Zinc oxide smoke dust and zinc calcine combined leaching method
Through the joint leaching method of zinc oxide fume and zinc roasting sand, the solution containing copper and ferric iron in the zinc roasting sand leaching process is used to solve the problem of low leaching rate of zinc oxide fume and zinc roasting sand in the traditional wet zinc smelting process. Complex problems are achieved, efficient metal recovery and impurity removal are achieved, and the process flow is simplified.
Patent Information
- Application Number
- CN202410933374.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-12
AI Technical Summary
In the traditional hydrometallurgical zinc smelting process, the leaching process of zinc oxide dust and zinc baking sand is complex, the zinc leaching rate is low, and there are problems of metal loss and difficulty in separating impurities.
The joint leaching method of zinc oxide smoke and zinc roasting sand is adopted, and the copper-containing solution and ferric iron-containing solution in the zinc roasting sand leaching process are used to achieve efficient leaching and impurity removal of zinc oxide smoke, simplify the process flow, and improve the copper content. leaching rates and recovery rates, and reducing the complexity of arsenic and chlorine removal.
It improves the leaching rate of valuable metal copper in zinc oxide dust and zinc roasting sand, simplifies the removal process of arsenic and chlorine in zinc hydrometallurgy solution, reduces the amount of zinc roasting slag leaching and neutralizing slag, and improves It improves the recovery efficiency of zinc and copper and reduces the complexity of the process.
Smart Images

Figure CN118726752A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a combined leaching method of zinc oxide smoke and zinc roasted sand, belonging to the technical field of hydrometallurgy. Background Art
[0002] The traditional hydrometallurgical zinc smelting process is roasting-leaching (neutral leaching + weak acid leaching)-purification-electrodeposition, and the zinc leaching slag is produced after weak acid leaching. The methods for treating zinc leaching slag include pyrometallurgical process and hydrometallurgical process. The pyrometallurgical process mainly includes rotary kiln volatilization method and fuming furnace method. Zinc oxide dust is obtained by high-temperature reduction volatilization, and then the zinc oxide dust is leached. Therefore, zinc roasted sand and zinc oxide dust are two types of zinc-containing materials in traditional hydrometallurgical enterprises.
[0003] Zinc oxide dust contains sulfides, which leads to low zinc leaching rate. When adding oxidants for high acid leaching, the amount of oxidants used is large and the effect is poor. In particular, the chloride ions brought into the solution system by zinc oxide dust need to be removed by a special process. The typical process is the copper slag dechlorination process, which makes the leaching process long, complex, and has a large amount of metal loss. The traditional leaching process of zinc roasted sand has a low copper leaching rate, and it cannot be directly separated and enriched and can only be sent to the purification process for treatment. Summary of the invention
[0004] Aiming at the problems of long process flow, complex process and low leaching rate of wet leaching of two types of zinc-containing materials, zinc oxide dust and zinc roasted sand, the present invention provides a combined leaching method of zinc oxide dust and zinc roasted sand. The present invention combines zinc oxide dust and zinc roasted sand for leaching, utilizes the copper-containing solution and the trivalent iron-containing solution obtained in the zinc roasted sand leaching process, realizes efficient leaching of zinc oxide dust and removal of impurities; improves the leaching rate and recovery rate of valuable metal copper in the two types of zinc-containing materials, zinc oxide dust and zinc roasted sand, and simplifies the removal of arsenic and chlorine in the wet zinc smelting solution.
