Water-based colorant for dust suppression as well as preparation method and application thereof
By using compound pigments of phthalocyanine green and iron oxide green and other additives in the colorant, the problems of poor color development performance and insufficient stability of the colorant in the existing technology are solved, and the control of landfill materials is realized. The effective coloring and rain erosion resistance are improved, which reduces the cost.
Patent Information
- Application Number
- CN202411015980.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-10-01
AI Technical Summary
Existing colorant products have problems such as poor coloring performance, instability, poor rain resistance and high cost when used in landfills. In particular, the color development of darker materials is not obvious, and their suspension and dispersion properties are poor. Insufficient water resistance.
A compound pigment of phthalocyanine green and iron oxide green is used as the main pigment, combined with rheological aids, thickening suspending agents, surfactants and defoaming agents, and the proportion of each component is controlled to prepare a water-based dust suppressor. The colorant is stirred and ground to form a stable compound system, which is used to spray on the surface of the dust residue to achieve dust suppression and coloring.
It improves the hiding power, stability and rain erosion resistance of the colorant, reduces the cost, ensures the viscosity and suspension of the colorant, and has a significant color development effect, and is suitable for different types of landfill materials.
Smart Images

Figure BDA0004965668010000171 
Figure BDA0004965668010000182 
Figure BDA0004965668010000191
Abstract
Description
Technical Field
[0001] The invention relates to the field of dust suppressants, and in particular to a water-based dust suppressant colorant and a preparation method and application thereof. Background Art
[0002] Various types of landfills are prone to serious dust pollution when encountering strong winds. The current dust suppression methods mainly include covering with dust nets and spraying dust suppressant products. Due to the poor quality of existing dust nets and their easy weathering, they need to be covered with nets for reinforcement from time to time. The non-naturally degradable nature of dust nets will cause a large amount of plastic to be introduced into the landfill, which is prone to secondary pollution. In addition, due to the high height of the material landfill, the dust nets cannot be recycled, which will lead to high dust suppression costs. Now, the spraying of dust suppressants has been gradually promoted to replace the dust suppression method of covering with nets.
[0003] Dust suppressant products have excellent dust suppression performance, long dust suppression cycle, and wide application scenarios. In order to comply with environmental protection requirements and facilitate subsequent operation and maintenance management, dust suppressants are usually combined with colorants to control dust pollution. The following are several colorant products:
[0004] CN114958093B reports a water-based organic color paste, which is mainly prepared by organic pigment, dispersant, defoamer and dustproof agent, wherein the dispersant is 2-naphthalenesulfonic acid formaldehyde polymer sodium salt, the defoamer is polydimethylsilane, and the dustproof agent is a mixture of polyurea polymer and N-methylpyrrolidone. The water-based color paste prepared by this formula has better color development ability and dyeability, and solves the problems of color powder sedimentation, stratification, insufficient dyeing power, insufficient weather resistance, etc.
[0005] CN116458598A reports a color paste and its preparation method and application. The invention uses curcumin, Tween 80 and glycerol to mix with modified starch and citric acid aqueous solution, and then adds capsanthin, glycerol and mono- and di-glycerol oleate. The color paste prepared by this formula solves the problems of unstable paste powder, easy fading and dark color after production.
[0006] CN116369460A reports a compound colorant, a color paste mixture, and its preparation method and application, which contain capsanthin, lycopene and an emulsifier. The formula has good coloring stability, and can still maintain a high color difference retention rate after exposure to light, repeated freezing and thawing, and boiling in water. It is easy to apply and the coloring is uniform and stable.
[0007] However, there are many problems with existing colorant products, such as high pigment content in color fillers, resulting in high cost of colorant products; poor suspension and dispersion of pigments, easy sedimentation and stratification, resulting in poor coloring performance; insufficient viscosity of colorants leads to the deposition of components with higher density, making colorant products unstable and poor in resistance to rain erosion. In addition, there are still deficiencies in the research on the actual production application of existing coloring dust suppression products. The coloring performance of existing commercially available products applied to landfills of different materials was investigated and it was found that the coloring performance was acceptable for lighter materials such as fly ash and loess, but the coloring was not obvious for darker materials such as coal and gasified slag. At the same time, its water resistance is poor, and the coloring degree decreases significantly after being washed by rain.
[0008] In short, the current domestic research on the actual production application of colorants is not perfect in terms of the addition ratio of pigments, the suspension and dispersion of pigments, and the color rendering of colorant products. There are no reports on the ratio of colorants to dust suppressants and the spraying method on landfills. Based on this, it is urgent to develop a water-based dust suppression colorant compound dust suppressant product with low cost, stable system, good colorability, and erosion resistance to overcome the defects in the existing technology and solve the dust problem in the storage and transportation of various landfills. Summary of the invention
[0009] The main purpose of the present invention is to provide a water-based dust suppression colorant to solve the problems of poor coloring performance, product instability, poor resistance to rain erosion, high cost and the like of colorant products in this field in the prior art.
[0010] In order to achieve the above-mentioned purpose, the present invention provides a water-based dust suppression colorant, which comprises, by weight percentage: 30-50% of color fillers, 8-20% of rheological additives, 3-15% of thickening suspending agents, 1-5% of surfactants, 0.5-1% of defoaming agents, 0.05-1% of preservatives, and the balance is water; the color fillers comprise pigments and fillers, wherein the pigment is a composite pigment of phthalocyanine green and iron oxide green.
[0011] Furthermore, the filler is one or more of barium sulfate, calcium carbonate, silicon dioxide, calcium sulfate and calcium silicate; preferably, the weight ratio of the pigment to the filler is (8-15):(22-35); more preferably, the weight ratio of the pigment to the filler is (10-15):(20-35); preferably, the weight ratio of phthalocyanine green and iron oxide green in the pigment is 1:(2-3.5).
[0012] Furthermore, the water-based dust suppression colorant includes, by weight percentage: 30-50% pigments and fillers, 10-18% rheological additives, 5-12% thickening and suspending agents, 1-3% surfactants, 0.5-1% defoaming agents, 0.1-0.5% preservatives, and the balance is water; preferably, 30-50% pigments and fillers, 10-15% rheological additives, 5-10% thickening and suspending agents, 1-3% surfactants, 0.5-1% defoaming agents, 0.1-0.5% preservatives, and the balance is water.
[0013] Further, the thickening suspending agent is one or more of cellulose ether, alginate, and polyvinyl alcohol; preferably, the thickening suspending agent is a mixture of alginate, cellulose ether, and polyvinyl alcohol; more preferably, by weight percentage, the content of cellulose ether in the thickening suspending agent is 5-25%, the content of polyvinyl alcohol is 1-5%, and the balance is alginate; further preferably, the content of cellulose ether is 5-15%; preferably, the cellulose ether is one or more of methyl cellulose, ethyl cellulose, carboxymethyl cellulose, hydroxypropyl methyl cellulose, and benzyl cellulose; more preferably, the alginate is sodium alginate and / or potassium alginate.
[0014] Furthermore, the rheological additive is an inorganic silicate clay; preferably, the inorganic silicate clay is one or more of kaolin, montmorillonite, bentonite, sepiolite, attapulgite and diatomaceous earth.
[0015] Furthermore, the surfactant is a nonionic surfactant and / or an anionic surfactant; preferably, the nonionic surfactant and the anionic surfactant are used in combination; preferably, the nonionic surfactant is an alkylphenol polyoxyethylene ether; further preferably, the alkylphenol polyoxyethylene ether is octylphenol polyoxyethylene ether and / or nonylphenol polyoxyethylene ether; preferably, the anionic surfactant is isopropylamine dodecylbenzenesulfonate and / or sodium p-methoxy fatty amide benzenesulfonate; preferably, the defoamer is a polyether-modified silicone defoamer; further preferably, the polyether-modified silicone defoamer is a polyether-modified trisiloxane and / or a polyether-modified heptamethyl trisiloxane.
[0016] Furthermore, the preservative is a compound preservative of ethylene glycol and at least one of the following: chlorphenesin, phenoxyethanol, benzyl alcohol, chlorphenesin; preferably, the content of ethylene glycol in the preservative is 0.5-2% by weight.
[0017] According to another aspect of the present invention, there is also provided a method for preparing a water-based dust suppression colorant, the preparation method comprising the following steps: S1, stirring and mixing water, a surfactant, a thickening suspending agent, a defoaming agent and a rheological additive to obtain a premixed solution; S2, adding a pigment filler to the premixed solution, stirring and grinding to obtain a grinding slurry; S3, adding a preservative to the grinding slurry, and mixing to obtain a water-based dust suppression colorant.
