Plastic optical fiber, optical cable and active optical cable

By arranging an outer edge area with a constant refractive index and a low refractive index trench layer in the POF core, the problem of frequency band reduction within short distances of POF is solved, and the effect of high frequency band and low bending loss is achieved, which is suitable for home use. signal transmission.

CN118732147AInactive Publication Date: 2024-10-01NITTO DENKO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410361449.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-27
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In existing POF, the frequency band is reduced due to light reflection from the trench layer within a short distance, and there is a lack of technology to improve the frequency band, especially in terms of bending loss reduction.

Method used

Design a POF whose core has a refractive index distribution that decreases from the center to the outer edge, and set a constant refractive index region with a thickness of more than 2 μm and less than 5 μm at the outer edge of the core, and the refractive index of the trench layer is lower than this area, this structure suppresses light reflection and improves the frequency band.

Benefits of technology

It achieves an increase in frequency band within a short distance and reduces bending loss, making it suitable for short-distance signal transmission within homes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118732147A_ABST
    Figure CN118732147A_ABST
Patent Text Reader

Abstract

The invention provides a plastic optical fiber, an optical cable and an active optical cable. Provided is a plastic optical fiber having a trench layer for improving bending loss, the plastic optical fiber having an improved frequency band in a short distance. This plastic optical fiber is provided with a core (11) and a trench layer (12) disposed on the outer periphery of the core (11). The core (11) has a first region (111) having a refractive index (n1) that decreases in a direction from the center toward the outer edge, and a second region (112) that is located on the outer periphery of the first region (111), includes the outer edge of the core (12), and has a constant refractive index (n2). The refractive index (n2) of the second region is equal to or less than the refractive index (n1) of the first region, the thickness of the second region is 2 [mu] m or more and less than 5 [mu] m, and the refractive index (n3) of the trench layer is lower than the refractive index (n2) of the second region.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to plastic optical fibers, optical cables, and active optical cables. Background Art

[0002] An optical fiber includes a core at the center portion that transmits light, and a region called a cladding or a trench (English: trench, Japanese original: レンチ) provided on the periphery of the core to confine light in the core.

[0003] Optical fibers include plastic optical fibers (hereinafter referred to as "POF") whose cores are formed of resin materials and glass optical fibers (hereinafter referred to as "GOF") whose cores are formed of glass materials. POF is more flexible than GOF and has better bending resistance (i.e., bending properties) and processability than GOF. Therefore, POF is generally used for short-distance applications at the end of an optical fiber transmission network (e.g., wiring within a home, etc.).

[0004] There are SI (Step-Index) type POF and GI (Graded-Index) type POF. SI type POF is a POF with a uniform refractive index in the core. GI type POF is a POF with a refractive index distribution in which the refractive index of the core decreases from the center of the core toward the outer edge of the core. In SI type, the propagation time varies depending on the path (mode) of light, so the signal pulse is wide and the bandwidth is low. In contrast, GI type POF greatly reduces the propagation time difference through the refractive index distribution, so the bandwidth is high and high-speed communication is possible.

[0005] In addition, in GI type POF, in order to make the bending loss smaller and thus be able to accept a wider range of light (that is, to achieve a larger numerical aperture (NA)), a groove layer optically designed in a manner to have a refractive index lower than the refractive index of the outer edge of the core is provided on the periphery of the core.

[0006] For example, Patent Document 1 discloses a multimode optical fiber having high bending resistance and in which the influence of a leakage mode is suppressed by an optical design of a trench layer.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application No. 2016-527547 Summary of the invention

[0010] Problems to be solved by the invention

[0011] However, the groove layer provided for the purpose of reducing bending loss, etc., reduces the frequency band due to the reflected light of the light incident on the groove layer. It should be noted that when the distance of the POF is short, the reduction of the frequency band caused by the reflection of the light in the groove layer becomes significant, and if the distance of the POF becomes longer, the influence becomes smaller. The reason is that when the light is guided in the POF, the light components that cause the reduction of the frequency band, such as the light incident on the POF at an angle larger than the numerical aperture (NA) of the POF and the scattered light, are lost. That is, as the distance of the POF becomes longer, the component of the light that reduces the frequency band is reduced.

[0012] As described above, POF is generally used for short-distance applications (e.g., 1 m to 100 m), and is easily affected by light components that reduce the frequency band in a short distance. However, conventionally, no technology has been proposed for improving the frequency band in a short distance with respect to POF in an optical fiber, especially with respect to POF provided with a groove layer for reducing bending loss.

[0013] The present disclosure aims to provide a POF having a groove layer for improving bending loss, the POF improving the frequency band in a short distance. In addition, the present disclosure aims to provide an optical cable and an active optical cable having such a POF having an improved frequency band in a short distance.

[0014] Means for solving problems

[0015] The POF according to the first aspect of the present disclosure includes:

[0016] a fiber core; and

[0017] A groove layer is arranged on the outer periphery of the core.

[0018] The above-mentioned fiber core has:

[0019] A first region having a refractive index n1 that decreases in a direction from the center toward the outer edge;

[0020] a second region, which is located at the periphery of the first region, includes the outer edge of the core, and has a constant refractive index n2,

[0021] The refractive index n2 of the second region is less than the refractive index n1 of the first region,

[0022] The thickness of the second region is greater than or equal to 2 μm and less than 5 μm.

[0023] A refractive index n3 of the trench layer is lower than the refractive index n2 of the second region.

