Method for improving impact resistance of float glass and float glass treatment device
Through the five-sided pickling process, hydrofluoric acid is used to etch the air surface and side of the float glass, which improves the impact resistance and ball drop strength of the glass, solves the problem of insufficient strength of float glass, and maintains the Appearance quality and simplified process flow.
Patent Information
- Application Number
- CN202410827428.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-01
AI Technical Summary
The strength of float glass is low. The existing method of strengthening glass by changing the glass formula requires a lot of experiments and process changes, and may affect the appearance quality of the glass.
Using a five-sided pickling process, the air surface and side of the float glass are exposed to hydrofluoric acid in the acid pool assembly, while the tin surface is not exposed to the acid. The acid etching rate and etching amount are controlled to ensure the resistance of the glass. The improved impact capability does not affect the appearance quality.
It effectively improves the impact resistance and ball drop strength of float glass, while maintaining the appearance quality of the glass, simplifying the process flow, and reducing the need for experiments and process changes.
Smart Images

Figure CN118724472A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of float glass processing, and in particular to a method for improving the impact resistance of float glass and a float glass processing device. Background Art
[0002] With the rapid development of the smart technology industry and the popularization of digital products in recent years, smartphones and tablets equipped with touch screens have become an indispensable part of our lives, and the outermost cover glass of the touch screen has become armor to protect the touch screen.
[0003] The cover glass needs to be strengthened. Strengthened glass can resist the erosion of most gases and liquids. Some existing technologies usually adopt the method of changing the formula of glass to improve the strength of glass. However, changing the formula to strengthen glass requires a lot of experiments, a lot of manpower and material resources, and the processing technology also needs to be changed. Summary of the invention
[0004] A technical problem to be solved by the present application is that the strength of float glass is relatively low.
[0005] To solve the above technical problems, an embodiment of the present application provides a method for improving the impact resistance of float glass, comprising the following steps: S10 preparing acid liquid of a predetermined concentration in an acid liquid tank assembly; S20 transferring the float glass with its air side facing downward into the acid liquid tank assembly, and both the air side and the side surface of the float glass are in contact with the acid liquid, and the tin surface of the float glass is not in contact with the acid liquid; S30 transferring the float glass from the acid liquid tank assembly to a rinsing tank assembly for cleaning at a predetermined time; S40 transferring the float glass from the rinsing tank assembly to a pure water tank assembly for cleaning; S50 discharging the float glass that has been cleaned in the pure water tank assembly.
[0006] In some embodiments, the acid pool assembly includes an acid pool, an acid driving structure and a plurality of roller structures, wherein the plurality of roller structures are rotatably arranged in the acid pool at intervals, and the plurality of roller structures are connected to the acid driving structure.
[0007] In some embodiments, the roller structure includes a carbon fiber central shaft and a rubber coating layer, wherein the rubber coating layer is disposed on the circumferential outer side of the carbon fiber central shaft, and the carbon fiber central shaft is rotatably sealed and disposed on the upper part of the acid liquid pool.
[0008] In some embodiments, the float glass is transferred from a first transition assembly to an acid tank assembly, and then transferred to a second transition assembly through the acid tank assembly. The conveying roller of the first transition assembly close to the acid tank assembly has an inclination angle of 0.5° to 3.5° with respect to a cross section of a roller structure of the acid tank assembly close to the first transition assembly.
[0009] In some embodiments, the acid is hydrofluoric acid.
[0010] In some embodiments, etching amount = etching rate * etching segment length L / roller speed.
[0011] In some embodiments, the acid etching rate is between 1 and 3 um / min, and the etching amount is between 0.5 and 5 um.
[0012] In some embodiments, the float glass after the pure water pool assembly has been cleaned needs to be blown dry between steps S40 and S50.
[0013] In some embodiments, the pH value of the rinsing solution is between 8 and 11, and the pure water tank assembly includes multiple separate pure water tanks.
[0014] According to another aspect of the present application, a float glass processing device is provided. The float glass processing device adopts the above method and comprises in sequence: an inlet assembly, a first transition assembly, an acid tank assembly, a second transition assembly, a rinsing assembly, a pure water cleaning assembly, a drying assembly and a discharge assembly.
