Chip bonding sheet, dicing chip bonding film, semiconductor device, and electronic apparatus

By rationally formulating thermoplastic resin and inorganic filler in the chip bonding sheet and optimizing its modulus and glass transition temperature, the problem of difficulty in balancing the pick-up and bonding performance of the chip bonding sheet in the existing technology is solved, and efficient semiconductor device manufacturing is achieved. .

CN118725762APending Publication Date: 2024-10-01NITTO DENKO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410305907.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-02-09
Filing Date
2024-03-18
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

It is difficult to balance the pick-up performance and bonding performance of chip bonding sheets in semiconductor devices with the existing technology, making it difficult to simultaneously improve the efficiency and quality of the pick-up process and chip bonding process during the manufacturing process.

Method used

A die bonding sheet containing a thermoplastic resin and an inorganic filler is used. Its elastic modulus at 50°C is 2.0MPa or more and 10.0MPa or less, and its elastic modulus at 130°C is 0.1MPa or more and 1.5MPa or less. By adjusting the resin combination The proportion of materials and the content of inorganic fillers can be optimized to optimize the glass transition temperature and molecular weight distribution of the resin and improve the pick-up and bonding performance of the chip bonding sheet.

Benefits of technology

Good pickup performance at high temperatures and good chip bonding performance at low temperatures are achieved, improving the manufacturing efficiency and product quality of semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725762A_ABST
    Figure CN118725762A_ABST
Patent Text Reader

Abstract

The invention relates to a chip bonding sheet, a dicing chip bonding film, a semiconductor device, and an electronic apparatus. Provided is a die-bonding sheet containing at least a thermoplastic resin and an inorganic filler, the thermoplastic resin containing a first thermoplastic resin and a second thermoplastic resin having an average molecular weight smaller than that of the first thermoplastic resin, the die-bonding sheet having an elastic modulus of 2-10 MPa at 50 DEG C before curing, and the elastic modulus at 130 DEG C is from 0.1 MPa to 1.5 MPa (inclusive).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a die bonding sheet used, for example, when manufacturing a semiconductor device having a semiconductor integrated circuit, and a dicing die bonding film having the die bonding sheet. In addition, it relates to a semiconductor device having the die bonding sheet. In addition, it relates to an electronic device having the semiconductor device. Background Art

[0002] In the past, there is known a dicing die bonding film used in the manufacture of semiconductor devices. Such a dicing die bonding film, for example, comprises: a dicing tape, and a die bonding sheet laminated on the dicing tape and bonded to a wafer. The dicing tape comprises: a base material layer, and an adhesive layer in contact with the die bonding sheet. Such a dicing die bonding film is used, for example, as follows in the manufacture of semiconductor devices.

[0003] The method of manufacturing a semiconductor device generally includes a front process of forming a circuit surface on one side of a wafer with a highly integrated electronic circuit, and a back process of cutting out chips from the wafer with the circuit surface formed thereon and assembling them.

[0004] The post-process includes, for example, a fragile portion forming process, in which a fragile portion is formed on a semiconductor wafer by using a laser or the like, for cutting a wafer (semiconductor wafer) having a circuit surface formed thereon into small chips (die); a back grinding process, in which the surface of the wafer having the fragile portion formed thereon, which is on the opposite side to the circuit surface, is ground and cut; a mounting process, in which the surface of the wafer on the opposite side to the circuit surface is attached to a die bonding sheet, and the semiconductor wafer is fixed to a dicing tape by means of the die bonding sheet; a dicing process, in which the semiconductor wafer is singulated into chips (die) with the fragile portion as the boundary by stretching the dicing tape in the surface direction, and the gap between adjacent chips (die) is widened; a picking process, in which the die bonding sheet is peeled off from the adhesive layer, and the die in a state of being attached with the die bonding sheet is taken out; a die bonding process, in which the die in a state of being attached with the die bonding sheet is attached to an adherend by means of the die bonding sheet; and a curing process, in which the die bonding sheet attached to the adherend is cured. The semiconductor integrated circuit in the semiconductor device is manufactured, for example, through these processes.

[0005] In the manufacturing method of the semiconductor device as described above, in the picking-up process, the chip (die) with the chip bonding sheet attached is peeled off from the adhesive layer of the dicing tape, and then, in the chip bonding process, the chip (die) with the chip bonding sheet attached is pressed onto the adherend while being heated. These processes are continuously and repeatedly implemented using, for example, a picking-up chuck. Therefore, when the picking-up process and the chip bonding process are repeatedly performed, the heat of the picking-up chuck that rises due to heating is transferred to the chip bonding sheet. When the temperature of the chip bonding sheet rises, the above-mentioned peeling in the picking-up process sometimes does not occur well due to reasons such as changes in the physical properties of the chip bonding sheet.

[0006] In order to improve the peeling in the pickup step, that is, to improve the pickup performance, there is known a die-bonding sheet in which the surface roughness of the die-bonding sheet on the side in contact with the adhesive layer is designed to a specific value (eg, Patent Document 1).

[0007] Specifically, the die bond sheet described in Patent Document 1 has an arithmetic mean roughness Ra1 of 0.05 to 2.50 μm on the surface in contact with the adhesive layer, and a ratio of Ra1 to an arithmetic mean roughness Ra2 of the surface opposite to the surface in contact with the adhesive layer is 1.05 to 28.00.

[0008] According to the die bonding sheet described in Patent Document 1, even if the temperature of the pickup collet rises, a decrease in pickup performance can be suppressed.

[0009] Prior art literature

[0010] Patent Literature

[0011] Patent Document 1: Japanese Patent Application Publication No. 2022-150243 Summary of the invention

[0012] Problem that the invention aims to solve

[0013] However, even if a die bonding sheet with a surface roughness designed as described above is used, in the subsequent die bonding process, it is not necessarily possible to bond the die (die) well to the adherend with the help of the die bonding sheet. That is, for a die bonding sheet with a surface roughness designed only to a specific value, it is impossible to take into account both the pickup performance and the bonding performance (die bonding performance). Therefore, a die bonding sheet with both good pickup performance and good die bonding performance is desired.

[0014] However, it can be said that sufficient research has not yet been conducted on a die-bonding sheet having both good pickup performance and good die-bonding performance, and a dicing die-bonding film having the die-bonding sheet.

[0015] Therefore, the present invention aims to provide a die-bonding sheet and a dicing die-bonding film having both good pickup performance and good die-bonding performance. In addition, the present invention aims to provide a semiconductor device having the die-bonding sheet and an electronic device having the semiconductor device.

[0016] Solutions for solving problems

[0017] In order to solve the above-mentioned problems, the die-bonding sheet of the present invention is characterized in that:

[0018] The die-bonding sheet comprises at least a thermoplastic resin and an inorganic filler.

[0019] The thermoplastic resin comprises a first thermoplastic resin and a second thermoplastic resin having an average molecular weight smaller than that of the first thermoplastic resin.

[0020] The die-bonding sheet has an elastic modulus of 2.0 MPa to 10.0 MPa at 50° C. before curing, and an elastic modulus of 0.1 MPa to 1.5 MPa at 130° C.

[0021] The dicing die-bonding film of the present invention includes the above-mentioned die-bonding sheet and a dicing tape bonded to the die-bonding sheet.

[0022] A semiconductor device according to the present invention includes the above-mentioned die-bonding sheet.

[0023] An electronic device according to the present invention includes the above-mentioned semiconductor device. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a cross-sectional view of the dicing die-bonding film of the present embodiment cut along the thickness direction.

[0025] Figure 2A This is a cross-sectional view schematically showing a state of a stealth dicing step in a method of manufacturing a semiconductor device.

[0026] Figure 2B This is a cross-sectional view schematically showing a state of a stealth dicing step in a method of manufacturing a semiconductor device.

[0027] Figure 2C This is a cross-sectional view schematically showing a state of a stealth dicing step in a method of manufacturing a semiconductor device.

[0028] Figure 2D This is a cross-sectional view schematically showing a state of a backside grinding step in a method for manufacturing a semiconductor device.

[0029] Figure 3A It is a cross-sectional view schematically showing a state of a mounting step in a method of manufacturing a semiconductor device.

[0030] Figure 3B It is a cross-sectional view schematically showing a state of a mounting step in a method of manufacturing a semiconductor device.

[0031] Figure 4A This is a cross-sectional view schematically showing a state of a low-temperature expansion step in a method for manufacturing a semiconductor device.

[0032] Figure 4B This is a cross-sectional view schematically showing a state of a low-temperature expansion step in a method for manufacturing a semiconductor device.

[0033] Figure 4C This is a cross-sectional view schematically showing a state of a low-temperature expansion step in a method for manufacturing a semiconductor device.

[0034] Figure 5A This is a cross-sectional view schematically showing a state of an expansion step at room temperature in a method for manufacturing a semiconductor device.

[0035] Figure 5B This is a cross-sectional view schematically showing a state of an expansion step at room temperature in a method for manufacturing a semiconductor device.

[0036] Figure 6 This is a cross-sectional view schematically showing a state of a pickup step in a method of manufacturing a semiconductor device.

[0037] Figure 7 This is a cross-sectional view schematically showing a state of a die bonding step in a method of manufacturing a semiconductor device.

[0038] Figure 8 This is a cross-sectional view schematically showing a state of a wire bonding step in a method of manufacturing a semiconductor device.

[0039] Fig. 9 It is a cross-sectional view schematically showing a state of a sealing step in a method of manufacturing a semiconductor device.

[0040] Description of Reference Numerals

[0041] 1: dicing die-bonding film, 10: die-bonding sheet, 20: dicing tape, 21: base material layer, 22: adhesive layer. DETAILED DESCRIPTION

[0042] Hereinafter, one embodiment of a die-bonding sheet and a dicing die-bonding film including the die-bonding sheet of the present invention will be described with reference to the drawings.

[0043] The dicing die-bonding film 1 of this embodiment is as follows Figure 1As shown, it includes a dicing tape 20 and a die bonding sheet 10 laminated on the dicing tape 20 and bonded to a semiconductor wafer. The die bonding sheet 10 is bonded to an adherend such as a circuit board or a semiconductor chip in the manufacture of a semiconductor device having a semiconductor integrated circuit.

[0044] It should be noted that the figures in the accompanying drawings are schematic diagrams and may not be the same as the length ratios of the vertical and horizontal aspects in the actual objects.

[0045] <Die-bonding sheet of diced die-bonding film>

[0046] The die-bonding sheet 10 contains at least a thermoplastic resin and an inorganic filler. The thermoplastic resin contains a first thermoplastic resin and a second thermoplastic resin having an average molecular weight smaller than that of the first thermoplastic resin.

[0047] The die-bonding sheet 10 before curing has an elastic modulus of 2.0 MPa to 10.0 MPa at 50° C. and an elastic modulus of 0.1 MPa to 1.5 MPa at 130° C.

[0048] The die-bonding sheet 10 may further include a thermosetting resin.

[0049] Since the elastic modulus of the die bonding sheet 10 of the present embodiment at 50°C is 2.0 MPa or more and 10.0 MPa or less, the pick-up performance in the pick-up process (described in detail later) is good. In addition, since the elastic modulus at 130°C is 0.1 MPa or more and 1.5 MPa or less, the die bonding performance in the die bonding process (described in detail later) is also good.

[0050] In detail, the tensile modulus (tensile storage modulus E' measured by the following measurement method) of the die bonding sheet 10 at 50°C before heat curing treatment is 2.0 MPa or more and 10.0 MPa or less. The tensile modulus can be 3.0 MPa or more, or 4.0 MPa or more. By making the tensile modulus at 50°C larger, better pickup performance can be achieved.

[0051] It should be noted that the tensile modulus may be 9.0 MPa or less, or 8.0 MPa or less.

