Powder containing hollow particles and method for producing same

By using hollow particle powder with cavities inside the shell, combined with spray drying and acid neutralization firing processes, the problem of low dielectric constant and low dielectric loss tangent of the insulating layer is solved, and a high filling rate is achieved and high porosity, which improves the thin film and dielectric properties of insulating materials.

CN118724005APending Publication Date: 2024-10-01JGC CATALYSTS & CHEMICALS LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410364324.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-03-14
Filing Date
2024-03-28
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

It is difficult to achieve low dielectric constant, low dielectric loss tangent and thin film of the insulating layer at the same time with the existing technology, and filler particles are prone to cracking and sticking, resulting in low filling rate and poor dielectric properties.

Method used

Powder containing hollow particles with cavities inside the shell is used to prepare hollow particles with an average particle size of 0.1 μm to 5.0 μm through spray drying of a silicate alkali aqueous solution, and is fired after neutralization and cleaning in an acid solution to control Particle size distribution and porosity ensure a silica shell of more than 70%.

Benefits of technology

While achieving low dielectric constant and low dielectric loss tangent of the insulating layer, it also improves the thinning ability and dielectric properties of the insulating layer, ensuring high filling rate and high porosity, avoiding particle breakage and adhesion, and improving performance of the insulating material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004763735170000211
    Figure BDA0004763735170000211
Patent Text Reader

Abstract

[Problem] To provide a filler capable of achieving a low dielectric constant and a low dielectric loss tangent of an insulating layer, and also capable of achieving a thin film of the insulating layer. [Solution] A powder containing hollow particles having a cavity inside a shell, the powder having an average particle diameter (D50) of 0.1 [mu] m to 5.0 [mu] m and a maximum particle diameter (D100) of 20.0 [mu] m or less, the sum of the particle volumes in the range of peak particle diameters (Ps) * 0.75 [mu] m * 1.25 [mu] m in the particle size distribution of the powder being 50% or less of the total volume of all the particles, and the particle size distribution of the powder being less than or equal to 100 [mu] m. The porosity of the powder is 10%-50%, the rate of fractured particles of the powder is 10% by volume or less, and the outer shell contains 70% by mass or more of silica.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a powder suitable for use as a filler in an insulating material, and in particular to a powder containing hollow particles having a cavity inside an outer shell. Background Art

[0002] In recent years, high speed and large capacity are developing in information communication. Therefore, materials used in communication equipment require low dielectric constant (low Dk) and low dielectric loss tangent (low Df). For example, for printed wiring boards equipped with semiconductor elements, insulating materials with low dielectric constant and low dielectric loss tangent are required. If the dielectric constant of the insulating material is high, dielectric loss will occur; if the dielectric loss tangent of the insulating material is high, not only dielectric loss but also the possibility of increased heat generation.

[0003] In order to achieve lower dielectric constant and lower dielectric loss tangent of insulating materials, the development of resin materials, which are the main body of insulating materials, is in progress. As such resin materials, epoxy resins, polyphenylene ether resins, fluorine resins, etc. have been proposed.

[0004] Fillers are blended into such resin materials from the viewpoints of durability (rigidity), heat resistance, etc. It is known to use hollow silica particles as fillers in order to lower the dielectric constant (for example, refer to Patent Document 1).

[0005] Recently, along with the development of thinning of semiconductor devices, the thin film of insulating layer is required. Therefore, the filler deployed in the insulating layer (insulating material) also needs to reduce the particle size (maximum particle size). As a method for manufacturing hollow particles with small particle size, there are known emulsion method (e.g., patent document 1), core-shell method (e.g., with reference to patent document 2 and patent document 3), thermal decomposition method (e.g., with reference to patent document 4 and patent document 5), spray drying method (e.g., with reference to patent document 6).

[0006] The emulsion method and the core-shell method can control the particle size to be uniform, and can also prepare small diameter particles of less than 1 μm. However, due to deformation caused by shrinkage force and adhesion between particles in the drying process for obtaining the powder from the liquid phase, it is difficult to obtain monodisperse hollow particles. Even if monodisperse hollow particles are obtained, it is difficult to fill more hollow particles in the resin material due to the sharp particle size distribution.

[0007] In addition, in the thermal decomposition method that utilizes the expansion of raw material powder for granulation, in order to efficiently obtain small particles, the raw material powder must be extremely small (micronized). Therefore, this is not a realistic method.

[0008] In the spray drying method, since particles are formed in the gas phase of hot air, a powder in a monodisperse state can be obtained. Usually, since a two-fluid nozzle that atomizes a liquid using compressed air is used to form droplets, there is a distribution in the actual droplet diameter. That is, droplets with small diameters to large diameters are mixed and present. Therefore, a powder in which small-diameter particles formed from small-diameter droplets and large-diameter particles formed from large-diameter droplets are mixed and present is recovered. In order to reduce the maximum particle size, it is necessary to remove large-diameter particles by classification or the like, but large-diameter particles are prone to breakage during drying and granulation, and are also prone to breakage in the recovery container. The broken particles reduce the overall porosity of the powder and do not contribute to low dielectric constant (low Dk) and low dielectric loss tangent (low Df). Since the broken particles are small, it is difficult to remove them by classification.

[0009] In addition, generally, the smaller the particle size, the larger the specific surface area of the particles, and the easier it is for the particles to adhere to each other. Therefore, the dispersibility in the resin is reduced. As a result, the particles cannot be uniformly dispersed in the resin, and problems such as being removed as aggregates by the filter and clogging the filter occur. Furthermore, it is impossible to fill the amount of filler required to reduce the dielectric constant and dielectric loss tangent (low filling rate). In addition, there is a problem that the underfill material cannot be filled into narrow gaps. Furthermore, if the shear force during kneading is increased or the kneading time is extended in order to uniformly disperse the filler, it will cause the hollow particles to break. Prior art documents Patent documents

[0010] Patent Document 1: Japanese Unexamined Patent Application Publication No. 2012-136363 Patent Document 2: Japanese Unexamined Patent Application Publication No. 2022-19357 Patent Document 3: Japanese Unexamined Patent Application Publication No. 2022-172938 Patent Document 4: Japanese Unexamined Patent Application Publication No. 2005-206436 Patent Document 5: Japanese Unexamined Patent Application Publication No. 2020-45263 Patent Document 6: Japanese Unexamined Patent Application Publication No. 2022-103683 Summary of the invention Technical problem to be solved by the invention

[0011] The technical problem of the present invention is to provide a filler that can achieve low dielectric constant and low dielectric loss tangent of the insulating layer while achieving thinning of the insulating layer. Technical means for solving the technical problem

[0012] The present inventor found that a powder satisfying the following characteristics can solve the above technical problems.