[0015] By applying the technical solution of the present application, the five sides of the float glass are pickled and then cleaned, which can effectively increase the impact height of the process drop ball, and will not damage the structure of the tin surface of the float glass. For example, since the composition of the tin surface is relatively complex, the tin surface will be etched unevenly after pickling, and even the traces are relatively obvious, affecting the appearance quality of the float glass. The technical solution of the present application effectively increases the drop ball impact height of the float glass, and will not affect the appearance quality of the float glass. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0017] Figure 1 A schematic flow chart of a method for improving the impact resistance of float glass according to an embodiment of the present application is shown;
[0018] Figure 2 The overall structural schematic diagram of the float glass processing device according to the embodiment of the present application is shown.
[0019] Description of reference numerals:
[0020] 10. Feeding assembly; 20. First transition assembly; 30. Acid tank assembly; 40. Second transition assembly; 50. Rinse assembly; 60. Pure water cleaning assembly; 70. Drying assembly; 80. Discharging assembly. DETAILED DESCRIPTION
[0021] The following is a further detailed description of the implementation methods of the present application in conjunction with the accompanying drawings and examples. The detailed descriptions of the following examples and the accompanying drawings are used to exemplarily illustrate the principles of the present application, but cannot be used to limit the scope of the present application. The present application can be implemented in many different forms and is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.
[0022] The present application provides these embodiments to make the present application thorough and complete, and to fully express the scope of the present application to those skilled in the art. It should be noted that unless otherwise specifically stated, the relative arrangement of the parts and steps, the composition of the materials, the numerical expressions and the numerical values set forth in these embodiments should be interpreted as being merely exemplary, and not as limiting.
[0023] It should be noted that, in the description of this application, unless otherwise specified, the meaning of "multiple" is greater than or equal to two; the terms "upper", "lower", "left", "right", "inner", "outer", etc., indicating the orientation or positional relationship, are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on this application. When the absolute position of the object being described changes, the relative positional relationship may also change accordingly.
[0024] In addition, the words "first", "second" and similar words used in this application do not indicate any order, quantity or importance, but are only used to distinguish different parts. "Vertical" does not mean vertical in the strict sense, but is within the tolerance range. "Parallel" does not mean parallel in the strict sense, but is within the tolerance range. "Include" or "comprising" and similar words mean that the elements before the word include the elements listed after the word, and do not exclude the possibility of including other elements.
[0025] It should also be noted that in the description of this application, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be directly connected or indirectly connected through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to the specific circumstances. When a specific device is described as being located between a first device and a second device, there may or may not be an intermediate device between the specific device and the first device or the second device.
[0026] All terms used in this application have the same meaning as those understood by those of ordinary skill in the art to which this application belongs, unless otherwise specifically defined. It should also be understood that terms defined in general dictionaries, such as general dictionaries, should be interpreted as having a meaning consistent with their meaning in the context of the relevant technology, and should not be interpreted in an idealized or extremely formal sense, unless explicitly defined herein.
[0027] Technologies, methods, and equipment known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, the technologies, methods, and equipment should be considered part of the specification.
[0028] When float glass comes into contact with a solution containing hydrofluoric acid, chemically strengthened glass is easily corroded. Therefore, the controllable hydrofluoric acid corrosion process is also used as an effective glass surface etching technology. At the same time, hydrofluoric acid treatment, through chemical reaction with the glass surface, removes the micro-crack layer on the glass surface or clocks the crack tip to hinder the crack propagation, thereby achieving the effect of improving the strength of the glass. Treating chemically strengthened glass with hydrofluoric acid for a certain period of time can improve the surface mechanical properties, especially the impact resistance.
[0029] At present, more than 90% of the flat glass used is produced by the float process. In the production process of float glass, the molten glass liquid needs to be spread on the surface of the molten tin liquid, causing some tin ions to diffuse into the glass surface in contact with the tin liquid, thus forming two surfaces with different chemical compositions and structures, usually referred to as the "air surface" and the "tin surface". The difference in composition and structure causes different surface compressive stresses and stress layer depths on the two surfaces of float glass during the chemical strengthening process. In addition, in order to prevent the glass from being scratched during the production process of float glass, sulfide gas is used to support the glass, which will cause some sulfides to enter the glass surface. When the glass is etched with acid, it will show a dot-shaped "sulfur mark", resulting in a poor appearance of the cover glass.
[0030] like Figure 1 and Figure 2 As shown, the method for improving the impact resistance of float glass in an embodiment of the present application comprises the following steps: S10: preparing acid of a predetermined concentration in an acid tank assembly. S20: transferring the float glass with its air side facing downward to the acid tank assembly, and both the air side and the side of the float glass are in contact with the acid, while the tin side of the float glass is not in contact with the acid. S30: transferring the float glass from the acid tank assembly to the rinsing tank assembly for cleaning at a predetermined time. S40: transferring the float glass from the rinsing tank assembly to the pure water tank assembly for cleaning. S50: discharging the float glass after cleaning the pure water tank assembly.