[0005] A method for combined leaching of zinc oxide smoke and zinc roasted sand, the specific steps are as follows:
[0006] (1) adding zinc oxide smoke to a simulated high-leaching solution for neutral leaching, and separating the liquid and solid to obtain intermediate leaching residue and intermediate leaching solution; the simulated high-leaching solution is prepared from a waste electrolyte of hydrometallurgical zinc smelting and a zinc sulfate solution;
[0007] (2) adding zinc roasted sand into the waste electrolyte of hydrometallurgical zinc smelting to carry out weak acid leaching, and liquid-solid separation to obtain weak leaching residue and weak leaching liquid;
[0008] (3) The weak leaching residue from step (2) is added to the waste electrolyte of hydrometallurgical zinc smelting for hot acid leaching, and the zinc leaching residue and hot acid leaching solution are obtained by liquid-solid separation; the zinc leaching residue is sent to pyrometallurgical volatilization treatment;
[0009] (4) the leaching residue in step (1) is added to a high acid solution for high acid leaching, and liquid-solid separation is performed to obtain a high acid leaching solution and a high acid leaching residue, wherein the high acid leaching residue is lead-silver slag; the high acid leaching solution is returned to step (1) to replace the simulated high acid leaching solution for neutral leaching; the high acid solution is a mixture of hot acid leaching solution and wet process waste electrolyte;
[0010] (5) mixing the leaching solution in step (1) and the weak leaching solution in step (2), adding a purifier to perform copper precipitation, arsenic removal and chlorine removal to obtain copper-rich arsenic-chlorine slag and copper precipitation solution;
[0011] (6) The zinc roasted sand is added to the copper precipitation solution of step (5) for neutralization and impurity removal, and the liquid-solid separation is performed to obtain a neutralized solution and a neutralized slag; the neutralized slag is sent to a pyrometallurgical volatilization treatment, and the neutralized solution is sent to a purification electrowinning process.
[0012] In the step (1), the copper content of the zinc oxide fume is greater than 0.5wt.%, the sulfur content is greater than 2wt.%, and the chlorine content is less than 0.5wt.%.
[0013] Preferably, the concentration of sulfuric acid in the simulated high-temperature leaching solution in step (1) is 80-120 g / L, and the solid-liquid ratio (g:mL) of zinc oxide fume to the simulated high-temperature leaching solution is 1:6-8.
[0014] The sulfuric acid concentration in the waste electrolyte of hydrometallurgical zinc smelting is 160-165 g / L.
[0015] Preferably, in the step (2), the solid-liquid ratio of zinc roasted sand to the waste electrolyte of hydrometallurgical zinc smelting is 1:6-7, the weak acid leaching temperature is 80-90°C, the leaching time is 1.5-2h, and the end point pH is 1.5-3; zinc and copper are leached while iron is not leached.
[0016] Preferably, the solid-liquid ratio of the weak leaching residue in step (3) to the waste electrolyte of hydrometallurgical zinc smelting is 1:3-4 in g:mL, the hot acid leaching temperature is 80-90°C, the time is 2-3h, and the final acid is 40-60g / L; during the hot acid leaching process, while leaching zinc and copper, part of the iron is leached to achieve the balance and concentration control of iron in the hot acid leaching solution, and obtain a hot acid leaching solution containing iron and 5-10g / L of trivalent iron.
[0017] Preferably, the concentration of sulfuric acid in the high acid solution in step (4) is 100-150 g / L, the temperature of high acid leaching is 80-90° C., the time is 3-5 h, and the final acid is 80-120 g / L; no oxidant is needed in the high acid leaching process, and the trivalent iron ions in the hot acid leaching solution are used to leach zinc sulfide in the zinc oxide dust, thereby improving the leaching rate of zinc in the zinc oxide dust.
[0018] Preferably, the purifier in step (5) is zinc-copper-iron alloy powder, which is added according to a stoichiometric amount, and the temperature for copper displacement, arsenic removal and chlorine removal is 50-60° C., and the time is 20-30 min, and copper, arsenic and chlorine are separated from the solution in the form of cuprous arsenide and cuprous chloride, respectively.
