Difunctional self-assembly hole transport material and preparation method and application thereof

By developing bifunctional self-assembled hole transport materials, using amphiphilic compounds formed by anthracene, thianthene or xanthene rings and cyanophosphate, the problem of insufficient performance and stability of hole transport materials in perovskite solar cells has been solved. problem, achieving efficient photoelectric conversion and improving stability, reducing costs.

CN118724948APending Publication Date: 2024-10-01深圳普太科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410646006.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-23
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The performance and stability of hole transport materials in existing perovskite solar cells are insufficient, affecting photoelectric conversion efficiency and cost-effectiveness.

Method used

Develop a bifunctional self-assembled hole transport material based on amphiphilic compounds formed by anthracene, thianthene or xanthene rings and cyanophosphoric acid, with high hole transport properties and air stability, through cyanophosphonic acid anchors The fixed group realizes self-assembly and interface passivation, and is suitable for use between the electrode and the perovskite material layer of perovskite solar cells.

Benefits of technology

It improves the photoelectric conversion efficiency and stability of perovskite solar cells, reduces production costs, and achieves high energy conversion efficiency of more than 23.80%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724948A_ABST
    Figure CN118724948A_ABST
Patent Text Reader

Abstract

The invention discloses a difunctional self-assembly hole transport material and a preparation method and application thereof, and belongs to the technical field of photovoltaic materials. The difunctional self-assembly hole transport material provided by the invention comprises a compound with a chemical formula as shown in a formula I: # imgabs0 #, wherein X is selected from CH2, S or O; in the formula (I), R1 to R2 are respectively and independently selected from one of H, substituted C1-30 alkyl, unsubstituted C1-30 alkyl, substituted C1-30 alkoxy, unsubstituted C1-30 alkoxy, substituted C1-30 alkylthio, unsubstituted C1-30 alkylthio, substituted C6-30 aryl and unsubstituted C6-30 aryl. The dual-function self-assembly hole transport material provided by the invention can effectively improve the hole transport efficiency in a photovoltaic device, thereby improving the photoelectric conversion efficiency and stability of the photovoltaic device. The invention also provides a preparation method and application of the difunctional self-assembly hole transport material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of photovoltaic materials, and in particular to a dual-functional self-assembled hole transport material and a preparation method and application thereof. Background Art

[0002] Energy is one of the key factors to promote economic development. With the booming economy and the improvement of people's living standards, the development of renewable energy has become an indispensable path. Optoelectronic technology is increasingly closely related to human life, and the development of solar cells has attracted much attention in recent years. Perovskite solar cells (PSCs) stand out in the field of optoelectronics for their excellent optoelectronic performance, and their importance in the field of renewable energy is becoming increasingly prominent; perovskite solar cells have become a promising alternative to traditional thin-film solar cells.

[0003] Perovskite materials have good light absorption properties and high charge mobility, which make them perform well in solar cells. Hole transport materials also play a vital role in perovskite solar cells. The hole transport layer (HTL) is responsible for receiving and transferring positive charges (holes) from the photosensitive perovskite layer to the electrode of the cell. Selecting the right hole transport material is crucial to improving the performance of solar cells. A good hole transport layer material needs to have not only good conductivity, but also an appropriate energy level structure to ensure efficient electron transport and photoelectric conversion.

[0004] Therefore, one of the keys to researching and developing perovskite solar cells lies in continuously optimizing hole transport materials to improve the overall performance, stability and production cost-effectiveness of perovskite solar cells, thereby promoting the development of renewable energy technology. Summary of the invention

[0005] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention proposes a bifunctional self-assembled hole transport material, which can effectively improve the hole transport efficiency in photovoltaic devices, thereby improving their photoelectric conversion efficiency and stability.

[0006] The present invention also provides a method for preparing the bifunctional self-assembled hole transport material.

[0007] The present invention also provides application of the bifunctional self-assembled hole transport material.

[0008] According to an embodiment of the first aspect of the present invention, there is provided a bifunctional self-assembled hole transport material, wherein the bifunctional self-assembled hole transport material comprises a compound having a chemical formula as shown in Formula I:

[0009]

[0010] wherein X is selected from CH2, S or O;

[0011] R1 to R2 are independently selected from H, substituted C 1~30 Alkyl, unsubstituted C 1~30 Alkyl, substituted C 1~30 Alkoxy, unsubstituted C 1~30 Alkoxy, substituted C 1~30 Alkylthio, unsubstituted C 1~30 Alkylthio, substituted C 6~30 Aryl and unsubstituted C 6~30 One of the aromatic groups.

[0012] The bifunctional self-assembled hole transport material according to the embodiment of the present invention has at least the following beneficial effects:

[0013] The chemical formula of the bifunctional self-assembled hole transport material in the present invention is shown in Formula I, which is an amphiphilic hole transport material formed based on anthracene, thioanthene or xanthene ring and cyanophosphoric acid, with an anthracene derivative with a rigid conjugated plane as the parent core, giving the molecule high hole transport performance and air stability; at the same time, it has π-π stacking between single molecules, which is conducive to the transmission of holes; cyanophosphonic acid is an anchoring group to achieve complete coverage and bonding of the self-assembled hole transport material on the substrate surface. Specifically:

[0014] The bifunctional self-assembled hole transport material of the present invention is used in photovoltaic devices, especially between the electrode and the perovskite material layer (also referred to as the perovskite photoactive layer) in a perovskite solar cell: the cyanophosphate in the compound shown in Formula I can modify the perovskite material layer, and the defect passivation effect of the phosphate can enhance the uniformity of the perovskite material layer; wherein the PO bond, the C≡N bond and the S and O in the anthracene heterocycle are reacted with the Pb commonly contained in the perovskite material layer. 2+ The chemical reaction between them effectively modifies the perovskite material layer and passivates the surface defects of the perovskite, significantly inhibiting non-radiative recombination. Therefore, when the compound shown in Formula I is used in a perovskite solar cell, it exhibits unique properties based on its amphiphilicity: as a hole transport layer material, it can be anchored to the adjacent substrate interface (such as a glass substrate containing a TIO layer), and can interact with the adjacent perovskite material layer, and the passivated perovskite material layer exhibits an excellent charge transport interface layer, thereby increasing the stability of the perovskite cell while improving the photoelectric conversion efficiency of the perovskite cell.