[0031] By applying the technical solution of this embodiment, the five sides of the float glass are pickled and then cleaned, which can effectively increase the impact height of the process drop ball, and will not damage the structure of the tin surface of the float glass. For example, due to the complex composition of the tin surface, the tin surface will be etched unevenly after pickling, and even the traces will be obvious, affecting the appearance quality of the float glass. The technical solution of this embodiment effectively increases the drop ball impact height of the float glass, while not affecting the appearance quality of the float glass.
[0032] In certain embodiments, the acid pool assembly 30 comprises an acid pool, an acid driving structure and a plurality of roller structures, and a plurality of roller structures are rotatably arranged in the acid pool at intervals, and a plurality of roller structures are all connected with the acid driving structure. The acid driving structure comprises an acid driving motor, and the acid driving motor is connected with the roller structure through a gear, and a plurality of roller structures are connected by being connected. Float glass is transmitted by the roller structures that are arranged at intervals, and such a transmission mode can both realize the transmission of float glass and ensure that the contact of float glass with acid is not affected. It should be noted that the highest point of the acid pool is slightly higher than the section on the top of the roller structure, high 0.8mm to 3.5mm.
[0033] In some embodiments, the roller structure includes a carbon fiber central shaft and a rubber coating, the rubber coating is arranged on the circumferential outer side of the carbon fiber central shaft, and the carbon fiber central shaft is rotatably sealed and arranged on the upper part of the acid tank. The above structure ensures that the conveying efficiency and accuracy of the roller structure for float glass are relatively controllable on the one hand, and on the other hand, it also ensures that the roller structure does not react with the acid, thereby extending the service life. The acid tank and the roller structure are sealed and installed. It should be noted that the outer surface of the rubber coating has an anti-slip surface, and the anti-slip surface includes a plurality of protrusions, which not only increases the friction between the rubber coating and the float glass, but also ensures that the acid passes through the gaps between the protrusions, so that the reaction between the float glass and the acid is more uniform.
[0034] In the technical solutions of some embodiments, the float glass is transferred from the first transition component to the acid tank component, and then transferred to the second transition component through the acid tank component. The angle of inclination between the conveying roller of the first transition component close to the acid tank component and the cross section of the roller structure of the acid tank component close to the first transition component is between 0.5° and 3.5°. The above structure ensures that the float glass can smoothly enter the acid tank. If the inclination angle is too small, the acid is easy to overflow from the acid tank. If the inclination angle is too large, the float glass is easy to get stuck with the roller structure, resulting in the float glass being unable to smoothly pass through the acid tank component 30. It should be noted that the free end of each protrusion is an arc surface, and the height of each protrusion is the same, between 3.6mm and 8mm. The height of the protrusion is higher than the thickness of the float glass. In this way, even if the float glass and the roller structure are stuck, the float glass can be driven to move forward by the rotation of the roller structure. The height of each protrusion cannot be too high, otherwise the conveying of the float glass will be unstable.
[0035] In some embodiments, the acid is hydrofluoric acid. The concentration of hydrofluoric acid is between 2% and 6%, so that the surface effect of the float glass after the reaction is better. The reaction product of hydrofluoric acid and float glass will not remain on the float glass.
[0036] In the technical solutions of some embodiments, etching amount = etching rate * etching section length L / roller speed. Through the above formula, the relationship between the acid tank assembly 30 and the float glass can be accurately estimated, for example, the length of the acid tank assembly 30 is between 1.2m and 3.2m. The roller speed refers to the roller speed of the roller structure.
[0037] In the technical solutions of some embodiments, the acid etching rate is between 1um / min and 3um / min, and the etching amount is between 0.5um and 5um. If the etching amount is too large, the strength of the float glass will be affected, and if the etching amount is too small, the defects on the five surfaces of the float glass will not be easily eliminated. The above etching rate and etching amount can not only eliminate defects such as microcracks on the five surfaces of the float glass, but also improve the drop ball strength of the float glass.
[0038] In the technical solutions of some embodiments, the float glass after the pure water pool assembly is cleaned needs to be blown dry between steps S40 and S50. This can increase the discharge rate of the float glass and is also conducive to ensuring the cleanliness of the float glass. The drying air needs to be clean gas with a certain temperature, such as compressed air, which needs dust removal, filtration and other processes to ensure the cleanliness of the float glass.