[0024] An optical cable according to a second aspect of the present disclosure includes the POF according to the first aspect of the present disclosure.

[0025] An active optical cable according to a third aspect of the present disclosure includes the optical cable according to the second aspect of the present disclosure and an optoelectronic hybrid module.

[0026] Effects of the Invention

[0027] According to the present disclosure, it is possible to provide a POF having an improved frequency band within a short distance. In addition, the present disclosure can provide an optical cable and an active optical cable having such a POF having an improved frequency band within a short distance. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a schematic diagram showing an example of a cross-sectional structure of a POF according to an embodiment of the present disclosure.

[0029] Figure 2 This is a graph showing a curve of the refractive index of the POF according to the embodiment of the present disclosure.

[0030] Figure 3 It is a schematic diagram showing an example of a cross-sectional structure of a modified example of the POF according to the embodiment of the present disclosure.

[0031] Figure 4 This is a schematic cross-sectional view showing an example of a production apparatus that can be used to produce POF according to an embodiment of the present disclosure.

[0032] Figure 5 1 is a schematic diagram showing an example of an optical cable according to an embodiment of the present disclosure.

[0033] Figure 6 1 is a schematic diagram showing an example of an active optical cable according to an embodiment of the present disclosure.

[0034] Figure 7 It is a schematic diagram showing a measurement system for measuring the bending loss of POF in Examples and Comparative Examples. DETAILED DESCRIPTION

[0035] (definition)

[0036] In this specification, the refractive index refers to a value measured by a prism coupling method.

[0037] In this specification, "optical loss when a plastic optical fiber (POF) is bent into a U-shape with a bending radius of R mm" refers to the optical loss obtained by the following procedure.

[0038] (a) Connect a light source to the incident side of the POF (length: 5 m) and connect an optical power meter to the light receiving side of the POF.

[0039] (b) Wrap the 1m portion of the incident side of the POF around a φ12.5mm cylinder 10 times to remove the cladding mode

[0040] (c) The central part (2.5 m part) of the POF is placed on a plate having a U-shaped groove with a bending radius R to bend the POF.

[0041] (d) Check the change in insertion loss associated with the change from a straight state to a curved state and calculate the optical loss

[0042] (Embodiments of the present disclosure)

[0043] The POF according to the embodiment of the present disclosure will be described.

[0044] Figure 1 It is a schematic diagram showing an example of a cross-sectional structure of a POF according to an embodiment of the present disclosure. Figure 2 This is a graph showing a curve of the refractive index of the POF according to the embodiment of the present disclosure.

[0045] The POF 10 of the present embodiment includes a core 11 and a groove layer 12 arranged on the periphery of the core 11. The core 11 has a first region 111 and a second region 112. The first region 111 has a refractive index n1 that decreases in a direction from the center 11a of the core 11 toward the outer edge 11b. The second region 112 is located on the periphery of the first region 111, includes the outer edge 11b of the core 11, and has a constant refractive index n2. The refractive index n2 of the second region 112 is less than the refractive index n1 of the first region 111. The thickness of the second region 112 is greater than 2 μm and less than 5 μm. The refractive index n3 of the groove layer 12 is lower than the refractive index n2 of the second region 112 of the core 11. It should be noted that the refractive index of the core 11 (the first region 111 and the second region 112 ) and the trench layer 12 refers to the refractive index for light of the wavelength (eg, 850 nm) of light propagating in the core 11 .

[0046] The refractive index n1 of the first region 111 of the core 11 of the POF 10 of the present embodiment has a refractive index distribution. Therefore, the POF 10 of the present embodiment is a GI type. Specifically, Figure 2 As shown, the center of the first region 111 of the core 11 has the largest refractive index, and the refractive index of the first region 111 gradually decreases toward the second region 112. In addition, the refractive index in the second region 112 is constant. Here, "the refractive index in the second region 112 is constant" means that the difference between the maximum refractive index and the minimum refractive index in the second region 112 is less than 0.005. In addition, the refractive index in the groove layer 12 may also be constant, for example. "The refractive index in the groove layer 12 is constant" means that the difference between the maximum refractive index and the minimum refractive index in the groove layer 12 is less than 0.005. As shown in FIG. Figure 2 As shown, the POF diameter refers to the diameter of the POF having the core 11 and the trench layer 12. In addition, Figure 2 The longitudinal direction refers to the relative height of the refractive index.

[0047] The POF10 of this embodiment has the following structure: a second region 112 having a constant refractive index n2 and satisfying the relationship of n1≥n2>n3 is provided between the first region 111 (refractive index n1) of the core 11 having a refractive index distribution and the groove layer 12 (refractive index n3) provided to seal light into the core 11. In addition, the thickness of the second region 112 is greater than 2μm and less than 5μm. Through this structure, it is possible to prevent the light propagating in the core 11 from reaching the groove layer 12, that is, the light is not incident on the groove layer 12. Therefore, the POF10 of this embodiment can suppress the reduction of the frequency band due to the reflection of the light incident on the groove layer 12. As a result, the POF10 of this embodiment has a lower bending loss and can achieve a higher frequency band within a short distance.

[0048] Here, the short-distance POF is, for example, 30 m or less, preferably 10 m or less, and more preferably 5 m or less. The short-distance POF is, for example, 1 m or more.