[0015] The bifunctional self-assembled hole transport material provided by the present invention is amphiphilic and comprises -PO3H2 and -CN. It is an organic small molecule bifunctional self-assembled hole transport material with an anchoring group, which can obtain a HOMO energy level that is more matched with the energy level of the perovskite material layer. The perovskite material layer is passivated by the bifunctional self-assembled hole transport material to make the perovskite solar cell more efficient and stable.

[0016] The bifunctional self-assembled hole transport material of the present invention can be used as HTMs in inverted perovskite solar cells and large-area modules. It is simple to prepare and low in cost. It can passivate the perovskite material layer in the cell or module (having the function of interface passivation), which helps to improve the efficiency and life of the cell, optimize the cell structure, reduce the cost, and realize large-scale production and industrialization. The bifunctional self-assembled hole transport material of the present invention is used for photovoltaic devices. The prepared device has high Voc, Jsc, FF and PCE, the highest energy conversion efficiency reaches more than 23.80%, and good environmental stability can be obtained. It has great commercial prospects in improving the efficiency and stability of perovskite solar cells and reducing their costs.

[0017] According to some embodiments of the invention, the aryl group includes at least one of a phenyl group, a methylphenyl group, an ethylphenyl group, and a propylphenyl group.

[0018] According to some embodiments of the present invention, the substituted C 1~30 Alkyl, substituted C 1~30 Alkoxy, substituted C 1~30 Alkylthio, substituted C 6~30 The substituent in the aryl group includes at least one of cyano, fluorine, chlorine, bromine or iodine.

[0019] According to some embodiments of the invention, in the compound represented by formula I, R1 to R2 are independently selected from H, substituted C 1~6 Alkyl, unsubstituted C 1~6 Alkyl, substituted C 1~6 Alkoxy, unsubstituted C 1~6 Alkoxy, substituted C 1~6 Alkylthio, unsubstituted C 1~6 One of an alkylthio group, a substituted phenyl group and an unsubstituted phenyl group.

[0020] According to some embodiments of the invention, in the compound represented by formula I, R1 to R2 are independently selected from at least one of H, methyl, methoxy, methylthio and phenyl.

[0021] Specifically, in the compound represented by formula I, R1 and R2 may be the same or different.

[0022] According to some embodiments of the present invention, the bifunctional self-assembled hole transport material comprises at least one of the compounds represented by chemical formulae I-1 to I-15:

[0023]

[0024]

[0025] According to some embodiments of the present invention, the color of the bifunctional self-assembled hole transport material may be any color from light yellow to dark brown.

[0026] According to some embodiments of the present invention, the ultraviolet-visible absorption peak of the bifunctional self-assembled hole transport material is 320-350 nm, for example, about 330 nm, 335 nm, 340 nm or about 345 nm.

[0027] According to some embodiments of the present invention, the ultraviolet-visible absorption sideband of the bifunctional self-assembled hole transport material is 380-410 nm, for example, about 385 nm, 400 nm or about 405 nm.

[0028] According to some embodiments of the present invention, the optical band gap of the bifunctional self-assembled hole transport material is 3 to 3.3 eV, for example, about 3.05 eV, 3.1 eV, 3.2 eV or about 3.25 eV.

[0029] According to an embodiment of the second aspect of the present invention, a method for preparing the bifunctional self-assembled hole transport material is provided, the method comprising the following steps:

[0030] S1. Knoevenagel condensation reaction of the compound represented by formula III with the cyanomethyl phosphate compound represented by formula IV to obtain a compound represented by formula II;

[0031] S2. subjecting the compound represented by formula II to a hydrolysis reaction;

[0032]

[0033] Wherein R3 and R4 are independently selected from substituted C 1~10 Alkyl or unsubstituted C 1~10 alkyl.

[0034] The preparation method according to the embodiment of the present invention has at least the following beneficial effects:

[0035] Since the preparation method adopts all the technical solutions of the bifunctional self-assembled hole transport material of the above embodiment, it at least has all the beneficial effects brought by the technical solutions of the above embodiment.

[0036] Furthermore, the preparation method provided by the present invention is simple and easy to implement, and the preparation raw materials are cheap and readily available.

[0037] According to some embodiments of the present invention, in step S1, the cyanomethyl phosphate compound includes at least one of dimethyl cyanomethyl phosphate, diethyl cyanomethyl phosphate (CAS: 2537-48-6), dipropyl cyanomethyl phosphate, dibutyl cyanomethyl phosphate, dipentyl cyanomethyl phosphate, dihexyl cyanomethyl phosphate, ethyl methyl cyanomethyl phosphate and ethyl propyl cyanomethyl phosphate.

[0038] According to some embodiments of the present invention, in step S1, the compound represented by formula III includes at least one of thioxanthone (CAS: 126395-12-8), xanthenone (CAS: 90-47-1), 3,6-dimethylanthraquinone (CAS: 54159-95-4) and 3,6-diphenylthioxanthone (CAS: 854661-66-8).

[0039] According to some embodiments of the present invention, in step S1, the molar ratio of the compound represented by formula III to the cyanomethyl phosphate compound represented by formula IV is 1:(1-5), for example, about 1:2, 1:3, 1:3.5 or about 1:4.

[0040] According to some embodiments of the present invention, in step S1, the Knoevenagel condensation reaction is carried out under the action of an organic base.

[0041] According to some embodiments of the present invention, the organic base includes at least one of piperidine, pyridine, triethylamine and TiCl4 / Et3N, wherein TiCl4 / Et3N represents a mixture of TiCl4 and Et3N.

[0042] According to some embodiments of the present invention, the mass volume ratio of the compound represented by formula III and the organic base is 1 g: (1-5) mL, for example, about 1 g: 1.5 mL, 1 g: 2 mL, 1 g: 2.5 mL, 1 g: 3 mL or about 1 g: 4 mL.

[0043] According to some embodiments of the present invention, in step S1, the Knoevenagel condensation reaction is carried out in an environment of solvent B.

[0044] The solvent B includes at least one of toluene, chlorobenzene, N,N-dimethylformamide, dichloromethane, chloroform, 1,4-dioxane and dimethyl sulfoxide.