[0013] That is, the powder of the present invention includes hollow particles having a cavity inside an outer shell, and satisfies the following requirements (a) to (f). (a) The average particle size (D50) of the powder is 0.1 μm to 5.0 μm, (b) The maximum particle size (D100) of the powder is less than 20.0 μm, (c) the sum of the volume of particles in the range of peak particle size (Ps)×0.75 μm to (Ps)×1.25 μm in the particle size distribution of the powder is less than 50% of the total volume of all particles, (d) The porosity of the powder is 10% to 50%, (e) the powder has a broken particle ratio of 10% by volume or less, (f) The outer shell contains 70 mass % or more of silicon dioxide.

[0014] In addition, the powder manufacturing method of the present invention comprises: a first step, using an alkaline silicate aqueous solution to form droplets with an average particle size of less than 10.0 μm, spraying and drying in a hot air flow to granulate hollow particles; a second step, neutralizing the alkali contained in the hollow particles in an acid solution and then washing them; a third step, calcining the neutralized and washed hollow particles. Beneficial Effects

[0015] The powder of the present invention can achieve a low dielectric constant and a low dielectric loss tangent of the insulating layer, and can also cope with a reduction in the thickness of the insulating layer. DETAILED DESCRIPTION

[0016] The powder of the present invention contains hollow particles having a cavity inside the shell, and the average particle size and the maximum particle size are small, and the particle size distribution is wide. Therefore, the filling rate to the insulating material (resin) is high, and excellent dielectric properties can be obtained even if the insulating layer is thin-filmed. Furthermore, since the content of the broken particles is low, a high porosity can be obtained despite the small particle size, and the dielectric constant and the dielectric loss tangent can be further reduced.

[0017] That is, the average particle size (D50) of the powder of the present invention is 0.1 μm to 5.0 μm, the maximum particle size (D100) is 20.0 μm or less, when the peak particle size in the particle size distribution is set to "Ps" μm, the sum of the volume of particles having a particle size of (Ps) × 0.75 or more and (Ps) × 1.25 or less is 50% or less of the total volume of all particles, the fractured particle rate is 10% or less by volume, and the porosity is 10% to 50%. In addition, the shell contains 70% by mass or more of silicon dioxide.

[0018] Each requirement is described below. a) Average particle size (D50) is 0.1 μm to 5.0 μm Since the average particle size is less than 0.1 μm, it contains more tiny particles, so the specific surface area (SiOH group content) becomes larger, and excellent dielectric properties cannot be obtained. In addition, powders with an average particle size greater than 5.0 μm are difficult to be highly filled in thin-film insulating materials (resins). Considering the insulating materials used for thin film, the average particle size is preferably 0.3 μm to 4.5 μm, and more preferably 0.5 μm to 4.0 μm.

[0019] b) Maximum particle size (D100) is less than 20.0 μm If the maximum particle size (D100) is larger than 20.0 μm, it is difficult to highly fill the resin in a thin film. The maximum particle size (D100) is preferably 15.0 μm or less, more preferably 10.0 μm or less, and even more preferably 8.0 μm or less.

[0020] c) Expansion of particle size distribution When the peak particle size in the particle size distribution is set to "Ps" μm, the sum of the volume of particles with a particle size of (Ps×0.75) μm or more and (Ps×1.25) μm or less is less than 50% of the total volume of all particles. If the volume ratio of particles in the range of (Ps)×0.75μm to (Ps)×1.25μm is greater than 50%, the particle size is uniform and the width (broadness) of the particle size distribution is low. Therefore, it is difficult to highly fill in the thin film resin and excellent dielectric properties cannot be obtained. The volume ratio is preferably less than 45%, and more preferably less than 40%.

[0021] In addition, the wider the particle size distribution, the more preferred (the higher the width of the particle size distribution, the more preferred). Therefore, there can be more than two peaks in the particle size distribution. That is, the particle size distribution can also be bimodal (multimodal). Thus, the filling rate of the thin film resin can be further improved. In addition, when there are multiple peaks, the volume ratio of the above particles is less than 50% relative to each peak.

[0022] d) The cracked particle rate is less than 10% by volume Since the cracked particles do not contribute to low dielectric constant and low dielectric loss tangent (reducing overall porosity), if the cracked particles are greater than 10% by volume, excellent dielectric properties cannot be obtained, and in addition, it will become an obstacle to high filling rate. The cracked particle rate is preferably less than 8% by volume, more preferably less than 6% by volume. In addition, the cracked particles refer to particles with the original shape of hollow particles such as C-shaped particles remaining, excluding crushed small pieces.

[0023] e) Porosity: 10% to 50% If the porosity of the powder is less than 10%, the effect of reducing the dielectric constant and dielectric loss tangent is insufficient, and the desired dielectric constant and dielectric loss tangent cannot be obtained. In addition, if the porosity exceeds 50%, the strength of the particles decreases and the particles are prone to breakage. The porosity is preferably 15% to 45%, and more preferably 20% to 40%.

[0024] f) The outer shell contains 70 mass % or more of silicon dioxide. As a component constituting the shell, 70% by mass or more of silicon dioxide is contained. That is, the shell is formed by an inorganic oxide containing 70% by mass or more of silicon dioxide. In addition to silicon dioxide, inorganic oxides such as aluminum oxide, zirconium dioxide, and titanium dioxide may also be contained. The amount of silicon dioxide contained in the shell is more preferably 90% by mass or more, further preferably 95% by mass or more, and it is particularly preferably formed essentially only by silicon dioxide.

[0025] Furthermore, the powder preferably satisfies any one of the following requirements. g) The alkali content of the powder is less than 100 ppm This can reduce the dielectric constant and dielectric loss tangent. In addition, it is suitable for semiconductor mounting. In addition, it can prevent particle adhesion in subsequent processes and prevent the generation of sintered particles in the firing process. The alkali content is more preferably 90 ppm or less, and more preferably 80 ppm or less.