[0018] Furthermore, the stirring speed in step S1 is controlled to be 1400-2000 rpm, and the mixing time is 10-30 min; and / or, the stirring speed in step S2 is controlled to be 500-800 rpm, the grinding time is 20-40 min, and the fineness of the grinding slurry is ≤50 μm; preferably, the fineness of the grinding slurry is controlled to be ≤20 μm; more preferably, the fineness of the grinding slurry is controlled to be ≤5 μm.
[0019] According to another aspect of the present invention, there is also provided a method for using the above-mentioned aqueous dust suppression colorant to treat the surface of dust residue for dust suppression, and the aqueous dust suppression colorant is used to treat the surface of dust residue for dust suppression in one of the following two spraying methods: Method 1: spraying the aqueous dust suppression colorant and the dust suppressant on the surface of the dust residue at the same time; Method 2: first spraying the dust suppressant on the surface of the dust residue, and then spraying the aqueous dust suppression colorant.
[0020] The water-based dust suppression colorant provided by the present invention uses a composite pigment of phthalocyanine green and iron oxide green, which effectively improves the bluish color phenomenon of the iron oxide green product used alone, and the base filler is added in combination to improve the hiding power and storage stability of the colorant, enhance the brightness of the colorant, and further reduce the cost of the pigment. In addition, the present invention uses components such as pigments, fillers, rheological additives, thickening suspending agents, surfactants, defoamers, etc. at the same time, and strictly controls the proportion of the components, while reducing the cost of the pigment, so that the synergistic effect between the components can be fully exerted, and the compatibility of the components in the colorant product is also improved, the viscosity of the colorant product is increased, and the coloring, stability, and rainwater scouring resistance of the colorant product are improved, so that the water-based dust suppression colorant has the advantages of low cost, stable system, good coloring, and scouring resistance. DETAILED DESCRIPTION
[0021] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.
[0022] As described in the background technology section of the present invention, spraying dust suppressants is an important means to solve the dust pollution problem in landfills. The use of dust suppressants and colorants to treat dust pollution is, on the one hand, to comply with environmental protection requirements, and on the other hand, to facilitate subsequent operation and maintenance management. However, the high proportion of existing colorants and pigments added will lead to a correspondingly high product cost. There are also problems such as poor coloring performance of colorant products due to poor suspension and dispersion of pigments, as well as instability of colorant products and poor resistance to rainwater erosion. In addition, there have been no reports on the compounding ratio of colorants and dust suppressants and the spraying method for landfills.
[0023] In order to solve the above problems, the present invention provides a water-based dust suppression colorant and a preparation method thereof. The water-based dust suppression colorant comprises: 30-50% of pigments and fillers, 8-20% of rheological additives, 3-15% of thickening suspending agents, 1-5% of surfactants, 0.5-1% of defoaming agents, 0.05-1% of preservatives, and the balance is water; the above-mentioned pigments and fillers comprise pigments and fillers, wherein the pigment is a composite pigment of phthalocyanine green and iron oxide green.
[0024] The color filler of the present invention includes a pigment and a filler, and in particular, a composite pigment of phthalocyanine green and iron oxide green is used to replace the traditional chromium oxide green pigment. First, the pigment in the present invention has a non-toxic characteristic, which ensures the safety and environmental protection of the colorant; second, the phthalocyanine green pigment also has the characteristics of good transparency, good light resistance, and excellent coloring performance, which can effectively solve the problem of bluish color when using iron oxide green alone for coloring, and make the colorant present a bright dark green color. At the same time, it is precisely because of the use of the above-mentioned composite pigment that the colorant of the present invention can achieve good coloring performance without adding too much pigment, which is beneficial to reducing costs on the one hand, and on the other hand, it also has a good improvement on the stability of the colorant. In addition, the use of a base filler in the colorant with a pigment compound can further improve the hiding power of the pigment and the stability of the storage process, and enhance the brightness of the colorant.
[0025] In addition, the present invention adds rheological additives, thickening suspending agents, surfactants and defoaming agents in combination with the above-mentioned special pigments and fillers, and controls the dosage of each component within the above-mentioned range, which can effectively regulate the viscosity, suspension, dispersion uniformity, etc. of the colorant system, maximize the coordination of the effects of each component, have better synergistic effects, promote good compatibility between the various components of the colorant, stable system, good coloring, and erosion resistance, so that it can be better applied to landfill sites to solve dust pollution problems.
[0026] In a preferred embodiment, the filler in the above-mentioned color filler is one or more of barium sulfate, calcium carbonate, silicon dioxide, calcium sulfate and calcium silicate. The above-mentioned inorganic filler is cheaper than the pigment, and when compounded with the pigment, the cost of the colorant can be reduced as a whole. In addition, compounding the pigment with the filler as the base can improve the hiding power of the pigment, and can also make the colorant have better stability during storage, and is not easy to settle and stratify. Preferably, when the weight ratio of the pigment and the filler is controlled to (8-15): (22-35), a good coloring effect can be achieved, and at the same time, controlling the amount of the pigment can further reduce the cost of the water-based dust suppression colorant; further preferably, when the weight ratio of the pigment and the filler is controlled to (10-15): (20-35), the coloring effect of the colorant is better. In order to further improve the coloring performance of the colorant, in a preferred embodiment, the weight ratio of phthalocyanine green and iron oxide green in the pigment is 1: (2-3.5). Using them together at this ratio can more effectively avoid the problem of bluish color when using iron oxide green alone, so that the colorant presents better coloring properties. When the two fillers are mixed and used, any mixing ratio is acceptable.
[0027] In a preferred embodiment, the water-based dust suppression colorant includes: 30-50% of pigments and fillers, 10-18% of rheological additives, 5-12% of thickening and suspending agents, 1-3% of surfactants, 0.5-1% of defoaming agents, 0.1-0.5% of preservatives, and the balance is water. Rheological additives, thickening and suspending agents, and surfactants will affect the stability of the water-based dust suppression colorant. Each component within this range can better play a synergistic role, so that the water-based dust suppression colorant has better material compatibility, stability, coloring, scouring resistance and other properties. Preservatives can improve the antibacterial and mildew-proof effects of the water-based dust suppression colorant.
[0028] Further preferably, the water-based dust suppression colorant comprises: 30-50% of pigment filler, 10-15% of rheological additive, 5-10% of thickening suspending agent, 1-3% of surfactant, 0.5-1% of defoaming agent, 0.1-0.5% of preservative, and the balance is water. Controlling the content of each component within this range will make the synergistic effect of each component better, and can further improve the comprehensive performance of the colorant.
[0029] In order to further improve the stability of the water-based dust suppression colorant, in a preferred embodiment, the thickening suspending agent is one or more of cellulose ether, alginate, and polyvinyl alcohol. The thickening suspending agent can increase the viscosity between the various components in the colorant product, improve the suspension and dispersion characteristics of each component, and make the pigment difficult to settle and stratify. In a preferred embodiment, the thickening suspending agent is a mixture of alginate, cellulose ether, and polyvinyl alcohol. In this way, the thickening suspending agent selects cellulose ether and alginate for compounding, and the two can be combined by intermolecular electrostatic attraction, so that they have good compatibility. In addition, the two can synergistically play a hygroscopic and bonding role, increase the viscosity of the colorant to make it present a suspended state, and then by compounding with polyvinyl alcohol, the excellent film-forming properties of polyvinyl alcohol can be further exerted, so that the ductility of the product is increased. Based on the above reasons, after the obtained water-based dust suppression colorant and dust suppressant are compounded and sprayed on the surface of dust residue, it can effectively prevent its brittle fracture failure, and its excellent water retention effect can more significantly enhance the product's anti-rainwater scouring characteristics.
[0030] Further preferably, in terms of weight percentage, the proportion of cellulose ether in the thickening suspending agent is 5-25%, the proportion of polyvinyl alcohol is 1-5%, and the balance is alginate. Cellulose ether, polyvinyl alcohol and alginate are different types of thickening suspending agents, and each of them can play a role in regulating the viscosity of the product liquid. However, mixing the three and controlling the ratio of the three within the above range can, while playing the role of regulating viscosity, improve the compatibility between the thickening suspending agent itself and with other components in the colorant on the one hand; on the other hand, within the above range, the three can cooperate with each other and further exert the hygroscopic effect, bonding effect and film-forming performance of the three components, which has a further promoting effect on improving the stability of the water-based dust suppression colorant. More preferably, when the above-mentioned cellulose ether accounts for 5-15%, the effect is better.
[0031] In a preferred embodiment, the cellulose ether includes, but is not limited to, one or more of methyl cellulose, ethyl cellulose, carboxymethyl cellulose, hydroxypropyl methyl cellulose, and benzyl cellulose. The cellulose ether and alginate are selected to be compounded so that the two can be better combined under the action of intermolecular electrostatic attraction, further improving their compatibility and thus improving the stability of the colorant. The alginate includes, but is not limited to, sodium alginate and / or potassium alginate.
