Green light emitting fluorescent powder with broadband emission as well as preparation method and application of green light emitting fluorescent powder
By developing a broadband green light-emitting phosphor of the AO-SiO2-Si3N4-EuO system in the field of white light LEDs, the problem of insufficient green light emission spectrum range in the existing technology has been solved, and wider emission spectrum coverage and improved stability have been achieved. Suitable for a variety of LED applications.
Patent Information
- Application Number
- CN202410777631.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-01
AI Technical Summary
In the field of existing white light LEDs, the emission spectrum range of green light-emitting fluorescent materials is insufficient to meet the needs of a wider emission spectrum, affecting luminous efficiency and lighting effects.
Develop a broadband-emitting green light-emitting phosphor, which belongs to the AO-SiO2-Si3N4-EuO system. It is prepared through specific raw material ratios and process steps, including pre-calcination, calcination and sintering processes, to prepare a phosphor covering the 200-500nm excitation band and Phosphors with emission spectrum range of 450-800nm.
It achieves broadband emission of green light-emitting phosphor with a center wavelength of 538 nm, improves structural and chemical stability, is suitable for white LEDs, solar-like LEDs and full-spectrum LEDs, simplifies the preparation process, and is suitable for industrial production.
Smart Images

Figure CN118725854A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fluorescent materials, and in particular relates to a broadband green light emitting fluorescent powder and a preparation method and application thereof. Background Art
[0002] White light LED is the main way for humans to achieve green, energy-saving and healthy lighting. There are two main ways to achieve white light lighting: one is multi-chip combination, which obtains white light through a circuit control system; the other is phosphor conversion technology. The circuit control system of the first method is complex and costly, and it is difficult to promote commercially. The second method is generally a mixture of red, green and blue primary color phosphors, and white light driven by a near-ultraviolet chip. This method has simple process, low cost, and the white light has good color rendering and adjustable color temperature. It has become the main lighting method for current commercial promotion. Among the three primary color phosphors, the emission wavelength peak of the green phosphor can well match the wavelength peak of the human visual perception curve, thereby maximizing the luminous efficiency of the three primary color phosphors. Therefore, in the field of white light LEDs, the research and development of green phosphors has always been an important topic.
[0003] Due to Eu 2+ The luminescence energy level of Eu is attributed to the fd electron transition. The 5d orbit of its electron is in the outer layer and is easily affected by the coordination crystal field. Therefore, the regulation of the coordination crystal field can realize the 2+ The excitation and emission spectra are clipped, so Eu 2+ Commonly used as an activator for phosphors, Eu 2+ Ions have become important doping ions in rare earth doped phosphors. In addition, oxynitride phosphors have been widely used in LEDs due to their excellent fluorescence properties and good stability.
[0004] Therefore, in order to meet the urgent needs of white light LED / sunlight-like LED / full spectrum LED / health lighting LED light sources and cover a wider emission spectrum range, it is urgent to develop new green light emitting fluorescent materials. Summary of the invention
[0005] The purpose of the present invention is to provide a broadband emission green light emitting phosphor and its preparation method and application, so as to cover a wider emission spectrum range and meet the current urgent demand for green light emitting fluorescent materials in the field of white light LEDs.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] The present invention provides a broadband green light emitting phosphor, which belongs to the AO-SiO2-Si3N4-EuO system; wherein A includes one or more of Ca, Sr and Ba;
[0008] The mass percentages of the substances in the green light emitting phosphor are: AO 60.36%-80.86%, SiO2 18.00%-38.50%, Si3N4 0.00%-20.46%, and EuO 0.11%-0.65%.
[0009] Furthermore, the excitation band of the green light emitting phosphor covers 200-500nm.
[0010] Furthermore, the emission spectrum of the green light emitting phosphor under ultraviolet excitation covers a range of 450-800 nm, with a central wavelength at 538 nm.
[0011] The present invention also provides a method for preparing a broadband green light emitting phosphor, comprising the following steps:
[0012] S1: Weigh appropriate amounts of A-containing compound, Si-containing compound, N-containing compound and Eu-containing compound as raw material powders, mix and grind them evenly;
[0013] S2: The mixed powder ground in S1 is placed in an alumina crucible, pre-fired in an air atmosphere, and then naturally cooled to room temperature;
[0014] S3: grinding the pre-calcined powder in S2 again, calcining it in an air atmosphere, and cooling it naturally to room temperature to obtain a phosphor precursor;
[0015] S4: Grind the phosphor precursor obtained in S3 evenly again, place it in a reducing atmosphere for sintering, and cool it to room temperature to obtain the green light emitting phosphor.