[0026] h) The oil absorption per unit volume of the powder is 0.60 ml / cm 3 the following The oil absorption per unit volume is expressed as 1 cm 3 The amount of oil required to make a fluid paste of particles of 1 cm2. Therefore, the smaller the value, the easier it is to fill the resin. For example, 0.60 ml of oil can make a particle of 1 cm2. 3 When fluidized, the particle filling rate in the paste is 62.5 vol%. If the oil absorption is 0.60 ml / cm 3 If the oil absorption is less than 0.50 ml / cm, the resin can be highly filled when dispersed. 3 Below, more preferably 0.40ml / cm 3 the following.

[0027] Furthermore, the powder preferably satisfies any one of the following requirements, and more preferably satisfies all of the requirements i) to m).

[0028] i) Sears number (ml / SiO21.5g) less than 0.30 Generally, the Sears number is an index of the amount of OH groups (silanol groups) of silica particles. If the Sears number is large, the amount of OH groups present in the particles is large. When the Sears number is above 0.30, the dielectric constant and the dielectric loss tangent are high. In addition, moisture absorption occurs over time, and the dielectric constant and the dielectric loss tangent tend to increase. Furthermore, the particles have high adhesion to each other, and it is possible to produce agglomeration of particles. The Sears number is more preferably less than 0.29, and more preferably less than 0.28.

[0029] In addition, the Sears number is measured by titration of sodium hydroxide according to the description of Sears' Analytical Chemistry 28 (1956), 12, 1981-1983. This determination method is used to measure the number of OH groups on the particle surface. The Sears number (ml / SiO21.5g) represents the titration amount of 0.1N sodium hydroxide aqueous solution relative to 1.5g of silicon dioxide.

[0030] j) The ratio of the BET specific surface area obtained by the water vapor adsorption method to the nitrogen adsorption method is less than 0.30 The ratio of the BET specific surface area obtained by the water vapor adsorption method to the BET specific surface area obtained by the nitrogen adsorption method (water vapor specific surface area / nitrogen specific surface area) indicates the degree of hydrophilicity and hydrophobicity, and the larger the value, the more hydrophilic. The material with a ratio of 0.30 or more is easy to absorb moisture. The ratio is more preferably less than 0.20, and more preferably less than 0.15.

[0031] k) Water vapor adsorption is less than 0.20% by mass The water vapor adsorption amount indicates the temporal stability related to moisture absorption. A substance with a water vapor adsorption amount of 0.20 mass % or more is prone to moisture absorption and has poor temporal stability. The water vapor adsorption amount is more preferably less than 0.15, and even more preferably less than 0.10.

[0032] m) 29 In Si-NMR structural analysis, the peak area of ​​Q4 structure is more than 90% of the total peak area of ​​Q0 structure to Q4 structure

[0033] 29In Si-NMR structural analysis, the silicon atoms in the particles are divided into five types, namely Q0, Q1, Q2, Q3, and Q4, according to the number of silicon atoms sharing oxygen around the silicon atoms. Specifically, the chemical shift of the Q0 structure appears at -73.0ppm to -73.5ppm, the chemical shift of the Q1 structure appears at -73.5ppm to -78.0ppm, the chemical shift of the Q2 structure appears at -78.0ppm to -82.0ppm, the chemical shift of the Q3 structure appears at -82.0ppm to -100.0ppm, and the chemical shift of the Q4 structure appears at -100.0ppm to -120.0ppm. Among these structures, the Q4 structure has a smaller number of OH groups (more siloxane bonds) than the Q0 to Q3 structures. The larger the existence ratio (area ratio) of the Q4 structure, the fewer unstable OH groups and the greater the bonding ratio between silicon. Therefore, it becomes a particle with high stability. When such particles are used as fillers, an insulating material with little change over time can be obtained. The peak area of ​​the Q4 structure is more preferably 93% or more of the total peak area (areas of the Q0 structure to the Q4 structure), and even more preferably 95% or more. In particular, it is preferred that the Q3 structure and the Q4 structure are substantially present.

[0034] The powder of the present invention is mostly spherical hollow particles, but may also contain solid particles. The hollow particles are preferably 80% or more of the total, more preferably 90% or more. The proportion of hollow particles can be calculated, for example, based on the cross-sectional SEM images of any 100 particles.

[0035] The dielectric constant of the powder is preferably 2.8 or less, and more preferably 2.5 or less. The dielectric loss tangent of the powder is preferably less than 0.0010, and more preferably less than 0.0005.

[0036] Furthermore, the specific surface area of ​​the powder is preferably 1 m 2 / g~50m 2 / g. If the specific surface area is too large, the amount of SiOH groups will be high, which may have an adverse effect on the dielectric properties. In addition, the adhesion between particles will also increase, and the dispersibility into the resin may become poor. The specific surface area is more preferably 2m 2 / g~20m 2 / g, more preferably 3m 2 / g~10m 2 / g.

[0037] [Method for producing powder] The method for producing the powder of the present invention comprises: a first step of spraying and drying droplets with an average particle size of 10.0 μm or less formed by an alkaline silicate aqueous solution in a hot air flow to prepare hollow particles; a second step of neutralizing the alkali contained in the hollow particles in an acid solution and then washing them; and a third step of calcining the neutralized and washed hollow particles. The powder of the present invention can be produced by such a production method. In addition, other steps such as a classification step and a drying step may be provided before and after each step.

[0038] In spray drying, by adjusting the spray droplet diameter to be smaller than before and not containing large-diameter droplets, the generation of large-diameter particles can be prevented. Regarding large-diameter particles, the ratio of shell thickness to particle diameter (shell thickness / particle diameter) is small, and it is easy to break compared with small-diameter particles. Therefore, it is possible to obtain small-diameter hollow particles with a high void ratio while suppressing the generation of broken particles. If only small-diameter hollow particles are finally obtained, classification can be achieved, but, from the viewpoint of reducing the content of broken particles, the droplet diameter must be reduced so that the large-diameter particles that are easy to break are not granulated. Usually, compared with emulsion methods, spray drying methods can manufacture particles with a wide particle size distribution.

[0039] Hereinafter, each step will be described in detail. (First process) In this process, droplets with an average particle size of 10.0 μm or less are formed by an alkaline silicate aqueous solution, sprayed and dried in a hot air flow, and spherical hollow particles are granulated. That is, the spray droplet diameter is adjusted to be smaller than before and does not contain large-diameter droplets, and hollow particles are granulated.

[0040] The average particle size of the droplets is preferably 9.0 μm or less, more preferably 8.0 μm or less. The lower limit is 5.0 μm. Here, the average particle size of the droplets (Sauter average particle size) is measured by a liquid immersion method.