[0032] In order to further improve the stability of the water-based dust suppression colorant, in a preferred embodiment, the rheological additive is an inorganic silicate clay. The rheological additive can adjust the viscosity of the colorant so that the various components in the colorant can be more evenly distributed. Inorganic silicate clay has excellent suspension properties and gelling effects, which can more effectively reduce the sedimentation of denser pigments and fillers in the colorant, and further maintain the stability of the colorant, so that the colorant is not prone to stratification or precipitation during storage and use. Preferably, the inorganic silicate clay is one or more of kaolin, montmorillonite, bentonite, sepiolite, attapulgite, and diatomaceous earth. When two types of inorganic silicate clays are compounded for use, any compounding ratio is acceptable, and it is preferred that the weight ratio of the two is 1: (0.8 to 1.2).
[0033] In a preferred embodiment, the surfactant used in the present invention is a nonionic surfactant and / or an anionic surfactant. Preferably, the nonionic surfactant and the anionic surfactant are used in combination. The combination of the two surfactants can make the pigment and filler better miscible with water, and further improve the uniformity and dispersibility of the colorant system. Preferably, the nonionic surfactant is an alkylphenol polyoxyethylene ether, and further preferably, the alkylphenol polyoxyethylene ether is an octylphenol polyoxyethylene ether and / or a nonylphenol polyoxyethylene ether. Preferably, the anionic surfactant is isopropylamine dodecylbenzenesulfonate and / or sodium p-methoxy fatty amide benzenesulfonate. Alkylphenol polyoxyethylene ether is a nonionic surfactant, and this type of active agent has a good emulsifying and dispersing effect; isopropylamine dodecylbenzenesulfonate and / or sodium p-methoxy fatty amide benzenesulfonate are anionic surfactants that can form hydrophobic anions in water. The combination of the two can further improve the stability of the colorant system. In addition, a good effect can be achieved by controlling the mass ratio of the nonionic surfactant and the anionic surfactant when used in combination to be 1:(0.7-1.5), more preferably (0.9-1.2):1.
[0034] Further preferably, the defoamer in the above-mentioned water-based dust suppression colorant is a polyether-modified silicone defoamer. The use of polyether-modified silicone defoamers has the excellent properties of both silicone defoamers and polyether defoamers, and is non-toxic and non-polluting. Preferably, the polyether-modified silicone defoamer is polyether-modified trisiloxane and / or polyether-modified heptamethyl trisiloxane. Both of the above silicone defoamers have the advantages of fast defoaming speed, excellent ductility and rain erosion resistance, which can further improve the stability and erosion resistance of the colorant.
[0035] In order to improve the comprehensive performance of the water-based dust suppression colorant, in a preferred embodiment, the above-mentioned preservative is one or more of kason, phenoxyethanol, benzyl alcohol, and chlorphenesin compounded with ethylene glycol. The use of kason and / or compounding other types of water-soluble preservatives is low-cost and cost-effective. It is also well soluble in various surfactants and emulsifiers, and only a small amount of addition can achieve antibacterial and mildew-proof effects. Preferably, when the proportion of ethylene glycol in the preservative is 0.5-2% by weight, the preservative and the various components in the system can be better soluble in each other. When two preservatives are compounded for use, any compounding ratio is acceptable, and it is preferred that the mass ratio of the two is within the range of 1: (0.8-1.2).
[0036] In a preferred embodiment, the preparation method of the above-mentioned water-based dust suppression colorant includes the following steps: S1: stirring and mixing water, surfactant, thickening suspending agent, defoaming agent, and rheological additive to obtain a premixed solution; S2: adding color fillers to the premixed solution, stirring and grinding to obtain a grinding slurry; S3: adding a preservative to the grinding slurry, and mixing to obtain a water-based dust suppression colorant.
[0037] Specifically, in step S1, water, surfactant, thickening suspending agent, defoaming agent, and rheological additive are added in sequence at room temperature and under high-speed stirring conditions, and the mixture is stirred and mixed to form a premixed solution; in step S2, pigments and fillers are mixed in proportion, added to the premixed solution formed above, and transferred to a sand mill while being stirred, and after grinding for a period of time, the grinding fineness is tested to obtain a grinding slurry; in step S3, a preservative is added to the grinding slurry, and a water-based dust suppression colorant is obtained after mixing. This method can make the various components mixed more evenly, and the obtained water-based dust suppression colorant has better comprehensive performance.
[0038] The various components in the colorant are mixed evenly, which can make the various components play a better synergistic role. In a preferred embodiment, in the preparation method, the stirring speed in S1 is controlled to be 1400-2000rpm, and the mixing time is 10-30min; and / or, the stirring speed in S2 is controlled to be 500-800rpm, the grinding time is 20-40min, and the fineness of the grinding slurry is ≤50μm. The small fineness of the grinding slurry is conducive to better mixing of the various components and easier to form a stable system. Further preferably, the fineness of the grinding slurry is controlled to be ≤20μm; more preferably, the fineness of the grinding slurry is controlled to be ≤5μm.
[0039] In order to better play the role of the water-based dust suppression colorant in the present invention, in a preferred embodiment, the water-based dust suppression colorant is used to suppress dust on the surface of the dust slag in one of the following two spraying methods: Method 1: spray the water-based dust suppression colorant and the dust suppressant on the surface of the dust slag at the same time. Method 2: first spray the dust suppressant on the surface of the dust slag, and then spray the water-based dust suppression colorant. For slag samples with lighter colors such as fly ash, loess, and desulfurized gypsum, the method of spraying the water-based dust suppression colorant and the dust suppressant on the surface of the dust slag at the same time in method 1 is selected. This spraying method has excellent color development effect for lighter color slag samples and can be sprayed once, which is convenient to use; for samples with darker colors such as gasification slag, boiler slag, and different types of coal, the method 2 is selected to first spray the dust suppressant on the surface of the dust slag, and then spray the water-based dust suppression colorant. This spraying method has a better color development effect for dark slag samples.
[0040] Preferably, in method 1, the dust suppressant is first diluted to an aqueous solution with a mass concentration of 2 to 3.5% by weight, and then an aqueous dust suppressant colorant is added to make its mass concentration 4 to 7.5%, and the spraying amount is 4 to 7 L / m 2 ;
[0041] Preferably, in the second method, according to the weight percentage, the dust suppressant aqueous solution with a mass concentration of 2 to 3.5% is first sprayed, and after the dust suppressant is agglomerated, the aqueous solution of the water-based dust suppression colorant with a mass concentration of 5 to 8% is sprayed, and the spraying amount of the two is controlled to be 2.5 to 4 L / m 2 .
[0042] The dust suppressant may be a type commonly used in the art, for example, a liquid coal dust suppressant.
[0043] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0044] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0045] Example 1
[0046] A method for preparing a colorant product for dust suppression, which includes 35% pigment filler, 5% thickening suspending agent, 12% rheological additive, 1.5% surfactant, 1% defoamer, 0.2% preservative, and the rest is water, by weight percentage. The filler is calcium carbonate, the weight ratio of pigment to filler is 12:28, and the mass ratio of pigment phthalocyanine green to iron oxide green is 1:2.5; the thickening suspending agent is methyl cellulose, sodium alginate and polyvinyl alcohol, wherein the weight proportion of methyl cellulose in the thickening suspending agent is 13%, the weight proportion of polyvinyl alcohol is 3%, and the balance is sodium alginate; the rheological additive is diatomaceous earth; the surfactant is octylphenol polyoxyethylene ether and isopropylamine dodecylbenzenesulfonate, and the mass ratio of the two is 1:1. The defoamer is polyether-modified trisiloxane; the preservative is kason with 1% ethylene glycol content.
[0047] It comprises the following preparation steps:
[0048] Step 1: at room temperature and a stirring speed of 1500 rpm, water, octylphenol polyoxyethylene ether, isopropylamine dodecylbenzenesulfonate, methyl cellulose, sodium alginate, polyvinyl alcohol, polyether-modified trisiloxane and diatomaceous earth were added in sequence, and stirred for 20 minutes to form a uniform solution;
[0049] Step 2: After mixing phthalocyanine green, iron oxide green and calcium carbonate, add them to the solution obtained in the above step 1 at room temperature and a stirring speed of 600 rpm, stirring while adding. After stirring, transfer to a sand mill and grind for 20 minutes. Test the fineness with a scraper fineness meter until the fineness is controlled to ≤5μm to obtain a grinding slurry.
[0050] Step 3: Add a preservative to the grinding slurry of step 2, mix well to obtain a water-based dust suppression colorant.