[0052] In addition, the tensile modulus of the die bonding sheet 10 at 130°C before heat curing (tensile storage modulus E' measured by the following measurement method) is 0.1 MPa or more and 1.5 MPa or less. The tensile modulus can be 1.3 MPa or less, or 1.0 MPa or less. By making the tensile modulus at 130°C smaller, better die bonding performance can be achieved.

[0053] It should be noted that the tensile modulus may be 0.2 MPa or more, or 0.3 MPa or more.

[0054] The tensile modulus of the chip bonding sheet 10 can be increased, for example, by increasing the ratio of the total amount of the thermoplastic resin and the thermosetting resin in the chip bonding sheet 10, or by reducing the content of the inorganic filler in the chip bonding sheet 10. On the other hand, for example, by reducing the ratio of the total amount of the thermoplastic resin and the thermosetting resin in the chip bonding sheet 10, or by increasing the content of the inorganic filler in the chip bonding sheet 10, the tensile modulus can be reduced.

[0055] The above-mentioned tensile modulus is measured under the following measurement conditions.

[0056] ·Measurement device: Solid viscoelasticity measurement device

[0057] For example, Rheometric Scientific (TA Instruments) manufactures "RSA-G2"

[0058] ·Measurement sample: thickness 200 μm (made by laminating die-bonding sheets)

[0059] Test piece: strip with a width of 10 mm and a length of 50 mm, initial distance between chucks 22.5 mm

[0060] ·Measurement mode: stretch mode

[0061] Frequency 1 Hz, heating rate 10°C / min, strain 0.1%

[0062] ·Measurement temperature range: -20℃~200℃

[0063] · Read the tensile storage modulus E' [MPa] at 50°C and 130°C

[0064] The glass transition temperature of the first thermoplastic resin and the glass transition temperature of the second thermoplastic resin may both be above 0°C and below 30°C. When the glass transition temperature is within the above range, by changing the amount ratio of the first thermoplastic resin and the second thermoplastic resin, the above elastic modulus of the die bonding sheet 10 at 50°C can be more easily adjusted (controlled). In addition, the elongation at break and the breaking strength of the die bonding sheet 10 at -15°C can be more easily adjusted (controlled). In addition, the peeling force at 50°C between the die bonding sheet 10 and the dicing tape 20 can be more easily adjusted (controlled) (described in detail later).

[0065] By making the glass transition temperature of the first thermoplastic resin and the second thermoplastic resin above 0°C, the pickup performance in the pickup process (described in detail later) can be improved. In addition, the cutting property of the die bonding sheet 10 can be improved. On the other hand, by making the above-mentioned glass transition temperature below 30°C, the adhesion of the die bonding sheet 10 to the adherend can be further increased.

[0066] The glass transition temperatures of the first thermoplastic resin and the second thermoplastic resin can be increased, for example, by synthesizing each resin with a monomer composition that adds a monomer that further increases the glass transition temperature of each thermoplastic resin. On the other hand, for example, by synthesizing each resin with a monomer composition that adds a monomer that further decreases the glass transition temperature of each thermoplastic resin, the glass transition temperatures of the first thermoplastic resin and the second thermoplastic resin can be decreased.

[0067] The glass transition temperature is measured before the die-bonding sheet 10 is subjected to a curing treatment, and is calculated based on the storage modulus E′ and the loss modulus E″ obtained when the tensile modulus is measured.

[0068] Specifically, the storage modulus E' and the loss modulus E", are measured while the temperature is raised, and Tan δ is calculated for each temperature using the calculation formula Tan δ = E", / E'. A higher Tan δ indicates a higher viscosity.

[0069] The temperature at which Tan δ becomes maximum (the top of the portion where Tan δ shows a peak shape) is defined as the above-mentioned glass transition temperature.

[0070] In this embodiment, the thermoplastic resin includes a first thermoplastic resin and a second thermoplastic resin having different average molecular weights. Specifically, the average molecular weight of the first thermoplastic resin is larger than the average molecular weight of the second thermoplastic resin.

[0071] The thermoplastic resin preferably includes an acrylic resin obtained by polymerizing at least a (meth)acrylate monomer. More preferably, the thermoplastic resin includes a first acrylic resin and a second acrylic resin having a mass average molecular weight less than that of the first acrylic resin as measured by gel permeation chromatography (GPC). Further preferably, the mass average molecular weight Mw of the first acrylic resin as measured by GPC is 500,000 to 1,500,000, and the mass average molecular weight Mw of the second acrylic resin is 10,000 to 100,000.

[0072] The first acrylic resin and the second acrylic resin, which are the thermoplastic resins, are each a polymer obtained by polymerizing at least a (meth)acrylic acid ester monomer.

[0073] In addition, in this specification, the expression "(meth)acrylic acid" means at least one of methacrylic acid and acrylic acid, and the expression "(meth)acrylate" means at least one of methacrylate and acrylate.

[0074] Among the above-mentioned acrylic resins (the first acrylic resin and the second acrylic resin), the mass ratio of the structural unit of the (meth)acrylic acid alkyl ester is preferably the highest. As the (meth)acrylic acid alkyl ester, for example, (meth)acrylic acid C2~C8 alkyl esters can be listed, and (meth)acrylic acid C2~C4 alkyl esters can be preferably listed. It should be noted that the expression such as C2 in the above-mentioned (meth)acrylic acid C2~C8 alkyl esters, etc., represents the carbon number of the alkyl part (hydrocarbon part) of the (meth)acrylic acid alkyl ester. The alkyl part is usually a saturated hydrocarbon. For example, the expression C2~C8 means that the carbon number is greater than 2 and less than 8. The same applies to the following.

[0075] The acrylic resin may further include a structural unit derived from a glycidyl group-containing monomer in addition to the structural unit derived from the (meth)acrylic acid alkyl ester monomer.

[0076] In addition, in addition to the structural units derived from the (meth)acrylic acid alkyl ester monomer, the above-mentioned acrylic resin may further contain structural units derived from, for example, carboxyl group-containing monomers, acid anhydride monomers, hydroxyl (hydroxyl) group-containing monomers, sulfonic acid group-containing monomers, phosphoric acid group-containing monomers, acrylamide, acrylonitrile and other polar functional group-containing monomers, or other various multifunctional monomers.

[0077] The acrylic resin is preferably a copolymer of at least an alkyl (meth)acrylate, particularly an alkyl (meth)acrylate having an alkyl moiety with 8 or less carbon atoms, and a glycidyl group-containing (meth)acrylate.

[0078] When the acrylic resin has a glycidyl group, a carboxyl group, a hydroxyl group or the like in the molecule, the glycidyl group or the like may be present in a side chain, and specifically, may be present at a terminal of a side chain.

[0079] When the thermoplastic resin (including the first acrylic resin and the second acrylic resin) is measured by gel permeation chromatography (GPC), since the average molecular weight of the second acrylic resin is smaller than that of the first acrylic resin, the graph showing the molecular weight distribution obtained by the measurement has at least two peaks separated from each other on the low molecular side and the high molecular side. In the graph showing the molecular weight distribution, the two peak vertices are separated from each other. In other words, even if the peak tails of the two peaks overlap each other, the above graph also has two peaks whose vertices are separated from each other.

[0080] The mass average molecular weight Mw and the like of the first acrylic resin and the second acrylic resin are determined by GPC measurement, which will be described in detail later.

[0081] The mass average molecular weight Mw of the first acrylic resin may be 500,000 or more and 1,500,000 or less, or 600,000 or more and 1,300,000 or less.

[0082] By making the mass average molecular weight of the first acrylic resin greater than or equal to 500,000, the cohesive force of the die bonding sheet 10 is further improved in the die bonding process (described in detail later), and the adhesive force of the die bonding sheet 10 can be further improved. In addition, by making the mass average molecular weight of the first acrylic resin less than or equal to 1.5 million, the wettability of the die bonding sheet 10 is further improved in the die bonding process (described in detail later), and the adhesive force of the die bonding sheet 10 can be further improved.

[0083] The mass average molecular weight Mw of the second acrylic resin may be 10,000 or more and 100,000 or less, or 20,000 or more and 80,000 or less.

[0084] By making the mass average molecular weight of the second acrylic resin greater than or equal to 10,000, the reliability of the die bonding sheet 10 in the reflow process (described in detail later) can be more fully ensured. In addition, by making the mass average molecular weight of the second acrylic resin less than or equal to 100,000, the wettability of the die bonding sheet 10 in the die bonding process (described in detail later) can be further improved.

[0085] Details of GPC measurement conditions are as follows.

[0086] [Preparation of measurement samples]

[0087] (1) A sample of about 0.2 g was obtained from the die-bonding sheet before the curing treatment.

[0088] (2) The sample wrapped in the mesh sheet was immersed in about 30 mL of toluene at room temperature for one week.

[0089] (3) The mesh sheet is taken out from toluene to remove the toluene insoluble components remaining in the mesh sheet, thereby obtaining a toluene solution containing toluene soluble components.

[0090] (4) The toluene solution is subjected to a reduced pressure treatment at a temperature of 45° C. or lower to remove toluene from the toluene solution to obtain a solid substance of a toluene-soluble component.

[0091] (5) The solid substance was dissolved in tetrahydrofuran (THF) so that the concentration of the solid substance became 0.2 mass % to prepare a THF solution, and the solution was left to stand overnight.

[0092] (6) The THF solution left overnight was filtered through a membrane filter (0.45 μm), and the obtained filtrate was used as a measurement sample.

[0093] [GPC measurement conditions]

[0094] · Apparatus: Gel Permeation Chromatography Apparatus

[0095] (For example, the product name of Tosoh Corporation is "HLC-8220GPC")

[0096] · Columns: 3 in total

[0097] 1 TSKgel quaudcolumn SuperHZ-L (hereinafter referred to as the first column) manufactured by Tosoh Corporation, and 2 TSKgel SuperHAM-M (hereinafter referred to as the second column) manufactured by Tosoh Corporation

[0098] Two second columns are connected in series on the downstream side of the first column, and the columns are arranged so that an eluent described later can flow in from the first column side.

[0099] Column temperature: 40℃

[0100] ·Eluent: Tetrahydrofuran (THF)

[0101] Flow rate: Sample pump flow rate 0.3mL / min

[0102] Reference pump flow rate 1.0mL / min

[0103] Injection volume: 10 μL (sample concentration is 0.2 mass % as described above)

[0104] Detector: Differential refractive index detector (RI)

[0105] ·Standard material: Standard polyethylene

[0106] In order to obtain a molecular weight distribution curve based on GPC measurement, two standard polystyrenes with different molecular weights were used as standard substances. Specifically, each standard polyethylene was measured in a manner to obtain a predetermined blending mass, and each measured standard polyethylene was dissolved in 100 mL of THF to prepare a standard polyethylene solution STD1 and a standard polyethylene solution STD2. These standard polyethylene solutions were also subjected to GPC measurement using the above-mentioned measuring device and the above-mentioned measuring conditions.

[0107] The GPC measurement results of the measurement sample and the standard polyethylene solution were analyzed using analysis software GPC-8020 Model II (data management Version 5.10) manufactured by Tosoh Corporation.

[0108] In the data analysis using the above analysis software, first, calibration curves for STD1 and STD2 are prepared (calibration curves with time (min) on the horizontal axis and logarithm of mass average molecular weight on the vertical axis). Data analysis related to the molecular weight of the above measurement sample is performed based on these calibration curves.

[0109] The data analysis related to the molecular weight of the above-mentioned measured sample is performed after obtaining the molecular weight distribution curve of the peak P1 (the peak on the highest molecular weight side) detected earliest on the chromatographic column. The data analysis is performed on the molecular weight distribution curve of the peak P1 to obtain the mass average molecular weight Mw of the peak P1. Since the chip bonding sheet contains both the first acrylic resin and the second acrylic resin, the peak P1 is equivalent to the peak of the first acrylic resin.