[0039] In the technical solutions of some embodiments, the pH value of the rinsing solution is between 8 and 11, and the pure water tank assembly includes multiple separate pure water tanks. Such a rinsing solution can not only neutralize the acid solution on the float glass, but also ensure that the rinsing solution will not cause adverse effects on the float glass, such as the reaction between the alkali solution and the float glass.
[0040] It can be seen from the above that the five-sided etching equipment of the present application includes eight parts: a feeding section (feeding component 10), a first transition section (first transition component 20), an acid etching section (acid tank component 30), a second transition section (second transition component 40), a pure water rinsing (alkali neutralization) section (rinsing component 50), a pure water washing 1 / 2+DT washing section (pure water cleaning component 60), an air knife drying section (drying component 70), and a discharging section (discharging component 80). The entire system is in a negative pressure state, and the negative pressure pipe is connected to the acid treatment tower. The acid etching section is the key section of the equipment, which requires high operating accuracy, stable glass operation, and liquid level control accuracy controllable within ±0.1mm. Acid etching section liquid level control description: The etching section is equipped with an etching liquid level sensor, which is interlocked with the etching liquid replenishing pump to achieve the purpose of precise liquid level control.
[0041] High-precision roller structure (roller structure) requires that the material should be resistant to hydrofluoric acid, have good rigidity, no deformation, and high coaxiality to ensure the stability of glass operation: the core of the rubber-coated shaft is The through shaft is made of carbon fiber. The coaxiality tolerance of the rubber-coated shaft is 0.02mm, and the total runout tolerance is 0.05mm. The hardness of the rubber coating is 40 degrees, and it is not easy to bend.
[0042] In the etching section, the rotation of the roller structure drives it to run. During the operation, the air surface of the glass and the surrounding areas (four raised surfaces) undergo chemical etching reaction with the etching liquid (acid solution).
[0043] The amount of etching can be controlled by the speed of the roller (i.e. the residence time of the glass in the acid solution) and the concentration of fluoride ions in the acid solution. Etching amount = etching rate * etching section length L / roller speed.
[0044] The key points of the process technology for improving the impact resistance of float high-aluminum glass include two aspects: one is that the etching rate requires the acid etching rate to be optimal at 1-3um / min, and the other is that the etching amount is required to be 0.5-5um. Under this process condition, the impact resistance of the glass is significantly improved. This patent solution takes 1.3mm thick float high-aluminum glass as an example, but the verification test is not a condition to limit the scope of the patent. Other types of process types for five-sided etching of float glass to improve the impact resistance of glass are all within the scope of protection of the patent (including but not limited to tin surface coating, inkjet printing, etc.). The verification reference data are as follows:
[0045] Table 1
[0046]
[0047] Note: The drop ball test is carried out in accordance with the standard GB4943.1-2011.
[0048] As shown in Table 1, the average impact height of the ring drop in the five-side etching process is about 150 cm, which is about 50 cm higher than that of the glass substrate (96 cm) that has not been etched.
[0049] The design of the acid etching section of the five-sided etching equipment requires high operating accuracy, smooth glass operation, and liquid level control accuracy of ±0.1mm. The etching section is equipped with a liquid level sensor and is interlocked with the liquid replenishment pump to achieve dynamic liquid replenishment to ensure that the etching liquid height is at a controlled height.
[0050] During the process, it is necessary to ensure that the tin surface of the glass substrate does not react with the acid solution, that is, the tin surface must be higher than the etching solution level. In this case, the high-precision rubber roller of the etching section is required to be processed according to the following requirements:
[0051] The core of the rubber-coated shaft is The through shaft is made of carbon fiber. The coaxiality tolerance of the rubber-coated shaft is 0.02mm, and the total runout tolerance is 0.05mm. The hardness of the rubber-coated shaft is 40 degrees, and it is not easy to bend. The improvement of impact performance requires that the etching rate of the acid solution is 1-3um / min, and the etching amount is 0.5-5um.
[0052] Description of the etching rate control method: by controlling the hydrofluoric acid concentration Wt in the etching reaction acid solution to be 3-5%.
[0053] Description of the etching amount control method: The etching amount can be controlled by the roller speed (i.e. the residence time of the glass in the acid solution) and the fluoride ion concentration in the acid solution. Etching amount = etching rate * etching section length L / roller speed.