[0045] The mass volume ratio of the compound represented by formula III and the solvent B is 1 g: (10-50) mL. For example, it can be about 1 g: 15 mL, 1 g: 20 mL, 1 g: 25 mL or about 1 g: 30 mL.

[0046] According to some embodiments of the present invention, in step S1, the temperature of the Knoevenagel condensation reaction is 25-140°C, for example, about 30°C, 40°C or about 50°C.

[0047] According to some embodiments of the present invention, in step S1, the Knoevenagel condensation reaction is carried out for 8 to 20 hours. To further increase the mass transfer rate, the Knoevenagel condensation reaction is carried out under stirring. The specific duration of the Knoevenagel condensation reaction is 10 hours, 12 hours, 15 hours or about 18 hours.

[0048] According to some embodiments of the present invention, step S1 further comprises purifying the compound shown in formula II after the Knoevenagel condensation reaction. The purification comprises cooling, desolventizing, extraction, drying and column separation performed in sequence. The desolventizing operation comprises rotary evaporation. The extractant used in the extraction comprises dichloromethane. The eluent for the column separation is a mixture of dichloromethane and petroleum ether, wherein the volume ratio of dichloromethane to petroleum ether is 2.5 to 3.5:1; more specifically, it may be about 3:1.

[0049] According to some embodiments of the present invention, in step S2, the hydrolysis reaction comprises reacting the compound represented by formula II with trimethylhalosilane.

[0050] According to some embodiments of the present invention, the trimethylhalosilane is selected from at least one of trimethylchlorosilane, trimethylbromosilane and trimethyliodosilane.

[0051] According to some embodiments of the present invention, the molar ratio of the trimethylhalosilane to the compound represented by formula II is (0.5-5): 1. For example, it can be about 2:1, 2.5:1, 3:1, 3.5:1 or about 4:1.

[0052] According to some embodiments of the present invention, step S2 is performed in a protective atmosphere.

[0053] According to some embodiments of the present invention, in step S2, the hydrolysis reaction is carried out in solvent A. The solvent A comprises at least one of dichloromethane and chloroform.

[0054] According to some embodiments of the present invention, in step S2, the specific step of the hydrolysis reaction includes dissolving the compound shown in formula II in the solvent A, and then mixing the resulting mixture with the trimethylhalosilane. More specifically, it includes dropping the trimethylhalosilane into the mixture of the compound shown in formula II and the solvent A.

[0055] According to some embodiments of the present invention, the mass volume ratio of the compound represented by Formula II and the solvent A is 1 g: (10-50) mL. For example, it can be about 1 g: 15 mL, 1 g: 20 mL, 1 g: 25 mL or about 1 g: 30 mL.

[0056] According to some embodiments of the present invention, in step S2, the hydrolysis reaction is carried out under stirring, thereby increasing the mass transfer rate.

[0057] According to some embodiments of the present invention, in step S2, the temperature of the hydrolysis reaction is 15-40°C, for example, about 25°C or about 30°C.

[0058] According to some embodiments of the present invention, in step S2, the duration of the hydrolysis reaction is 5 to 30 hours, for example, about 10 hours, 12 hours, 15 hours or about 20 hours.

[0059] According to some embodiments of the present invention, in step S2, in the compound represented by formula II, R3 and R4 are independently selected from unsubstituted C 1~10 For example, it can be unsubstituted C 1~5 The alkyl group may be at least one of a methyl group, an ethyl group, a propyl group and an isopropyl group.

[0060] According to some embodiments of the present invention, the preparation method further comprises purification after step S2. The purification comprises desolventizing and recrystallization. The recrystallization solvent used in the recrystallization comprises dichloromethane and methanol. The volume ratio of dichloromethane to methanol is 1.5 to 2.5:1. For example, it can be about 2:1.

[0061] According to some embodiments of the present invention, the compound represented by formula II is a compound represented by formula II-1 or a compound represented by formula II-2:

[0062]

[0063] The mechanism of the preparation method is briefly described as follows:

[0064]

[0065] It should be noted that the above reaction formula is not unique, and in actual production, the types of organic base, trimethyl halide, solvent A and solvent B can be adjusted according to production conditions.

[0066] According to an embodiment of the third aspect of the present invention, there is provided a hole transport layer, wherein the raw materials for preparing the hole transport layer include the bifunctional self-assembled hole transport material.

[0067] Since the hole transport layer adopts all the technical solutions of the bifunctional self-assembled hole transport material of the above embodiment, it at least has all the beneficial effects brought by the technical solutions of the above embodiment.

[0068] According to some embodiments of the present invention, the hole transport layer is a monomolecular layer. The reason for achieving such an effect is the self-assembly property of the bifunctional self-assembly hole transport material.

[0069] According to some embodiments of the present invention, the thickness of the hole transport layer is 5-100 nm.

[0070] According to some embodiments of the present invention, the hole transport layer has a thickness of 10 to 20 nm.

[0071] According to an embodiment of the fourth aspect of the present invention, a photovoltaic device is provided, wherein the photovoltaic device comprises the hole transport layer; and / or the raw materials for preparing the photovoltaic device comprise the bifunctional self-assembled hole transport material.

[0072] Since the photovoltaic device adopts all the technical solutions of the hole transport layer or the bifunctional self-assembled hole transport material of the above embodiments, it at least has all the beneficial effects brought by the technical solutions of the above embodiments.

[0073] According to some embodiments of the present invention, the photovoltaic device includes at least one of a solar cell type device and an organic light emitting diode.

[0074] According to some embodiments of the present invention, the solar cell device includes at least one of an organic solar cell, a perovskite solar cell, a perovskite solar cell, and their corresponding large-area modules.

[0075] According to some embodiments of the present invention, the area of ​​the module of the perovskite solar cell is 10 to 500 cm 2 For example, it can be 10 to 200 cm 2 .

[0076] According to some embodiments of the present invention, the perovskite solar cell comprises a substrate, the hole transport layer, the perovskite material layer, the electron transport layer and the metal electrode layer which are stacked.

[0077] The substrate includes at least one of ITO glass or fluorine tin oxide (FTO). The ITO glass is transparent.

[0078] The ITO glass includes a base glass and an ITO layer, and the ITO layer is located between the base glass and the hole transport layer.