[0110] It should be noted that, when the descending portion of the earliest detected peak P1 overlaps with the ascending portion of the peak P2 detected next to the peak P1, a baseline is drawn in a manner extending in the horizontal direction with the ascending start portion of the peak P1 as the base point. Next, a line is drawn vertically from the aforementioned baseline toward the valley portion (the most depressed portion) generated between the descending portion of the peak P1 and the ascending portion of the peak P2. Then, the area divided by the line from the ascending start portion of the peak P1 to the aforementioned valley portion, the aforementioned baseline, and the line drawn vertically from the aforementioned baseline toward the aforementioned valley portion is taken as the analysis object, and the mass average molecular weight Mw of the peak P1 is obtained.

[0111] The same operation is performed to obtain the mass average molecular weight Mw of peak P2. The baseline of peak P2 is drawn in a manner extending horizontally toward the descending part of peak P2 with the rising beginning part of peak P1 as the base point. A line is drawn vertically from the baseline of peak P2 toward the valley part (the most depressed part) generated between the descending part of peak P1 and the rising part of peak P2. Then, the area divided by the line from the valley part to the descending end part of peak P2, the baseline of the aforementioned peak P2, and the line drawn vertically from the baseline of the aforementioned peak P2 toward the aforementioned valley part is taken as the analysis object of peak P2 to obtain the mass average molecular weight Mw of peak P2.

[0112] The peak P2 appears on the right side of the peak P1 in the GPC measurement chart, and corresponds to the peak of the second acrylic resin.

[0113] When the acrylic resin has a glycidyl group in the molecule, the epoxy equivalent of the acrylic resin may be 200 [g / eq] or more and 7000 [g / eq] or less. The epoxy equivalent may be 400 [g / eq] or more and 5000 [g / eq] or less.

[0114] <Epoxy Equivalent of Acrylic Resin>

[0115] The epoxy equivalent of the acrylic resin is measured by nuclear magnetic resonance analysis (NMR analysis) as follows.

[0116] [Sample preparation]

[0117] About 350 mg of chromium (III) acetylacetonate (molecular weight 349.32 g / mol) as a relaxation reagent was weighed and fixed to 20 mL with CDCl3 to a concentration of 50 mM. Thereafter, about 50 mg of a hexamethyldisiloxane standard (molecular weight 162.38 g / mol) as an internal standard was weighed and fixed to 10 mL with CDCl3 (the aforementioned liquid) containing chromium (III) acetylacetonate as a quantitative standard solution for NMR measurement.

[0118] Next, weigh about 40 mg of the sample to be measured, add 0.5 mL of the quantitative standard solution to dissolve it, and perform 13 Determination of epoxy equivalent [g / eq] by C NMR (NNE, absolute quantitative method).

[0119] [Analysis device]

[0120] Magnetic resonance imaging device

[0121] [Measurement conditions]

[0122] Observation frequency: 150MHz( 13 C)

[0123] Determination solvent: CDCl3

[0124] Measurement temperature: 300K

[0125] Chemical shift standard: Determination of solvent ( 13 C: 77.05ppm)

[0126] [Calculation formula of epoxy equivalent]:

[0127]

[0128] In the chip bonding sheet 10 of the present embodiment, the mass ratio of the second acrylic resin to the first acrylic resin is preferably less than 1.5, and more preferably less than 1.0. In other words, it is more preferred that the content of the first acrylic resin is greater than the content of the second acrylic resin. By making the above-mentioned mass ratio less than 1.5, the proportion of the first acrylic resin increases, so the cohesive force of the chip bonding sheet 10 is further improved at high temperatures (e.g., 130° C.), and the adhesive force of the chip bonding sheet 10 can be further improved. In addition, the reliability of the chip bonding sheet 10 in the reflow process (described in detail later) can be more fully ensured.

[0129] The mass ratio may be 0.1 or more, or 0.2 or more. By making the mass ratio 0.1 or more, the die bonding sheet 10 can be cut better in the expansion process (described later). In addition, the adhesion of the die bonding sheet 10 to the adherend can be better when the die bonding sheet 10 is bonded to the adherend.

[0130] The die-bonding sheet 10 of the present embodiment preferably contains 50.0 mass % or more and 95.0 mass % or less of a thermoplastic resin (particularly the above-mentioned acrylic resin), and more preferably contains 70 mass % or less.

[0131] By making the die bonding sheet 10 contain more thermoplastic resin (especially the acrylic resin mentioned above), there is an advantage that the elastic modulus of the die bonding sheet 10 at high temperature can be easily controlled by changing the type of thermoplastic resin. On the other hand, by making the die bonding sheet 10 contain a smaller amount of thermoplastic resin (especially the acrylic resin mentioned above), the cohesive force of the die bonding sheet 10 after thermal curing can be improved, and the reliability of the die bonding sheet 10 can be more fully ensured.

[0132] The die-bonding sheet 10 of this embodiment preferably contains 20.0 mass % or more of the first acrylic resin, more preferably 30.0 mass % or more, and further preferably 40.0 mass % or more. The die-bonding sheet 10 may contain 70.0 mass % or less of the first acrylic resin, preferably 65.0 mass % or less.

[0133] By making the die bonding sheet 10 contain 20.0 mass % or more and 65.0 mass % or less of the first acrylic resin, it is easy to control the elastic modulus of the die bonding sheet 10 at high temperature by changing the type of thermoplastic resin. In addition, both the cohesive force and wettability of the die bonding sheet 10 after thermal curing can be appropriately improved.

[0134] The die-bonding sheet 10 of the present embodiment preferably contains 40.0 mass % or less, more preferably 35.0 mass % or less of the second acrylic resin. The die-bonding sheet 10 may contain 5.0 mass % or more, preferably 10.0 mass % or more of the second acrylic resin.

[0135] When the die-bonding sheet 10 contains 5.0 mass % or more and 40.0 mass % or less of the second acrylic resin, the wettability of the die-bonding sheet 10 at high temperatures becomes better, and the splitting property of the die-bonding sheet 10 can be easily controlled by changing the type of the thermoplastic resin.

[0136] Commercially available products can be used as the first acrylic resin and the second acrylic resin, respectively. The first acrylic resin and the second acrylic resin can be synthesized by, for example, performing a polymerization reaction using an acrylic monomer such as (meth)acrylic acid alkyl ester by a common method.

[0137] In the die-bonding sheet 10 of the present embodiment, the elongation at break at -15° C. may be 0.2% or more. The elongation at break may be 2.0% or less, or 1.5% or less.

[0138] By setting the elongation at break at -15°C to 0.2% or more, the die-bonding sheet 10 can be further prevented from being cracked during processing or transportation. In addition, by setting the elongation at break to 2.0% or less, the splitting property of the die-bonding sheet 10 in the low-temperature expansion process (described in detail later) can be further improved.

[0139] The elongation at break at -15°C can be increased, for example, by reducing the amount of the second acrylic resin in the die-bonding sheet 10. On the other hand, the elongation at break at -15°C can be reduced, for example, by increasing the amount of the second acrylic resin in the die-bonding sheet 10.

[0140] In the die-bonding sheet 10 of the present embodiment, the breaking strength at -15°C can be 1.0 kg / mm 2 The breaking strength can be 7.5kg / mm 2 Below, can also be 6.0kg / mm 2 the following.

[0141] By making the breaking strength at -15°C 1.0 kg / mm 2 As described above, it is possible to further prevent the die-bonding sheet 10 from being broken during processing or transportation. 2 Thereby, the dividing property of the die-bonding sheet 10 in the low-temperature expansion process (described in detail later) can be further improved.

[0142] The breaking strength at -15°C can be increased, for example, by reducing the amount of the second acrylic resin in the die-bonding sheet 10. On the other hand, for example, by increasing the amount of the second acrylic resin in the die-bonding sheet 10, the breaking strength can be reduced.

[0143] The elongation at break (elongation at break) and the breaking strength of the die-bonding sheet 10 at −15° C. were measured under the following measurement conditions before the die-bonding sheet 10 was cured.

[0144] ·Measurement device: Solid viscoelasticity measurement device

[0145] ·Measurement sample: Thickness 20 μm (If the thickness is less than 20 μm, for example, in the case of a 5 μm die-bonding sheet, the sheets are stacked so that the total thickness becomes 20 μm)

[0146] Test piece: strip with a width of 10 mm and a length of 50 mm, initial distance between chucks 20 mm

[0147] ·Stretching speed: 1mm / sec,

[0148] ·Measurement temperature: -15℃ (start measurement after keeping at -15℃ for 5 minutes)

[0149] The elongation at break is taken as the elongation at break (elongation at break), and the test force at break is taken as the breaking strength.

[0150] The die-bonding sheet 10 of the present embodiment further contains, for example, a thermosetting resin.

[0151] Examples of thermosetting resins include epoxy resins, phenolic resins, amino resins, unsaturated polyester resins, polyurethane resins, silicone resins, and thermosetting polyimide resins. As the thermosetting resins, only one type or two or more types may be used. The thermosetting resin may include, for example, at least one of an epoxy resin and a phenolic resin, or may include a phenolic resin.

[0152] In the die bonding sheet 10 of the present embodiment, the content of the thermosetting resin is preferably 40% by mass or less, more preferably 30% by mass or less, and further preferably 20% by mass or less. By making the content of the thermosetting resin in the die bonding sheet 10 lower, the curing of the die bonding sheet 10 can be made to proceed more slowly.

[0153] In the chip bonding sheet 10 of the present embodiment, the content of the thermosetting resin is, for example, 5% by mass or more. By making the content of the thermosetting resin in the chip bonding sheet 10 higher, the chip bonding sheet 10 can be bonded to the adherend with a higher bonding strength, and the heat-resistant reliability of the chip bonding sheet 10 at high temperatures such as during reflow can be improved.

[0154] In the die-bonding sheet 10 of the present embodiment, the content of the thermosetting resin may be 0% by mass or more (ie, may be 0% by mass or more). The content of the thermosetting resin is preferably 5% by mass or more, and more preferably 7% by mass or more.

[0155] Examples of the epoxy resin include bisphenol A type, bisphenol F type, bisphenol S type, brominated bisphenol A type, hydrogenated bisphenol A type, bisphenol AF type, biphenyl type, naphthalene type, fluorene type, phenol novolac type, o-cresol novolac type, trihydroxyphenylmethane type (trisphenolmethane type), tetraphenolethane type, hydantoin type, triglycidyl isocyanurate type, and glycidylamine type epoxy resins.

[0156] The epoxy equivalent [g / eq] of the epoxy resin may be, for example, 90 or more and 220 or less.

[0157] Phenolic resin can function as a curing agent for epoxy resin. In addition, the hydroxyl group of phenolic resin can undergo a cross-linking reaction with a glycidyl group. Therefore, when the acrylic resin has a glycidyl group in the molecule, the acrylic resin and the phenolic resin can undergo a cross-linking reaction.

[0158] Examples of the phenolic resin include novolac-type phenolic resins, resol-type phenolic resins, and polyoxystyrene such as polyoxystyrene.

[0159] Examples of the novolac type phenol resin include phenol novolac resin, phenol aralkyl resin (biphenyl aralkyl type resin phenol resin, etc.), cresol novolac resin, tert-butylphenol novolac resin, nonylphenol novolac resin, and phenol xylylene resin.

[0160] The hydroxyl equivalent [g / eq] of the phenol resin may be, for example, 150 or more and 250 or less.

[0161] As the phenol resin, a biphenyl aralkyl type resin phenol resin having a relatively large hydroxyl equivalent is preferred from the viewpoint that the elastic modulus of the die-bonding sheet 10 can be appropriately reduced.

[0162] As the phenol resin, only one type may be used or two or more types may be used.