[0051] Example 2
[0052] A method for preparing a colorant product for dust suppression, which includes 30% pigment filler, 5% thickening suspending agent, 10% rheological additive, 1% surfactant, 0.5% defoamer, 0.2% preservative, and the rest is water, by weight percentage. The filler is calcium sulfate, the weight ratio of pigment to filler is 14:26, and the weight ratio of pigment phthalocyanine green to iron oxide green is 1:3; the thickening suspending agent is carboxymethyl cellulose, sodium alginate and polyvinyl alcohol, wherein the weight proportion of carboxymethyl cellulose in the thickening suspending agent is 12%, the weight proportion of polyvinyl alcohol is 3.3%, and the balance is sodium alginate; the rheological additive is kaolin; the surfactant is nonylphenol polyoxyethylene ether; the defoamer is polyether-modified heptamethyl trisiloxane; and the preservative is chlorphenesin with an ethylene glycol content of 1.5%.
[0053] It comprises the following preparation steps:
[0054] Step 1: at room temperature and a stirring speed of 1400 rpm, water, nonylphenol polyoxyethylene ether, carboxymethyl cellulose, sodium alginate, polyvinyl alcohol, polyether-modified heptamethyl trisiloxane, and kaolin were added in sequence, and stirred for 15 minutes to form a uniform solution;
[0055] Step 2: After mixing phthalocyanine green, iron oxide green and calcium sulfate, add them to the solution obtained in the above step 1 at room temperature and a stirring speed of 500 rpm, stirring while adding. After stirring, transfer to a sand mill and grind for 20 minutes. Test the fineness with a scraper fineness meter until the fineness is controlled to ≤5μm to obtain a grinding slurry.
[0056] Step 3: Add a preservative to the grinding slurry of step 2, mix well to obtain a water-based dust suppression colorant.
[0057] Example 3
[0058] A method for preparing a colorant product for dust suppression, which includes 40% pigment filler, 7% thickening suspending agent, 15% rheological additive, 2% surfactant, 0.5% defoamer, 0.3% preservative, and the rest is water, by weight percentage. The filler is calcium silicate, the weight ratio of pigment to filler is 12:24, the weight ratio of pigment phthalocyanine green to iron oxide green is 1:3.5; the thickening suspending agent is ethyl cellulose, sodium alginate and polyvinyl alcohol, wherein the weight proportion of ethyl cellulose in the thickening suspending agent is 11.4%, the weight proportion of polyvinyl alcohol is 3.6%, and the balance is sodium alginate; the rheological additive is bentonite; the surfactant is nonylphenol polyoxyethylene ether and sodium p-methoxy fatty amide benzene sulfonate, and the weight ratio of the two is 1.2:1; the defoamer is polyether modified trisiloxane; the preservative is Kasson compound phenoxyethanol with 1.5% ethylene glycol content.
[0059] It comprises the following preparation steps:
[0060] Step 1: at room temperature and a stirring speed of 1800 rpm, water, nonylphenol polyoxyethylene ether, sodium p-methoxy fatty amide benzene sulfonate, ethyl cellulose, sodium alginate, polyvinyl alcohol, polyether modified trisiloxane, and bentonite were added in sequence, and stirred for 20 minutes to form a uniform solution;
[0061] Step 2: After mixing phthalocyanine green, iron oxide green and calcium silicate, add them to the solution obtained in the above step 1 at room temperature and a stirring speed of 800 rpm, stirring while adding. After stirring, transfer to a sand mill and grind for 30 minutes. Test the fineness with a scraper fineness meter until the fineness is controlled to ≤5μm to obtain a grinding slurry.
[0062] Step 3: Add a preservative to the grinding slurry of step 2, mix well to obtain a water-based dust suppression colorant.
[0063] Example 4
[0064] A method for preparing a colorant product for dust suppression, which includes 50% pigment filler, 9% thickening suspending agent, 15% rheological additive, 2% surfactant, 1% defoaming agent, 0.5% preservative, and the rest is water, by weight percentage. The filler is barium sulfate, the weight ratio of pigment to filler is 13:21, and the weight ratio of pigment phthalocyanine green to iron oxide green is 1:3.5; the thickening suspending agent is hydroxypropyl methylcellulose, sodium alginate and polyvinyl alcohol, wherein the weight proportion of hydroxypropyl methylcellulose in the thickening suspending agent is 11.3%, the weight proportion of polyvinyl alcohol is 3.8%, and the balance is sodium alginate; the rheological additive is montmorillonite; the surfactant is octylphenol polyoxyethylene ether; the defoaming agent is polyether modified trisiloxane; the preservative is phenoxyethanol compounded with benzyl alcohol with 1% ethylene glycol content, wherein the weight ratio of phenoxyethanol to benzyl alcohol is 1:1.
[0065] It includes the following steps:
[0066] Step 1: at room temperature and a stirring speed of 1800 rpm, water, octylphenol polyoxyethylene ether, hydroxypropyl methylcellulose, sodium alginate, polyvinyl alcohol, polyether-modified trisiloxane, and montmorillonite were added in sequence, and stirred for 25 minutes to form a uniform solution;
[0067] Step 2: After mixing phthalocyanine green, iron oxide green and barium sulfate, add them to the solution obtained in the above step 1 at room temperature and a stirring speed of 800 rpm, stirring while adding. After stirring, transfer to a sand mill and grind for 40 minutes. Test the fineness with a scraper fineness meter until the fineness is controlled to ≤10μm to obtain a grinding slurry.
[0068] Step 3: Add a preservative to the grinding slurry of step 2, mix well to obtain a water-based dust suppression colorant.
[0069] Example 5
[0070] A method for preparing a colorant product for dust suppression, which includes 35% pigment filler, 10% thickening suspending agent, 10% rheological additive, 3% surfactant, 1% defoamer, 0.5% preservative, and the rest is water, by weight percentage. The filler is calcium carbonate, the weight ratio of pigment to filler is 13:27, and the weight ratio of pigment phthalocyanine green to iron oxide green is 1:2; the thickening suspending agent is benzyl cellulose, potassium alginate and polyvinyl alcohol, wherein the weight proportion of benzyl cellulose in the thickening suspending agent is 11.1%, the weight proportion of polyvinyl alcohol is 3.9%, and the balance is potassium alginate; the rheological additive is attapulgite; the surfactant is octylphenol polyoxyethylene ether and sodium p-methoxy fatty amide benzene sulfonate, and the weight ratio of the two is 0.9:1; the defoamer is polyether-modified heptamethyl trisiloxane; the preservative is kason with 2% ethylene glycol content.
[0071] It comprises the following preparation steps:
[0072] Step 1: at room temperature and a stirring speed of 1500 rpm, water, octylphenol polyoxyethylene ether, sodium p-methoxy fatty amide benzene sulfonate, benzyl cellulose, potassium alginate, polyvinyl alcohol, polyether-modified heptamethyl trisiloxane, and attapulgite were added in sequence, and stirred for 20 minutes to mix into a uniform solution;
[0073] Step 2: After mixing phthalocyanine green, iron oxide green and calcium carbonate, add them to the solution obtained in the above step 1 at room temperature and a stirring speed of 600 rpm, stirring while adding. After stirring, transfer to a sand mill and grind for 20 minutes. Test the fineness with a scraper fineness meter until the fineness is controlled to ≤5μm to obtain a grinding slurry.
[0074] Step 3: Add a preservative to the grinding slurry of step 2, mix well to obtain a water-based dust suppression colorant.
[0075] Example 6
[0076] A method for preparing a colorant product for dust suppression, which comprises, by weight percentage, 30% pigment filler, 3% thickening suspending agent, 8% rheological additive, 1% surfactant, 0.5% defoamer, 0.05% preservative, and the rest is water. The filler is silicon dioxide, the weight ratio of pigment to filler is 15:22, and the weight ratio of pigment phthalocyanine green to iron oxide green is 1:2; the thickening suspending agent is benzyl cellulose, potassium alginate and polyvinyl alcohol, wherein the weight proportion of benzyl cellulose in the thickening suspending agent is 5%, the weight proportion of polyvinyl alcohol is 1%, and the balance is potassium alginate; the rheological additive is sepiolite; the surfactant is nonylphenol polyoxyethylene ether; the defoamer is polyether-modified heptamethyl trisiloxane; and the preservative is kason with an ethylene glycol content of 0.5%.
[0077] Step 1: at room temperature and a stirring speed of 1400 rpm, water, nonylphenol polyoxyethylene ether, benzyl cellulose, potassium alginate, polyvinyl alcohol, polyether-modified heptamethyl trisiloxane, and sepiolite were added in sequence, and stirred for 10 minutes to mix into a uniform solution;
[0078] Step 2: After mixing phthalocyanine green, iron oxide green and silicon dioxide, add them to the solution obtained in the above step 1 at room temperature and a stirring speed of 500 rpm, stirring while adding. After stirring, transfer to a sand mill and grind for 20 minutes. Test the fineness with a scraper fineness meter until the fineness is controlled to ≤5μm to obtain a grinding slurry.