[0041] As a spray drying method for stably forming small-diameter droplets, there can be cited methods using a collision-type two-fluid nozzle, a nozzle that crushes a liquid by collision of two relative air streams, a four-fluid nozzle, etc., wherein the collision-type two-fluid nozzle has a structure that further homogenizes and refines the droplets discharged from the two-fluid nozzle that atomizes the liquid by compressed air. Specifically, there can be cited methods using a collision-type two-fluid nozzle manufactured by Mist Noise Co., Ltd., a nozzle (Microflow) manufactured by Nozul Net Works Co., Ltd., a four-fluid nozzle manufactured by GF Co., Ltd., etc. In addition, the droplets can be made smaller by increasing the volume ratio (gas / liquid volume ratio) of the gas supply amount and the raw material liquid supply amount in the nozzle injection. In order to make the average particle size of the droplets less than 10 μm, the gas / liquid volume ratio needs to be 6000 or more, preferably 7000 or more, and more preferably 8000 or more.

[0042] In spray drying, the inlet temperature of the spray dryer is preferably 300° C. to 600° C., more preferably 350° C. to 550° C. In addition, the outlet temperature is preferably 120° C. to 350° C., more preferably 200° C. to 300° C. By increasing the inlet temperature and the outlet temperature, the drying speed can be increased and the porosity can be increased.

[0043] The concentration of SiO2 in the alkaline silicate aqueous solution is preferably 1% to 30% by mass, more preferably 5% to 28% by mass, and further preferably 10% to 25% by mass. The lower the concentration of the alkaline silicate aqueous solution, the lower the viscosity, which can make the droplets smaller. As the alkaline silicate, water-soluble sodium silicate and potassium silicate can be exemplified, preferably sodium silicate.

[0044] The molar ratio (SiO2 / M2O) of the silicate base is preferably 1 to 5, more preferably 2 to 4. When the molar ratio is less than 1, the amount of alkali is too much, not only the acid cleaning becomes difficult when removing the alkali, but also the deliquescent property of the spray-dried product becomes large, making it difficult to obtain the desired hollow particles. If the molar ratio is greater than 5, the solubility of the silicate base decreases, making it difficult to prepare an aqueous solution. Even if an aqueous solution is prepared, there is a case where the desired hollow particles cannot be obtained by spray drying.

[0045] (Second process) In this step, the alkali contained in the granulated hollow particles is neutralized and removed in an acid solution under predetermined conditions. Specifically, the hollow particles are immersed in an acid solution to remove the alkali contained in the hollow particles.

[0046] In the second process, the hollow particles obtained in the first process are neutralized (de-alkalized) by a large amount of acid. That is, neutralization is performed under a low pH state. The pH is preferably below 2.0. Usually, the alkali is removed from the particles (shell) to form pores on the particles (shell). By rapidly neutralizing (de-alkalizing) by a large amount of acid, the dissolution of silicon dioxide in the shell is suppressed, and the formation of large pores can be prevented. That is, the pores can be made into a size (structure) that is easily blocked in the subsequent firing process. The result is to obtain particles with a small amount of SiOH groups, and the low dielectric constant and low dielectric loss tangent of the insulating material are achieved. In addition, since the firing process causes the pores to be blocked, the change of the dielectric loss tangent caused by moisture absorption over time can also be suppressed, and the low dielectric loss tangent can be maintained for a long time. In addition, the adhesion of particles to each other can be suppressed, and the dispersibility of the particles can be improved. Furthermore, since no large pores remain on the shell, the particle strength is also improved.

[0047] In this process, it is preferred to add the hollow particles to the acid solution rather than to add the acid solution to the hollow particles. This can prevent the pH state near the particles from dissolving, and can prevent the particles from dissolving. In addition, in the column flow method, the H of the acid solution during the period of flowing from the upper part of the column to the lower part + When the concentration decreases (pH increases), the particles may be in contact with each other at an insufficiently low pH state, causing the particles to dissolve. As a result, large pores are easily formed, and the desired effect may not be obtained.

[0048] In this step, it is preferred to use the molar number of hydrogen ions (M H+ ) relative to the value obtained by multiplying the number of moles of alkali metal ions in the hollow particle by the valence number (M SP ) ratio (M H+ / M SP ) is greater than 4.7. Such a high value of acid solution has not been used in the past. For example, paragraph 0032 of Japanese Patent Publication No. 2013-103850 states that "even if it exceeds 4.7, no further skeletonization will be carried out, and there will be excess acid, which is not economical." In addition, in the examples of Japanese Patent Publication No. 04-104907, the ratio is 3.0 (200L) and 4.4 (300L). In the present invention, by deliberately performing a neutralization treatment with such an acid solution, it is possible to remove alkali ions (and H + The ratio (M H+ / M SP ) is preferably 5.0 or more, more preferably 5.2 or more, and further preferably 5.5 or more. The upper limit is not limited, and is, for example, 7.0 or less.

[0049] In this process, the alkali component in the particle (shell) is removed and the mass is reduced, but the particle shape, hollow structure, etc. (volume) change is very small, so the density of the particle decreases according to the amount of alkali removed when compared before and after this process. The density of the particle can be measured based on the gas specific gravity method (Gaspicnometry) (JIS Z8837). The particles before this process (the first process end product) are directly measured, and the particles after this process are measured after drying at 120°C for 24 hours (after washing).

[0050] By removing the alkali (alkaline removal) in this step, pores are formed on the particles (shell). Therefore, the particle density measurement result is different depending on whether the gas used for density measurement passes through the pores. In the case of using helium, since helium penetrates the pores and fills the cavities inside the particles, the measured particle density is similar to the density of silica (about 2.2 g / cm 3 ) is almost the same value (2.1g / cm 3 ~2.3g / cm 3 ).

[0051] On the other hand, when nitrogen is used, the pores of the outer shell are not penetrated, and the particle density reflecting the existence of the internal cavity can be measured. In this step, if no pores into which nitrogen can penetrate are formed in the particle (the outer shell) and the alkali component is completely removed, the particle density after this step can be calculated by the following formula (X) (theoretical value: ρ 2T ).