[0163] The chip bonding sheet 10 of the present embodiment may include a thermoplastic resin other than the acrylic resin. Examples of thermoplastic resins other than the acrylic resin include natural rubber, butyl rubber, isoprene rubber, chloroprene rubber, ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, polybutadiene resin, polycarbonate resin, thermoplastic polyimide resin, polyamide resins such as 6-polyamide resin and 6,6-polyamide resin, phenoxy resin, saturated polyester resins such as PET and PBT, polyamide-imide resin, and fluororesin.

[0164] As the above-mentioned thermoplastic resin, only one kind may be used or two or more kinds may be used.

[0165] The die-bonding sheet 10 of this embodiment contains an inorganic filler. By changing the amount of the inorganic filler in the die-bonding sheet 10 , the elasticity and viscosity of the die-bonding sheet 10 can be more easily adjusted, and the physical properties such as electrical conductivity, thermal conductivity, and elastic modulus of the die-bonding sheet 10 can also be adjusted.

[0166] As the inorganic filler, for example, fillers containing silicon dioxide such as aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, calcium silicate, magnesium silicate, calcium oxide, magnesium oxide, aluminum oxide, aluminum nitride, boron nitride, crystalline silicon dioxide, amorphous silicon dioxide, etc. can be listed. In addition, as the material of the inorganic filler, metal single substances, alloys, etc. such as aluminum, gold, silver, copper, and nickel can be listed. The inorganic filler can also be aluminum borate whiskers, amorphous carbon black, graphite, etc. The shape of the inorganic filler can be various shapes such as spherical, needle-shaped, and flaky. As the inorganic filler, only one or more of the above-mentioned can be used.

[0167] As the inorganic filler, a silica filler is preferred. The -OH group on the surface of the silica particles reacts easily with the acrylic resin (containing a glycidyl group in the molecule) during the curing process, which has the advantage that the die-bonding sheet 10 can be cured more fully.

[0168] The average particle size of the inorganic filler (average particle size of primary particles) can be, for example, more than 1 nm and less than 500 nm. The average particle size of the inorganic filler is preferably more than 5 nm and less than 200 nm, more preferably less than 100 nm, further preferably less than 50 nm, particularly preferably less than 20 nm, and most preferably less than 15 nm. From the perspective that the cutting property of the chip bonding sheet 10 before the curing treatment can be better, the average particle size is preferably less than 500 nm, more preferably less than 200 nm, and further preferably less than 100 nm. In addition, in order to obtain a thinner chip bonding sheet 10, it is preferred that the average particle size of the inorganic filler is smaller.

[0169] The average particle size of the inorganic filler (the average particle size of the primary particles) is measured as follows. For example, a dispersion in which an inorganic filler is dispersed is added dropwise to a flat plate, and then a drying process is implemented to prepare a sample for measurement. Using a field emission scanning electron microscope (FE-SEM), an observation image of the inorganic filler particles in the sample for measurement is obtained. For example, a scanning electron microscope "HITACHI S-4800" (accelerating voltage 5kV) is used to obtain a reflected electron image. Alternatively, for example, a scanning electron microscope "HITACHI SU8020" (accelerating voltage 5kV) is used to obtain a phase contrast image. Thereafter, each particle size of more than 1000 inorganic fillers is measured by image analysis (Image J, Image Pro), and the average value is calculated, thereby determining the average particle size of the inorganic filler. It should be noted that the above-mentioned dispersion can be prepared by mixing an inorganic filler and a solvent in a manner such that the inorganic filler concentration (solid content concentration) is less than 1% by mass.

[0170] The above-mentioned dispersion can also be prepared, for example, as follows. In detail, the organic components contained in the chip bonding sheet 10 are burned by a calcination treatment (for example, under air conditions, 500°C, 5 hours). The above-mentioned dispersion can be prepared by diluting with a solvent in a manner such that the concentration of the residual ash (solid content concentration) is less than 1% by mass. As a solvent, for example, pure water, methanol, ethanol, isopropanol, methyl ethyl ketone, chloroform, or pH-adjusted water adjusted to a pH away from the isoelectric point of the inorganic filler, etc., can be used, in which the inorganic filler can be dispersed in the form of primary particles.

[0171] In the die-bonding sheet 10 , the mass ratio of the inorganic filler to the thermoplastic resin (acrylic resin) is preferably 0.1 or more and 0.5 or less. Thereby, the die-bonding sheet 10 can have appropriate viscoelasticity.

[0172] The content of the inorganic filler is preferably 5.0 mass % or more, more preferably 10.0 mass % or more, relative to the total mass of the die-bonding sheet 10. The content of the inorganic filler is preferably 30.0 mass % or less, more preferably 25.0 mass % or less.

[0173] The die-bonding sheet 10 may contain other components as necessary. Examples of the other components include a curing catalyst, a flame retardant, a silane coupling agent, an ion scavenger, and a dye.

[0174] Examples of the flame retardant include antimony trioxide, antimony pentoxide, and brominated epoxy resins.

[0175] Examples of the silane coupling agent include β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, and γ-glycidoxypropylmethyldiethoxysilane.

[0176] Examples of the ion scavenger include hydrotalcites, bismuth hydroxide, and benzotriazole.

[0177] As the above-mentioned other additives, only one kind or two or more kinds may be used.

[0178] From the viewpoint of facilitating adjustment of elasticity and viscosity, the die-bonding sheet 10 preferably contains the first acrylic resin, the second acrylic resin, a phenolic resin, and a silica filler.

[0179] The thickness of the chip bonding sheet 10 is not particularly limited, for example, it is greater than 1 μm and less than 100 μm. The thickness can be greater than 3 μm, greater than 5 μm, or greater than 7 μm. The thickness of the chip bonding sheet 10 can be less than 50 μm, or less than 40 μm. It should be noted that when the chip bonding sheet 10 is a laminate, the above thickness is the total thickness of the laminate.

[0180] The die bonding sheet 10 is, for example, Figure 1 As shown, it may have a single-layer structure. In this specification, a single layer means a layer consisting of only one composition. A stacked state of multiple layers consisting of the same composition is also a single layer.

[0181] On the other hand, the die-bonding sheet 10 may have a multilayer structure in which layers formed of two or more different compositions are stacked. When the die-bonding sheet 10 has a multilayer structure, at least one layer constituting the die-bonding sheet 10 may contain the first acrylic resin and the second acrylic resin.

[0182] Next, embodiments of the dicing die-bonding film of the present invention will be described.

[0183] The dicing die-bonding film 1 of the present embodiment includes the above-mentioned die-bonding sheet 10 and a dicing tape 20 bonded to the die-bonding sheet 10 . The dicing tape 20 includes a base material layer 21 and an adhesive layer 22 superimposed on the base material layer 21 .

[0184] The dicing die bonding film 1 of the present embodiment is cured by irradiating active energy rays (e.g., ultraviolet rays) during use. Specifically, in a state where the die bonding sheet 10 having a semiconductor wafer bonded to one side and the adhesive layer 22 bonded to the other side of the die bonding sheet 10 are stacked, at least the adhesive layer 22 is irradiated with ultraviolet rays or the like. For example, ultraviolet rays or the like are irradiated from the side where the base material layer 21 is arranged, and the ultraviolet rays or the like pass through the base material layer 21 and reach the adhesive layer 22. The adhesive layer 22 is cured by irradiation with ultraviolet rays or the like.

[0185] The adhesive layer 22 is cured after irradiation, thereby reducing the adhesive force of the adhesive layer 22 . Therefore, the die-bonding sheet 10 (in a state where the semiconductor wafer is bonded) can be relatively easily peeled from the adhesive layer 22 after irradiation.

[0186] <Dicing tape for dicing die-bonding film>

[0187] In this embodiment, the dicing tape 20 is usually a long sheet and is stored in a rolled state until use. The dicing die-bonding film 1 of this embodiment is attached to an annular frame having an inner diameter slightly larger than the silicon wafer to be cut and used.

[0188] The elastic modulus (tensile modulus) of the dicing tape 20 at 50° C. is preferably 10 MPa or more. Therefore, in the pickup process (described in detail later), when the semiconductor chip is picked up using the adsorption jig J at a raised temperature (e.g., 50° C.), the adhesive layer 22 and the die bonding sheet 10 are easily peeled off. Therefore, the semiconductor chip can be picked up more satisfactorily.

[0189] It should be noted that the elastic modulus (tensile modulus) of the dicing tape 20 at 50° C. is preferably 100 MPa or less. This can further suppress cracking of the adhesive layer 22 in the expansion step (described in detail later).

[0190] The elastic modulus (tensile modulus) of the dicing tape 20 at 50° C. is measured in the same manner as the method for measuring the tensile modulus of the die-bonding sheet 10 before the adhesive layer 22 described in detail later is cured by active energy rays.

[0191] The base material layer 21 may be a single layer or may be composed of a plurality of layers (for example, three layers). The thickness (total thickness) of the base material layer 21 may be 80 μm or more and 150 μm or less.

[0192] Each layer of the base material layer 21 is, for example, a metal foil, a fiber sheet such as paper or cloth, a rubber sheet, a resin film, or the like.

[0193] Examples of the fiber sheet constituting the base layer 21 include paper, woven fabric, and nonwoven fabric.

[0194] As the material of the resin film, for example, polyolefins such as polyethylene (PE), polypropylene (PP), and ethylene-propylene copolymers; copolymers of ethylene such as ethylene-vinyl acetate copolymers (EVA), ionomer resins, ethylene-(meth)acrylic acid copolymers, and ethylene-(meth)acrylate (random, alternating) copolymers; polyesters such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), and polybutylene terephthalate (PBT); polyacrylates; polyvinyl chloride (PVC); polyurethane; polycarbonate; polyphenylene sulfide (PPS); polyamides such as aliphatic polyamides and wholly aromatic polyamides (aramid); polyetheretherketone (PEEK); polyimide; polyetherimide; polyvinylidene chloride; ABS (acrylonitrile-butadiene-styrene copolymer); cellulose or cellulose derivatives; silicone-containing polymers; fluorine-containing polymers, etc. These can be used alone or in combination of two or more.

[0195] The base material layer 21 is preferably made of a polymer material such as a resin film.

[0196] When the base material layer 21 includes a resin film, the resin film may be subjected to a stretching treatment or the like to control deformability such as elongation.

[0197] In order to improve the adhesion with the adhesive layer 22, the surface of the base material layer 21 may be subjected to a surface treatment. As the surface treatment, for example, a corona treatment, an antistatic treatment, a chromic acid treatment, an oxidation treatment based on a chemical method or a physical method such as ozone exposure, flame exposure, high voltage electric shock exposure, ionizing radiation treatment, etc. may be adopted. In addition, a coating treatment using a coating agent such as an anchor coating agent, a primer, an antistatic agent, an adhesive, etc. may be performed.

[0198] In order to impart releasability, the back side of the base layer 21 (the side not overlapping the adhesive layer 22 ) may be subjected to a release treatment using a release agent (release agent) such as a silicone resin or a fluorine resin.

[0199] The base material layer 21 is preferably a light-transmitting (ultraviolet-transmitting) resin film or the like, from the viewpoint of being able to apply active energy rays such as ultraviolet rays to the pressure-sensitive adhesive layer 22 from the back side.

[0200] The dicing tape 20 may include a release liner covering one surface of the adhesive layer 22 (the surface of the adhesive layer 22 not overlapping the base layer 21) before use. The release liner is used to protect the adhesive layer 22 and is removed before attaching the die-bonding sheet 10 to the adhesive layer 22.

[0201] In the present embodiment, the adhesive layer 22 includes, for example, an acrylic polymer, an isocyanate compound, and a polymerization initiator.

[0202] The adhesive layer 22 may have a thickness of 5 μm to 40 μm. The thickness of the adhesive layer 22 is preferably 10 μm or less in order to better cut the die-bonding sheet 10 . The shape and size of the adhesive layer 22 are usually the same as those of the base layer 21 .