[0079] Step 3: Add a preservative to the grinding slurry of step 2, mix well to obtain a water-based dust suppression colorant.
[0080] Example 7
[0081] A method for preparing a colorant product for dust suppression, which comprises, by weight percentage, 50% pigment filler, 15% thickening suspending agent, 20% rheological additive, 5% surfactant, 1% defoamer, 1% preservative, and the rest is water. The filler is barium sulfate and calcium carbonate, and the weight ratio of the two is 1:1, the weight ratio of the pigment to the filler is 8:35, and the weight ratio of the pigment phthalocyanine green and iron oxide green is 1:3; the thickening suspending agent is benzyl cellulose, potassium alginate and polyvinyl alcohol, wherein the weight proportion of benzyl cellulose in the thickening suspending agent is 25%, the weight proportion of polyvinyl alcohol is 5%, and the balance is potassium alginate; the rheological additive is a mixture of kaolin and montmorillonite, and the weight ratio of the two is 1:1; the surfactant is octylphenol polyoxyethylene ether; the defoamer is polyether-modified heptamethyl trisiloxane; and the preservative is kason with an ethylene glycol content of 2%.
[0082] Step 1: at room temperature and a stirring speed of 2000 rpm, water, octylphenol polyoxyethylene ether, benzyl cellulose, potassium alginate, polyvinyl alcohol, polyether-modified heptamethyl trisiloxane, kaolin and montmorillonite mixture were added in sequence, and stirred for 30 minutes to form a uniform solution;
[0083] Step 2: After mixing phthalocyanine green, iron oxide green, barium sulfate and calcium carbonate, add them to the solution obtained in the above step 1 at room temperature and a stirring speed of 800 rpm, stirring while adding. After stirring, transfer to a sand mill and grind for 40 minutes. Test the fineness with a scraper fineness meter until the fineness is controlled to ≤5μm to obtain a grinding slurry.
[0084] Step 3: Add a preservative to the grinding slurry of step 2, mix well to obtain a water-based dust suppression colorant.
[0085] Example 8
[0086] A method for preparing a colorant product for dust suppression, which comprises, by weight percentage, 30% pigment filler, 5% thickening suspending agent, 10% rheological additive, 1% surfactant, 0.5% defoamer, 0.1% preservative, and the rest is water. The filler is calcium carbonate and calcium silicate, the weight ratio of pigment to filler is 10:20, and the weight ratio of pigment phthalocyanine green and iron oxide green is 1:2.5; the thickening suspending agent is benzyl cellulose, potassium alginate and polyvinyl alcohol, wherein the weight proportion of benzyl cellulose in the thickening suspending agent is 15%, the weight proportion of polyvinyl alcohol is 2%, and the balance is potassium alginate; the rheological additive is bentonite; the surfactant is isopropylamine dodecylbenzenesulfonate; the defoamer is polyether-modified heptamethyl trisiloxane; and the preservative is benzyl alcohol with an ethylene glycol content of 0.5%.
[0087] Step 1: at room temperature and a stirring speed of 1500 rpm, water, isopropylamine dodecylbenzenesulfonate, benzyl cellulose, potassium alginate, polyvinyl alcohol, polyether-modified heptamethyl trisiloxane, and bentonite were added in sequence, and stirred for 30 minutes to form a uniform solution;
[0088] Step 2: After mixing phthalocyanine green, iron oxide green, calcium carbonate and calcium silicate, add them to the solution obtained in the above step 1 at room temperature and a stirring speed of 800 rpm, stirring while adding. After stirring, transfer to a sand mill and grind for 40 minutes. Test the fineness with a scraper fineness meter until the fineness is controlled to ≤5μm to obtain a grinding slurry.
[0089] Step 3: Add a preservative to the grinding slurry of step 2, mix well to obtain a water-based dust suppression colorant.
[0090] Example 9
[0091] A method for preparing a colorant product for dust suppression, which comprises, by weight percentage, 50% pigment filler, 12% thickening suspending agent, 18% rheological additive, 3% surfactant, 1% defoamer, 0.5% preservative, and the rest is water. The filler is calcium carbonate, the weight ratio of pigment to filler is 15:35, and the weight ratio of pigment phthalocyanine green to iron oxide green is 1:2.5; the thickening suspending agent is benzyl cellulose, potassium alginate and polyvinyl alcohol, wherein the weight proportion of benzyl cellulose in the thickening suspending agent is 20%, the weight proportion of polyvinyl alcohol is 4%, and the balance is potassium alginate; the rheological additive is sepiolite and diatomaceous earth, and the ratio of the two is 1:1; the surfactant is sodium p-methoxy fatty amide benzene sulfonate; the defoamer is polyether modified trisiloxane; and the preservative is a compound of kason and benzyl alcohol with an ethylene glycol content of 1%.
[0092] Step 1: at room temperature and a stirring speed of 1800 rpm, water, sodium p-methoxy fatty amide benzene sulfonate, benzyl cellulose, potassium alginate, polyvinyl alcohol, polyether-modified trisiloxane, sepiolite and diatomaceous earth were added in sequence, and stirred for 30 minutes to form a uniform solution;
[0093] Step 2: After mixing phthalocyanine green, iron oxide green and calcium carbonate, add them to the solution obtained in the above step 1 at room temperature and a stirring speed of 800 rpm, stirring while adding. After stirring, transfer to a sand mill and grind for 40 minutes. Test the fineness with a scraper fineness meter until the fineness is controlled to ≤5μm to obtain a grinding slurry.
[0094] Step 3: Add a preservative to the grinding slurry of step 2, mix well to obtain a water-based dust suppression colorant.
[0095] Example 10
[0096] A method for preparing a colorant product for dust suppression, which comprises, by weight percentage, 50% pigment filler, 10% thickening suspending agent, 15% rheological additive, 3% surfactant, 1% defoamer, 0.5% preservative, and the rest is water. The filler is calcium carbonate, the weight ratio of pigment to filler is 10:20, and the weight ratio of pigment phthalocyanine green to iron oxide green is 1:2.5; the thickening suspending agent is benzyl cellulose, potassium alginate and polyvinyl alcohol, wherein the weight proportion of benzyl cellulose in the thickening suspending agent is 11%, the weight proportion of polyvinyl alcohol is 4%, and the balance is potassium alginate; the rheological additive is diatomaceous earth; the surfactant is octylphenol polyoxyethylene ether and sodium p-methoxy fatty amide benzene sulfonate, and the mass ratio of the two is 1:1; the defoamer is polyether-modified heptamethyl trisiloxane; and the preservative is kason with an ethylene glycol content of 2%.
[0097] Step 1: at room temperature and a stirring speed of 1800 rpm, water, octylphenol polyoxyethylene ether, sodium p-methoxy fatty amide benzene sulfonate, benzyl cellulose, potassium alginate, polyvinyl alcohol, polyether-modified heptamethyl trisiloxane, and diatomaceous earth were added in sequence, and stirred for 30 minutes to mix into a uniform solution;
[0098] Step 2: After mixing phthalocyanine green, iron oxide green and calcium carbonate, add them to the solution obtained in the above step 1 at room temperature and a stirring speed of 800 rpm, stirring while adding. After stirring, transfer to a sand mill and grind for 40 minutes. Test the fineness with a scraper fineness meter until the fineness is controlled to ≤5μm to obtain a grinding slurry.
[0099] Step 3: Add a preservative to the grinding slurry of step 2, mix well to obtain a water-based dust suppression colorant.
[0100] Embodiment 11
[0101] A method for preparing a colorant product for dust suppression, which includes 35% pigment filler, 5% thickening suspending agent, 12% rheological additive, 1.5% surfactant, 1% defoamer, 0.2% preservative, and the rest is water, by weight percentage. The filler is calcium carbonate, the weight ratio of pigment to filler is 12:28, and the weight ratio of pigment phthalocyanine green to iron oxide green is 1:2.5; the thickening suspending agent is methyl cellulose, sodium alginate and polyvinyl alcohol, wherein the weight proportion of methyl cellulose in the thickening suspending agent is 13%, the weight proportion of polyvinyl alcohol is 3%, and the balance is sodium alginate; the rheological additive is diatomaceous earth; the surfactant is octylphenol polyoxyethylene ether and isopropylamine dodecylbenzenesulfonate, and the mass ratio of the two is 1:1; the defoamer is polyether modified trisiloxane; and the preservative is kason with 1% ethylene glycol content.