[0079] The thickness of the substrate is 0.5 mm to 10 mm, for example, about 1 mm, 1.1 mm, 1.2 mm or about 1.5 mm.

[0080] The hole transport layer is prepared from the bifunctional self-assembled hole transport material and has a thickness of 5 to 100 nm, for example, about 10 nm, 15 nm or about 20 nm.

[0081] The thickness of the perovskite material layer is 100-1000 nm, for example, about 500 nm, 600 nm, 700 nm or about 800 nm.

[0082] The electron transport layer includes a C60 layer and a BCP layer stacked together, wherein the C60 layer is located between the perovskite material layer and the BCP layer. The thickness of the electron transport layer is 10 to 100 nm; for example, it can be 10 to 50 nm. For example, it can be about 20 nm, 25 nm or about 30 nm.

[0083] The thickness of the C60 layer is 10 to 40 nm; for example, it may be about 15 nm, 20 nm or about 25 nm;

[0084] The thickness of the BCP layer is 1-10 nm; for example, it may be about 3 nm, 5 nm or about 8 nm.

[0085] The material of the metal electrode layer includes at least one of Au, Ag, Al or Cu.

[0086] The thickness of the metal electrode layer is 50-300 nm, for example, about 70 nm, 80 nm, 90 nm, 100 nm or about 200 nm.

[0087] According to some embodiments of the present invention, in the method for preparing the perovskite solar cell, a slurry containing the bifunctional self-assembled hole transport material is coated on the surface of the substrate and annealed to form the hole transport layer.

[0088] According to some embodiments of the present invention, the concentration of the slurry comprising the bifunctional self-assembled hole transport material is 0.5 to 5 mg / mL, and specifically may be 1 to 3 mg / mL.

[0089] According to some embodiments of the present invention, the annealing temperature is 80-120°C.

[0090] According to some embodiments of the present invention, the annealing time is 5 to 50 minutes.

[0091] Unless otherwise specified, the terms in this invention have the following definitions:

[0092] The "protective atmosphere" includes at least one of an inert gas or nitrogen, wherein the inert gas includes a Group 0 gas.

[0093] "Unsubstituted" means that H in the corresponding group is not substituted.

[0094] "Substituted" means that at least one H in the group may be further substituted by one of the following groups: alkyl, alkenyl, alkynyl, aryl, halogen, haloalkyl, haloalkenyl, haloalkynyl, haloaryl, hydroxy, alkoxy, alkenyloxy, aryloxy, benzyloxy, haloalkoxy, haloalkenyloxy, haloaryloxy, nitro, nitroalkyl, nitroalkenyl, nitroalkynyl, nitroaryl, nitroheterocyclyl, amino, alkylamino, dialkylamino, alkenylamino, alkynylamino, arylamino, diarylamino, phenylamino, diphenylamino, benzylamino, dibenzylamino, hydrazino, acyl, acylamino, diacylamino, acyloxy, heterocyclyl, heterocyclyloxy, heterocyclylamino, halogenated heterocyclyl, carboxyl ester, carboxyl, carboxylamide, thiol, alkylthio, benzylthio, acylthio and phosphorus-containing groups.

[0095] "Alkyl" refers to a group derived from a branched or straight chain saturated aliphatic alkane having the specified number of carbon atoms by removing one hydrogen.

[0096] “C 1~30 "alkyl" means an alkyl group having 1 to 30 carbon atoms, including C 1~30 Straight chain alkyl, C 1~30 The branched alkyl and C 3~30 Cycloalkyl; for "C 1~6 The "alkyl" etc. have a similar explanation, except that the number of carbon atoms is different.

[0097] "Alkoxy" refers to an alkyl group as defined herein attached to another group through an oxygen atom, i.e., "alkyl-O-". 1~30 "alkoxy" means an alkoxy group having a total of 1 to 30 carbon atoms, including C 1~30 Straight chain alkoxy, C 1~30 Branched alkoxy and C 2~30 The cycloalkoxy group of "C" may be, for example, methoxy, ethoxy, n-propoxy, isopropoxy, etc. 1~6 The explanation of "alkoxy" is similar to this, except that the number of carbon atoms is different.

[0098] "Alkylthio" refers to an alkyl group as defined herein attached to another group through a sulfur atom, i.e., "alkyl-S-". 1~30 "alkylthio" means an alkylthio group having a total carbon number of 1 to 30, including C 1~30 Straight chain alkylthio, C 1~30 Branched alkylthio and C 2~30The cycloalkylthio group may be, for example, methylthio, ethylthio, n-propylthio, isopropylthio, etc. 1~6 The "alkylthio" etc. have a similar explanation, except that the number of carbon atoms is different.

[0099] The "halogen" includes any one or two or more of fluorine, chlorine, bromine and iodine.

[0100] “C 6~30 The term "aryl" refers to an all-carbon monocyclic or fused polycyclic group having a completely conjugated π electron system. It refers to an all-carbon monocyclic or fused polycyclic group of 6 to 30 carbon atoms; for example, benzene, naphthalene, indene, fluorene, etc.

[0101] If there is no special explanation, the actual meaning of “about” in the present invention is that the error is allowed to be within the range of ±2%, for example, about 100 is actually 100±2%×100.

[0102] Unless otherwise specified, “between” in the present invention includes the number itself, for example, “between 2 and 3” includes the endpoint values ​​2 and 3.

[0103] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0104] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0105] Figure 1 is a schematic structural diagram of a perovskite solar cell in Application Example 1 of the present invention;

[0106] Figure 2 It is a UV-visible spectrum curve diagram of the bifunctional self-assembled hole transport material obtained in Examples 1 and 2 of the present invention;

[0107] Figure 3 It is a UV-visible spectrum curve diagram of the bifunctional self-assembled hole transport material obtained in Examples 3 to 4 of the present invention;

[0108] Figure 4 It is a JV curve diagram of some perovskite solar cells obtained in Application Example 1 of the present invention. DETAILED DESCRIPTION

[0109] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.

[0110] In the description of the present invention, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0111] If there is no special explanation, the temperature in the specific implementation mode is room temperature, that is, in the range of 20 to 30° C., and fluctuation within this range will not have a significant impact on the test results.

[0112] If the experimental method of specific conditions is not indicated in the specific implementation mode, it is usually based on the conventional conditions in the art or the conditions recommended by the manufacturer.