[0016] Furthermore, in step S1, the A-containing compound includes oxides, halides or carbonates of Ca, Sr and Ba.
[0017] Furthermore, the Si-containing compound includes Si oxide, preferably SiO2.
[0018] Furthermore, the N-containing compound includes N oxide or silicate, preferably Si3N4.
[0019] Furthermore, the Eu-containing compound includes an oxide or a halide of Eu.
[0020] Furthermore, in steps S1, S3 and S4, the grinding time is 20-50 min.
[0021] Furthermore, in step S2, the pre-burning temperature is 300-800°C and the time is 3-10h.
[0022] Furthermore, in step S3, the calcination temperature is 1000-1400° C. and the calcination time is 5-10 h.
[0023] Furthermore, in step S4, the reducing atmosphere is CO.
[0024] Furthermore, the sintering temperature is 1000-1400° C. and the sintering time is 6-20 hours.
[0025] The present invention also provides an application of a broadband-emitting green light-emitting phosphor, wherein the green light-emitting phosphor is used for preparing a UV chip white light LED, a UV chip-like solar light LED, a UV chip full-spectrum LED or a UV chip high-quality white light LED.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] (1) The green light emitting phosphor prepared by the present invention emits a spectrum covering 450 to 800 nm under ultraviolet light excitation, with a central wavelength of green light at 538 nm, which is broadband emission and broadens the range of the emission spectrum.
[0028] (2) The doped Si3N4 of the present invention can effectively improve the structural stability and chemical stability of the green light emitting phosphor and has application potential in high-power device applications.
[0029] (3) The green light emitting phosphor of the present invention is Eu 2+ The doped broadband green light emitting phosphor has the advantage of stable physical and chemical properties. At the same time, the phosphor can be prepared by a conventional solid phase reaction method, has the characteristics of simple preparation process and is conducive to industrial production. It is a good candidate material that can be widely used.
[0030] (4) The emission wavelength of the green light emitting phosphor of the present invention includes 450 to 800 nm, and it can effectively absorb light in the wavelength range of 200 to 500 nm. It has the characteristics of a wide emission spectrum range and can be well matched with existing commercial near-ultraviolet LED chips. It is suitable for applications such as ultraviolet chip white light LEDs, ultraviolet chip solar LEDs, ultraviolet chip full-spectrum LEDs, and ultraviolet chip high-quality white light LEDs. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a photoexcitation-emission spectrum diagram of the green light emitting phosphor of Example 1 of the present invention.
[0032] Figure 2 The photoluminescence spectra of the green light emitting phosphors of Examples 1-3 of the present invention are shown. DETAILED DESCRIPTION
[0033] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.
[0034] Unless otherwise specified, the reagents, methods, instruments and equipment used in the present invention are conventional reagents, methods, instruments and equipment in the art. Unless otherwise specified, the reagents and materials used in the following examples are commercially available.
[0035] Embodiment 1:
[0036] This embodiment provides a broadband green light emitting phosphor, which belongs to the AO-SiO2-Si3N4-EuO system, and the specific preparation method is as follows:
[0037] S1: Select CaCO3, SiO2, Si3N4, Eu2O3 as starting materials, Ca:Si:Eu=2.985:2:0.0075 (molar ratio). Weigh CaCO3, SiO2, Eu2O3 respectively, and control the total mass of the raw material mixture to be 20g.
[0038] S2: Grind the above raw material mixture in an agate mortar for 20-50 minutes. After the materials are evenly mixed, load the mixture into an alumina crucible. Then, pre-sinter the alumina crucible with the raw materials at 500°C for 5 hours in an air atmosphere, and then naturally cool it to room temperature. Grind the cooled powder for 30 minutes and put it into an alumina crucible. Then, calcine it at 1300°C for 6 hours in an air atmosphere, and then cool it to room temperature. Grind the mixed product again, calcine it at 1000°C for 6 hours in a reducing atmosphere of carbon monoxide, and then cool it to room temperature to obtain the target product.
[0039] The spectral properties of the phosphor in this system were tested using a fluorescence spectrometer (HITACHI F-7000). Figure 1 and Figure 2 As shown. The results show that the phosphor of this system has a wide excitation band, covering the ultraviolet, purple and blue light regions (200-500nm), with a peak near 380nm, and a high spectral peak, indicating that it can be effectively excited by ultraviolet and purple chips and matches well with n-UV LED chips. Under the excitation of a 380nm ultraviolet light source, the phosphor emits bright green light, and the emission spectrum consists of a wide emission band (480-800nm) with a peak at 538nm.
