative Example 2
[0120] This comparative example is a commercially available direct X-ray detector based on α-Se. The detector is manufactured by KA Imaging of Canada and its model is BrillianSe. TM .
[0121] Comparative Example 3
[0122] This comparative example is a commercially available direct X-ray detector based on CZT, the manufacturer of the detector is Shaanxi Ditech New Materials Co., Ltd., and the model is DT-P01.
[0123] The performance of the X-ray detectors obtained in Examples 1 to 3 was analyzed, and the results are as follows:
[0124] (1) The current density-time response diagrams of the X-ray detectors prepared in Examples 1 to 3 under different bias voltages and different dose rates of X-rays are shown in FIG. Figures 8 to 10 The results show that the X-ray detectors prepared in Examples 1 to 3 are effective for 13nGy air s -1 ~244nGy air s -1 It has fast and good response to different dose rates.
[0125] (2) The X-ray sensitivity S of a photoconductive detector is defined as the ability to convert the received radiation into current per unit area. The sensitivity S can be calculated using the following formula:
[0126]
[0127] in, I ph is the photocurrent, D is the dose rate of X-ray radiation, A is the effective area of the detector; sensitivity S It is an important indicator to measure the performance of X-ray detectors. High sensitivity can reduce the radiation measurement of the detector and increase the dynamic range of the detector. In order to avoid the calculation error caused by dark current, the photocurrent I ph The net photocurrent is obtained by subtracting the dark current from the actual photocurrent; Figures 8 to 10 The actual photocurrent density and dark current density corresponding to different bias voltages and different dose rates can be obtained. Current density = photocurrent I ph / Detector effective area A , combined with the sensitivity S calculation formula, it can be seen that the current density and dose rate are linearly related, and the slope is the sensitivity. Since the current density is different under different bias voltages, and thus the sensitivity is different, the data relationship between dose rate and current density under different bias voltages can be obtained based on the sensitivity data. The data relationship between dose rate and current density of the X-ray detectors prepared in Examples 1 to 3 under different bias voltages is shown in FIG. Figures 11 to 13 shown.
[0128] The results show that the sensitivity of the X-ray detector prepared in Example 1 can reach 1696μCGy air -1 cm -2 The sensitivity of the X-ray detector prepared in Example 2 can reach 1767μCGy air -1 cm -2 The sensitivity of the X-ray detector prepared in Example 3 can reach 549μCGy air -1 cm -2 , and compared it with some commercial high-performance X-ray detectors. The results are shown in Table 1 below.
[0129] Table 1
[0130]
[0131] The sensitivities in the above Table 1 are all calculated under a bias voltage of -1V. It can be seen from the data in Table 1 that the sensitivities of the X-ray detectors prepared in Examples 1 to 3 of the present invention are all better than the commercial high-performance X-ray detectors in Comparative Examples 1 to 3.
[0132] (3) The X-ray detectors prepared in Examples 1 to 3 were subjected to dark current drift tests. The results are as follows: Figures 14 to 16 As shown, Fig.14 It shows that the long-term dark current drift level of the X-ray detector of Example 1 in a dark environment is 2.57×10 -9 nA -1 V -1 S -1 , Fig.15 It shows that the long-term dark current drift level of the X-ray detector of Example 2 in a dark environment is 3.65×10 -9 nA -1 V -1 S -1 , Fig.16 It shows that the long-term dark current drift level of the X-ray detector of Example 3 in a dark environment is 8.15×10 -9 nA -1 V -1 S -1 It can be seen that the X-ray detectors prepared in Examples 1 to 3 have excellent dark current drift stability during long-term use.
[0133] In addition, the X-ray detector prepared in Example 1 was tested for stability under light conditions. air S -1 After long-term irradiation with a dose rate of 100 nm, the dark current drift test was carried out. The dark current drift level of the X-ray detector was 3.98×10 -8 nA -1 V -1 S -1 It can be seen that the X-ray detector of the present invention has excellent working stability even when working for a long time under a large radiation dose.
[0134] The above-described embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that, for a person of ordinary skill in the art, several modifications and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the attached claims.
Claims
1. An X-ray detector based on a halide metal complex gel, characterized in that: The X-ray detector comprises a substrate, a modification layer, a gel active layer and an electrode stacked in sequence from bottom to top; The gelling material is coated on the surface of the substrate to form the modified layer; The material of the gel active layer is a halogenated metal complex formed by mixing a phosphorus-containing complex and a metal halide in a solvent; the halogenated metal complex is annealed to form the gel active layer on the modified layer on the surface of the substrate; The general structural formula of the phosphorus-containing complex is: ; The general structural formula of the halogenated metal complex is: ; Wherein, R1, R2, R3, R4 are all cycloalkyl, benzene ring or chain alkyl; R5 is chain hydrocarbon group; X is halogen; MX a is a metal halide, a is the valence number of the metal M, and b is the molar ratio of the metal halide to the phosphorus-containing complex; The cycloalkyl group is C3 to C6; R5 is C3 to C6 chain hydrocarbon group; When the metal M is divalent, b=2; when the metal M is trivalent, b=1.2~1.4; when the metal M is monovalent, b=2~4; when the metal M is tetravalent, b=1~1.
2.
2. The X-ray detector based on halide metal complex gel according to claim 1, characterized in that: The halogen is F, Cl or Br.
3. The X-ray detector based on halide metal complex gel according to claim 1, characterized in that: The solvent is any one of amide solvents, hydrazide solvents, alcohol solvents, ester solvents, sulfone solvents, sulfoxide solvents, ketone solvents, nitrile solvents, pyridine, and tetrahydrofuran.
4. A method for preparing an X-ray detector based on a halide metal complex gel, characterized in that: The preparation method is used to prepare the X-ray detector based on the halide metal complex gel according to any one of claims 1 to 3, and the preparation method comprises the following steps: The phosphorus-containing complex is mixed with a metal halide, and then fully dissolved in a solvent to prepare a gel precursor solution; The liquid gelling material is coated on the substrate and forms a finishing layer after drying; A gel precursor solution is dripped onto the surface of the modified layer of the substrate to cover the modified layer, and a gel active layer is obtained after annealing; Conductive electrodes are arranged on the surface of the gel active layer to produce an X-ray detector.
5. The method for preparing an X-ray detector based on a halide metal complex gel according to claim 4, characterized in that: The general structural formula of the phosphorus-containing complex is: ; Wherein, R1, R2, R3, and R4 are all cycloalkyl, benzene ring, or chain alkyl; R5 is a chain hydrocarbon group; X is a halogen; The metal halide is MX a , a is the valence number of the metal M, and X is the same halogen as in the phosphorus-containing complex.
6. The method for preparing an X-ray detector based on a halide metal complex gel according to claim 4, characterized in that: The annealing treatment is performed at a temperature of 100° C. to 120° C. and for a time of 9 h to 11 h.
7. The method for preparing an X-ray detector based on a halide metal complex gel according to claim 5, characterized in that: The cycloalkyl group is C3 to C6; R5 is C3 to C6 chain hydrocarbon group.
8. The method for preparing an X-ray detector based on a halide metal complex gel according to claim 5, characterized in that: The molar ratio of the metal halide to the phosphorus-containing complex is b; when the metal M in the metal halide is divalent, b=2; when the metal M is trivalent, b=1.2-1.4; when the metal M is monovalent, b=2-4; when the metal M is tetravalent, b=1-1.2.