[0113] Unless otherwise specified, the raw materials and reagents used are all commercially available from conventional markets.

[0114] ITO glass: purchased from Liaoning Youxuan Technology Co., Ltd., using indium tin oxide (ITO) glass with a resistance of 15Ω / sq, including a base glass and an ITO layer arranged on the surface of the base glass, wherein the ITO layer thickness is 150nm and the base glass thickness is 1.1mm.

[0115] Example 1

[0116] In this example, a bifunctional self-assembled hole transport material was prepared. The specific reaction mechanism is shown in the following formula:

[0117]

[0118] The specific steps are as follows:

[0119] S1. Preparation of the compound of formula II-1: Add the compound of formula III-1 (2 g, 10.20 mmol, CAS: 90-47-1) and diethyl cyanomethyl phosphate (5.9 g, 33 mmol, CAS: 2537-48-6) to a 100 mL round-bottom flask equipped with a stirring bar, then add 40 mL of dichloromethane (DCM for short), and then add 4 mL of titanium tetrachloride (TiCl4 for short) dropwise into the round-bottom flask, and then add 4 mL of Et3N (triethylamine) (the two are mixed as an organic base TiCl4 / Et3N), and react at room temperature (set temperature is about 30°C) for 12 hours.

[0120] The obtained reaction mixture was cooled to room temperature, the solvent was removed by rotary evaporation, extracted with dichloromethane, dried, and separated and purified by rotary column chromatography (the eluent was a mixture of dichloromethane and petroleum ether, wherein the volume ratio of dichloromethane to petroleum ether was 3:1). Finally, the compound represented by formula II-1 (3.11 g, yield 86%) was obtained.

[0121] The compound of formula II-1 obtained in this example was characterized by nuclear magnetic resonance, and the results were as follows:

[0122] 1 H NMR (400MHz, CDCl3) δ8.47(ddd,J=20.8,8.1,1.4Hz,2H),7.66–7.48(m,2H),7.43–7.22(m,4H),4.12(dd,J=7.6,6.5Hz,4H),1.30–1.19(m,6H).

[0123] 13 C NMR (101MHz, CDCl3) δ154.93,152.25,152.08,133.01,132.67,129.52,126.84,123.83 ,121.31,121.15,120.07,118.45,116.96,116.48,93.40,63.78,63.72,16.02,15.96.

[0124] S2. Synthesis of the compound shown in formula I-3: Add the compound shown in formula II-1 (2 g, 5.63 mmol) to a 100 mL Schlenk reaction bottle and replace the gas with argon three times, then inject dichloromethane (40 mL) into the reaction bottle. Slowly add trimethylsilyl bromide (2 mL, 15.16 mmol, CAS: 2857-97-8, referred to as BrSiMe3) to the reaction bottle at room temperature, and stir the reaction for 12 h at room temperature. The reaction was stopped after TLC monitoring.

[0125] The obtained reaction solution was directly dried using a vacuum rotary evaporator and recrystallized with 50 mL of a mixture of dichloromethane and methanol (the volume ratio of dichloromethane to methanol was 2:1) to obtain a compound of formula I-3. The product was shown to be a light yellow powder (1.51 g, yield 90%).

[0126] The compound represented by formula I-3 was characterized by nuclear magnetic resonance and mass spectrometry, and the data statistics are as follows:

[0127] 1 H NMR (400MHz, DMSO) δ8.62(dd,J=8.2,1.4Hz,1H),8.03(dd,J=8.2,1.4Hz,1H),7.65(dddd,J=19.9,8.5,7.2,1.5Hz,2H),7.50–7.32(m,4H).

[0128] 13 C NMR (101MHz, DMSO) δ151.19,150.44,142.93,133.46,133.14,126.04,125.13,124.93,124.55,120.27,119.56,118.48,118.22,117.91,84.41.

[0129] HRMS-ESI(m / z):[M+H] + :(C 15 H 10 NO4P),m / z:calculate:299.2218,found:299.3466.

[0130] Example 2

[0131] In this example, a bifunctional self-assembled hole transport material was prepared. The specific reaction mechanism is shown in the following formula:

[0132]

[0133] S1. Preparation of the compound of formula II-2: A 100mL round-bottom flask equipped with a stirring bar is charged with thioxanthone (2g, 9.43mmol, CAS: 126395-12-8) and diethyl cyanomethylphosphonate (5.83g, 32.95mmol, CAS: 2537-48-6) of formula III-2, and then 40mL of dichloromethane is added, and then 4mL of titanium tetrachloride is added dropwise into the round-bottom flask, and then 4mL of Et3N is added dropwise, and the reaction is carried out at room temperature for 12h.

[0134] The obtained reaction mixture was cooled to room temperature, the solvent was removed by rotary evaporation, extracted with dichloromethane, dried, and separated and purified by rotary column chromatography (the eluent was a mixture of dichloromethane and petroleum ether, wherein the volume ratio of dichloromethane to petroleum ether was 3:1). Finally, the compound represented by formula II-2 (2.94 g, yield 84%) was obtained.

[0135] The product obtained in this step was characterized by nuclear magnetic resonance, and the statistical results are as follows:

[0136] 1 H NMR (400MHz, CDCl3) δ8.22–8.00(m,2H),7.67–7.51(m,2H),7.51–7.32(m,4H),4.02(s,4H),1.17(s,6H).

[0137] 13 C NMR (101MHz, CDCl3) δ162.49,162.42,133.48,133.22,132.46,132.30,131.34,131.29, 129.97,129.84,129.78,128.11,126.72,126.40,126.30,126.17,63.90,15.98,15.91.

[0138] S2. Synthesis of the compound shown in formula I-2: Add the product obtained in step S1 (1 g, 2.93 mmol) to a 100 mL Schlenk reaction bottle in sequence and replace the gas with argon three times, then inject dichloromethane (30 mL) into the reaction bottle. Slowly add trimethylsilyl bromide (1 mL, the same specifications as in Example 1) to the reaction bottle at room temperature, and stir the reaction at room temperature for 12 h. The reaction was stopped after TLC monitoring.

[0139] The reaction solution was directly dried by vacuum rotary evaporator and recrystallized with 50 mL of a mixture of dichloromethane and methanol (the volume ratio of dichloromethane to methanol was 2:1) to obtain a compound of formula I-2. The product was dark brown powder (0.75 g) with a yield of 89%.