[0052] ρ 2T =ρ1×(1-Wa)···Formula (X) ρ1: Particle density after the first process ρ 2T : Theoretical value of particle density after the second process W a : Mass ratio of alkali components in the raw material solid content

[0053] In the second step, more pores are formed into which nitrogen can penetrate. The actual measured particle density (ρ2) (after the second step) is different from the theoretical value (ρ 2T ) the greater the difference. Although the pores formed in this process can be made smaller by heat treatment in the subsequent process, if the size of the pores formed in this process is too large or the amount is too large, they cannot be fully blocked and eventually remain in the particle (shell), which increases the hygroscopicity. Therefore, it is preferred that the size of the pores is small and the amount is small, and the particle density (ρ2) measured by nitrogen is close to the theoretical value (ρ 2T ) is more preferred as the deviation is smaller. Specifically, ρ2 / ρ 2TIt is preferably 1.0 to 1.4, more preferably 1.0 to 1.3, and even more preferably 1.0 to 1.2. In addition, as described above, the particle density (ρ2) after the second step is obtained by measuring the particles washed and then dried at 120° C. for 24 hours.

[0054] In addition, when the hollow particles are broken from the end of the first step to the end of the second step, the particle density (ρ2) is different from the theoretical value (ρ 2T In the present invention, compared with the conventional method of granulating easily ruptured large-diameter hollow particles, since the granulation of small-diameter hollow particles that are not easily ruptured is carried out in the first step, the deviation from the theoretical value is reduced.

[0055] In addition, about the concentration of hollow particles, it is preferred that SiO2 is immersed in an acid solution in a manner of 1 mass % to 30 mass %. In the case of less than 1 mass %, there is no problem with alkali removal and cleaning, but the manufacturing efficiency is reduced. If it is greater than 30 mass %, the concentration is too high, and there is a situation where alkali removal and cleaning efficiency are reduced. In addition, there are problems such as contact and friction between particles causing particle rupture. More preferably, 5 mass % to 25 mass %. The immersion treatment can be carried out in multiple times.

[0056] The temperature condition for the immersion treatment is usually 5°C or higher and below the boiling point of the solution. From the viewpoint of forming better pores and more reliably achieving a lower dielectric constant and a lower dielectric loss tangent of the insulating material, the temperature is preferably 50°C or higher, and more preferably 55°C or higher. The treatment time is, for example, 0.5 to 24 hours.

[0057] After the immersion treatment, the hollow particles are thoroughly cleaned by a conventionally known method, for example, by filtering and cleaning with pure water.

[0058] The residual amount (mass ratio) of the alkali (M) after the alkali is removed is preferably 100 ppm or less, more preferably 90 ppm or less, and further preferably 80 ppm or less. By fully removing the alkali in this step, the particles can be prevented from adhering in the subsequent steps, and the generation of sintered particles in the firing step can be prevented.

[0059] The amount of residual alkali was measured using an atomic absorption spectrophotometer using a sample obtained by dissolving particles in an acid to measure Na or K. When sodium silicate was used, Na was measured, and when potassium silicate was used, K was measured.

[0060] The amount of alkali in the final product (powder) is also preferably within the above range, and is usually equal to the amount of alkali after the alkali removal step.

[0061] Examples of the acid used in this step include inorganic acids such as hydrochloric acid, nitric acid, and sulfuric acid; and organic acids such as acetic acid, tartaric acid, and malic acid. Inorganic acids are preferably used, and sulfuric acid is particularly preferred from the viewpoint of valence. In addition, the acid solution is usually an aqueous solution, but an alcohol or the like may also be used as a mixture.

[0063] (Third process) In this process, the hollow particles after neutralization and cleaning are fired. The firing temperature is preferably above 900°C, more preferably above 1000°C. There is no upper limit, for example, 1200°C. The alkali is fully removed by the second process, so the adhesion of the particles can be prevented, and the generation of sintered particles can be prevented even if fired at a high temperature. The pores formed when the alkali is removed can be blocked by high-temperature firing, so the shell becomes non-porous. As a result, the SiOH group can be reduced, and particles with low dielectric constant and dielectric loss tangent can be obtained. For example, particles with a dielectric loss tangent less than 0.0010 cannot be obtained in the invention of Japanese Patent Gazette No. 2013-103850, but particles less than 0.0010 can be obtained in the present invention. In addition, particles with high strength can be obtained.

[0064] (Grading process) Furthermore, it is preferred to provide a classification step between the second step and the third step. In the classification step, the hollow particles obtained in the second step are subjected to classification treatment. The classification step preferably removes coarse particles. For example, there can be cited a method for removing coarse particles larger than 20.0 μm, a method for removing coarse particles larger than 15.0 μm, and a method for removing coarse particles larger than 10.0 μm. That is, in this step, it is preferred that coarse particles larger than 20.0 μm are substantially not contained, coarse particles larger than 15.0 μm are substantially not contained, and coarse particles larger than 10.0 μm are substantially not contained. In addition, the content of coarse particles in the final product is usually not significantly different from the content after the classification step.

[0065] In order to make the particle diameter consistent, it is generally believed that it is preferred to carry out classification treatment after firing, but the present invention is specially classified before the firing process (the third process). If the classification treatment is not carried out and the firing is carried out, there will also be coarse particles with high porosity that should be removed. Because the coarse particles with high porosity are easily broken, there is the possibility of causing the shrinkage stress caused by heating to break. The fragments produced by the rupture can not be removed even if the classification process is carried out afterwards because the particle diameter is small. In addition, because the fragments are dense silicon dioxide without spaces, they become the obstruction of low dielectric constant and low dielectric loss tangent. Such disadvantages can be avoided by carrying out classification treatment before firing. In addition, classification treatment can be further carried out after firing.

[0066] The classification in this step refers to the particle size classification for separating the powder according to the particle size in order to make the particle size of the powder uniform. The operation of the particle size classification can be fluid classification, which can be divided into dry classification and wet classification.

[0067] In principle, the classifier used for dry classification can be roughly divided into a gravity classifier, an inertial classifier, and a centrifugal classifier. By using an inertial classifier and a centrifugal classifier that classify using the inertial force of particles, more precise classification can be performed. As a classifier that can exert its characteristics even on light particles that are not easily subjected to centrifugal force, there can be cited the Elbow Classifier manufactured by Nippon Steel & Mining Co., Ltd., the SG Semiconductor manufactured by Nippon Sleeve Co., Ltd., the Airophiian Classia manufactured by Nissin Engineering Co., Ltd., and the Microspin manufactured by Nymax Industries, Ltd. Among them, Elastrol and Elastrol, which can accurately classify light particles, are preferred.