[0102] It comprises the following preparation steps:
[0103] Step 1: at room temperature and a stirring speed of 1500 rpm, water, octylphenol polyoxyethylene ether, isopropylamine dodecylbenzenesulfonate, methyl cellulose, sodium alginate, polyvinyl alcohol, polyether-modified trisiloxane and diatomaceous earth were added in sequence, and stirred for 20 minutes to form a uniform solution;
[0104] Step 2: After mixing phthalocyanine green, iron oxide green and calcium carbonate, add them to the solution obtained in the above step 1 at room temperature and a stirring speed of 600 rpm, stirring while adding. After stirring, transfer to a sand mill and grind for 20 minutes. Test the fineness with a scraper fineness meter until the fineness is controlled to 20 μm to obtain a grinding slurry.
[0105] Step 3: Add a preservative to the grinding slurry of step 2, mix well to obtain a water-based dust suppression colorant.
[0106] Example 12
[0107] A method for preparing a colorant product for dust suppression, which includes 35% pigment filler, 5% thickening suspending agent, 12% rheological additive, 1.5% surfactant, 1% defoamer, 0.2% preservative, and the rest is water, by weight percentage. The filler is calcium carbonate, the weight ratio of pigment to filler is 12:28, and the weight ratio of pigment phthalocyanine green to iron oxide green is 1:2.5; the thickening suspending agent is methyl cellulose, sodium alginate and polyvinyl alcohol, wherein the weight proportion of methyl cellulose in the thickening suspending agent is 13%, the weight proportion of polyvinyl alcohol is 3%, and the balance is sodium alginate; the rheological additive is diatomaceous earth; the surfactant is octylphenol polyoxyethylene ether and isopropylamine dodecylbenzenesulfonate, and the mass ratio of the two is 1:1; the defoamer is polyether modified trisiloxane; and the preservative is kason with 1% ethylene glycol content.
[0108] It comprises the following preparation steps:
[0109] Step 1: at room temperature and a stirring speed of 1500 rpm, water, octylphenol polyoxyethylene ether, isopropylamine dodecylbenzenesulfonate, methyl cellulose, sodium alginate, polyvinyl alcohol, polyether-modified trisiloxane and diatomaceous earth were added in sequence, and stirred for 20 minutes to form a uniform solution;
[0110] Step 2: After mixing phthalocyanine green, iron oxide green and calcium carbonate, add them to the solution obtained in the above step 1 at room temperature and a stirring speed of 600 rpm, stirring while adding. After stirring, transfer to a sand mill and grind for 20 minutes. Test the fineness with a scraper fineness meter until the fineness is controlled to 50 μm to obtain a grinding slurry.
[0111] Step 3: Add a preservative to the grinding slurry of step 2, mix well to obtain a water-based dust suppression colorant.
[0112] Embodiment 13
[0113] A method for preparing a colorant product for dust suppression, which includes 35% pigment filler, 5% thickening suspending agent, 12% rheological additive, 1.5% surfactant, 1% defoamer, 0.2% preservative, and the rest is water, by weight percentage. The filler is calcium carbonate, the weight ratio of pigment to filler is 12:28, and the weight ratio of pigment phthalocyanine green to iron oxide green is 1:2.5; the thickening suspending agent is methyl cellulose, sodium alginate and polyvinyl alcohol, wherein the weight proportion of methyl cellulose in the thickening suspending agent is 13%, the weight proportion of polyvinyl alcohol is 3%, and the balance is sodium alginate; the rheological additive is diatomaceous earth; the surfactant is octylphenol polyoxyethylene ether; the defoamer is polyether modified trisiloxane; and the preservative is kason with 1% ethylene glycol content.
[0114] It comprises the following preparation steps:
[0115] Step 1: at room temperature and a stirring speed of 1500 rpm, water, octylphenol polyoxyethylene ether, methyl cellulose, sodium alginate, polyvinyl alcohol, polyether-modified trisiloxane and diatomaceous earth were added in sequence, and stirred for 20 minutes and then mixed into a uniform solution;
[0116] Step 2: After mixing phthalocyanine green, iron oxide green and calcium carbonate, add them to the solution obtained in the above step 1 at room temperature and a stirring speed of 600 rpm, stirring while adding. After stirring, transfer to a sand mill and grind for 20 minutes. Test the fineness with a scraper fineness meter until the fineness is controlled to ≤5μm to obtain a grinding slurry.
[0117] Step 3: Add a preservative to the grinding slurry of step 2, mix well to obtain a water-based dust suppression colorant.
[0118] Embodiment 14
[0119] A method for preparing a colorant product for dust suppression, which includes 35% pigment filler, 5% thickening suspending agent, 12% rheological additive, 1.5% surfactant, 1% defoamer, 0.2% preservative, and the rest is water, by weight percentage. The filler is calcium carbonate, the weight ratio of pigment to filler is 12:28, the weight ratio of pigment phthalocyanine green to iron oxide green is 1:2.5; the thickening suspending agent is methyl cellulose and sodium alginate, wherein the weight proportion of methyl cellulose in the thickening suspending agent is 25%, and the balance is sodium alginate; the rheological additive is diatomaceous earth; the surfactant is octylphenol polyoxyethylene ether and isopropylamine dodecylbenzenesulfonate, and the mass ratio of the two is 1:1; the defoamer is polyether modified trisiloxane; the preservative is kason with 1% ethylene glycol content.
[0120] It comprises the following preparation steps:
[0121] Step 1: at room temperature and a stirring speed of 1500 rpm, water, octylphenol polyoxyethylene ether, isopropylamine dodecylbenzenesulfonate, methyl cellulose, sodium alginate, polyether-modified trisiloxane and diatomaceous earth were added in sequence, and stirred for 20 minutes to form a uniform solution;
[0122] Step 2: After mixing phthalocyanine green, iron oxide green and calcium carbonate, add them to the solution obtained in the above step 1 at room temperature and a stirring speed of 600 rpm, stirring while adding. After stirring, transfer to a sand mill and grind for 20 minutes. Test the fineness with a scraper fineness meter until the fineness is controlled to ≤5μm to obtain a grinding slurry.
[0123] Step 3: Add a preservative to the grinding slurry of step 2, mix well to obtain a water-based dust suppression colorant.
[0124] Comparative Example 1
[0125] A method for preparing a colorant product for dust suppression, which includes 35% pigment filler, 20% rheological additive, 1.5% surfactant, 1% defoamer, 0.2% preservative, and the rest is water, by weight percentage. The filler is calcium carbonate, the weight ratio of pigment to filler is 12:28, the weight ratio of pigment phthalocyanine green to iron oxide green is 1:2.5; the rheological additive is diatomaceous earth; the surfactant is octylphenol polyoxyethylene ether and dodecylbenzenesulfonic acid isopropylamine, the mass ratio of the two is 1:1; the defoamer is polyether modified trisiloxane; the preservative is kason with 1% ethylene glycol content.
[0126] It comprises the following preparation steps:
[0127] Step 1: under the condition of room temperature and stirring speed of 1500 rpm, water, octylphenol polyoxyethylene ether, isopropylamine dodecylbenzenesulfonate, polyether-modified trisiloxane and diatomaceous earth were added in sequence, and stirred for 20 minutes and then mixed into a uniform solution;
[0128] Step 2: After mixing phthalocyanine green, iron oxide green and calcium carbonate, add them to the solution obtained in the above step 1 at room temperature and a stirring speed of 600 rpm, stirring while adding, and after stirring, transfer to a sand mill and grind for 20 minutes, and test the fineness with a scraper fineness meter until the fineness is controlled to ≤5μm to obtain a grinding slurry;
[0129] Step 3: Add a preservative to the grinding slurry of step 2, mix well to obtain a water-based dust suppression colorant.
[0130] Comparative Example 2
[0131] A method for preparing a colorant product for dust suppression, which includes 35% pigment filler, 15% thickening suspending agent, 1.5% surfactant, 1% defoamer, 0.2% preservative, and the rest is water, by weight percentage. The filler is calcium carbonate, the weight ratio of pigment to filler is 12:28, and the weight ratio of pigment phthalocyanine green to iron oxide green is 1:2.5; the thickening suspending agent is methyl cellulose, sodium alginate and polyvinyl alcohol, wherein the weight proportion of methyl cellulose in the thickening suspending agent is 13%, the weight proportion of polyvinyl alcohol is 3%, and the balance is sodium alginate; the surfactant is octylphenol polyoxyethylene ether and isopropylamine dodecylbenzenesulfonate, and the mass ratio of the two is 1:1; the defoamer is polyether modified trisiloxane; and the preservative is kason with 1% ethylene glycol content.