[0140] The compound represented by formula I-2 was characterized by nuclear magnetic resonance and mass spectrometry, and the statistical results are as follows:

[0141] 1 H NMR (400MHz, DMSO) δ8.11(d,J=9.2Hz,1H),8.01(dd,J=7.8,1.2Hz,1H),7.87–7.73(m,2H),7.66–7.37(m,4H).

[0142] 13C NMR (101MHz, DMSO) δ152.03,132.45,132.12,131.27,130.68,130.38,129.47,128.37,128.07,127.41,127.01,126.97,126.40,118.94,96.08.

[0143] HRMS-ESI(m / z):[M+H] + :(C 15 H 10 NO3PS),m / z:calculate:315.2828,found:315.5480.

[0144] Example 3

[0145] In this example, a bifunctional self-assembled hole transport material was prepared. The specific reaction mechanism is shown in the following formula:

[0146]

[0147] S1. Preparation of the compound shown in formula II-3: A 100mL round-bottom flask equipped with a stirring bar is charged with 3,6-dimethylanthraquinone (2g, 9.01mmol, CAS: 54159-95-4) shown in formula III-3 and diethyl cyanomethylphosphonate (5.83g, 32.95mmol, CAS: 2537-48-6), and then 40mL of dichloromethane is added, and then 4mL of titanium tetrachloride is added dropwise into the round-bottom flask, and then 4mL of Et3N is added dropwise, and the reaction is carried out at room temperature for 12h.

[0148] The obtained reaction mixture was cooled to room temperature, the solvent was removed by rotary evaporation, extracted with dichloromethane, dried, and separated and purified by rotary column chromatography (the eluent was a mixture of dichloromethane and petroleum ether, wherein the volume ratio of dichloromethane to petroleum ether was 3:1). Finally, the compound represented by formula II-3 (2.65 g, yield 77%) was obtained.

[0149] S2. Synthesis of the compound shown in formula I-4: Add the product obtained in step S1 (1 g, 2.60 mmol) to a 100 mL Schlenk reaction bottle in sequence and replace the gas with argon three times, then inject dichloromethane (30 mL) into the reaction bottle. Slowly add trimethylsilyl bromide (1 mL, the same specifications as in Example 1) to the reaction bottle at room temperature, and stir the reaction at room temperature for 12 h. The reaction was stopped after TLC monitoring.

[0150] The reaction solution was directly dried by vacuum rotary evaporator and recrystallized with 50 mL of a mixture of dichloromethane and methanol (the volume ratio of dichloromethane to methanol was 2:1) to obtain a compound of formula I-4, the product having the appearance of dark brown powder (0.75 g) and a yield of 85%.

[0151] The compound represented by formula I-2 was characterized by nuclear magnetic resonance and mass spectrometry, and the statistical results are as follows:

[0152] 1 H NMR (400MHz, DMSO) δ7.58 (d, J = 9.2 Hz, 1H), 7.42 (dd, J = 7.8, 1.2 Hz, 1H), 7.11–7.18 (m, 2H), 7.01–7.08 (m, 2H), 4.80 (s, 2H), 3.28 (s, 6H).

[0153] 13 C NMR(101MHz,DMSO)δ173.91,138.19,136.48,131.27,131.08,130.38,129.47,128 .37,128.07,127.41,127.01,126.97,126.40,117.24,89.08,38.43,21.62,21.80.

[0154] HRMS-ESI(m / z):[M+H] + :(C 18 H 16 NO3P),m / z:calculate:325.3038,found:326.1480.

[0155] Example 4

[0156] In this example, a bifunctional self-assembled hole transport material was prepared. The specific reaction mechanism is shown in the following formula:

[0157]

[0158] S1. Preparation of the compound shown in formula II-4: A 100mL round-bottom flask equipped with a stirring bar is charged with 3,6-diphenylthioxanthone (2g, 5.74mmol, CAS: 854661-66-8) shown in formula III-4 and diethyl cyanomethylphosphonate (5.83g, 17.24mmol, CAS: 2537-48-6), and then 40mL of dichloromethane is added, and then 4mL of titanium tetrachloride is added dropwise into the round-bottom flask, and then 4mL of Et3N is added dropwise, and the reaction is carried out at room temperature for 12h.

[0159] The obtained reaction mixture was cooled to room temperature, the solvent was removed by rotary evaporation, extracted with dichloromethane, dried, and separated and purified by rotary column chromatography (the eluent was a mixture of dichloromethane and petroleum ether, wherein the volume ratio of dichloromethane to petroleum ether was 3:1). Finally, the compound represented by formula II-2 (2.35 g, yield 81%) was obtained.

[0160] S2. Synthesis of the compound shown in formula I-15: Add the product obtained in step S1 (1 g, 1.97 mmol) to a 100 mL Schlenk reaction bottle in sequence and replace the gas with argon three times, then inject dichloromethane (30 mL) into the reaction bottle. Slowly add trimethylsilyl bromide (1 mL) to the reaction bottle at room temperature, and stir the reaction at room temperature for 12 hours. The reaction is stopped after TLC monitoring.

[0161] The reaction solution was directly dried by vacuum rotary evaporator and recrystallized with 50 mL of a mixture of dichloromethane and methanol (the volume ratio of dichloromethane to methanol was 2:1) to obtain a compound of formula I-15, the product having the appearance of dark brown powder (0.68 g) and a yield of 88%.

[0162] The compound represented by formula I-15 was characterized by nuclear magnetic resonance and mass spectrometry, and the statistical results are as follows:

[0163] 1 H NMR (400MHz, DMSO) δ7.71-7.75 (d, J=6.2Hz, 4H), δ7.49-7.51 (d, J=7.8Hz, 4H), δ7.48 ( d,J=9.8Hz,2H), δ7.40(d,J=7.4Hz,2H),7.31(d,J=9.2Hz,2H),7.28(d,J=6.8Hz,2H),

[0164] 13 C NMR (101MHz, DMSO) δ173.95,152.21,152.17,144.61,140.67,140.91,140.89,131.27,131.08,129.31,129.25,127.67,1 27.61,127.59,127.56,127.51,127.47,126.52,126.40,120.59,120.62,117.2,115.01,115.04,114.82,114.76,89.08.