[0019] Preferably, the specific method of neutralization and impurity removal in step (6) is as follows: zinc roasted sand is added to the copper precipitation solution of step (5); when the pH value of the copper precipitation solution is not greater than 3, hydrogen peroxide is added to oxidize the iron precipitation to generate ferrocyanide and goethite precipitation instead of iron hydroxide to reduce the amount of neutralization slag; then the pH value of the solution is adjusted to 5.0-5.2, air is introduced to oxidize the iron precipitation and hydrolyze to obtain iron hydroxide; and impurities are removed by utilizing the adsorption of ferrocyanide, goethite and iron hydroxide to different impurities.
[0020] The beneficial effects of the present invention are:
[0021] (1) The present invention utilizes the copper-containing solution and the ferric iron-containing solution obtained in the zinc roasting sand leaching process to achieve efficient leaching of zinc oxide dust and removal of impurities;
[0022] (2) The present invention can achieve efficient leaching of zinc oxide dust and improve the quality of lead-silver slag: the hot acid leaching solution of zinc roasted sand is used for high-acid leaching of zinc oxide dust, and the trivalent iron ions in the hot acid leaching solution are used to leach zinc sulfide in the zinc oxide dust, and the zinc leaching rate in the oxidized powder can be improved without adding an external oxidant. At the same time, the amount of lead-silver slag can be reduced, and the quality of the lead-silver slag can be improved;
[0023] (3) The present invention can realize the direct separation and enrichment of copper and the removal of arsenic and chlorine in zinc roasted sand: the zinc oxide fume leaching solution is mixed with the zinc roasted sand weak acid solution to adjust the pH at the same time, and the copper is replaced by precipitation to remove arsenic and chlorine. During the leaching process, the copper is separated and enriched as a marketable copper slag, thereby avoiding the precipitation loss of copper caused by the return of weak acid leaching to the leaching process in the traditional process and simplifying the subsequent purification process. At the same time, when the copper is converted into cuprous ions, the arsenic and chlorine in the solution are converted into precipitates and removed from the solution, thereby realizing the efficient utilization and recovery of copper and the simultaneous removal of arsenic and chlorine, and avoiding the separate copper slag dechlorination process;
[0024] (4) The present invention can achieve the reduction of zinc roasted sand leaching residue and the opening of impurities in the pre-purification liquid: the iron in the zinc roasted sand hot acid leaching liquid is not returned to the zinc roasted sand leaching system, and the iron is opened from the roasted sand leaching system, thereby reducing the amount of zinc leaching residue; the copper precipitation liquid controls the solution acidity in stages during the neutralization process, and the iron in the copper precipitation liquid is converted into iron alum, goethite, and iron hydroxide during the neutralization process instead of completely oxidizing the iron to precipitate iron hydroxide colloid, thereby reducing the amount of neutralization residue (and the sum of the neutralization residue and the zinc leaching residue is less than the amount of leaching residue in the traditional leaching process), and at the same time, the adsorption of different iron precipitates relative to different impurities is used to deeply remove impurities in the solution, so as to facilitate subsequent solution purification. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0026] The present invention is further described in detail below in conjunction with specific implementation modes, but the protection scope of the present invention is not limited to the described contents.