[0132] It comprises the following preparation steps:
[0133] Step 1: at room temperature and a stirring speed of 1500 rpm, water, octylphenol polyoxyethylene ether, isopropylamine dodecylbenzenesulfonate, methyl cellulose, sodium alginate, polyvinyl alcohol, and polyether-modified trisiloxane were added in sequence, and stirred for 20 minutes to form a uniform solution;
[0134] Step 2: After mixing phthalocyanine green, iron oxide green and calcium carbonate, add them to the solution obtained in the above step 1 at room temperature and a stirring speed of 600 rpm, stirring while adding. After stirring, transfer to a sand mill and grind for 20 minutes. Test the fineness with a scraper fineness meter until the fineness is controlled to ≤5μm to obtain a grinding slurry.
[0135] Step 3: Add a preservative to the grinding slurry of step 2, mix well to obtain a water-based dust suppression colorant.
[0136] Comparative Example 3
[0137] A method for preparing a colorant product for dust suppression, which includes 35% pigment filler, 2% thickening suspending agent, 5% rheological additive, 1% surfactant, 0.5% defoamer, 0.1% preservative, and the rest is water, by weight percentage. The filler is calcium sulfate, the weight ratio of pigment to filler is 12:28, and the ratio of pigment phthalocyanine green to iron oxide green is 1:2.5; the thickening suspending agent is carboxymethyl cellulose, sodium alginate and polyvinyl alcohol, wherein the weight proportion of carboxymethyl cellulose in the thickening suspending agent is 13%, the weight proportion of polyvinyl alcohol is 3%, and the balance is sodium alginate; the rheological additive is kaolin; the surfactant is octylphenol polyoxyethylene ether; the defoamer is polyether-modified heptamethyl trisiloxane; and the preservative is chlorphenesin with an ethylene glycol content of 0.5%.
[0138] It comprises the following preparation steps:
[0139] Step 1: at room temperature and a stirring speed of 1500 rpm, water, octylphenol polyoxyethylene ether, carboxymethyl cellulose, sodium alginate, polyvinyl alcohol, polyether-modified heptamethyl trisiloxane, and kaolin were added in sequence, and stirred for 20 minutes to form a uniform solution;
[0140] Step 2: After mixing phthalocyanine green, iron oxide green and calcium sulfate, add them to the solution obtained in the above step 1 at room temperature and a stirring speed of 600 rpm, stirring while adding. After stirring, transfer to a sand mill and grind for 20 minutes. Then test the fineness with a scraper fineness meter until the fineness is controlled to ≤5μm to obtain a grinding slurry.
[0141] Step 3: Add a preservative to the grinding slurry of step 2, mix well to obtain a water-based dust suppression colorant.
[0142] Comparative Example 4
[0143] A method for preparing a colorant product for dust suppression, which includes 35% pigment filler, 5% thickening suspending agent, 12% rheological additive, 1.5% surfactant, 1% defoamer, 0.2% preservative, and the rest is water, by weight percentage. The filler is calcium carbonate, the weight ratio of pigment to filler is 12:28, and the pigment is iron oxide green; the thickening suspending agent is methyl cellulose, sodium alginate and polyvinyl alcohol, wherein the weight proportion of methyl cellulose in the thickening suspending agent is 13%, the weight proportion of polyvinyl alcohol is 3%, and the balance is sodium alginate; the rheological additive is diatomaceous earth; the surfactant is octylphenol polyoxyethylene ether and isopropylamine dodecylbenzenesulfonate, and the mass ratio of the two is 1:1; the defoamer is polyether modified trisiloxane; the preservative is kason with 1% ethylene glycol content.
[0144] It comprises the following preparation steps:
[0145] Step 1: at room temperature and a stirring speed of 1500 rpm, water, octylphenol polyoxyethylene ether, isopropylamine dodecylbenzenesulfonate, methyl cellulose, sodium alginate, polyvinyl alcohol, polyether-modified trisiloxane and diatomaceous earth were added in sequence, and stirred for 20 minutes to form a uniform solution;
[0146] Step 2: After mixing the iron oxide green and calcium carbonate, add them to the solution obtained in the above step 1 at room temperature and a stirring speed of 600 rpm, stirring while adding. After stirring, transfer to a sand mill and grind for 20 minutes. Test the fineness with a scraper fineness meter until the fineness is controlled to ≤5μm to obtain a grinding slurry.
[0147] Step 3: Add a preservative to the grinding slurry of step 2, mix well to obtain a water-based dust suppression colorant.
[0148] Comparative Example 5
[0149] A method for preparing a colorant product for dust suppression, which includes 35% pigment, 5% thickening suspending agent, 12% rheological additive, 1.5% surfactant, 1% defoaming agent, 0.2% preservative, and the rest is water, by weight percentage. The ratio of pigment phthalocyanine green to iron oxide green is 1:2.5; the thickening suspending agent is methyl cellulose, sodium alginate and polyvinyl alcohol, wherein the weight proportion of methyl cellulose in the thickening suspending agent is 13%, the weight proportion of polyvinyl alcohol is 3%, and the balance is sodium alginate; the rheological additive is diatomaceous earth; the surfactant is octylphenol polyoxyethylene ether and isopropylamine dodecylbenzenesulfonate, and the mass ratio of the two is 1:1; the defoaming agent is polyether modified trisiloxane; the preservative is kason with 1% ethylene glycol content.
[0150] It comprises the following preparation steps:
[0151] Step 1: at room temperature and a stirring speed of 1500 rpm, water, octylphenol polyoxyethylene ether, isopropylamine dodecylbenzenesulfonate, methyl cellulose, sodium alginate, polyvinyl alcohol, polyether-modified trisiloxane and diatomaceous earth were added in sequence, and stirred for 20 minutes to form a uniform solution;
[0152] Step 2: After mixing phthalocyanine green and iron oxide green, add them to the solution obtained in the above step 1 at room temperature and a stirring speed of 600 rpm, stirring while adding. After stirring, transfer to a sand mill and grind for 20 minutes. Test the fineness with a scraper fineness meter until the fineness is controlled to ≤5μm to obtain a grinding slurry.
[0153] Step 3: Add a preservative to the grinding slurry of step 2, mix well to obtain a water-based dust suppression colorant.
[0154] The dust suppression colorant products prepared in Examples 1 to 14 and Comparative Examples 1 to 5 were tested for viscosity, stability, and particle size, and were compounded with dust suppressants to test their resistance to rain erosion. It should be noted that the dust suppressant used in the embodiments of the present invention is a biomass dust suppressant produced by Inner Mongolia Hongshun Da Industry and Trade Co., Ltd.
[0155] The specific detection methods are as follows:
[0156] (1) Viscosity test: Use LVDV-2T intelligent touch digital viscometer to measure the sample to be tested. The rotor is selected from 1 to 4 and the speed is adjusted from large to small. During the test, read 3 values in succession and take the average value as the viscosity of the product. At the same time, record the ambient temperature.
[0157] (2) Stability test: Dilute the dust suppression colorant product to a solid content of 4-5%, place it at room temperature for 72 hours, and observe the stratification.
[0158] (3) Particle size test: The scraper fineness is measured by a scraper fineness meter with a range of 0 to 50 μm, and the overall particle size distribution of the product is measured by an S3500 series Bluewavel laser particle size analyzer. Finally, the grinding time is tested when the particle size is ≤5 μm.
[0159] (4) Test of anti-rainwater erosion performance: Place the coal sample in a stainless steel top plate, dry it in a 50°C oven for 5 hours to remove moisture, spray the colorant compound dust suppressant product, wait for it to be completely moistened, dry it at room temperature for 24 hours, use a sprayer to simulate natural rainfall and spray vertically on various samples, continue spraying for 10 minutes, then dry it and observe the color change. The specific method of spraying the colorant compound dust suppressant product on the sample is: first spray an aqueous solution of a dust suppressant with a mass concentration of 3% by weight, wait for the dust suppressant to agglomerate, and then spray an aqueous solution of a water-based dust suppressant colorant with a mass concentration of 7%, and control the spraying amount of the two to be 3L / m 2 .
[0160] In addition, in order to further describe the relevant performance when using each colorant, the specific performance is graded, specifically:
[0161] The coloring ability is graded as follows: Grade 1: uniform coloring; Grade 2: some dust residue will be exposed; Grade 3: uneven coloring; Grade 4: the dust residue sample does not show color.
[0162] The color brightness is graded as follows: Level 1: bright green; Level 2: light green; Level 3: bluish; Level 4: unclear color.
[0163] The ability to resist rain erosion is graded: Level 1: after simulated rain erosion, the coloring is uniform; Level 2: after simulated rain erosion, the color powder is lost and some dust is exposed; Level 3: after simulated rain erosion, the color powder is seriously lost and the coloring is uneven, with the upper dust sample basically not showing color; Level 4: after erosion, the dust sample has no obvious color.