[0049] The POF10 of this embodiment can, for example, set the -1.5dB band value to be above 40MHz·km when the overflow light is incident at 5m. In this way, the POF10 of this embodiment can achieve a high frequency band of above 40MHz·km even in a very short distance of 5m. It should be noted that the band of the POF10 of this embodiment is a value measured by the pulse method in accordance with the method of IEC60793-1-41, under the excitation condition of full-mode excitation using the overflow light. Overflow light refers to light whose numerical aperture (NA) of the incident light is greater than the numerical aperture (NA) of the POF under test and whose beam diameter of the incident light is greater than the core diameter of the POF under test.

[0050] Here, in this specification, the core diameter of POF refers to the outer diameter of the core. The outer diameter of the core is the diameter of the light intensity of 5% measured by the near field pattern method (hereinafter referred to as "NFP method") using light of wavelength 850nm in accordance with the method of IEC60793-1-20 and IEC60793-2-40subcategory A4h. The diameter of the light intensity of 5% refers to the diameter of an approximate circle determined by a portion having a light intensity of 5% relative to the peak value of the light intensity. In addition, the place with a brightness of 100% refers to the place with the highest brightness in the core. It should be noted that the outer edge 11b of the core 11 can be determined by the same method as the core diameter, namely the NFP method.

[0051] In the POF 10 of the present embodiment, the first region 111 and the second region 112 of the core 11 can be determined using the NFP method in the same manner as the method for measuring the core diameter of the above-mentioned POF. The refractive index in the core 11 can be confirmed based on the surface distribution of the light intensity of the emitted light obtained by the measurement based on the NFP method. Therefore, by using the surface distribution of the emitted light intensity and differentiating the surface distribution to obtain the inflection point, the first region 111 having a refractive index distribution and the second region 112 having a constant refractive index can be distinguished. The outer edge of the second region 112 is the outer edge 11b of the core 11, that is, it is equivalent to the interface (core / groove layer interface) between the core 11 and the groove layer 12. Therefore, the second region 112 is the region between the above-mentioned inflection point and the core / groove layer interface. The outer diameter of the first region 111 can be determined by the above-mentioned inflection point, and the outer diameter of the second region 112 can be determined by the core / groove layer interface. By determining the outer diameter of each region, the thickness of the second region 112 can be obtained.

[0052] The outer diameter of the trench layer 12 can also be obtained using the NFP method in the same manner as the core diameter.

[0053] The refractive index n1 of the first region 111 of the core 11, the refractive index n2 of the second region 112, and the refractive index n3 of the groove layer 12 can be obtained by the following method. Using the core material and the groove layer material, sheet-shaped test pieces are made by hot pressing. Using the test piece, the refractive index of the core material and the groove layer material is obtained by the prism coupling method. Next, the opening angle is measured by the far-field pattern method to obtain the refractive index difference between the core and the groove layer. Then, referring to 2.4 of the paper (Tachibana Hirohiro, "Measurement Method of Refractive Index Distribution of Optical Fiber", Applied Physics Vol. 48 No. 8), the refractive index n1 of the first region 111 of the core 11, the refractive index n2 of the second region 112, and the refractive index n3 of the groove layer 12 are calculated.

[0054] In the POF10 of the present embodiment, the first optical loss when bent into a U shape with a bending radius of 1.5 mm is, for example, preferably less than 3.0 dB, and more preferably less than 1.0 dB. In the POF10 of the present embodiment, since the core 11 is a POF formed of a resin material, the bending loss is lower than that of a GOF, and since the groove layer 12 is provided, the bending loss can be suppressed to a smaller value within the above range. With this configuration, the POF10 of the present embodiment can suppress the bending loss to a smaller value within the above range, and can achieve a higher frequency band within a short distance. The above-mentioned first optical loss is, for example, more than 0.5 dB, more than 0.7 dB, or more than 0.75 dB. It should be noted that the method for measuring the first optical loss as the bending loss is described in the embodiments described later.

[0055] In addition, in the POF 10 of the present embodiment, the second optical loss when bent into a U shape with a bending radius of 2.0 mm is preferably, for example, 0.5 dB or less. According to this configuration, the POF 10 of the present embodiment can suppress the bending loss to be smaller within the above range, and can achieve a higher frequency band in a short distance. The above-mentioned second optical loss is, for example, 0.1 dB or more, 0.3 dB or more, or 0.4 dB or more. It should be noted that the method for measuring the second optical loss as the bending loss is described in the embodiment described later.

[0056] In order to further improve the frequency band, the thickness of the second region 112 in the core 11 of the POF 10 of the present embodiment is preferably, for example, 2.9 μm or more and 4.8 μm or less. In order to further improve the frequency band, the thickness of the second region 112 is more preferably 2.9 μm or more and 4.5 μm or less. In order to further improve the frequency band, the thickness of the second region 112 is more preferably 3.5 μm or more and 4.4 μm or less.

[0057] The POF 10 of this embodiment can achieve a larger numerical aperture (NA) by providing the groove layer 12. Therefore, the POF 10 of this embodiment can receive light in a wider range. The POF 10 of this embodiment has a numerical aperture (NA) of, for example, 0.190 or more and 0.235 or less.

[0058] Hereinafter, each structure of the POF 10 of this embodiment will be described in more detail.

[0059] (Core 11)

[0060] The core 11 is a region for transmitting light. As described above, the core 11 has a first region 111 having a refractive index distribution (refractive index n1) and a second region 112 having a constant refractive index n2. The refractive indexes of the first region 111 and the second region 112 (i.e., refractive index n1 and refractive index n2) are higher than the refractive index n3 of the groove layer 12. According to this configuration, light incident into the core 11 is confined inside the core 11 by the groove layer 12 and propagates in the POF 10.