[0027] Example 1: The main components (wt%) of zinc oxide smoke in this example are: Zn: 54.85, Fe: 2.58, S: 3.19, Pb: 10.28, Ag: 0.0485, Cl: 0.51; the main components (wt%) of zinc roasted sand are: Zn: 50.27, Fe: 10.16, S: 2.53, Cu: 0.85, Pb: 1.98, Ag: 0.068; the waste electrolyte of hydrometallurgical zinc smelting contains 45.28 g / L zinc and 160.51 g / L sulfuric acid;
[0028] A method for leaching zinc oxide dust and zinc roasted sand (see Figure 1 ), the specific steps are as follows:
[0029] (1) adding zinc oxide smoke into a simulated high-leaching solution for neutral leaching, and separating liquid from solid to obtain intermediate leaching residue and intermediate leaching solution;
[0030] The simulated high-liquid leaching solution is prepared from waste electrolyte of hydrometallurgical zinc smelting and zinc sulfate solution, the concentration of sulfuric acid in the simulated high-liquid leaching solution is 105 g / L, and the solid-liquid ratio of zinc oxide smoke to the simulated high-liquid leaching solution is 1:6.2 g:mL;
[0031] (2) adding zinc roasted sand to the waste electrolyte of hydrometallurgical zinc smelting for weak acid leaching, and separating the liquid and solid to obtain weak leaching residue and weak leaching solution; the solid-liquid ratio of the zinc roasted sand to the waste electrolyte of hydrometallurgical zinc smelting is 1:7 g:mL, the temperature of the weak acid leaching is 80° C., the time is 2 h, the end point pH is 1.5, zinc and copper are leached but iron is not leached, and weak leaching residue and weak leaching solution are obtained;
[0032] (3) The weak leaching residue of step (2) is added to the waste electrolyte of zinc hydrometallurgy for hot acid leaching, and the zinc leaching residue and the hot acid leaching solution are obtained by liquid-solid separation; the zinc leaching residue is sent to the pyrometallurgical volatilization treatment to obtain zinc oxide smoke; the solid-liquid ratio of the weak leaching residue to the waste electrolyte of zinc hydrometallurgy is 1:4 g:mL, the hot acid leaching temperature is 90°C, the time is 2h, and the final acid is 50g / L; during the hot acid leaching process, while leaching zinc and copper, part of the iron is leached, so as to achieve the balance and concentration control of iron in the hot acid leaching solution, and obtain a hot acid leaching solution containing iron and 9.6g / L of trivalent iron;
[0033] (4) adding the leaching residue from step (1) into a high acid solution for high acid leaching, and performing liquid-solid separation to obtain a high acid leaching solution and a high acid leaching residue, wherein the high acid leaching residue is lead-silver slag; the high acid leaching solution is returned to step (1) to replace the simulated high acid leaching solution for neutral leaching; the high acid solution is a mixture of hot acid leaching solution and wet process waste electrolyte, the sulfuric acid concentration in the high acid solution is 123 g / L, the high acid leaching temperature is 80° C., the leaching time is 5 h, and the final acid is 100 g / L; no oxidant is added during the high acid leaching process, and the trivalent iron ions in the hot acid leaching solution are used to leach zinc sulfide in the zinc oxide dust, thereby improving the leaching rate of zinc in the zinc oxide dust;
[0034] (5) the leaching solution in step (1) and the weak leaching solution in step (2) are mixed, and a purifier (zinc-copper-iron alloy powder) is added to perform copper displacement precipitation, arsenic removal and chlorine removal to obtain copper-rich arsenic-chlorine slag and copper precipitation solution; the purifier (zinc-copper-iron alloy powder) is added according to a stoichiometric amount, the temperature of the copper displacement precipitation, arsenic removal and chlorine removal is 60° C., and the time is 20 min, and copper, arsenic and chlorine are separated from the solution in the form of cuprous arsenide and cuprous chloride, respectively;
[0035] (6) adding zinc roasted sand to the copper precipitation solution of step (5) for neutralization and impurity removal, and separating liquid from solid to obtain neutralized solution and neutralized slag; the neutralized solution is sent to a purification electrolytic process; the neutralized slag is sent to a pyrometallurgical volatilization process to obtain zinc oxide smoke; the specific method of neutralization and impurity removal (two-step method) is as follows: adding zinc roasted sand to the copper precipitation solution of step (5), when the pH value of the copper precipitation solution is not greater than 3, adding hydrogen peroxide (oxidant) to oxidize the precipitated iron to generate ferrocyanide and goethite precipitation instead of iron hydroxide to reduce the amount of neutralized slag; then adjusting the pH value of the solution to 5.0-5.2, introducing air to oxidize the remaining iron in the precipitate and hydrolyze to obtain iron hydroxide; removing impurities by utilizing the adsorption of ferrocyanide, goethite and iron hydroxide to different impurities;
[0036] In this embodiment, the zinc leaching rate in the zinc oxide smoke is 94.12%, and the lead-silver slag rate is 31.05%; the zinc leaching rate in the zinc roasted sand is 93.52%, the copper leaching rate is 75.63%, and the zinc leaching slag rate is 28.83%; the copper content in the copper-rich arsenic-chlorine slag is 52.23%, the copper precipitation rate is 99.67%, the arsenic removal rate is 90.22%, and the chlorine removal rate is 60.34%.