[0203] The acrylic polymer has at least: a structural unit of an alkyl (meth)acrylate, a structural unit of a hydroxyl (meth)acrylate, and a structural unit of a (meth)acrylate containing a polymerizable group in the molecule. The structural unit is a unit constituting the main chain of the acrylic polymer. Each side chain in the acrylic polymer is included in each structural unit constituting the main chain.

[0204] In the acrylic polymer contained in the adhesive layer 22, the above-mentioned structural units can be 1 H-NMR, 13 The molar ratio of the above structural units in the acrylic polymer is usually calculated from the amount (charge amount) when the acrylic polymer is obtained by polymerization.

[0205] The structural unit of the alkyl (meth)acrylate is derived from the alkyl (meth)acrylate monomer. In other words, the molecular structure after the alkyl (meth)acrylate monomer is polymerized is the structural unit of the alkyl (meth)acrylate. The term "alkyl" means a hydrocarbon part that is ester-bonded to (meth)acrylic acid.

[0206] The hydrocarbon in the alkyl portion in the structural unit of the (meth)acrylic acid alkyl ester may be a saturated hydrocarbon or an unsaturated hydrocarbon.

[0207] It should be noted that the alkyl portion preferably does not contain polar groups having oxygen (O), nitrogen (N), etc. Thus, the polarity of the acrylic polymer can be suppressed from being extremely increased. Therefore, the adhesive layer 22 can be suppressed from having excessive affinity for the chip bonding sheet 10. Therefore, the dicing tape 20 can be peeled off from the chip bonding sheet 10 more effectively. The number of carbon atoms in the alkyl portion can be 6 or more and 12 or less.

[0208] Examples of the structural unit of the alkyl (meth)acrylate include hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, and lauryl (meth)acrylate.

[0209] The acrylic polymer has a structural unit of a hydroxyl group-containing (meth)acrylate, and the hydroxyl group of the structural unit easily reacts with an isocyanate group.

[0210] By allowing the acrylic polymer having a structural unit containing a hydroxyl (meth)acrylate and an isocyanate compound to coexist in the adhesive layer 22 in advance, the adhesive layer 22 can be appropriately cured. Therefore, the acrylic polymer can be fully gelled. Therefore, the adhesive layer 22 can maintain its shape and exhibit adhesive properties.

[0211] The structural unit of the hydroxyl-containing (meth)acrylate is preferably a structural unit of a hydroxyl-containing C2-C4 alkyl (meth)acrylate. The expression "C2-C4 alkyl" indicates a hydrocarbon part and its carbon number to which (meth)acrylic acid is ester-bonded. In other words, the hydroxyl-containing C2-C4 alkyl (meth)acrylate monomer refers to a monomer obtained by ester-bonding (meth)acrylic acid and an alcohol (usually a dihydric alcohol) having a carbon number of 2 or more and 4 or less.

[0212] The hydrocarbon part of the C2-C4 alkyl group is usually a saturated hydrocarbon. For example, the hydrocarbon part of the C2-C4 alkyl group is a straight-chain saturated hydrocarbon or a branched saturated hydrocarbon. The hydrocarbon part of the C2-C4 alkyl group preferably does not contain a polar group having oxygen (O), nitrogen (N), etc.

[0213] As the structural unit of the hydroxyl group-containing C2-C4 alkyl (meth)acrylate, for example, there can be mentioned structural units of hydroxybutyl (meth)acrylate such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxyn-butyl (meth)acrylate, or hydroxyisobutyl (meth)acrylate. It should be noted that in the structural unit of hydroxybutyl (meth)acrylate, the hydroxyl group (-OH group) may be bonded to the carbon (C) at the terminal of the hydrocarbon part, or may be bonded to the carbon (C) other than the terminal of the hydrocarbon part.

[0214] The acrylic polymer described above includes a structural unit of a polymerizable group-containing (meth)acrylate having a polymerizable unsaturated double bond in a side chain.

[0215] The acrylic polymer mentioned above can be cured by irradiation of active energy rays (ultraviolet rays, etc.) before the pick-up process by containing a structural unit of (meth) acrylate containing a polymerizable group. In detail, by irradiation of active energy rays such as ultraviolet rays, free radicals are generated by a photopolymerization initiator, and by the action of the free radicals, the acrylic polymers can be cross-linked with each other. As a result, the adhesive force of the adhesive layer 22 before irradiation can be reduced by irradiation. In addition, the chip bonding sheet 10 can be well peeled off from the adhesive layer 22.

[0216] In addition, as active energy rays, ultraviolet rays, radiation rays, and electron beams can be used.

[0217] Specifically, the structural unit of the polymerizable group-containing (meth)acrylate may have a molecular structure in which an isocyanate group of an isocyanate group-containing (meth)acrylate monomer and a hydroxyl group in the structural unit of the hydroxyl group-containing (meth)acrylate are urethane-bonded.

[0218] The structural unit of the polymerizable group-containing (meth)acrylate having a polymerizable group can be prepared after the polymerization reaction of synthesizing an acrylic polymer. For example, after copolymerization of an alkyl (meth)acrylate monomer and a hydroxyl group-containing (meth)acrylate monomer, a hydroxyl group in a part of the structural unit of the hydroxyl group-containing (meth)acrylate is subjected to a urethanization reaction with an isocyanate group of an isocyanate group-containing polymerizable monomer, thereby obtaining the structural unit of the polymerizable group-containing (meth)acrylate.

[0219] The above-mentioned isocyanate group-containing (meth)acrylate monomer preferably has one isocyanate group and one (meth)acryloyl group in the molecule. Examples of such a monomer include 2-isocyanatoethyl (meth)acrylate.

[0220] The adhesive layer 22 of the dicing tape 20 in the present embodiment further contains an isocyanate compound. A part of the isocyanate compound may be in a state after reacting by a urethanization reaction or the like.

[0221] The isocyanate compound has a plurality of isocyanate groups in the molecule. By making the isocyanate compound have a plurality of isocyanate groups in the molecule, a cross-linking reaction between acrylic polymers in the adhesive layer 22 can be performed. Specifically, by making one isocyanate group of the isocyanate compound react with a hydroxyl group of an acrylic polymer and making another isocyanate group react with a hydroxyl group of another acrylic polymer, a cross-linking reaction via the isocyanate compound can be performed.

[0222] Examples of the isocyanate compound include diisocyanates such as aliphatic diisocyanates, alicyclic diisocyanates, and aromatic aliphatic diisocyanates.

[0223] Furthermore, as an isocyanate compound, polymeric polyisocyanate, such as a dimer and a trimer of a diisocyanate, and polymethylene polyphenylene polyisocyanate are mentioned, for example.

[0224] Examples of the isocyanate compound include polyisocyanates obtained by reacting an excess amount of the above isocyanate compound with an active hydrogen-containing compound. Examples of the active hydrogen-containing compound include active hydrogen-containing low molecular weight compounds and active hydrogen-containing high molecular weight compounds.

[0225] In addition, as an isocyanate compound, allophanate polyisocyanate, biuret polyisocyanate, etc. can also be used.

[0226] The above-mentioned isocyanate compounds can be used alone or in combination of two or more.

[0227] As the above-mentioned isocyanate compound, the reaction product of an aromatic diisocyanate and an active hydrogen-containing low molecular weight compound is preferred. Since the reaction rate of the isocyanate group of the reaction product of the aromatic diisocyanate is relatively slow, the adhesive layer 22 containing the reaction product can be prevented from being excessively cured. As the above-mentioned isocyanate compound, it is preferred that the isocyanate compound has three or more isocyanate groups in the molecule.

[0228] The polymerization initiator contained in the adhesive layer 22 is a compound that can initiate a polymerization reaction using the energy of applied heat or light. By making the adhesive layer 22 contain a polymerization initiator, when heat energy or light energy is applied to the adhesive layer 22, a cross-linking reaction between acrylic polymers can be carried out. In detail, a polymerization reaction between polymerizable groups can be initiated between acrylic polymers having structural units of (meth)acrylates containing polymerizable groups, thereby curing the adhesive layer 22. As a result, the adhesive force of the adhesive layer 22 can be reduced, and the chip bonding sheet 10 can be easily peeled off from the cured adhesive layer 22 during the pickup process.

[0229] As the polymerization initiator, for example, a photopolymerization initiator or a thermal polymerization initiator can be used. As the polymerization initiator, a general commercially available product can be used.

[0230] The adhesive layer 22 may also contain other components in addition to the above components. Examples of other components include tackifiers, plasticizers, fillers, antioxidants, antioxidants, ultraviolet absorbers, light stabilizers, heat stabilizers, antistatic agents, surfactants, and light peeling agents. The types and amounts of other components may be appropriately selected according to the purpose.

[0231] The peeling force between the dicing tape 20 and the die-bonding sheet 10 may be within a predetermined range. Specifically, the peeling force between the adhesive layer 22 of the dicing tape 20 and the die-bonding sheet 10 at 50° C. may be 0.03 N / 20 mm or more and 0.20 N / 20 mm or less.

[0232] By setting the peeling force within the above range, the semiconductor chip X can be well picked up by the suction jig J even if the temperature of the suction jig J for peeling the semiconductor chip X and the small die-bonding sheet 10 ′ from the adhesive layer 22 rises in the pickup step described in detail later.

[0233] The peeling force between the die-bonding sheet 10 and the adhesive layer 22 (after curing treatment) of the dicing tape 20 was measured as follows.

[0234] A liner tape (product name "BT-315", manufactured by Nitto Denko Corporation) is attached to the die bonding sheet 10 of the cut die bonding film 1. Then, a test piece with a width of 50 mm and a length of 120 mm is cut out. Using the cut test piece, a T-type peel test is performed using a tensile testing machine (e.g., "Autograph AGS series", manufactured by Shimadzu Corporation) to measure the peeling force [N / 20 mm]. The temperature condition in the measurement is set to 50°C, and the peeling speed is set to 300 mm / min.

[0235] Before laminating the backing tape, the adhesive layer of the dicing tape was irradiated with 300 mJ / cm at a temperature of 22°C from the substrate layer side. 2 (Irradiation intensity 150mW / cm 2 , 2 seconds) of ultraviolet light to implement light curing treatment.

[0236] The dicing die bonding film 1 of this embodiment may have a release liner covering one surface of the die bonding sheet 10 (the surface of the die bonding sheet 10 that does not overlap with the adhesive layer 22) before use. The release liner is used to protect the die bonding sheet 10 and is peeled off before the adherend (e.g., semiconductor wafer) is attached to the die bonding sheet 10.

[0237] The release liner can be used as a supporting material for supporting the chip bonding sheet 10. The release liner is suitable for use when the chip bonding sheet 10 is overlapped on the adhesive layer 22. In detail, the chip bonding sheet 10 is overlapped on the adhesive layer 22 in a state where the release liner and the chip bonding sheet 10 are stacked, and the release liner is peeled off (transferred) after overlapping, thereby enabling the chip bonding sheet 10 to overlap the adhesive layer 22.

[0238] Next, a method for manufacturing the die-bonding sheet 10 and the dicing die-bonding film 1 according to the present embodiment will be described.

[0239] <Method for Manufacturing Dicing Die-Bond Film>

[0240] The method for manufacturing the dicing die-bonding film 1 according to the present embodiment includes:

[0241] A process for manufacturing the chip bonding sheet 10;

[0242] A process for making a cutting tape 20; and,

[0243] A step of overlapping the manufactured die-bonding sheet 10 and the dicing tape 20 .

[0244] <Step of Manufacturing Die-Bond Sheet>

[0245] The process of manufacturing the die bond sheet 10 includes:

[0246] a resin composition preparation step of preparing a resin composition for forming the die-bonding sheet 10; and,

[0247] In the die-bonding sheet forming step, the die-bonding sheet 10 is formed from the resin composition.