[0061] The core 11 contains the first resin. The core 11 may contain the first resin as a main component. Here, the core 11 contains the first resin as a main component means that the first resin is the largest component in the core 11 in terms of mass ratio. The core 11 may contain 75% by mass or more of the first resin, or 80% by mass or more, or 85% by mass or more.

[0062] The core 11 may further include an additive in addition to the first resin. The additive is, for example, a refractive index adjuster. That is, the core 11 may be formed of a resin composition including the first resin and an additive such as a refractive index adjuster. As the refractive index adjuster, for example, a known refractive index adjuster used in the material of the core 11 of the POF 10 may be used. The material of the core 11 may also include other additives in addition to the refractive index adjuster.

[0063] The first region 111 of the core 11 has a refractive index distribution in which the refractive index decreases in the direction from the center 11a of the core 11 toward the outer edge 11b. Such a refractive index distribution can be formed, for example, by adding a refractive index adjusting agent to the first resin and diffusing the refractive index adjusting agent in the first resin (for example, thermal diffusion). The second region 111 of the core 11 having a constant refractive index n2 can be formed, for example, by adjusting the conditions (for example, diffusion temperature and diffusion time) when diffusing the refractive index adjusting agent in the first resin (for example, thermal diffusion), adjusting the ejection amount of the core material when manufacturing the POF 10 of this embodiment by melt spinning, etc.

[0064] The first resin contained in the core 11 is not particularly limited as long as it has high transparency. Examples of the first resin include fluorine-containing resins, acrylic resins such as methyl methacrylate, styrene resins, and carbonate resins.

[0065] The first resin contained in the core 11 can be at least one selected from perfluoro resin, partial fluoro resin, partial chlorine resin and partial deuterated resin. Here, the partial fluoro resin, partial chlorine resin and partial deuterated resin refer to resins in which a part of the hydrogen atoms of the CH bond is replaced by fluorine, chlorine and deuterium respectively in the resin known in the technical field as the core material of POF. Here, the perfluoro resin refers to a resin in which all the hydrogen atoms of the CH bond are replaced by fluorine in the resin known in the technical field as the core material of POF. As examples of resins known in the technical field as core materials, acrylic resins such as methyl methacrylate, styrene resins and carbonate resins as described above can be cited. Polymers having an aliphatic ring structure such as a polymer having a dioxolane structure can be used.

[0066] The first resin is preferably at least one selected from a perfluorinated resin and a partially fluorinated resin. That is, the first resin is preferably a fluorinated resin.

[0067] The first resin of the core 11 is preferably a fluorine-containing resin containing a fluorine-containing polymer. Hereinafter, the fluorine-containing resin contained in the core 11 is referred to as a first fluorine-containing resin, and the fluorine-containing polymer contained in the first fluorine-containing resin is referred to as a first fluorine-containing polymer.

[0068] From the viewpoint of suppressing light absorption caused by the stretching energy of the CH bond, the first fluoropolymer contained in the first fluororesin preferably does not substantially contain hydrogen atoms, and it is particularly preferred that all hydrogen atoms bonded to carbon atoms are substituted by fluorine atoms. That is, the first fluoropolymer preferably does not substantially contain hydrogen atoms and is perfluorinated. In this specification, the fluoropolymer does not substantially contain hydrogen atoms means that the content of hydrogen atoms in the fluoropolymer is less than 1 mol%.

[0069] The first fluorinated polymer preferably has a fluorinated aliphatic ring structure. The fluorinated aliphatic ring structure may be contained in the main chain of the fluorinated polymer or in the side chain of the first fluorinated polymer. The first fluorinated polymer has, for example, a structural unit (A) represented by the following structural formula (1).

[0070]

Chemical formula 1

[0071]

[0072] In formula (1), R ff 1 ~R ff 4 Each independently represents a fluorine atom, a perfluoroalkyl group having 1 to 7 carbon atoms, or a perfluoroalkyl ether group having 1 to 7 carbon atoms. ff 1 and R ff 2 can be linked to form a ring. "Perfluoro" means that all hydrogen atoms bonded to carbon atoms are replaced by fluorine atoms. In formula (1), the number of carbon atoms in the perfluoroalkyl group is preferably 1 to 5, more preferably 1 to 3, and further preferably 1. The perfluoroalkyl group may be linear or branched. Examples of the perfluoroalkyl group include trifluoromethyl, pentafluoroethyl, heptafluoropropyl, and the like.

[0073] In formula (1), the number of carbon atoms in the perfluoroalkyl ether group is preferably 1 to 5, more preferably 1 to 3. The perfluoroalkyl ether group may be linear or branched. Examples of the perfluoroalkyl ether group include perfluoromethoxymethyl and the like.

[0074] In R ff 1 and R ff 2 When the rings are linked to form a ring, the ring may be a 5-membered ring or a 6-membered ring. Examples of the ring include a perfluorotetrahydrofuran ring, a perfluorocyclopentane ring, and a perfluorocyclohexane ring.

[0075] Specific examples of the structural unit (A) include structural units represented by the following formulae (A1) to (A8).

[0076]

Chemical formula 2

[0077]

[0078] The structural unit (A) is preferably a structural unit (A2) among the structural units represented by the above formulae (A1) to (A8), that is, a structural unit represented by the following formula (2).