[0037] Example 2: The zinc oxide fume, zinc roasted sand, and waste electrolyte of hydrometallurgical zinc smelting in this example are the same as those in Example 1;
[0038] A method for leaching zinc oxide dust and zinc roasted sand (see Figure 1 ), the specific steps are as follows:
[0039] (1) adding zinc oxide smoke into a simulated high-leaching solution for neutral leaching, and separating liquid from solid to obtain intermediate leaching residue and intermediate leaching solution;
[0040] The simulated high-liquid leaching solution is prepared from waste electrolyte of hydrometallurgical zinc smelting and zinc sulfate solution, the concentration of sulfuric acid in the simulated high-liquid leaching solution is 118 g / L, and the solid-liquid ratio of zinc oxide smoke to the simulated high-liquid leaching solution is 1:7.1 g:mL;
[0041] (2) adding zinc roasted sand to the waste electrolyte of hydrometallurgical zinc smelting for weak acid leaching, and separating the liquid and solid to obtain weak leaching residue and weak leaching solution; the solid-liquid ratio of the zinc roasted sand to the waste electrolyte of hydrometallurgical zinc smelting is 1:6.5, the temperature of weak acid leaching is 85° C., the time is 1.5 h, the end point pH is 2.3, zinc and copper are leached but iron is not leached, and weak leaching residue and weak leaching solution are obtained;
[0042] (3) The weak leaching residue of step (2) is added to the waste electrolyte of zinc hydrometallurgy for hot acid leaching, and the zinc leaching residue and the hot acid leaching solution are obtained by liquid-solid separation; the zinc leaching residue is sent to the pyrometallurgical volatilization treatment to obtain zinc oxide smoke; the solid-liquid ratio of the weak leaching residue to the waste electrolyte of zinc hydrometallurgy is 1:3.5 g:mL, the hot acid leaching temperature is 80°C, the time is 3h, and the final acid is 40g / L; during the hot acid leaching process, while leaching zinc and copper, part of the iron is leached, so as to achieve the balance and concentration control of iron in the hot acid leaching solution, and obtain a hot acid leaching solution containing iron and 7.8g / L of trivalent iron;
[0043] (4) adding the leaching residue from step (1) into a high acid solution for high acid leaching, and separating the liquid and solid to obtain a high acid leaching solution and a high acid leaching residue, wherein the high acid leaching residue is lead-silver residue; the high acid leaching solution is returned to step (1) to replace the simulated high acid leaching solution for neutral leaching; the high acid solution is a mixture of hot acid leaching solution and wet process waste electrolyte, the sulfuric acid concentration in the high acid solution is 149 g / L, the high acid leaching temperature is 85° C., the time is 3 h, and the final acid is 120 g / L; no oxidant is added during the high acid leaching process, and the trivalent iron ions in the hot acid leaching solution are used to leach zinc sulfide in the zinc oxide dust, thereby improving the leaching rate of zinc in the zinc oxide dust;
[0044] (5) the leaching solution in step (1) and the weak leaching solution in step (2) are mixed, and a purifier (zinc-copper-iron alloy powder) is added to perform copper displacement precipitation, arsenic removal and chlorine removal to obtain copper-rich arsenic-chlorine slag and copper precipitation solution; the purifier (zinc-copper-iron alloy powder) is added according to a stoichiometric amount, the temperature of the copper displacement precipitation, arsenic removal and chlorine removal is 55° C., and the time is 25 min, and copper, arsenic and chlorine are separated from the solution in the form of cuprous arsenide and cuprous chloride, respectively;