[0164] Table 1 shows the relevant performance test results of the colorant products for dust suppression prepared in Examples 1 to 14 and Comparative Examples 1 to 5, as follows:
[0165] Table 1
[0166]
[0167]
[0168] It can be seen from the data in the above table that the particle size of the colorant products with different proportions under this formula is controlled at ≤5μm. With the interaction between the raw material components, the viscosity of the system increases significantly, thereby effectively avoiding the problem of color powder deposition in the product. Testing its stability shows that the product has no obvious stratification phenomenon. The dust suppressant compound colorant spraying test was carried out in the laboratory. The results show that all kinds of materials are bright green.
[0169] Comparative Example 1 is a product obtained without adding a thickening suspending agent, and Comparative Example 2 is a product obtained without adding a rheological additive. The performance test results show that the viscosity of the two products is significantly reduced, the suspension dispersion effect is poor, and the grinding time is increased, resulting in a decrease in product stability and a significant stratification phenomenon. Comparative Example 3 is a product obtained with a relatively low weight percentage content of thickener, rheological additive and surfactant. At this time, the viscosity of the product is significantly reduced, the stratification is obvious, and the grinding time is long, indicating that each component of the colorant should be controlled within a suitable addition range to make the product stability better. Comparative Example 4 is a product obtained by using only a pigment of iron oxide green. When used, the product is blue in color and uneven in color. Especially after being washed by rain, the sample fades significantly. Comparative Example 5 is a product obtained without adding fillers. The toner has a significant deposition phenomenon, the product color is reduced, and the anti-rainwater scouring performance is deteriorated.
[0170] In summary, the product liquids of the water-based dust suppression colorant and dust suppressant compound obtained in Examples 1 to 14 were sprayed on the surface of each material. After being eroded by rain, the surface was flat and smooth, the color was evenly distributed, and it still showed bright green, with good comprehensive performance. However, the product liquids of the water-based dust suppression colorant and dust suppressant compound obtained in the comparative example were sprayed on the surface of each material, resulting in uneven coloring due to the deposition of color powder. After being washed by rain, the color powder was lost, the color of the material surface became lighter, and the comprehensive performance was poor. If a better coloring effect is to be achieved during use, it is necessary to spray twice or more times.
[0171] Example 15 to Example 21
[0172] In another aspect of the present invention, the color development of different color samples by different spraying methods is investigated. The coloring products for dust suppression prepared by the coloring agents for dust suppression in Examples 1 to 7 are selected and sprayed by Method 1 and Method 2 respectively to color and cover fly ash, desulfurized gypsum, and coal samples, and their color development capabilities are recorded. The specific classification standards for color development capabilities are described above, and the results are shown in Table 2.
[0173] Spraying method 1: Dilute the dust suppressant to a 3% aqueous solution by weight, then add a water-based dust suppression colorant to a 6% concentration. The spraying volume is 6L / m 2 .
[0174] Spraying method 2: First spray a 3% dust suppressant aqueous solution by weight percentage, and then spray a 7% water-based dust suppressant colorant aqueous solution after the dust suppressant agglomerates, and control the spraying volume of the two independently to 3L / m 2 .
[0175] Table 2
[0176]
[0177]
[0178] From the results in Table 2, it can be seen that for fly ash and desulfurization gypsum slag samples with lighter colors, the samples can show excellent color development effects by using spraying method 1, which is to spray the water-based dust suppression colorant and the dust suppressant on the surface of the dust slag at the same time, or by using method 2, which is to first spray the dust suppressant on the surface of the dust slag and then spray the water-based dust suppression colorant. However, method 1 only requires one spraying, which has the advantage of being easy to use. For samples with darker colors such as coal samples, spraying method 2 is used, which is to first spray the dust suppressant on the surface of the dust slag and then spray the water-based dust suppression colorant, and the color development effect is better.
[0179] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A water-based dust suppression colorant, characterized in that: By weight percentage, the water-based dust suppression colorant includes: Pigments and fillers 30-50%, rheological additives 8-20%, thickening and suspending agents 3-15%, surfactants 1-5%, defoamers 0.5-1%, preservatives 0.05-1%, and the balance is water; The color filler comprises a pigment and a filler, wherein the pigment is a composite pigment of phthalocyanine green and iron oxide green.
2. The water-based dust suppression colorant according to claim 1, characterized in that: The filler is one or more of barium sulfate, calcium carbonate, silicon dioxide, calcium sulfate and calcium silicate; Preferably, the weight ratio of the pigment to the filler is (8-15):(22-35); More preferably, the weight ratio of the pigment to the filler is (10-15):(20-35); Preferably, the weight ratio of the phthalocyanine green to the iron oxide green in the pigment is 1:(2-3.5).
3. The water-based dust suppression colorant according to claim 1, characterized in that: By weight percentage, the water-based dust suppression colorant includes: The pigment and filler are 30-50%, the rheological additive is 10-18%, the thickening suspending agent is 5-12%, the surfactant is 1-3%, the defoaming agent is 0.5-1%, the preservative is 0.1-0.5%, and the balance is water; Preferably, the pigment and filler are 30-50%, the rheological additive is 10-15%, the thickening and suspending agent is 5-10%, the surfactant is 1-3%, the defoaming agent is 0.5-1%, the preservative is 0.1-0.5%, and the balance is water.
4. The aqueous dust suppression colorant according to any one of claims 1 to 3, characterized in that The thickening suspending agent is one or more of cellulose ether, alginate, and polyvinyl alcohol; Preferably, the thickening suspending agent is a mixture of the alginate, the cellulose ether and the polyvinyl alcohol; more preferably, in terms of weight percentage, the content of the cellulose ether in the thickening suspending agent is 5-25%, the content of the polyvinyl alcohol is 1-5%, and the balance is the alginate; further preferably, the content of the cellulose ether is 5-15%; Preferably, the cellulose ether is one or more of methyl cellulose, ethyl cellulose, carboxymethyl cellulose, hydroxypropyl methyl cellulose, and benzyl cellulose; More preferably, the alginate is sodium alginate and / or potassium alginate.
5. The aqueous dust suppression colorant according to any one of claims 1 to 3, characterized in that The rheological additive is inorganic silicate clay; Preferably, the inorganic silicate clay is one or more of kaolin, montmorillonite, bentonite, sepiolite, attapulgite and diatomaceous earth.
6. The aqueous dust suppression colorant according to any one of claims 1 to 3, characterized in that The surfactant is a nonionic surfactant and / or an anionic surfactant; Preferably, the nonionic surfactant and the anionic surfactant are used in combination; Preferably, the nonionic surfactant is alkylphenol polyoxyethylene ether; further preferably, the alkylphenol polyoxyethylene ether is octylphenol polyoxyethylene ether and / or nonylphenol polyoxyethylene ether; Preferably, the anionic surfactant is isopropylamine dodecylbenzenesulfonate and / or sodium p-methoxy fatty amide benzenesulfonate; Preferably, the defoaming agent is a polyether-modified silicone defoaming agent; further preferably, the polyether-modified silicone defoaming agent is polyether-modified trisiloxane and / or polyether-modified heptamethyl trisiloxane.
7. The aqueous dust suppression colorant according to any one of claims 1 to 3, characterized in that The preservative is a compound preservative of ethylene glycol and at least one of the following: kathoson, phenoxyethanol, benzyl alcohol, chlorphenesin; Preferably, the content of ethylene glycol in the preservative is 0.5-2% by weight.
8. The method for preparing the water-based dust suppression colorant according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: S1, stirring and mixing water, a surfactant, a thickening suspending agent, a defoaming agent and a rheological additive to obtain a premixed solution; S2, adding pigments and fillers to the premixed solution, stirring and grinding to obtain a grinding slurry; S3, adding a preservative to the polishing slurry, and mixing to obtain the water-based dust suppression colorant.
9. The method for preparing the water-based dust suppression colorant according to claim 8, characterized in that: The stirring speed in step S1 is controlled to be 1400-2000 rpm, and the mixing time is 10-30 min; and / or, the stirring speed in step S2 is controlled to be 500-800 rpm, the grinding time is 20-40 min, and the fineness of the grinding slurry is ≤50 μm; Preferably, the fineness of the grinding slurry is controlled to be ≤20 μm; More preferably, the fineness of the grinding slurry is controlled to be ≤5 μm.
10. A method for treating the surface of dusty slag by using the water-based dust suppression colorant according to any one of claims 1 to 7, characterized in that: The water-based dust suppression colorant is sprayed on the dust slag surface in one of the following two ways to perform the dust suppression treatment: Method 1: Mix the water-based dust suppression colorant and the dust suppression agent and spray them on the surface of the dust residue at the same time; Method 2: first spray the dust suppressant on the surface of the dust residue, and then spray the water-based dust suppressant colorant.