[0165] HRMS-ESI(m / z):[M+H] + :(C 27 H 18NO4P),m / z:calculate:451.4178,found:452.2387.

[0166] Application Example 1

[0167] refer to Figure 1 This example provides a perovskite solar cell with an inverted planar structure. The perovskite solar cell provided in this example includes a substrate (ITO glass, referred to as ITO substrate), a hole transport layer (HTM, monomolecular layer, thickness of 10nm), a perovskite material layer (referred to as perovskite layer, thickness of 700nm), an electron transport layer (including C60 layer and BCP layer, total thickness of 25nm) and a metal electrode (Cu, thickness of 100nm) which are stacked in sequence. The preparation process includes:

[0168] The ITO conductive glass (including the ITO coating) was ultrasonically cleaned for 30 min using alkaline glass cleaning agent, deionized water, acetone and isopropanol in sequence. After drying with nitrogen, the ITO glass was plasma cleaned for 15 min.

[0169] The hole transport layer was prepared using the bifunctional self-assembled hole transport materials (Formula I-3, Formula I-2, Formula I-4 and Formula I-15) obtained in Examples 1 to 4, and the bifunctional self-assembled hole transport materials shown in Formula V (CAS: 6048-49-3) and Formula VI (CAS: 6788-63-2) as raw materials:

[0170]

[0171] The specific preparation steps of the hole transport layer are as follows: spin coating a methanol solution (2 mg / mL) of a bifunctional self-assembled hole transport material on the ITO coating surface of the ITO glass at a speed of 4000 rpm, followed by thermal annealing at 100° C. for 10 min to form a hole transport layer.

[0172] 1.5 mol / L Cs 0.05 (FA 0.9 MA 0.1 ) 0.95 The PbI3 perovskite solution is spin-coated onto the surface of the hole transport layer material and thermally annealed at 100°C for 30 minutes. After cooling, a perovskite material layer is formed.

[0173] A 20nm C60 layer and a 5nm BCP (2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline) layer were evaporated on the surface of the perovskite material layer to form an electron transport layer.

[0174] Finally, a layer of 80nm Cu was vacuum evaporated on the surface of the electron transport layer as an electrode, thus completing the preparation of the perovskite solar cell device;

[0175] The effective area of ​​the perovskite solar cell obtained in this example is 4mm 2 .

[0176] Application Example 2

[0177] This example discloses a large-area perovskite solar cell module, which differs from Application Example 1 only in that the thickness of the final perovskite material layer is 600nm and the effective area of ​​the device is 100cm 2 Large-area perovskite solar cell module.

[0178] Test Case

[0179] This example performs performance tests on the bifunctional self-assembled hole transport material obtained in the embodiment, the perovskite solar cell obtained in the application example, and the corresponding module, specifically including:

[0180] (1) The optical properties of the bifunctional self-assembled hole transport materials obtained in Examples 1 to 4 were studied by using UV-visible spectroscopy. The UV-visible spectroscopy test included: testing with a 1 g / mL methanol solution of the bifunctional self-assembled hole transport material, and the measured UV-visible spectral curve was as follows: Figures 2-3 As shown, the absorption peak of the bifunctional self-assembled hole transport material obtained in Example 1 is near 331nm, and the absorption sideband is 381nm; the absorption peak of the bifunctional self-assembled hole transport material obtained in Example 2 is near 342nm, and the absorption sideband is 402nm; the absorption peak of the bifunctional self-assembled hole transport material obtained in Example 3 is near 335nm, and the absorption sideband is 378nm; the absorption peak of the bifunctional self-assembled hole transport material obtained in Example 4 is near 351nm, and the absorption sideband is 396nm; according to the formula: Egap=1240 / λ, the optical band gap of the bifunctional self-assembled hole transport material obtained in Example 1 is calculated to be 3.25eV; the optical band gap of the bifunctional self-assembled hole transport material obtained in Example 2 is 3.08eV, and the optical band gap of the bifunctional self-assembled hole transport material obtained in Example 3 is 3.28eV; the optical band gap of the bifunctional self-assembled hole transport material obtained in Example 4 is 3.13eV.

[0181] (2) The electrochemical properties of the bifunctional self-assembled hole transport materials obtained in Examples 1 to 4 were studied by cyclic voltammetry. During the test, the bifunctional self-assembled hole transport material was coated on a working electrode. The electrochemical properties were tested by cyclic voltammetry, including: using a 1 mol / L ethanol solution of tetrabutylammonium hexafluorophosphate as an electrolyte for cyclic voltammetry testing at a scan rate of 10 mV / s. Ferrocene was used as an external standard reference;

[0182] It is calculated that the HOMO energy level of the bifunctional self-assembled hole transport material obtained in Example 1 is -5.13eV. The HOMO energy level of the bifunctional self-assembled hole transport material obtained in Example 2 is -5.22eV, and the HOMO energy level of the bifunctional self-assembled hole transport material obtained in Example 3 is -5.15eV. The HOMO energy level of the bifunctional self-assembled hole transport material obtained in Example 4 is -5.24eV. ​​The HOMO energy level of the bifunctional self-assembled hole transport material obtained in Examples 1 to 4 matches the HOMO energy level of perovskite (-5.48eV), satisfying the conditions for it to work as a hole transport layer in a perovskite solar cell device.

[0183] (3) Use a xenon lamp solar simulator and test the light source intensity to 100mW / cm 2 The open circuit voltage V of the perovskite solar cell obtained under AM1.5G simulated sunlight corresponding to Example 1 oc , short circuit current density J sc , fill factor FF and photoelectric energy conversion efficiency PCE were tested, and the test results are as follows Figure 4 As shown in Table 1:

[0184] Table 1 Performance results of perovskite solar cells obtained in Application Example 1

[0185] Bifunctional self-assembled hole transport materials <![CDATA[J sc (mA / cm 2 )]]> <![CDATA[V oc (V)]]> FF(%) PCE(%) Formula I-3 24.00 1.16 84.47 23.78 Formula I-2 24.68 1.17 83.51 23.96 Formula I-4 24.27 1.16 84.35 23.56 Formula I-15 24.38 1.16 83.56 23.28 Formula V 23.69 1.03 80.62 20.03 Formula VI 23.95 1.05 83.46 20.82

[0186] According to the above results, the perovskite solar cell using the bifunctional self-assembled hole transport material provided by the present invention has excellent performance. If the hole transport material shown in Formula V to Formula VI is used, although its structure is similar to the structure of the bifunctional self-assembled hole transport material provided by the present invention, its overall performance is significantly reduced; the reason is that the bifunctional self-assembled hole transport material shown in Formula V to Formula VI does not include phosphate, does not have an amphiphilic structure, and cannot produce an anchoring effect with the base, and its stability, self-assembly performance and interface contact are all reduced.