[0045] (6) adding zinc roasted sand to the copper precipitation solution of step (5) for neutralization and impurity removal, and separating liquid from solid to obtain neutralized solution and neutralized slag; the neutralized solution is sent to a purification electrolytic process; the neutralized slag is sent to a pyrometallurgical volatilization process to obtain zinc oxide smoke; the specific method of neutralization and impurity removal (two-step method) is as follows: adding zinc roasted sand to the copper precipitation solution of step (5), when the pH value of the copper precipitation solution is not greater than 3, adding hydrogen peroxide (oxidant) to oxidize the precipitated iron to generate ferrocyanide and goethite precipitation instead of iron hydroxide to reduce the amount of neutralized slag; then adjusting the pH value of the solution to 5.0-5.2, introducing air to oxidize the remaining iron in the precipitate and hydrolyze to obtain iron hydroxide; removing impurities by utilizing the adsorption of ferrocyanide, goethite and iron hydroxide to different impurities;
[0046] In this embodiment, the zinc leaching rate in the zinc oxide smoke is 95.68%, and the lead-silver slag rate is 29.75%; the zinc leaching rate in the zinc roasted sand is 92.08%, the copper leaching rate is 73.17%, and the zinc leaching slag rate is 30.15%; the copper content in the copper-rich arsenic-chlorine slag is 50.68%, the copper precipitation rate is 99.89%, the arsenic removal rate is 90.85%, and the chlorine removal rate is 63.53%.
[0047] Example 3: The zinc oxide fume, zinc roasted sand, and waste electrolyte of hydrometallurgical zinc smelting in this example are the same as those in Example 1;
[0048] A method for leaching zinc oxide dust and zinc roasted sand (see Figure 1 ), the specific steps are as follows:
[0049] (1) adding zinc oxide smoke into a simulated high-leaching solution for neutral leaching, and separating liquid from solid to obtain intermediate leaching residue and intermediate leaching solution;
[0050] The simulated high-liquid leaching solution is prepared from waste electrolyte of hydrometallurgical zinc smelting and zinc sulfate solution, the concentration of sulfuric acid in the simulated high-liquid leaching solution is 82 g / L, and the solid-liquid ratio of zinc oxide smoke to the simulated high-liquid leaching solution is 1:8 g:mL;
[0051] (2) adding zinc roasted sand to the waste electrolyte of hydrometallurgical zinc smelting for weak acid leaching, and separating the liquid and solid to obtain weak leaching residue and weak leaching solution; the solid-liquid ratio of the zinc roasted sand to the waste electrolyte of hydrometallurgical zinc smelting is 1:6.8, the temperature of the weak acid leaching is 90° C., the time is 2 h, the end point pH is 1.5, zinc and copper are leached but iron is not leached, and weak leaching residue and weak leaching solution are obtained;
[0052] (3) The weak leaching residue of step (2) is added to the waste electrolyte of zinc hydrometallurgy for hot acid leaching, and the zinc leaching residue and the hot acid leaching solution are obtained by liquid-solid separation; the zinc leaching residue is sent to the pyrometallurgical volatilization treatment to obtain zinc oxide smoke; the solid-liquid ratio of the weak leaching residue to the waste electrolyte of zinc hydrometallurgy is 1:3 g:mL, the hot acid leaching temperature is 85°C, the time is 2.5h, and the final acid is 30g / L; during the hot acid leaching process, while leaching zinc and copper, part of the iron is leached, so as to achieve the balance and concentration control of iron in the hot acid leaching solution, and obtain a hot acid leaching solution containing iron and 5.7g / L of trivalent iron;
[0053] (4) adding the leaching residue from step (1) into a high acid solution for high acid leaching, and performing liquid-solid separation to obtain a high acid leaching solution and a high acid leaching residue, wherein the high acid leaching residue is lead-silver slag; the high acid leaching solution is returned to step (1) to replace the simulated high acid leaching solution for neutral leaching; the high acid solution is a mixture of hot acid leaching solution and wet process waste electrolyte, the sulfuric acid concentration in the high acid solution is 103 g / L, the high acid leaching temperature is 90° C., the time is 4 h, and the final acid is 80 g / L; no oxidant is added during the high acid leaching process, and the trivalent iron ions in the hot acid leaching solution are used to leach zinc sulfide in the zinc oxide dust, thereby improving the leaching rate of zinc in the zinc oxide dust;