[0040] Embodiment 2:
[0041] This embodiment provides a broadband green light emitting phosphor, and the specific preparation method is as follows:
[0042] S1: Select CaCO3, SiO2, Si3N4, and Eu2O3 as starting raw materials, Ca:Si:N:Eu=2.985:1.85:0.05:0.0075, weigh the four raw materials separately, and control the total mass of the raw material mixture to be 20g of mixed raw materials.
[0043] S2: Grind the above raw material mixture in an agate mortar for 20-50 minutes. After the materials are evenly mixed, load the mixture into an alumina crucible. Then, pre-sinter the alumina crucible with the raw materials at 500°C for 5 hours in an air atmosphere, and then naturally cool it to room temperature. Grind the cooled powder for 30 minutes and put it into an alumina crucible. Then, calcine it at 1300°C for 6 hours in an air atmosphere, and then cool it to room temperature. Grind the mixed product again, calcine it at 1000°C for 6 hours in a reducing atmosphere of carbon monoxide, and then cool it to room temperature to obtain the target product.
[0044] The spectral properties of the phosphor in this system were tested using a fluorescence spectrometer (HITACHI F-7000), such as Figure 2 The results show that when excited by a 380nm ultraviolet light source, the phosphor emits bright green light, and the emission spectrum consists of a wide emission band (450-800nm) with a peak at 538nm.
[0045] Embodiment 3:
[0046] This embodiment provides a broadband emission green light emitting phosphor, the reaction conditions and steps are basically the same as those of Example 1, except that the ratio of the raw materials weighed in step 1 is Ca: Si: N: Eu = 2.985: 1.4: 0.2: 0.0075, and the four raw materials are weighed respectively to control the total mass of the raw material mixture to be 20g of mixed raw materials. The above raw material mixture is placed in an agate mortar and ground for 20 to 50 minutes. After the materials are mixed evenly, the mixture is loaded into an alumina crucible, and then the alumina crucible containing the raw materials is first placed in an air atmosphere and calcined at 700°C for 10 hours, and then naturally cooled to room temperature; the cooled powder is ground for 30 minutes and then loaded into an alumina crucible, and then placed in an air atmosphere and calcined at 1300°C for 8 hours, and then cooled to room temperature; the mixed product obtained is then fully ground again, and then placed in a carbon monoxide reducing atmosphere for calcination at 1100°C for 10 hours, and then cooled to room temperature to obtain the target product. The fluorescence spectrum properties of the green luminescent material are similar to those in Example 1.
[0047] Embodiment 4:
[0048] This embodiment provides a broadband emission green light emitting phosphor, the reaction conditions and steps are basically the same as those of Example 1, except that the ratio of the raw materials weighed in step 1 is Ca: Si: N: Eu = 2.985: 1.25: 0.25: 0.0075, and the four raw materials are weighed respectively to control the total mass of the raw material mixture to be 20g of mixed raw materials. The above raw material mixture is placed in an agate mortar and ground for 20 to 50 minutes. After the materials are mixed evenly, the mixture is loaded into an alumina crucible, and then the alumina crucible containing the raw materials is first placed in an air atmosphere and calcined at 700°C for 10 hours, and then naturally cooled to room temperature; the cooled powder is ground for 30 minutes and then loaded into an alumina crucible, and then placed in an air atmosphere and calcined at 1300°C for 8 hours, and then cooled to room temperature; the mixed product obtained is then fully ground again, and then placed in a reducing atmosphere of carbon monoxide for calcination at 1100°C for 10 hours, and then cooled to room temperature to obtain the target product. The fluorescence spectrum properties of the green luminescent material are similar to those in Example 1.
[0049] Embodiment 5:
[0050] This embodiment provides a broadband green light emitting phosphor, and the reaction conditions and steps are basically the same as those of Example 1, except that different raw materials are selected in step 1. This embodiment uses BaCO3, SiO2, Si3N4, and Eu2O3 as starting raw materials, Ba:Si:Eu=2.985:2:0.0075, and weighs the three raw materials respectively to control the total mass of the raw material mixture to be 20g of mixed raw materials. The raw material mixture is placed in an agate mortar and ground for 20 to 50 minutes. After the materials are evenly mixed, the mixture is loaded into an alumina crucible. The alumina crucible containing the raw materials is first placed in an air atmosphere and calcined at 700°C for 10 hours, and then naturally cooled to room temperature; the cooled powder is ground for 30 minutes and then loaded into an alumina crucible, and then placed in an air atmosphere and calcined at 1300°C for 8 hours, and then cooled to room temperature; the obtained mixed product is then fully ground again, and then placed in a reducing atmosphere of carbon monoxide and calcined at 1100°C for 10 hours, and then cooled to room temperature to obtain the target product. The fluorescence spectrum properties of this green luminescent material are similar to those in Example 1.