[0068] In principle, the classifiers used for wet classification can be roughly divided into gravity classifiers and centrifugal classifiers. By using a centrifugal classifier, more precise classification can be performed. As a classifier that can exert its characteristics even on light particles that are not easily subjected to centrifugal force, there can be cited the Hidrosicron manufactured by Nippon Chemical Machinery Industry Co., Ltd., the Supercron manufactured by Murata Industries, and the Icracy manufactured by Satake Marutimix. Among them, the Icracy that can precisely classify light particles is preferred.

[0069] In the classification step, although it does not prevent the removal of fine particles smaller than 0.1 μm, it is an operation in the direction of sharpening the particle size distribution, so it is preferable not to remove fine particles.

[0070] In order to suppress the generation of broken particles, classification may be performed at an early stage between the first step and the second step. However, since the hollow particles obtained in the first step are deliquescent, it is preferred to perform classification in dry air rather than wet classification.

[0071] (Drying process) A drying step may be provided before the third step, after the third step, etc. As a drying method, heat drying may be mentioned. The drying temperature is preferably 50°C to 400°C, more preferably 50°C to 200°C. Specifically, there may be exemplified a method of drying at a low temperature of about 50°C to 200°C for a period of time, a method of drying by gradually increasing the temperature, and a method of drying by changing the temperature in several stages. The drying step may be provided between the second step and the third step, after the third step, or in between. The drying treatment may also be repeated as required.

[0072] (Screening process) Furthermore, it is preferred that a sieving process for sieving the particle lumps is performed after the drying process or after the third process (firing). In addition, the particle lumps refer to foreign matter with a particle size greater than 150 μm, for example. A sieve with a mesh size (number of meshes) capable of removing such particle lumps is appropriately used for the sieving process.

[0073] [Resin composition] The resin composition of the present invention is dispersed with a powder containing the above-mentioned hollow particles. Such a resin composition can be manufactured by mixing the powder containing the hollow particles with a resin. Specifically, for example, a powder containing hollow particles, a thermosetting resin, etc. are mixed, and a resin composition (coating liquid) is prepared by mixing with a roller mill, etc. It is applied to a substrate and cured by heat, ultraviolet rays, etc.

[0074] Such resin composition can be used as an insulating material for electronic materials such as semiconductors. Specifically, it can be used in copper-clad laminates, prepregs, deposited films, etc. for forming printed wiring boards (including rigid substrates and flexible substrates). In addition, the resin composition is useful for film insulating materials, for example, for insulating materials with a thickness of less than 50 μm, preferably for insulating materials with a thickness of less than 25 μm. In addition, it can also be used for semiconductor packaging related materials such as molded resins, molded bottom filling materials, bottom filling materials, adhesives for flexible substrates, etc.

[0075] As the resin mixed with the powder, a curable resin commonly used for electronic materials such as semiconductors can be used. It can be a light-cured resin, but preferably a thermosetting resin. As such a curable resin, epoxy resins, polyphenylene ether resins, fluorine resins, polyimide resins, bismaleimide resins, acrylic resins, methacrylic resins, silicone resins, BT resins, cyanate resins, etc. can be cited. As epoxy resins, specifically bisphenol-type epoxy resins, novolac-type epoxy resins, trisphenol-alkane-type epoxy resins, epoxy resins with biphenyl skeletons, epoxy resins with naphthalene skeletons, dicyclopentadiene phenol novolac resins, phenol aralkyl-type epoxy resins, glycidyl ester-type epoxy resins, alicyclic epoxy resins, heterocyclic epoxy resins, halogenated epoxy resins, etc. can be illustrated. These resins can be used alone or in combination of two or more.

[0076] The resin composition preferably contains the powder A of the present invention and the curable resin B at a mass ratio (A / B) of 10 / 100 to 95 / 100, more preferably 30 / 100 to 80 / 100. With such a mass ratio, the filler function can be fully exhibited while maintaining properties such as fluidity.

[0077] The resin composition preferably contains a curing agent such as a phenol compound, an amine compound, and an acid anhydride. When an epoxy resin is used as the curable resin, the curing agent may include: a phenolic resin having two or more phenolic hydroxyl groups in one molecule; an acid anhydride such as methylhexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, and methylnadic anhydride (anhydrous methylnadic acid); wherein the phenolic resin is a bisphenol type resin, a novolac type resin, a trisphenol alkane type resin, a resol type phenolic resin, a phenol aralkyl resin, a biphenyl type phenolic resin, a naphthalene type phenolic resin, a cyclopentadiene type phenolic resin, and the like.

[0078] Various additives such as a colorant, a stress relaxant, a defoaming agent, a leveling agent, a coupling agent, a flame retardant, and a curing accelerator may be added to the resin composition as needed. Example

[0079] The embodiments of the present invention are described in detail below. [Example 1] First, prepare 30,000 g of a water glass aqueous solution (SiO2 / Na2O molar ratio 3.2, SiO2 concentration 20 mass%), spray the water glass aqueous solution from two nozzles of a four-fluid nozzle, and spray air from the other two nozzles to granulate the hollow particles (first step). In this embodiment, the inlet temperature is set to 450°C. In addition, the total flow rate of the water glass aqueous solution (i.e., the total flow rate of the liquid sprayed from the two nozzles) is set to 0.29 L / hr, and the total flow rate of the air (i.e., the total flow rate of the air sprayed from the two nozzles) is set to 2040 L / hr. That is, the air / liquid volume ratio is 7034. At this time, the outlet temperature is 250°C.

[0080] Next, 5000 g of the obtained hollow particles were added while stirring 40000 g of a 25% by mass sulfuric acid aqueous solution. The solution was stirred for 15 hours while adjusting the liquid temperature to maintain at 35°C, and then cooled to room temperature. At this time, the solid content (SiO2) concentration was 8.4% by mass, and the pH value of the cooled dispersion was less than 1.0. In addition, the number of moles of hydrogen ions (M H+ ) relative to the value obtained by multiplying the number of moles of alkali metal ions in the hollow particle by the valence number (M SP ) ratio (M H+ / M SP) is set to 5.2. After cooling, solid-liquid separation is performed, and further washing is performed in pure water (second step). Then, it is dried in a dryer at 120°C for 24 hours (drying step). The obtained dried product is crushed, and the particle lumps (foreign matter) are further removed through a sieve with a mesh of 75μm. After that, dry inertial classification is performed using the Elbow Filter (EJ-15) manufactured by Nippon Steel Mining Co., Ltd. The device can classify the powder into three types: F powder (fine powder), M powder (fine powder), and G powder (coarse powder). The F edge distance is adjusted so that the particles larger than 10μm contained in the F powder (fine powder) are less than 5% by volume, and a bag filter is used for recovery (classification step). Then, a powder containing hollow particles is obtained by heating at 1000°C for 10 hours (third step). In addition, after the firing in the third step, a sieve with a mesh of 150μm can be used to remove the particle lumps (foreign matter).