[0248] In the resin composition preparation process, for example, the first thermoplastic resin, the second thermoplastic resin, the inorganic filler, the solvent and the thermosetting resin as required are mixed, and each resin is dissolved in the solvent to prepare the resin composition. The viscosity of the composition can be adjusted by changing the amount of the solvent. It should be noted that commercially available products can be used as these resins.

[0249] In the chip bonding sheet forming process, for example, the resin composition prepared as described above is applied to a release liner. As a coating method, there is no particular limitation, for example, a common coating method such as roller coating, screen coating, gravure coating, etc. is adopted. Then, as needed, the applied composition is solidified by desolventizing treatment, curing treatment, etc. to form a chip bonding sheet 10.

[0250] <Process of Making Cutting Tape>

[0251] The process of making cutting tape includes:

[0252] A synthesis process for synthesizing acrylic polymers;

[0253] An adhesive layer preparation step of volatilizing a solvent from an adhesive composition to prepare an adhesive layer 22, wherein the adhesive composition comprises the above-mentioned acrylic polymer, an isocyanate compound, a polymerization initiator, a solvent, and other components appropriately added according to the purpose;

[0254] a base material layer manufacturing step of manufacturing the base material layer 21; and,

[0255] In the lamination step, the adhesive layer 22 and the base layer 21 are bonded together to laminate the base layer 21 and the adhesive layer 22 .

[0256] In the synthesis step, for example, an alkyl (meth)acrylate monomer and a hydroxyl group-containing (meth)acrylate monomer are radically polymerized to synthesize an acrylic polymer intermediate.

[0257] Free radical polymerization can be carried out by a common method. For example, the above-mentioned monomers can be dissolved in a solvent, stirred while heating, and a polymerization initiator can be added to synthesize an acrylic acid polymer intermediate. In order to adjust the molecular weight of the acrylic acid polymer, the polymerization can be carried out in the presence of a chain transfer agent.

[0258] Next, a part of the hydroxyl groups of the structural unit containing hydroxyl (meth)acrylate contained in the acrylic polymer intermediate is bonded to the isocyanate groups of the isocyanate group-containing polymerizable monomer by urethanization reaction. Thus, a part of the structural unit containing hydroxyl (meth)acrylate becomes a structural unit of (meth)acrylate containing a polymerizable group.

[0259] The urethanization reaction can be carried out by a common method. For example, the acrylic polymer intermediate and the isocyanate group-containing polymerizable monomer are stirred while heating in the presence of a solvent and a urethanization catalyst. In this way, the isocyanate group of the isocyanate group-containing polymerizable monomer can be urethanized with a part of the hydroxyl group of the acrylic polymer intermediate.

[0260] In the adhesive layer preparation process, for example, acrylic polymer, isocyanate compound and polymerization initiator are dissolved in solvent to prepare adhesive composition. By changing the amount of solvent, the viscosity of the composition can be adjusted. Then, the adhesive composition is applied to the release liner. As a coating method, for example, common coating methods such as roller coating, screen coating, gravure coating are adopted. By implementing desolventizing treatment, solidification treatment, etc. to the applied composition, the applied adhesive composition is solidified, thereby making adhesive layer 22.

[0261] In the substrate layer preparation process, the substrate layer can be prepared by film-making by a common method. As the film-making method, for example, a calendering film-making method, a casting method in an organic solvent, an inflation extrusion method in a closed system, a T-die extrusion method, a dry lamination method, etc. can be listed. Coextrusion molding can also be adopted. It should be noted that, as the substrate layer 21, a commercially available film, etc. can be used.

[0262] In the lamination step, the pressure-sensitive adhesive layer 22 in a state of being overlapped with the release liner is overlapped and laminated with the base layer 21. In addition, the release liner may be in a state of being overlapped with the pressure-sensitive adhesive layer 22 until before use.

[0263] In order to promote the reaction between the crosslinking agent and the acrylic polymer and the surface of the base layer 21 , an aging treatment step may be performed at 50° C. for 48 hours after the lamination step.

[0264] Through these steps, the dicing tape 20 can be manufactured.

[0265] <Step of Overlaying the Die-Bond Sheet 10 and the Dicing Tape 20>

[0266] In the step of overlapping the die-bonding sheet 10 and the dicing tape 20 , the die-bonding sheet 10 is attached to the pressure-sensitive adhesive layer 22 of the dicing tape 20 manufactured as described above.

[0267] During the pasting, the release liner is peeled off from the adhesive layer 22 of the dicing tape 20 and the die bonding sheet 10, respectively, and the two are bonded in a manner that the die bonding sheet 10 is in direct contact with the adhesive layer 22. For example, bonding can be performed by crimping. The temperature during bonding is not particularly limited, for example, it is a temperature above room temperature, above 30°C and below 50°C, preferably above 35°C and below 45°C. The linear pressure during bonding is not particularly limited, preferably above 0.1kgf / cm and below 20kgf / cm, more preferably above 1kgf / cm and below 10kgf / cm.

[0268] The dicing die-bonding film 1 manufactured as described above through the above steps is used as an auxiliary tool for manufacturing a semiconductor device having a semiconductor integrated circuit, for example.

[0269] <Method of using dicing die-bonding film when manufacturing semiconductor devices>

[0270] In a method for manufacturing a semiconductor device, generally, chips are cut out from a semiconductor wafer having a circuit surface formed thereon and assembled. In this case, the dicing die-bonding film of the present embodiment is used as a manufacturing auxiliary tool.

[0271] A general method for manufacturing a semiconductor device includes a step of cutting chips from a semiconductor wafer having a circuit surface formed thereon and assembling the chips.

[0272] The process includes, for example, a stealth dicing process, in which a fragile portion is formed inside a semiconductor wafer with a back grinding tape attached thereto by using a laser, and preparation is made for processing the semiconductor wafer into a chip (die) by cutting; a back grinding process, in which a semiconductor wafer with a back grinding tape attached thereto on a circuit surface is ground to reduce the thickness of the semiconductor wafer; a mounting process, in which one side of the semiconductor wafer with a reduced thickness (for example, the side on the opposite side to the circuit surface) is attached to a chip bonding sheet 10, and the semiconductor wafer is fixed to a dicing tape 20; and an expansion process, in which the dicing tape 20 is stretched, thereby bonding the semiconductor wafer and the chip bonding sheet. 10 is cut and the interval between the chips is enlarged at the same time; a picking process is performed to peel off the chip bonding sheet 10 and the adhesive layer 22 so as to take out the semiconductor chip (die) with the chip bonding sheet 10 attached; a chip bonding process is performed to bond the chip bonding sheet 10 attached to the semiconductor chip (die) to the adherend; a curing process is performed to cure the chip bonding sheet 10 attached to the adherend; a wire bonding process is performed to electrically connect the electrodes of the electronic circuit in the semiconductor chip (die) to the adherend using the wire; and a sealing process is performed to seal the semiconductor chip (die) and the wire on the adherend with a thermosetting resin. When implementing any of these processes, at least a part of the dicing tape (dicing chip bonding film) of this embodiment is used as a manufacturing auxiliary tool.

[0273] In the invisible cutting process, Figure 2A to Figure 2C As shown in FIG. 1 , a fragile portion for singulating the semiconductor wafer W into small pieces (dies) is formed inside the semiconductor wafer W. Specifically, the back grinding tape G is attached to the circuit surface of the semiconductor wafer W (see FIG. 1 ). Figure 2A ). With the back grinding tape G attached, grinding is performed using a grinding pad K until the semiconductor wafer W reaches a predetermined thickness (preliminary back grinding) (see Figure 2B ). By irradiating the thinned semiconductor wafer W with laser light, a fragile portion is formed inside the semiconductor wafer W (refer to Figure 2C ).

[0274] During the back grinding process, Figure 2D As shown, the semiconductor wafer W with the back grinding tape G attached thereto is further subjected to grinding to reduce the thickness of the semiconductor wafer W to a thickness corresponding to a chip (die) to be produced by subsequent dicing.

[0275] During the installation process, Figure 3A to Figure 3B As shown in FIG. 1 , the semiconductor wafer W is fixed to the dicing die bonding film 1. Specifically, a dicing ring R is mounted on the adhesive layer 22 of the dicing tape 20, and the semiconductor wafer W (see FIG. 1 ) thinned by cutting as described above is attached to the exposed surface of the die bonding sheet 10. Figure 3A ). Next, the back grinding tape G is peeled off from the semiconductor wafer W (see Figure 3B ).

[0276] In the expansion process, Figure 4A to Figure 4C As shown in FIG. 1 , the semiconductor wafer W is cut by stretching the dicing tape 20, thereby widening the interval between adjacent semiconductor chips (die) X. Specifically, after the dicing ring R is attached to the adhesive layer 22 of the dicing tape 20, the dicing ring R is fixed to the holder H (see FIG. 1 ) of the expansion device. Figure 4A ). The lifting member U provided in the expansion device is lifted from the lower side of the dicing die-bonding film 1, thereby stretching the dicing die-bonding film 1 to expand in the surface direction (refer to Figure 4B ). Thus, the semiconductor wafer W is cut under a specific temperature condition. The temperature condition is, for example, above -20°C and below 0°C, preferably above -15°C and below 0°C, and more preferably above -10°C and below -5°C. By lowering the lifting member U, the expanded state is released (see Figure 4C , so far it is a low temperature expansion process).

[0277] When the expansion process is performed at a low temperature like this, it is necessary to cut the die-bonding sheet 10. The die-bonding sheet 10 of the present embodiment described above is designed so as to be well cut at this time.

[0278] Furthermore, in the expansion process, Figure 5A to Figure 5B As shown, the dicing tape 20 is stretched under a higher temperature condition (e.g., 10°C to 25°C) to expand the area. Thus, the adjacent semiconductor chips X after cutting are separated in the plane direction of the film surface, and the cut (interval) is further expanded (room temperature expansion process).

[0279] During the picking process, Figure 6 As shown, the semiconductor chip X in a state where the die-bonding sheet 10' is attached is peeled off from the adhesive layer 22 of the dicing tape 20. Specifically, the pin member P is raised to lift up the semiconductor chip X to be picked up through the dicing tape 20. The lifted semiconductor chip X is held by a suction jig J. As the suction jig J, for example, a pickup chuck is used.

[0280] In the die bonding step, the semiconductor chip X with the die bonding sheet 10 ′ attached thereto is bonded to the adherend Z using the above-mentioned suction jig J. In the die bonding step, the semiconductor chip X is bonded to the adherend Z generally at a temperature of about 120° C. to 150° C.

[0281] It should be noted that in the chip bonding process, Figure 7 As shown, the semiconductor chips X in a state where the small pieces 10 ′ of the die-bonding sheet are attached are sometimes stacked multiple times.

[0282] In the pickup process and the chip bonding process, the adsorption jig J repeatedly performs the actions of picking up the semiconductor chip X and bonding the semiconductor chip X to the adherend Z under heating conditions. The adsorption jig J accumulates heat while repeatedly performing these actions, and the temperature may become, for example, above 100°C. When the pickup process is performed using the adsorption jig J with a rising temperature, the heat is transferred to the small piece 10' of the chip bonding sheet, and the small piece 10' is heated to, for example, about 50°C and may become soft. Moreover, it may lead to a situation where the small piece 10' may not be well peeled off from the adhesive layer 22 of the dicing tape 20. In addition, in the chip bonding process, the small piece 10' of the chip bonding sheet is bonded to the adherend Z at a relatively high temperature of about 130°C, so the small piece 10' needs to be well adhered to the adherend Z even at a relatively high temperature.

[0283] The die-bonding sheet 10 of this embodiment has a relatively high elastic modulus at 50° C. and a relatively low elastic modulus at 130° C., so both the pickup step and the die-bonding step can be performed well. That is, the die-bonding sheet 10 of this embodiment can have both good pickup performance and good die-bonding performance.