[0079]

Chemical formula 3

[0080]

[0081] The first fluoropolymer may include one or more structural units (A). In the first fluoropolymer, the content of the structural unit (A) is preferably more than 20 mol% relative to the total of all structural units, and more preferably more than 40 mol%. By including more than 20 mol% of the structural unit (A), the first fluoropolymer has a trend of having higher heat resistance. In the case of including more than 40 mol% of the structural unit (A), the first fluoropolymer has a trend of having higher transparency and high mechanical strength in addition to having high heat resistance. In the first fluoropolymer, the content of the structural unit (A) is preferably less than 95 mol% relative to the total of all structural units, and more preferably less than 70 mol%.

[0082] The structural unit (A) is derived from, for example, a compound represented by the following formula (3). ff 1 ~R ff 4 The same as formula (1). The compound represented by formula (3) can be obtained by a known production method such as the production method disclosed in JP-A-2007-504125.

[0083]

Chemical formula 4

[0084]

[0085] Specific examples of the compound represented by the above formula (3) include compounds represented by the following formulas (M1) to (M8).

[0086]

Chemical formula 5

[0087]

[0088] The fluorinated polymer may further contain other structural units in addition to the structural unit (A). Examples of the other structural units include the following structural units (B) to (D).

[0089] The structural unit (B) is represented by the following formula (4).

[0090]

Chemical formula 6

[0091]

[0092] In formula (4), R 1 ~R 3 Each independently represents a fluorine atom or a perfluoroalkyl group having 1 to 7 carbon atoms. 4 It represents a perfluoroalkyl group having 1 to 7 carbon atoms. The perfluoroalkyl group may have a ring structure. A part of the fluorine atoms may be substituted by a halogen atom other than a fluorine atom. A part of the fluorine atoms in the perfluoroalkyl group may be substituted by a halogen atom other than a fluorine atom.

[0093] The fluorinated polymer may contain one or more structural units (B). In the fluorinated polymer, the content of the structural unit (B) is preferably 5 to 10 mol% relative to the total of all structural units. The content of the structural unit (B) may be 9 mol% or less, or 8 mol% or less.

[0094] The structural unit (B) is derived from, for example, a compound represented by the following formula (5). 1 ~R 4 The same as formula (4). The compound represented by formula (5) is a fluorine-containing vinyl ether such as perfluorovinyl ether.

[0095]

Chemical formula 7

[0096]

[0097] The structural unit (C) is represented by the following formula (6).

[0098]

Chemical formula 8

[0099]

[0100] In formula (6), R 5 ~R 8 Each independently represents a fluorine atom or a perfluoroalkyl group having 1 to 7 carbon atoms. The perfluoroalkyl group may have a ring structure. A portion of the fluorine atoms may be substituted by a halogen atom other than a fluorine atom. A portion of the fluorine atoms in the perfluoroalkyl group may be substituted by a halogen atom other than a fluorine atom.

[0101] The fluorinated polymer may contain one or more structural units (C). In the fluorinated polymer, the content of the structural unit (C) is preferably 5 to 10 mol% relative to the total of all structural units. The content of the structural unit (C) may be 9 mol% or less, or 8 mol% or less.

[0102] The structural unit (C) is derived from, for example, a compound represented by the following formula (7). 5 ~R 8The same as formula (6). The compound represented by formula (7) is a fluorine-containing olefin such as tetrafluoroethylene and chlorotrifluoroethylene.

[0103]

Chemical formula 9

[0104]

[0105] The structural unit (D) is represented by the following formula (8).

[0106]

Chemical formula 10

[0107]

[0108] In formula (8), Z represents an oxygen atom, a single bond or -OC(R 19 R 20 )O-,R 9 ~R 20 Each independently represents a fluorine atom, a perfluoroalkyl group having 1 to 5 carbon atoms, or a perfluoroalkoxy group having 1 to 5 carbon atoms. A portion of the fluorine atoms may be substituted by a halogen atom other than a fluorine atom. A portion of the fluorine atoms in the perfluoroalkyl group may be substituted by a halogen atom other than a fluorine atom. A portion of the fluorine atoms in the perfluoroalkoxy group may be substituted by a halogen atom other than a fluorine atom. s and t each independently represent an integer from 0 to 5, and s+t is an integer from 1 to 6 (wherein, when Z is -OC(R 19 R 20 )O-, s+t can be 0).

[0109] The structural unit (D) is preferably represented by the following formula (9). The structural unit represented by the following formula (9) is the case where Z is an oxygen atom, s is 0, and t is 2 in the above formula (8).

[0110]

Chemical formula 11

[0111]

[0112] In formula (9), R 141 , R 142 , R 151 and R 152 Each independently represents a fluorine atom, a perfluoroalkyl group having 1 to 5 carbon atoms, or a perfluoroalkoxy group having 1 to 5 carbon atoms. A portion of the fluorine atoms may be substituted by a halogen atom other than a fluorine atom. A portion of the fluorine atoms in the perfluoroalkyl group may be substituted by a halogen atom other than a fluorine atom. A portion of the fluorine atoms in the perfluoroalkoxy group may be substituted by a halogen atom other than a fluorine atom.

[0113] The fluorinated polymer may contain one or more structural units (D). In the fluorinated polymer, the content of the structural unit (D) is preferably 30 to 67 mol% relative to the total of all structural units. The content of the structural unit (D) is, for example, 35 mol% or more, 60 mol% or less, or 55 mol% or less.