[0081] <Manufacturing of Resin Molded Body> The obtained powder was mixed with liquid acid anhydride "Rikacid MH700 manufactured by Shin Nippon Rika Co., Ltd." and imidazole epoxy resin curing agent "2PHZ-PW manufactured by Shikoku Chemical Co., Ltd." in liquid epoxy resin "ZX-1059 manufactured by Nippon Steel Chemical & Material Co., Ltd." Here, 100 parts by mass of "ZX-1059", 86 parts by mass of "Rikacid MH700", and 1 part by mass of "2PHZ-PW" were mixed so that the powder ratio in the mixture was 65% by volume. After pre-mixing with a planetary ball mill (Yusei Mill), a paste (resin composition) was prepared by mixing with a three-roll mill (Sanben Roll). The paste was heated at 170°C for 2 hours to cure it, and a plate-shaped resin composition of 50mm×50mm×1mm was obtained.

[0082] The physical properties of the powder and the resin molded product obtained above were measured and evaluated as follows. The results are shown together with the production conditions in Table 1. The other examples and comparative examples were basically carried out in the same manner. 1) Particle size distribution and broken particle rate 20 g of liquid diluted to 0.5% by pure water (Leodul TW-0120V manufactured by Kao Corporation) and 0.125 g of powder were placed in a 30 ml glass spiral tube and irradiated with ultrasound for 10 minutes using an ultrasonic cleaner (SC-20A manufactured by Shin Sun Electronics). 0.2 g of the liquid was taken into a 6 ml glass spiral tube, 1.8 g of pure water was added, and ultrasound was irradiated again using an ultrasonic cleaner for 10 minutes. The dispersion of the powder thus obtained was observed under a microscope. The particle size distribution of the powder was obtained from the observation results of about 50,000 particles by image analysis. The average particle size (D50), maximum particle size (D100), and peak particle size (Ps) were obtained from the particle size distribution. Furthermore, the particle volume with a particle size in the range of ±25% of the peak particle size (Ps) was calculated. In addition, the ratio (volume %) of broken particles was calculated from the observation results of about 50,000 particles by image analysis. Particles with an area envelope (Solidity) of less than 0.75 were regarded as broken particles.

[0083] 2) Porosity The particle density of the powder was measured by gas gravimetric method using Ultrapyc5000 manufactured by Quantachrome Instruments. The porosity (%) was calculated from the particle density using the formula "[2.2-(particle density)] / 2.2×100". In this formula, the density of silica is 2.2 g / cm 3 .

[0084] 3) Alkali content The powder was pre-treated with sulfuric acid and hydrofluoric acid and then dissolved in hydrochloric acid, and the alkali content was measured by atomic absorption spectrophotometry using an atomic absorption spectrophotometer (Z-2310 manufactured by Hitachi). In this example, the Na content was measured.

[0085] 4) Oil absorption The mass of the sample was weighed, and the oil absorption was measured using boiled linseed oil in accordance with JIS K 5421. The oil absorption was converted into the oil absorption per unit volume using the above-mentioned particle density.

[0086] 5) Number of Sears The Sears number is determined by titration using sodium hydroxide according to the description of Sears, Analytical Chemistry 28 (1956), 12, 1981-1983. Specifically, for 150 g of a solution in which the powder is diluted with pure water to a particle concentration of 1% by mass, 30 g of sodium chloride is added, and the pH is adjusted to 4.0 with hydrochloric acid. The solution is fixed at 0.1 ml / sec using an automatic titrator and titrated with a 0.01 N aqueous sodium hydroxide solution. The amount of aqueous sodium hydroxide solution required to reach pH 9.0 is one-tenth, which is converted to the titration amount of a 0.1 N aqueous sodium hydroxide solution (i.e., the titration amount of a 0.1 N aqueous sodium hydroxide solution relative to 1.5 g of silica).

[0087] 6) Water vapor specific surface area / nitrogen specific surface area The ratio of the BET specific surface area obtained by the nitrogen adsorption method to the BET specific surface area obtained by the water vapor adsorption method was calculated based on the BET specific surface area obtained by the nitrogen adsorption method. The BET specific surface area was measured using BELSORP-max manufactured by Microtrac Bell.

[0088] 7) Water vapor adsorption The water vapor adsorption method was used to measure the water vapor adsorption amount relative to the powder mass at a partial pressure of 0.9 (p / p0=0.9) using BELSORP-max manufactured by Microtrac Bell.

[0089] 8) 29 Si-NMR Silica particles 29 The structural analysis by Si-NMR was performed as follows. After drying the powder at 110°C for 1 hour, the relative humidity was adjusted for 24 hours at 60%. The obtained powder (sample) was filled into a 5 mm diameter NMR solid sample tube to make it uniform, and a 14.1T NMR device (VNMRS-600 manufactured by Agilent, 1H resonance frequency 600 MHz) was used to measure it by single pulse non-decoupling method (Single Pulse Nodcapling Method). Polydimethylsiloxane (-34.44 ppm) was used as the reference substance. The obtained spectrum was subjected to waveform analysis to calculate the area of ​​each peak. The ratio of each structure is calculated by the area ratio of the peak of each structure (Si / ST)×100[%] (wherein i is a number selected from 0, 1, 2, 3, and 4. ST is the total peak area of ​​each structure represented by ST=S0+S1+S2+S3+S4).

[0090] 9) Dielectric constant (Dk) and dielectric loss tangent (Df) The dielectric constant (Dk) and dielectric loss tangent (Df) of the powder were measured by a cavity resonator perturbation method using a network analyzer (manufactured by Anritsu Co., Ltd., MS46122B) and a cavity resonator (1 GHz) in accordance with ASTM D2520 (JIS C2565). The dielectric constant (Dk) and dielectric loss tangent (Df) of the plate-shaped resin molded body were measured at 9.4 GHz using a network analyzer (manufactured by Anritsu Co., Ltd., MS46122B) and a coaxial resonator. The results were compared with those of a resin molded body without powder (filler) blending and evaluated according to the following evaluation criteria.