[0284] In the curing step, in order to cure the small piece 10' of the die bonding sheet, a heat treatment is performed at a temperature of, for example, 100°C to 150°C. At this time, pressure may be applied to the small piece 10' of the die bonding sheet. Preferably, the heat treatment is performed while applying a pressure of 0.2 MPa to 2 MPa, more preferably 0.4 MPa to 1 MPa.

[0285] In the wire bonding process, Figure 8 As shown, the semiconductor chip X (die) and the adherend Z are heated and connected. Thus, the glycidyl group of the acrylic resin contained in the die-bonding sheet 10 becomes reactive by heating, and the curing reaction of the die-bonding sheet 10 can proceed.

[0286] In the sealing process, Fig. 9 As shown, the semiconductor chip X (die) and the die bonding sheet 10' are sealed with a thermosetting resin M such as epoxy resin. In the sealing process, the sealing process is performed under pressure while heating at a temperature of, for example, 150°C to 200°C in order to make the thermosetting resin M flow and then solidify.

[0287] After the sealing step, a reflow step of electrically joining electrodes using molten solder may be performed. In the reflow step, a heating treatment is performed at a temperature of, for example, 230° C. to 270° C. inclusive.

[0288] In the above-mentioned method for manufacturing a semiconductor device (method for using a dicing die-bonding film), an example in which the semiconductor wafer W having a fragile portion formed therein is divided into small pieces in the expansion step is described in detail, but the present invention is not limited to this example.

[0289] For example, instead of forming a fragile portion inside the semiconductor wafer W, the semiconductor wafer W may be cut into small pieces by performing a so-called half-cut process in the expansion step.

[0290] Furthermore, for example, even in the case of a semiconductor wafer W having a fragile portion formed therein or a semiconductor wafer W subjected to a half-cut process, the semiconductor wafer W may be fragmented when the above-described preliminary backside grinding process is performed.

[0291] It should be noted that in recent years, with the further advancement of integration technology in the semiconductor industry, there is a demand for thinner semiconductor chips (for example, a thickness of more than 20 μm and less than 50 μm) and thinner chip bonding sheets (for example, a thickness of more than 1 μm and less than 40 μm, preferably less than 7 μm, and more preferably less than 5 μm).

[0292] The die-bonding sheet and the dicing die-bonding film of the present embodiment are as exemplified above, but the present invention is not limited to the die-bonding sheet and the dicing die-bonding film exemplified above.

[0293] That is, various forms used in general die-bonding sheets and dicing die-bonding films can be adopted within a range that does not impair the effects of the present invention.

[0294] Matters disclosed in this specification include the following. (1)

[0296] A die bonding sheet comprising at least a thermoplastic resin and an inorganic filler.

[0297] The thermoplastic resin comprises a first thermoplastic resin and a second thermoplastic resin having an average molecular weight smaller than that of the first thermoplastic resin.

[0298] The die-bonding sheet has an elastic modulus of 2 MPa to 10 MPa at 50° C. before curing, and an elastic modulus of 0.1 MPa to 1.5 MPa at 130° C.

[0299] The die-bonding sheet having this structure can have both good pickup performance and good die-bonding performance. (2)

[0301] The die-bonding sheet according to (1) above, wherein the average molecular weight of the first thermoplastic resin is 500,000 to 1,500,000, and the average molecular weight of the second thermoplastic resin is 10,000 to 100,000.

[0302] The glass transition temperature of the first thermoplastic resin and the second thermoplastic resin are both 0° C. or higher and 30° C. or lower. (3)

[0304] The die-bonding sheet according to (1) or (2) above, wherein the elongation at break at -15°C is 0.2% to 2.0%. (4)

[0306] The die-bonding sheet according to any one of (1) to (3) above, wherein the breaking strength at -15°C is 1.0 kg / mm 2 Above and 7.5kg / mm 2 the following. (5)

[0308] The die-bonding sheet according to any one of (1) to (4) above, wherein the inorganic filler contains silica particles. (6)

[0310] The die-bonding sheet according to any one of (1) to (5) above, further comprising a thermosetting resin. (7)

[0312] A dicing die-bonding film comprising: the die-bonding sheet according to any one of (1) to (6) above; and a dicing tape bonded to the die-bonding sheet. (8)

[0314] The dicing die-bonding film according to the above (7), wherein the dicing tape comprises a base material layer and an adhesive layer superposed on one surface of the base material layer,

[0315] The pressure-sensitive adhesive layer comprises an acrylic polymer having a structural unit of a (meth)acrylate containing a polymerizable group in a molecule.

[0316] The peel force at 50° C. between the die-bonding sheet and the dicing tape is 0.03 N / 20 mm or more and 0.20 N / 20 mm or less after the adhesive layer is cured by irradiation with active energy rays. (9)

[0318] A semiconductor device comprising the die-bonding sheet according to any one of (1) to (6) above. (10)

[0320] An electronic device comprising the semiconductor device described in (9) above.

[0321] Example

[0322] Next, the present invention will be described in more detail using experimental examples, but the present invention is not limited to these.

[0323] The die-bonding sheet was manufactured as follows: Furthermore, the die-bonding sheet was bonded to a dicing tape to manufacture a dicing die-bonding film.

[0324] <Production of Die Bonding Sheet>

[0325] The raw materials having the blending compositions shown in Tables 1 and 2 were added to methyl ethyl ketone and mixed to obtain a die-bonding sheet composition having a solid content concentration of 15% by mass. The details of each raw material are shown below.

[0326] (First thermoplastic resin)

[0327] ·[SG-P3]

[0328] First acrylic resin (containing glycidyl group)

[0329] Mass average molecular weight: Mw = 850,000

[0330] Product name: Teisan Resin SG-P3, manufactured by Nagase ChemteX Corporation

[0331] Epoxy value: 0.21[eq / kg]

[0332] Glass transition temperature Tg: 13°C

[0333] [SG-708-6]

[0334] First acrylic resin (containing carboxyl and hydroxyl groups)

[0335] Mass average molecular weight: Mw = 700,000

[0336] Product name: Teisan Resin SG-708-6, manufactured by Nagase ChemteX Corporation

[0337] Acid value: 9[mgKOH / g]

[0338] Glass transition temperature Tg: 4°C

[0339] ·[SG-70L]

[0340] First acrylic resin (containing carboxyl and hydroxyl groups)

[0341] Mass average molecular weight: Mw = 900,000

[0342] Product name: Teisan Resin SG-70L, manufactured by Nagase ChemteX Corporation

[0343] Acid value: 5[mgKOH / g]

[0344] Glass transition temperature Tg: -15℃

[0345] (Second thermoplastic resin)

[0346] ·[Polymer A]

[0347] An acrylic resin solution (solid content 70% by mass) prepared by dissolving a copolymer of ethyl acrylate (EA), butyl methacrylate (BMA) and glycidyl methacrylate (GMA) (second acrylic resin) in methyl ethyl ketone (MEK)

[0348] Mass average molecular weight: 70000 (Mw = 70,000),

[0349] Epoxy equivalent: 444[g / eq],

[0350] Glass transition temperature Tg: 11°C

[0351] ·[Polymer B]

[0352] An acrylic resin solution (solid content 70% by mass) prepared by dissolving a copolymer of ethyl acrylate (EA), butyl methacrylate (BMA) and glycidyl methacrylate (GMA) (second acrylic resin) in methyl ethyl ketone (MEK)

[0353] Mass average molecular weight: 40,000 (Mw = 40,000), epoxy equivalent: 2029 [g / eq], glass transition temperature Tg: 2°C

[0354] (Thermosetting resin)

[0355] ·[MEHC-7851SS]

[0356] Biphenyl aralkyl phenolic resin

[0357] Product name: MEHC-7851SS Made by UBE

[0358] Hydroxyl equivalent: 203[g / eq]

[0359] ·[EPPN-501HY]

[0360] Triphenolmethane type epoxy resin

[0361] Product name: EPPN-501HY Made by Nippon Kayaku Co., Ltd.

[0362] Epoxy equivalent: 166[g / eq]

[0363] (Inorganic filler)

[0364] ·[MEK-AC-2140Z]

[0365] Spherical silica dispersion

[0366] Product name: MEK-AC-2140Z Made by Nissan Chemical Co., Ltd.

[0367] Chemically modified particles

[0368] Dispersion having an average particle size of 10 nm or more and 15 nm or less and a solid content of 40% by mass

[0369] ·[MEK-AC-5140Z]

[0370] Spherical silica dispersion

[0371] Product name: MEK-AC-5140Z Made by Nissan Chemical Co., Ltd.

[0372] Chemically modified particles

[0373] Dispersion having an average particle size of 70 nm or more and 100 nm or less and a solid content of 40% by mass

[0374] [SO-E2]

[0375] Spherical silica

[0376] Product name: "Admafine SO-E2" made by Admatechs

[0377] Average particle size 500nm

[0378] <Silane coupling agent>

[0379] ·[KBM-403]

[0380] 3-Glycidoxypropyltrimethoxysilane

[0381] Product name: "KBM-403" Made by Shin-Etsu Chemical Co., Ltd.

[0382] ·[KBM-303]

[0383] 2-(3,4-Epoxycyclohexyl)ethyltrimethoxysilane

[0384] Product name: "KBM-303" Made by Shin-Etsu Chemical Co., Ltd.

[0385] Using any of the above raw materials, a composition for a die bond sheet is prepared with the blending composition shown in Table 1 and Table 2. Then, the composition for a die bond sheet is applied to one surface of a release liner (the surface of a PET sheet with a thickness of 50 μm on which a silicone treatment is implemented) using an applicator. The coating is performed in such a way that the thickness after drying becomes 40 μm, and then a drying treatment is performed at 130° C. for 2 minutes, thereby volatilizing the solvent from the composition for a die bond sheet. In this way, a die bond sheet overlapping a single surface of the release liner is obtained.

[0386] <Base material layer of dicing tape>

[0387] The products shown below were used as resin raw materials to prepare a single-layer substrate layer (thickness 100 μm).

[0388] Product name: Evaflex P1007 (manufactured by DuPont-Mitsui Polychemicals Co., Ltd.)

[0389] Ethylene-vinyl acetate copolymer resin (EVA)

[0390] Contains 9% by mass of vinyl acetate monomer units

[0391] (Formation of base material layer)

[0392] The base layer was formed using an extrusion T-die molding machine. The extrusion temperature was 190° C. The base layer was wound into a roll and stored.

[0393] <Adhesive Layer of Dicing Tape>

[0394] (Preparation of Adhesive Layer (Adhesive Composition))

[0395] The following raw materials were mixed to prepare a first resin composition.

[0396] INA (isononyl acrylate) 150 parts by mass

[0397] HEA (hydroxyethyl acrylate) 62 parts by mass

[0398] ·AIBN (2,2'-azobisisobutyronitrile) 0.4 parts by mass

[0399] 350 parts by mass of ethyl acetate

[0400] Next, the first resin composition was placed in a round-bottom separable flask of a polymerization experimental apparatus equipped with a round-bottom separable flask (capacity 1 L), a thermometer, a nitrogen inlet tube, and a stirring blade. The first resin composition was stirred, the liquid temperature of the first resin composition was adjusted to room temperature (23° C.), and the inside of the round-bottom separable flask was replaced with nitrogen for 6 hours.

[0401] Next, nitrogen was flowed into the round-bottom separable flask, and the first resin composition was stirred while the liquid temperature of the first resin composition was maintained at 62° C. for 3 hours. Thereafter, the temperature was further maintained at 75° C. for 2 hours to carry out the polymerization reaction of INA, HEA and AIBN, thereby preparing a second resin composition. Thereafter, the flow of nitrogen into the round-bottom separable flask was stopped.

[0402] After the second resin composition was cooled to room temperature, the following raw materials were added to the second resin composition to prepare a third resin composition.