[0114] The structural unit (D) is derived from, for example, a compound represented by the following formula (10). 9 ~R 18 , s and t are the same as those in formula (4). The compound represented by formula (10) is a fluorine-containing compound having two or more polymerizable double bonds and capable of cyclopolymerization.

[0115]

Chemical formula 12

[0116]

[0117] The structural unit (D) is preferably derived from a compound represented by the following formula (11). In formula (11), R 141 , R 142 , R 151 and R 152 Same as formula (9).

[0118]

Chemical formula 13

[0119]

[0120] Specific examples of the compound represented by formula (10) or formula (11) include the following compounds.

[0121] CF2=CFOCF2CF=CF2

[0122] CF2=CFOCF(CF3)CF=CF2

[0123] CF2=CFOCF2CF2CF=CF2

[0124] CF2=CFOCF2CF(CF3)CF=CF2

[0125] CF2=CFOCF(CF3)CF2CF=CF2

[0126] CF2=CFOCFClCF2CF=CF2

[0127] CF2=CFOCCl2CF2CF=CF2

[0128] CF2=CFOCF2OCF=CF2

[0129] CF2=CFOC(CF3)2OCF=CF2

[0130] CF2=CFOCF2CF(OCF3)CF=CF2

[0131] CF2=CFCF2CF=CF2

[0132] CF2=CFCF2CF2CF=CF2

[0133] CF2=CFCF2OCF2CF=CF2

[0134] CF2=CFOCF2CFClCF=CF2

[0135] CF2=CFOCF2CF2CCl=CF2

[0136] CF2=CFOCF2CF2CF=CFCl

[0137] CF2=CFOCF2CF(CF3)CCl=CF2

[0138] CF2=CFOCF2OCF=CF2

[0139] CF2=CFOCCl2OCF=CF2

[0140] CF2=CClOCF2OCCl=CF2

[0141] The first fluorinated polymer may further contain other structural units other than the structural units (A) to (D), but preferably does not substantially contain other structural units other than the structural units (A) to (D). It should be noted that the fluorinated polymer does not substantially contain other structural units other than the structural units (A) to (D) means that the total amount of the structural units (A) to (D) is 95 mol% or more, preferably 98 mol% or more, relative to the total amount of all structural units in the fluorinated polymer.

[0142] The polymerization method of the first fluorinated polymer is not particularly limited, and for example, a common polymerization method such as radical polymerization may be used. The polymerization initiator used for polymerizing the fluorinated polymer may be a perfluorinated compound.

[0143] The first fluorinated polymer constitutes the first fluorinated resin used as the first resin. The first glass transition temperature Tg1 of the first resin is not particularly limited, and is, for example, 100°C to 140°C, may be 105°C or higher, or may be 120°C or higher. In this specification, Tg refers to the midpoint glass transition temperature (Tg1) determined in accordance with the provisions of JIS K7121:1987. mg ).

[0144] The refractive index n1 of the first region 111 of the core 11 preferably has a refractive index distribution such that g satisfies 1.9≤g≤2.1 in the following mathematical formula (1). Δ in the mathematical formula (1) is represented by the following mathematical formula (2).

[0145] n1(r)=n A [1-2Δ(r / a) g ] 1 / 2 Mathematical formula (1)

[0146] Δ=(n A 2 -n B 2 ) / 2h A 2 ···Mathematical formula (2)

[0147] In mathematical formulas (1) and (2), r, a, and n are A and n B as follows.

[0148] r: radius

[0149] a: radius of the first region 111 of the core 11

[0150] n A : The center of the core 11, i.e., the refractive index value of r = 0

[0151] n B : The refractive index value of the outer edge of the first region 111 of the core 11

[0152] The refractive index n1 of the first region 111 can be set to be within the range of 1.329 to 1.341, for example, at a wavelength of 850 nm.

[0153] The refractive index n2 of the second region 112 only needs to be equal to or less than the refractive index n1, and for example, can be set within the range of 1.327 to 1.331 at a wavelength of 850 nm.

[0154] (Groove layer 12)

[0155] In the POF 10 of the present embodiment, the groove layer 12 includes, for example, a second resin. The groove layer 12 may include the second resin as a main component. Here, the groove layer 12 includes the second resin as a main component means that, in the groove layer 12, the second resin is the largest component in terms of mass ratio. The groove layer 12 may include more than 80% by mass of the second resin, more than 90% by mass, or more than 95% by mass. The groove layer 12 may consist only of the second resin. The groove layer 12 may also include additives in addition to the second resin.

[0156] The second resin contained in the groove layer 12 is not particularly limited as long as it has high transparency. Examples of the second resin are the same as those exemplified as the resin that can be used as the first resin. As with the first resin, a fluorine-containing resin is preferably used as the second resin.

[0157] The second resin of the groove layer 12 is preferably a fluorine-containing resin containing a fluorine-containing polymer. Hereinafter, the fluorine-containing resin contained in the groove layer 12 is referred to as a second fluorine-containing resin, and the fluorine-containing polymer contained in the second fluorine-containing resin is referred to as a second fluorine-containing polymer.

[0158] As the second fluorine-containing resin, the fluorine-containing resins exemplified as the fluorine-containing resin that can be used as the first fluorine-containing resin can be used.

[0159] As the second fluorine-containing resin, a fluorine-containing resin comprising a fluorine-containing polymer and a fluorine-containing plasticizer, the fluorine-containing polymer comprising a structural unit (E) represented by the following formula (12) and having an amorphous structure.