[0095] Dielectric constant (Dk) reduction rate (%) = ((dielectric constant without filler added - dielectric constant with filler added) / dielectric constant without filler added) × 100 0:Reduction rate>0 △: Reduction rate = 0 ×: Reduction rate < 0

[0096] Dielectric loss tangent (Df) reduction rate (%) = ((Dielectric loss tangent without filler added - Dielectric loss tangent with filler added) / Dielectric loss tangent without filler added) × 100 ○: Reduction rate is more than 30% △: Reduction rate is 20% or more and less than 30% ×: The reduction rate is less than 20%

[0097] Furthermore, the dielectric constant (Dk) and dielectric loss tangent (Df) of the resin assembly before and after storage for 1000 hours under the conditions of a temperature of 80 degrees and a humidity of 80% were evaluated according to the following evaluation criteria (high temperature and high humidity test).

[0098] The relative ratio of the dielectric constant (Dk) before and after = Dk (after) / Dk (before) 〇:1.1 or less △: greater than 1.1 and less than 1.2 ×: greater than 1.2

[0099] The relative ratio of the dielectric loss tangent (Df) before and after = Df (after) / Df (before) 〇: 2.0 or less △: greater than 2.0 and less than 3.0 ×: greater than 3.0

[0100] The average particle size of the spray droplets in the first step was determined by the liquid immersion method. Specifically, the spray droplets were caught on a plate glass thickly coated with silicone oil, and an enlarged photograph was quickly taken.

[0101] The particle diameter was measured using the photograph to determine the average particle diameter (Sauter average particle diameter).

[0102] [Example 2] In the first step, a two-fluid nozzle spray dryer was used to spray the water glass aqueous solution at a flow rate of 0.29 L / hr from one nozzle and to spray air at a flow rate of 2040 L / hr from another nozzle, thereby granulating the hollow particles (the air / liquid volume ratio was 7034). In addition, 45000 g of a sulfuric acid aqueous solution with a concentration of 25% by mass was used in the second step. In addition, the same as in Example 1, a powder containing hollow particles was obtained.

[0103] [Example 3] In the second step, the liquid temperature was adjusted so as to be maintained at 60° C. Otherwise, in the same manner as in Example 1, a powder containing hollow particles was obtained.

[0104] [Example 4] In the second step, 5000 g of hollow particles were added while stirring 80000 g of 10% by mass hydrochloric acid aqueous solution. In addition, the same as in Example 1, a powder containing hollow particles was obtained. However, in the classification step, the F edge distance was adjusted so that the particles larger than 24 μm contained in the F powder (micro powder) were less than 5% by volume. In addition, in the second step, the solid content (SiO2) concentration was 4.4% by mass, the pH of the dispersion after cooling was less than 1.0, and the ratio (M H+ / M sp ) is 5.6.

[0105] [Example 5] In the first step, the flow rate of the water glass aqueous solution was set to 0.25 L / hr (air / liquid volume ratio 8160). Furthermore, in the second step, the solution was stirred for 15 hours while the liquid temperature was maintained at 60° C. Otherwise, a powder containing hollow particles was obtained in the same manner as in Example 1.

[0106] [Comparative Example 1] In the first step, the SiO2 concentration of the water glass aqueous solution was set to 24% by mass, and the flow rate of the water glass aqueous solution was set to 0.40 L / hr (air / liquid volume ratio 5100). Furthermore, in the second step, 32000 g of a 25% by mass sulfuric acid aqueous solution was used. In addition, the same as in Example 1, a powder containing hollow particles was obtained. In addition, in the second step, the solid content (SiO2) concentration was 10.2% by mass, the pH of the dispersion after cooling was less than 1.0, and the ratio (M H+ / M sp ) is 4.1.

[0107] [Comparative Example 2] In the first step, the SiO2 concentration of the water glass aqueous solution was set to 24% by mass, and the flow rate of the water glass aqueous solution was set to 0.48 L / hr (air / liquid volume ratio 4250). Furthermore, in the second step, 32000 g of a 25% by mass sulfuric acid aqueous solution was used. In addition, the same as in Example 1, a powder containing hollow particles was obtained. In addition, in the second step, the solid content (SiO2) concentration was 10.2% by mass, the pH of the dispersion after cooling was less than 1.0, and the ratio (M H+ / M sp ) is 4.1.

[0108] In Comparative Examples 1 and 2, since a resin composition could not be obtained if the proportion of the hollow particles was blended at 65% by volume, the hollow particles were blended at 60% by volume.

[0102] [Table 1]

Claims

1. A powder containing hollow particles having a cavity inside an outer shell, wherein: The shell contains 70% by mass or more of silicon dioxide, The average particle size (D50) of the powder is 0.1 μm to 5.0 μm, The maximum particle size (D100) of the powder is less than 20.0 μm, The volume ratio of particles in the range of peak particle diameter (Ps)×0.75 μm to (Ps)×1.25 μm in the particle size distribution of the powder is less than 50% of all particles. The porosity of the powder is 10% to 50%. The powder has a broken particle rate of 10 volume % or less.

2. The powder according to claim 1, wherein The alkali content is 100 ppm or less.

3. The powder according to claim 1, wherein The oil absorption per unit volume is 0.60ml / cm 3 the following.

4. The powder according to claim 1, wherein Sears number (ml / SiO21.5g) is less than 0.30, The BET specific surface area according to the water vapor adsorption method / the BET specific surface area according to the nitrogen adsorption method is less than 0.30, Water vapor adsorption is less than 0.20% by mass. 29 In Si-NMR structural analysis, the peak area of ​​the Q4 structure accounted for more than 90% of the total peak area.

5. The powder according to claim 1, wherein The dielectric constant is less than 2.8, and the dielectric loss tangent is less than 0.0010.

6. A method for producing a resin composition, characterized in that: The production method comprises the step of mixing the powder according to any one of claims 1 to 5 into a resin material.

7. A method for producing a powder containing hollow particles, characterized in that: The manufacturing method has the following features: In the first step, an alkaline silicate aqueous solution is used to form droplets with an average particle size of less than 10.0 μm, which are sprayed and dried in a hot air flow to granulate hollow particles; The second step is to neutralize the alkali contained in the hollow particles in an acid solution and then wash them; The third step is to sinter the neutralized and cleaned hollow particles.

8. The method for producing a powder according to claim 7, wherein: The acid solution used in the second step satisfies the following formula: (M H+ / M SP )>4.7···Formula Among them, M H+ is the number of moles of hydrogen ions in the acid solution, M SP It is the value obtained by multiplying the number of moles of alkali metal ions contained in the hollow particles by their valence.