[0054] (5) the leaching solution in step (1) and the weak leaching solution in step (2) are mixed, and a purifier (zinc-copper-iron alloy powder) is added to perform copper precipitation, arsenic removal and chlorine removal to obtain copper-rich arsenic-chlorine slag and copper precipitation solution; the purifier (zinc-copper-iron alloy powder) is added according to a stoichiometric amount, the temperature of the copper precipitation, arsenic removal and chlorine removal is 50° C., and the time is 30 min, and copper, arsenic and chlorine are separated from the solution in the form of cuprous arsenide and cuprous chloride, respectively;
[0055] (6) adding zinc roasted sand to the copper precipitation solution of step (5) for neutralization and impurity removal, and separating liquid from solid to obtain neutralized solution and neutralized slag; the neutralized solution is sent to a purification electrolytic process; the neutralized slag is sent to a pyrometallurgical volatilization process to obtain zinc oxide smoke; the specific method of neutralization and impurity removal (two-step method) is as follows: adding zinc roasted sand to the copper precipitation solution of step (5), when the pH value of the copper precipitation solution is not greater than 3, adding hydrogen peroxide (oxidant) to oxidize the precipitated iron to generate ferrocyanide and goethite precipitation instead of iron hydroxide to reduce the amount of neutralized slag; then adjusting the pH value of the solution to 5.0-5.2, introducing air to oxidize the remaining iron in the precipitate and hydrolyze to obtain iron hydroxide; removing impurities by utilizing the adsorption of ferrocyanide, goethite and iron hydroxide to different impurities;
[0056] In this embodiment, the zinc leaching rate in the zinc oxide smoke is 92.35%, and the lead-silver slag rate is 33.21%; the zinc leaching rate in the zinc roasted sand is 90.68%, the copper leaching rate is 70.52%, and the zinc leaching slag rate is 31.29%; the copper content in the copper-rich arsenic-chlorine slag is 53.16%, the copper precipitation rate is 99.76%, the arsenic removal rate is 90.39%, and the chlorine removal rate is 61.28%.
[0057] The specific implementation modes of the present invention are described in detail above, but the present invention is not limited to the above implementation modes, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.
Claims
1. A combined leaching method of zinc oxide fume and zinc roasted sand, It is characterized in that The specific steps are as follows: (1) adding zinc oxide smoke to a simulated high-leaching solution for neutral leaching, and separating the liquid and solid to obtain intermediate leaching residue and intermediate leaching solution; the simulated high-leaching solution is prepared from a waste electrolyte of hydrometallurgical zinc smelting and a zinc sulfate solution; (2) adding zinc roasted sand into the waste electrolyte of hydrometallurgical zinc smelting to carry out weak acid leaching, and liquid-solid separation to obtain weak leaching residue and weak leaching liquid; (3) The weak leaching residue from step (2) is added to the waste electrolyte of hydrometallurgical zinc smelting for hot acid leaching, and the zinc leaching residue and hot acid leaching solution are obtained by liquid-solid separation; the zinc leaching residue is sent to pyrometallurgical volatilization treatment; (4) adding the leaching residue in step (1) into a high acid solution for high acid leaching, and separating the liquid and solid to obtain a high acid leaching solution and a high acid leaching residue, wherein the high acid leaching residue is a lead-silver residue; The high-acid leaching solution is returned to step (1) to replace the simulated high-acid leaching solution for neutral leaching; the high-acid solution is a mixture of hot acid leaching solution and wet-process waste electrolyte; (5) mixing the leaching solution in step (1) and the weak leaching solution in step (2), adding a purifier to perform copper precipitation, arsenic removal and chlorine removal to obtain copper-rich arsenic-chlorine slag and copper precipitation solution; (6) The zinc roasted sand is added to the copper precipitation solution of step (5) for neutralization and impurity removal, and the liquid-solid separation is performed to obtain a neutralized solution and a neutralized slag; the neutralized slag is sent to a pyrometallurgical volatilization treatment, and the neutralized solution is sent to a purification electrowinning process.