[0051] Embodiment 6:
[0052] This embodiment provides a broadband green light emitting phosphor, and the reaction conditions and steps are basically the same as those of Example 1, except that different raw materials are selected in step 1. This embodiment uses BaCO3, SiO2, Si3N4, and Eu2O3 as starting raw materials, Ba:Si:N:Eu=2.985:1.85:0.05:0.0075, and weighs the four raw materials respectively to control the total mass of the raw material mixture to be 20g of mixed raw materials. The raw material mixture is placed in an agate mortar and ground for 20 to 50 minutes. After the materials are evenly mixed, the mixture is loaded into an alumina crucible. The alumina crucible containing the raw materials is then pre-fired at 500°C for 5 hours in an air atmosphere, and then naturally cooled to room temperature. The cooled powder is ground for 30 minutes and then loaded into an alumina crucible. The powder is then calcined at 1300°C for 6 hours in an air atmosphere, and then cooled to room temperature. The obtained mixed product is then fully ground again, and then calcined at 1000°C for 6 hours in a reducing atmosphere of carbon monoxide, and then cooled to room temperature to obtain the target product. The fluorescence spectrum properties of the green luminescent material are similar to those in Example 1.
[0053] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A broadband green light emitting phosphor, characterized in that: The green light emitting phosphor belongs to the AO-SiO2-Si3N4-EuO system; wherein A includes one or more of Ca, Sr and Ba; The mass percentages of the substances in the green light emitting phosphor are: AO 60.36%-80.86%, SiO2 18.00%-38.50%, Si3N4 0.00%-20.46%, and EuO 0.11%-0.65%.
2. A broadband green light emitting phosphor according to claim 1, characterized in that: The excitation band of the green light emitting phosphor covers 200-500nm.
3. A broadband green light emitting phosphor according to claim 2, characterized in that: The emission spectrum of the green light emitting phosphor under ultraviolet excitation covers a range of 450-800 nm, with a central wavelength at 538 nm.
4. A method for preparing the broadband green light emitting phosphor according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1: Weigh appropriate amounts of A-containing compound, Si-containing compound, N-containing compound and Eu-containing compound as raw material powders, mix and grind them evenly; S2: The mixed powder ground in S1 is placed in an alumina crucible, pre-fired in an air atmosphere, and then naturally cooled to room temperature; S3: grinding the pre-calcined powder in S2 again, calcining it in an air atmosphere, and cooling it naturally to room temperature to obtain a phosphor precursor; S4: Grind the phosphor precursor obtained in S3 evenly again, place it in a reducing atmosphere for sintering, and cool it to room temperature to obtain the green light emitting phosphor.
5. The method for preparing a broadband green light emitting phosphor according to claim 4, characterized in that: In step S1, the A-containing compound includes oxides, halides or carbonates of Ca, Sr and Ba; the Si-containing compound includes Si oxides; the N-containing compound includes N oxides or silicates; and the Eu-containing compound includes Eu oxides or halides.
6. The method for preparing a broadband green light emitting phosphor according to claim 4, characterized in that: In steps S1, S3 and S4, the grinding time is 20-50 min.
7. The method for preparing a broadband green light emitting phosphor according to claim 4, characterized in that: In step S2, the pre-burning temperature is 300-800°C and the time is 3-10 hours.
8. The method for preparing a broadband green light emitting phosphor according to claim 4, characterized in that: In step S3, the calcination temperature is 1000-1400° C. and the calcination time is 5-10 hours.
9. The method for preparing a broadband green light emitting phosphor according to claim 4, characterized in that: In step S4, the reducing atmosphere is CO; The sintering temperature is 1000-1400° C. and the sintering time is 6-20 hours.
10. Use of the broadband green light emitting phosphor according to any one of claims 1 to 3, characterized in that: The green light emitting phosphor is used for preparing ultraviolet chip white light LED, ultraviolet chip sunlight LED, ultraviolet chip full spectrum LED or ultraviolet chip high quality white light LED.
Citation Information
Patent Citations
Method for optimizing crystalline form of silicate green fluorescent powder material
CN102191057A
Fluorescent powder and preparation method thereof
CN109679654A
Cited By
Purple light excitation type sunlight LED green light fluorescent powder and preparation method and application thereof
CN122344468A