[0160]

Chemical formula 14

[0161]

[0162] (In formula (12), Z represents an oxygen atom, a single bond or -OC(R 31 R 32 )O-,R 21 ~R 32 Each independently represents a fluorine atom, a perfluoroalkyl group having 1 to 5 carbon atoms, or a perfluoroalkoxy group having 1 to 5 carbon atoms. "Perfluoro" means that all hydrogen atoms bonded to carbon atoms are substituted by fluorine atoms. A portion of the fluorine atoms may be substituted by halogen atoms other than fluorine atoms. A portion of the fluorine atoms in the perfluoroalkyl group may be substituted by halogen atoms other than fluorine atoms. A portion of the fluorine atoms in the perfluoroalkoxy group may be substituted by halogen atoms other than fluorine atoms. s and t each independently represent an integer from 0 to 5, and s+t is an integer from 1 to 6 (wherein, when Z is -OC(R 31 R 32 )O-, s+t can be 0). u and v are each independently 0 or 1. )

[0163] The fluorinated polymer containing the structural unit (E) may further contain a structural unit CF) represented by the following formula (13).

[0164]

Chemical formula 15

[0165]

[0166] (In formula (13), R 33 ~R 36Each independently represents a fluorine atom or a perfluoroalkyl group having 1 to 7 carbon atoms. The perfluoroalkyl group may have a ring structure. A portion of the fluorine atoms may be substituted by a halogen atom other than a fluorine atom. A portion of the fluorine atoms in the perfluoroalkyl group may be substituted by a halogen atom other than a fluorine atom.

[0167] When the second fluorinated polymer is the above-mentioned copolymer, the ratio of the structural unit (E) to the structural unit (F) is arbitrary and is not particularly limited.

[0168] The second fluorinated polymer is preferably at least one selected from the group consisting of, for example, a fluorinated polymer A and a fluorinated polymer B shown below.

[0169] The fluorinated polymer A contains a structural unit (G) represented by the following formula (14) and a structural unit (H) represented by the following formula (15). 23 , R 24 , R 31 and R 32 The same as the above formula (12).

[0170]

Chemical formula 16

[0171]

[0172]

Chemical formula 17

[0173]

[0174] (In formula (15), R 37 ~R 40 Each independently represents a fluorine atom or a perfluoroalkyl group having 1 to 7 carbon atoms. The perfluoroalkyl group may have a ring structure. A portion of the fluorine atoms may be substituted by a halogen atom other than a fluorine atom. A portion of the fluorine atoms in the perfluoroalkyl group may be substituted by a halogen atom other than a fluorine atom.

[0175] The fluorinated polymer B contains a structural unit (I) represented by the following formula (16). 21 ~R 24 , R 27 ~R 30 , R 31 and R 32 The same as the above formula (12).

[0176]

Chemical formula 18

[0177]

[0178] The fluoropolymer A and the fluoropolymer B have very high transparency, and can have a refractive index very low compared to the normal refractive index of the first fluororesin used as the material of the core 11. Therefore, the second fluororesin containing at least one selected from the fluoropolymer A and the fluoropolymer B as the second fluoropolymer can further reduce the refractive index while maintaining the high transparency of the groove layer 12. As a result, the difference between the refractive index of the core 11 and the refractive index of the groove layer 12 can be further increased, so the sealing effect of the groove layer 12 on light into the core 11 is further improved, and low transmission loss of the POF 10 can be easily achieved.

[0179] The second fluorinated polymer preferably contains a structural unit (J) represented by the following formula (17).

[0180]

Chemical formula 19

[0181]

[0182] (In formula (17), m and n are arbitrary integers)

[0183] The second fluorine-containing polymer constitutes the second fluorine-containing resin used as the second resin. The second glass transition temperature Tg2 of the second resin is not particularly limited, and is, for example, 100° C. to 150° C., may be 105° C. or higher, or may be 125° C. or higher.

[0184] The refractive index n3 of the groove layer 12 can be designed according to the refractive index n2 of the second region 112 of the core 11, and is therefore not particularly limited. The refractive index n3 of the groove layer 12 can be, for example, 1.34 or less, or 1.33 or less at a wavelength of 850 nm. The refractive index n3 of the groove layer 12 can be, for example, 1.32 or more at a wavelength of 850 nm.

[0185] The difference between the refractive index n3 of the trench layer 12 and the refractive index n2 of the second region 112 of the core 11 is preferably 0.005 or more and 0.010 or less.

[0186] (Variation of POF)

[0187] Figure 3 Modifications of the POF of this embodiment are shown. Figure 3The POF 20 shown has a structure in which a reinforcement layer 21 is further provided on the periphery of the groove layer 12 relative to the POF 10. The reinforcement layer 21 is provided to improve the mechanical strength of the POF 10. For example, the material and structure used as the reinforcement layer in the known POF can be applied to the reinforcement layer 21. As the material of the reinforcement layer 21, for example, various engineering plastics such as polycarbonate, polyester, cycloolefin polymer, cycloolefin copolymer, polytetrafluoroethylene (PTFE), modified PTFE and tetrafluoroethylene-perfluoroalkoxyethylene copolymer (PFA), or their copolymers, mixtures, etc. can be cited.