[0054] The present application also provides a float glass processing device. The float glass processing device adopts the above method, and the float glass processing device comprises: a feed assembly 10, a first transition assembly 20, an acid liquid pool assembly 30, a second transition assembly 40, a rinse assembly 50, a pure water cleaning assembly 60, a blow-drying assembly 70 and a discharge assembly 80 in sequence. The feed assembly 10 comprises a feed bracket and a feed roller, the feed roller is rotatably arranged on the feed bracket, and the feed roller can also be a feed conveyor belt, the first transition assembly 20 comprises a first transition shell and a first transition roller, the first transition roller is arranged in the first transition shell, and the first transition shell is provided with a negative pressure air induction channel. The acid liquid pool assembly 30 comprises an acid liquid shell, the acid liquid shell cover is arranged on the acid liquid pool, and the space formed by the acid liquid shell and the acid liquid pool is connected to the first transition shell, so that the acid mist in the acid liquid pool can be drawn out through the negative pressure air induction channel and processed, which is beneficial to the health of the operator.
[0055] So far, various embodiments of the present application have been described in detail. In order to avoid obscuring the concept of the present application, some details known in the art are not described. Based on the above description, those skilled in the art can fully understand how to implement the technical solution disclosed herein.
[0056] Although some specific embodiments of the present application have been described in detail by way of examples, it should be understood by those skilled in the art that the above examples are for illustration only and are not intended to limit the scope of the present application. It should be understood by those skilled in the art that the above embodiments may be modified or some technical features may be replaced by equivalents without departing from the scope and spirit of the present application. In particular, the various technical features mentioned in the various embodiments may be combined in any manner as long as there is no structural conflict.
Claims
1. A method for improving the impact resistance of float glass, characterized in that: The following steps are involved: S10: preparing an acid solution of a predetermined concentration in an acid solution pool assembly; S20: transferring the float glass with its air side facing downward into the acid liquid tank assembly, wherein both the air side and the side surface of the float glass are in contact with the acid liquid, and the tin side of the float glass is not in contact with the acid liquid; S30: at a predetermined time, the float glass is transferred from the acid tank assembly to the rinsing tank assembly for cleaning; S40 float glass is transferred from the rinse tank assembly to the pure water tank assembly for cleaning; S50 discharges the float glass after the pure water tank components have been cleaned.
2. The method for improving the impact resistance of float glass according to claim 1, characterized in that: The acid pool assembly comprises an acid pool, an acid driving structure and a plurality of roller structures. The plurality of roller structures are rotatably arranged in the acid pool at intervals, and the plurality of roller structures are all connected to the acid driving structure.
3. The method for improving the impact resistance of float glass according to claim 2, characterized in that: The roller structure comprises a carbon fiber central shaft and a rubber coating layer, wherein the rubber coating layer is arranged on the circumferential outer side of the carbon fiber central shaft, and the carbon fiber central shaft is rotatably sealed and arranged on the upper part of the acid liquid pool.
4. The method for improving the impact resistance of float glass according to claim 3, characterized in that: The float glass is transferred from the first transition component to the acid pool component, and then transferred to the second transition component through the acid pool component. The conveying roller of the first transition component close to the acid pool component has an inclination angle of 0.5° to 3.5° with respect to the cross section of the roller structure of the acid pool component close to the first transition component.
5. The method for improving the impact resistance of float glass according to claim 1, characterized in that: The acid liquid is hydrofluoric acid.
6. The method for improving the impact resistance of float glass according to claim 5, characterized in that: Etching amount = etching rate * etching section length L / roller speed.
7. The method for improving the impact resistance of float glass according to claim 6, characterized in that: The acid etching rate is between 1 and 3 um / min, and the etching amount is between 0.5 and 5 um.
8. The method for improving the impact resistance of float glass according to claim 1, characterized in that: Between steps S40 and S50, the float glass after the pure water pool assembly has been cleaned needs to be blown dry.
9. The method for improving the impact resistance of float glass according to claim 8, characterized in that: The pH value of the rinsing solution is between 8 and 11, and the pure water pool assembly includes multiple separate pure water pools.
10. A float glass processing device, characterized in that: The float glass processing device adopts the method according to any one of claims 1 to 9, and the float glass processing device comprises: An inlet assembly (10), a first transition assembly (20), an acid pool assembly (30), a second transition assembly (40), a rinsing assembly (50), a pure water cleaning assembly (60), a drying assembly (70), and an outlet assembly (80).
Citation Information
Patent Citations
Glass reinforcing method
CN103508674A
Processing method for reinforcing over-sized multi-curved glass
CN103936290A
Etching equipment and glass plate production system
CN115745413A
Conveyor for surface treating device
JP2008137733A