[0187] (4) This example also tests the performance of the perovskite solar cell module obtained in Application Example 2. From the current-voltage curve of the module, it is found that the open circuit voltage is 11.89 V and the short circuit current density is 2.21 mA / cm 2 , the filling factor is 74.04%, and the photoelectric energy conversion efficiency is 19.43%.

[0188] In summary, the present invention provides a class of amphiphilic bifunctional self-assembled hole transport materials that can self-assemble to form a monolayer. The bifunctional self-assembled hole transport material has interface passivation. The bifunctional self-assembled hole transport material has an anthracene heterocyclic derivative with a rigid conjugated plane as a parent core, which gives the bifunctional self-assembled hole transport material high hole transport performance and air stability; at the same time, it has π-π stacking between single molecules, which is beneficial to the transmission of holes; cyanophosphonic acid is an anchoring group to achieve complete coverage and bonding of the self-assembled bifunctional self-assembled hole transport material on the substrate surface. Furthermore, in the bifunctional self-assembled hole transport material provided by the present invention, anthrone, xanthene, thioanthene core and the like provide the main transport performance, cyanophosphonic acid plays an anchoring role, and the methyl, methoxy, methylthio, phenyl and other side chains on the core play a role in regulating the energy level; based on the fact that the present invention has proved that anthrone, xanthene, and thioanthene cores can all play a transport role, it can be reasonably predicted that all the bifunctional self-assembled hole transport materials provided by the present invention have relatively excellent transport effects, and are expected to be widely used in photovoltaic devices after being matched with suitable perovskite materials.

[0189] The preparation method of the bifunctional self-assembled hole transport material provided by the present invention has simple synthesis steps, mild synthesis conditions, low cost of substrates and catalysts, simple post-treatment, and a simple synthesis and purification process is adopted to obtain the target bifunctional self-assembled hole transport material with high yield (high yield of target product). The amphiphilic monolayer bifunctional self-assembled hole transport material of the synthesized anthracene heterocyclic derivative is used for the self-assembled hole transport material of the trans-perovskite solar cell, and the energy conversion efficiency of the device PCE of more than 23% can be obtained without doping. The obtained bifunctional self-assembled hole transport material has an interface passivation performance, anchoring metal oxides and ITO glass, which can improve the photoelectric conversion efficiency of the battery while improving the battery life, and is suitable for large-area perovskite solar device modules, and can obtain high photoelectric conversion efficiency. Therefore, the bifunctional self-assembled hole transport material of the present invention promotes charge transfer as a bifunctional self-assembled hole transport material of the trans-perovskite solar cell, and improves the energy conversion efficiency and stability of the solar cell.

[0190] The embodiments of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

Claims

1. A bifunctional self-assembled hole transport material, characterized in that: The bifunctional self-assembled hole transport material includes a compound as shown in Formula I: wherein X is selected from CH2, S or O; R1 to R2 are independently selected from H, substituted C 1~30 Alkyl, unsubstituted C 1~30 Alkyl, substituted C 1~30 Alkoxy, unsubstituted C 1~30 Alkoxy, substituted C 1~30 Alkylthio, unsubstituted C 1~30 Alkylthio, substituted C 6~30 Aryl and unsubstituted C 6~30 One of the aromatic groups.

2. The bifunctional self-assembled hole transport material according to claim 1, characterized in that: In the compound represented by formula I, R1 to R2 are independently selected from H, substituted C 1~6 Alkyl, unsubstituted C 1~6 Alkyl, substituted C 1~6 Alkoxy, unsubstituted C 1~6 Alkoxy, substituted C 1~6 Alkylthio, unsubstituted C 1~6 One of an alkylthio group, a substituted phenyl group and an unsubstituted phenyl group.

3. The bifunctional self-assembled hole transport material according to claim 1 or 2, characterized in that: The bifunctional self-assembled hole transport material comprises at least one of the compounds shown in chemical formulae I-1 to I-15:

4. A method for preparing a bifunctional self-assembled hole transport material as claimed in any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: S1. Knoevenagel condensation reaction of the compound represented by formula III with the cyanomethyl phosphate compound represented by formula IV to obtain a compound represented by formula II; S2. subjecting the compound represented by formula II to a hydrolysis reaction; Wherein R3 and R4 are independently selected from substituted C 1~10 Alkyl or unsubstituted C 1~10 alkyl.

5. The preparation method according to claim 4, characterized in that: In step S2, the hydrolysis reaction comprises reacting the compound represented by formula II with trimethylhalosilane; and / or the trimethylhalosilane is selected from at least one of trimethylchlorosilane, trimethylbromosilane and trimethyliodosilane.

6. The preparation method according to claim 5, characterized in that: The molar ratio of the trimethylhalosilane to the compound represented by formula II is (0.5-5):

1.

7. The preparation method according to claim 4, characterized in that: In step S2, the temperature of the hydrolysis reaction is 15 to 40°C; and / or, in step S2, the duration of the hydrolysis reaction is 5 to 30 hours.

8. The preparation method according to claim 4, characterized in that: In step S1, the Knoevenagel condensation reaction is carried out under the action of an organic base; and / or the organic base includes at least one of piperidine, pyridine, triethylamine and TiCl4 / Et3N.

9. A hole transport layer, characterized in that: The raw material for preparing the hole transport layer includes the bifunctional self-assembled hole transport material according to any one of claims 1 to 3.

10. A photovoltaic device, characterized in that: The photovoltaic device comprises the hole transport layer as claimed in claim 9; and / or, the raw materials for preparing the photovoltaic device comprise the bifunctional self-assembled hole transport material as claimed in any one of claims 1 to 3.