[0403] ·2-Methacryloyloxyethyl isocyanate

[0404] Compounds with polymerizable carbon-carbon double bonds

[0405] Product name: "Karenz MOI", manufactured by Showa Denko K.K.) 58 parts by mass

[0406] · Dibutyltin dilaurate IV (manufactured by Wako Pure Chemical Industries, Ltd.) 0.3 parts by mass

[0407] The obtained third resin composition was stirred at 50° C. for 24 hours in an air atmosphere.

[0408] Finally, the following raw materials were added to 100 parts by mass of the polymer solid content of the third resin composition.

[0409] Isocyanate compound (product name: "TAKENATE D-101A" (manufactured by Mitsui Chemicals, Inc.) 1.0 part by mass

[0410] (Trifunctional isocyanate compound)

[0411] · Photopolymerization initiator (product name "Omnirad 127", manufactured by IGM Resins Co., Ltd.) 3 parts by mass

[0412] Then, the third resin composition was diluted with ethyl acetate so as to have a solid content concentration of 20% by mass, thereby preparing an adhesive composition.

[0413] <Production of cutting tape>

[0414] The adhesive composition was applied to one surface of the base layer using an applicator so that the thickness after drying was 10 μm. After the adhesive composition was applied, it was heated and dried at 110° C. for 3 minutes to form an adhesive layer. In this way, a dicing tape was manufactured.

[0415] <Manufacturing of Dicing Die-Bonding Film>

[0416] (Attachment of die bonding sheet to dicing tape)

[0417] The adhesive layer of the dicing tape was bonded to the die-bonding sheet (the side on which the release liner was not laminated). Thereafter, the release liner was peeled off from the die-bonding sheet to prepare a dicing die-bonding film having the die-bonding sheet.

[0418] As above, the chip bonding sheets and dicing chip bonding films of the embodiment and the comparative example were manufactured respectively. The details of each chip bonding sheet are shown in Table 1 and Table 2. It should be noted that in Table 1 and Table 2, the mixing amounts [parts by mass] of the first thermoplastic resin, the second thermoplastic resin, the thermosetting resin, the inorganic filler (silica filler), etc. are shown in the form of solid content conversion values.

[0419] [Table 1]

[0420]

[0421] [Table 2]

[0422]

[0423] <Determination of Tensile Modulus of Die-Bond Sheet>

[0424] The chip bonding sheets before the heat curing treatment of each embodiment and each comparative example are stacked in a manner to have a thickness of 200μm. Next, the stacked sample is cut into strips with a width of 10mm and a length of 50mm with a cutting knife as a test piece. Using a solid viscoelasticity measuring device (measuring device: RSA-G2, Rheometric Scientific (manufactured by TA Instruments), the dynamic storage modulus is measured in a tensile mode in a temperature range of -20℃ to 200℃ under the conditions of a frequency of 1Hz, a heating rate of 10℃ / min, an initial chuck distance of 22.5mm, and a strain of 0.1%. Then, the values ​​at 50℃ and 130℃ are read respectively, and these values ​​are used as the tensile modulus (tensile storage modulus) [MPa] at 50℃ and 130℃.

[0425] <Measurement of Elongation at Break (Elongation at Break) and Breaking Strength of Die-Bond Sheet at Low Temperature>

[0426] Under the above-mentioned measurement conditions, the elongation at break (elongation at break) and the breaking strength of the die-bonding sheet were measured.

[0427] Specifically, a sheet sample is prepared by coating the chip bonding sheet of each embodiment and each comparative example before the heat curing treatment in a manner to become a thickness of 20μm, or a laminated sheet sample is prepared. Then, the sample is cut into strips with a width of 10mm and a length of 50mm using a cutting knife as a test piece. A tensile test is performed using a solid viscoelasticity measuring device (measuring device: RSA-G2, Rheometric Scientific (manufactured by TA Instruments) at a temperature of -15°C, a tensile speed of 1mm / sec, and an initial distance between chucks of 20mm. It should be noted that the measurement is started after keeping at -15°C for 5 minutes. Then, the elongation at break is taken as the elongation at break (elongation at break). In addition, the test force at break is confirmed as the breaking strength.

[0428] <Evaluation of Peel Force (Peel Force between Die-Bond Sheet and Adhesive Layer of Dicing Tape)>

[0429] The peeling force between the die-bonding sheet and the adhesive layer of the dicing tape was measured under the above-mentioned test conditions.

[0430] Specifically, after the backing tape is attached to the die bonding sheet of the diced die bonding film, a test piece with a width of 50 mm and a length of 120 mm is cut out. The cut test piece is used to perform a T-type peel test to measure the peeling force [N / 20 mm]. The temperature condition in the measurement is set to 50°C and the peeling speed is set to 300 mm / min.

[0431] Before laminating the backing tape, the adhesive layer of the dicing tape was irradiated with 300 mJ / cm at a temperature of 22°C from the substrate layer side. 2 (Irradiation intensity 150mW / cm 2 , 2 seconds) of ultraviolet light to cure the adhesive layer.

[0432] When the peeling force is 0.05 [N / 20 mm] or more and 0.20 [N / 20 mm] or less, the pickup performance is considered to be good.

[0433] <Evaluation of Pickup Performance (Picking Up Small Pieces of Die-bonding Sheets with Semiconductor Chips from Dicing Tape)>

[0434] Using each of the manufactured dicing die-bonding films, a mounting step, a low-temperature expansion step for cutting the semiconductor wafer, a room-temperature expansion step for separating the chips, and a die-bonding step were performed as described below.

[0435] During the installation process, a semiconductor wafer held on a wafer processing tape (product name "UB-3083D", manufactured by Nitto Denko Corporation) is adhered to the adhesive layer of the dicing chip bonding film, and then the wafer processing tape is peeled off from the semiconductor wafer. The semiconductor wafer has a thickness of 50 μm, and is formed with a dividing groove for small pieces (width 25 μm, one area is a 10 mm × 10 mm grid) after half-cutting, and is thinned by pre-back grinding. The above-mentioned pasting is performed using a laminator, and the pasting speed is 10 mm / second, the temperature condition is 60°C, and the pressure condition is 0.15 MPa. It should be noted that the surface of the semiconductor wafer on the opposite side of the surface where the dividing groove is formed is adhered to the adhesive layer of the dicing chip bonding film.

[0436] The low-temperature expansion process uses a chip separation device (product name "Die Separator DDS2300", manufactured by DISCO Corporation) and is implemented in the low-temperature expansion unit of the device. Specifically, after a ring frame is attached to the adhesive layer of the dicing chip bonding film to which the semiconductor wafer is attached, the dicing chip bonding film is set in the device. In the low-temperature expansion unit of the device, the dicing tape is expanded in a state accompanying the semiconductor wafer. In this low-temperature expansion process, the temperature is -15°C, the expansion speed is 200mm / second, and the expansion amount is 12mm. In this way, the semiconductor wafer is sliced ​​into small pieces on the dicing tape to obtain a plurality of semiconductor chips with chip bonding pieces.

[0437] The normal temperature expansion process uses a chip separation device (product name "Die Separator DDS2300", manufactured by DISCO Corporation), and is implemented using a normal temperature expansion unit in the device after the above-mentioned low temperature expansion process. Specifically, the dicing tape of the diced chip bonding film accompanied by the state of the small-piece semiconductor wafer (multiple semiconductor chips) is expanded in the normal temperature expansion unit of the device. In this normal temperature expansion process, the temperature is 23°C, the expansion speed is 1mm / sec, and the expansion amount is 10mm. Then, the cut piece is thermally shrunk by a thermal expansion unit to obtain a sample for evaluation. It should be noted that the conditions for thermal shrinkage are an expansion amount of 10mm, a heating temperature of 250°C, an air volume of 40L / min, a heating distance of 20mm, and a rotation speed of 3° / sec.

[0438] At 22°C, the adhesive layer was irradiated with 300 mJ / cm 2 (Irradiation intensity 150mW / cm 2 The adhesive layer was cured by ultraviolet light (1000 sec, 200 sec). Then, 1000 chips were picked up by a chip bonding machine to evaluate the pick-up performance. If there were more than 2 chips that could not be picked up, it was judged as bad (×), and if there were less than 1 chip, it was judged as good (O).

[0439] Picking was performed in a die bonder (manufactured by Shinkawa Co., Ltd., product name "Die Bonder SPA-300") with 5 pins and a pick-up height of 350 μm. The die bonding temperature was 130°C.

[0440] <Evaluation of Die Bonding Performance>

[0441] (Shear Adhesion Strength of Die Bonding Sheet at 130°C)

[0442] Each die-bonding sheet was attached to a bare chip (silicon chip) having a thickness of 0.5 mm and a size of 3 mm×3 mm. The attachment conditions were a temperature of 80° C., a speed of 10 mm / s, and a pressure of 0.15 MPa.

[0443] Furthermore, each die bonding sheet was bonded to a bare chip (0.5 mm, 10 mm×10 mm) to obtain each test piece. For bonding, a die bonding machine (manufactured by Shinkawa Co., Ltd., product name “Die Bonder SPA-300”) was used. In addition, the bonding conditions were a workbench temperature of 130° C., a die bonding load of 0.2 MPa, and a die bonding time of 1 second.

[0444] Next, a shear tester (Dage 4000, manufactured by Dage) was used to apply shear force to each test piece, and the shear adhesion (MPa) was measured. The conditions for the measurement were: speed 500 μm / s, measurement gap 100 μm, and workbench temperature 130°C. It should be noted that the test piece was placed on the measurement table and the measurement was performed after 20 seconds.

[0445] A value of 0.02 MPa or more was judged as good (○), and a value less than this was judged as poor (×).

[0446] From the above evaluation results, it can be seen that the die-bonding sheet of the example can have both good pickup performance and good die-bonding performance.

[0447] On the other hand, the die-bonding sheet of the comparative example cannot have both good pickup performance and good die-bonding performance.

[0448] By using the die-bonding sheet (dicing die-bonding film) of the embodiment having the above-described physical properties in manufacturing a semiconductor device, a so-called NAND type flash memory or the like can be efficiently manufactured.

[0449] Industrial Applicability

[0450] The die-bonding sheet and dicing die-bonding film of the present invention are suitably used as auxiliary tools when manufacturing a semiconductor device having a semiconductor integrated circuit, for example.

Claims

1. A die-bonding sheet comprising at least a thermoplastic resin and an inorganic filler, The thermoplastic resin includes a first thermoplastic resin and a second thermoplastic resin having an average molecular weight smaller than that of the first thermoplastic resin. The die-bonding sheet has an elastic modulus of 2.0 MPa to 10.0 MPa at 50° C. before curing, and an elastic modulus of 0.1 MPa to 1.5 MPa at 130° C.

2. The die bonding sheet according to claim 1, in, The first thermoplastic resin has an average molecular weight of 500,000 to 1,500,000, and the second thermoplastic resin has an average molecular weight of 10,000 to 100,000. The glass transition temperatures of the first thermoplastic resin and the second thermoplastic resin are both 0° C. or higher and 30° C. or lower. 3 . The die-bonding sheet according to claim 1 , wherein the elongation at break at −15° C. is 0.2% to 2.0%.

4. The die-bonding sheet according to claim 1 or 2, which has a breaking strength of 1.0 kg / mm ​​at -15°C 2 Above and 7.5kg / mm 2 the following.

5. The die bonding sheet according to claim 1 or 2, in, The inorganic filler contains silicon dioxide particles. 6 . A dicing die-bonding film comprising: the die-bonding sheet according to claim 1 or 2, and a dicing tape bonded to the die-bonding sheet.

7. The dicing die-bonding film according to claim 6, in, A peel force at 50° C. between the die-bonding sheet and the dicing tape is 0.03 N / 20 mm or more and 0.20 N / 20 mm or less. 8 . A semiconductor device comprising the die-bonding sheet according to claim 1 . 9 . An electronic device comprising the semiconductor device according to claim 8 .