2. The combined leaching method of zinc oxide smoke and zinc roasted sand according to claim 1, Features: In step (1), the sulfur content in the zinc oxide fume is greater than 2wt% and the chlorine content is less than 0.5%.
3. According to the combined leaching method of zinc oxide smoke and zinc roasted sand described in claim 1, Features: The concentration of sulfuric acid in the simulated high-temperature leaching solution in step (1) is 80-120 g / L, and the solid-liquid ratio (g:mL) of zinc oxide fume to the simulated high-temperature leaching solution is 1:6-8.
4. The combined leaching method of zinc oxide smoke and zinc roasted sand according to claim 1, Features: The concentration of sulfuric acid in the waste electrolyte of hydrometallurgical zinc smelting is 160-165 g / L.
5. The combined leaching method of zinc oxide smoke and zinc roasted sand according to claim 1, Features: In step (2), the solid-liquid ratio of zinc roasted sand to the waste electrolyte of hydrometallurgical zinc smelting is 1:6-7, the weak acid leaching temperature is 80-90° C., the leaching time is 1.5-2 h, and the endpoint pH is 1.5-3.
6. The combined leaching method of zinc oxide fume and zinc roasted sand according to claim 1, Features: In step (3), the solid-liquid ratio of the weak leaching residue to the waste electrolyte of hydrometallurgical zinc smelting is 1:3-4, the hot acid leaching temperature is 80-90° C., the time is 2-3 h, and the final acid is 40-60 g / L.
7. The combined leaching method of zinc oxide smoke and zinc roasted sand according to claim 1, Features: In step (4), the concentration of sulfuric acid in the high acid solution is 100-150 g / L, the temperature of high acid leaching is 80-90° C., the time is 3-5 h, and the final acid is 80-120 g / L.
8. The combined leaching method of zinc oxide fume and zinc roasted sand according to claim 1, Features: In step (5), the purifier is zinc-copper-iron alloy powder, and the temperature for replacement copper precipitation, arsenic removal and chlorine removal is 50-60° C., and the time is 20-30 min.
9. The combined leaching method of zinc oxide fume and zinc roasted sand according to claim 1, Features: The specific method of neutralization and impurity removal in step (6) is as follows: zinc roasted sand is added to the copper precipitation solution in step (5); when the pH value of the copper precipitation solution is not greater than 3, hydrogen peroxide is added to oxidize the iron precipitation to generate iron alum and goethite precipitation; then the pH value of the solution is adjusted to 5.0-5.2, air is introduced to oxidize the iron precipitation and hydrolyze to obtain ferric hydroxide.
Citation Information
Patent Citations
Synergistic leaching-copper arsenate removing method for leaching residues in high-iron zinc calcine and high-iron zinc sulfide concentrate
CN103789544A
Treatment technique of copper-containing high-indium high-iron zinc sulfide concentrate
CN104745810A
Environmentally-friendly and highly-efficient recovery and separation technology of lithium ion batteries in waste mobile phones
CN106558739A
Continuous iron removing process in zinc hydrometallurgy
CN107287422A
Method for removing arsenic and chlorine in waste acid
CN111003834A
Cited By
Method for deeply removing arsenic in zinc sulfate solution with high arsenic content
CN120060641A