[0188] (Manufacturing method of POF)

[0189] The POF of the present embodiment is manufactured, for example, using a melt spinning method. That is, an example of a method for manufacturing the POF of the present embodiment includes:

[0190] The step of melting and extruding the core material into a fiber shape to produce a fiber-shaped molded body including the core material; and

[0191] The groove layer material is melted and extruded so as to cover the surface of the molded body, thereby producing a laminated body in which the core material and the groove layer material are concentrically laminated. The core material, for example, includes a first resin. The groove layer material, for example, includes a second resin.

[0192] When manufacturing a fibrous molded body formed of a core material, first, a first core material containing a refractive index adjusting agent is extruded to form a core inner layer portion, and then a second core material is extruded to cover the outer periphery of the core inner layer portion 2 formed of the first core material 1a. In this case, the first region 111 and the second region 112 of the core 11 can be formed by diffusing the refractive index adjusting agent contained in the first core material toward the core outer periphery formed by the second core material. In order to form the second region 111 of the core 11 having a constant refractive index n2, for example, the conditions (e.g., diffusion temperature and diffusion time) when diffusing the refractive index adjusting agent (e.g., thermal diffusion), the ejection amounts of the first core material and the second core material, etc. are adjusted.

[0193] Figure 4 Yes means Figure 3 Schematic cross-sectional view of an example of a manufacturing apparatus that can be used to manufacture the POF 20 shown.

[0194] Figure 4The device 1000 shown includes a first extrusion device 101a for extruding a first core material, a second extrusion device 101b for extruding a second core material, a third extrusion device 101c for extruding a groove layer material, and a fourth extrusion device 101d for forming a coating layer.

[0195] The first extrusion device 101a includes a first receiving portion 102a for receiving the first core material 1a and a first extrusion portion 103a for extruding the first core material 1a received in the first receiving portion 102a from the first receiving portion 102a. The first extrusion device 101a is further provided with a heating portion (not shown) so that the first core material 1a can be melted in the first receiving portion 102a and the molten state can be maintained until the molten first core material 1a is formed. The rod-shaped first core material (preform) 1a is inserted into the first receiving portion 102a through the opening at the top of the first receiving portion 102a and is heated and melted in the first receiving portion 102a.

[0196] In the first extrusion device 101a, the first core material 1a is extruded by gas, and is extruded outward from the first accommodation portion 102a through the first extrusion unit 103a to form the core inner layer portion 2. The first core material 1a extruded through the first extrusion unit 103a to form the core inner layer portion 2 then moves downward in the vertical direction and is supplied to the first chamber 110.

[0197] The second extrusion device 101b includes a second housing portion 102b for housing the second core material 1b and a second extrusion portion 103b for extruding the second core material 1b housed in the second housing portion 102b from the second housing portion 102b. The second extrusion device 101b extrudes the molten second core material so as to cover the outer periphery of the core inner layer portion 2 formed by the first core material 1a extruded from the first extrusion device 101a. Specifically, the second core material extruded from the second extrusion device 101b is supplied to the first chamber 110. In the first chamber 110, by covering the core inner layer portion 2 formed by the first core material 1a with the second core material, the core outer peripheral portion 3 covering the outer periphery of the core inner layer portion 2 can be formed. The stacked body 4 formed of the core inner layer portion 2 and the core outer peripheral portion 3 covering the outer periphery of the core inner layer portion 2 moves from the first chamber 110 to the diffusion tube 120 arranged vertically below the first chamber 110. A heater (not shown) for heating the stacked body is arranged in the diffusion tube 120. The diffusion tube 120 diffuses the dopant such as the refractive index adjusting agent contained in the core inner layer portion 2 of the stacked body 4 passing through the diffusion tube 120 toward the core outer peripheral portion 3. That is, the core is finally formed by the core inner layer portion 2 and the core outer peripheral portion 3.

[0198] The third extrusion device 101c has a third housing portion 102c for housing the groove layer material 1c and a third extrusion portion 103c for extruding the groove layer material 1c housed in the third housing portion 102c from the third housing portion 102c. The third extrusion device 101c extrude the molten groove layer material 1c in a manner of covering the outer periphery of the stacked body 4 passing through the diffusion tube 120. Specifically, the groove layer material 1c extruded from the third extrusion device 101c is supplied to the second chamber 130. In the second chamber 130, by covering the stacked body 4 (i.e., the core) with the groove layer material 1c, the groove layer 5 covering the outer periphery of the core can be formed. It should be noted that, hereinafter, the stacked body 4 is referred to as the core 4. The stacked body formed by the core 4 and the groove layer 5 moves from the second chamber 130 to the third chamber 140 arranged vertically below the second chamber 130.

[0199] The fourth extrusion device 101d includes a fourth housing portion 102d for housing the coating material 1d, a screw 104 disposed in the fourth housing portion 102d, and a hopper 105 connected to the fourth housing portion 102d. In the fourth extrusion device 101d, for example, the coating material 1d in the form of pellets is supplied to the fourth housing portion 102d through the hopper 105. The coating material 1d supplied to the fourth housing portion 102d is kneaded by the screw 104 while being heated, thereby softening and being able to flow. The softened coating material 1d is extruded from the fourth housing portion 102d by the screw 104.

[0200] The coating material 1d extruded from the fourth extruder 101d is supplied to the third chamber 140. In the third chamber 140, the surface of the stacked body formed of the core 4 and the trench layer 5 is coated with the coating material 1d, thereby forming the coating layer 6 covering the outer periphery of the trench layer 5.

[0201] The stacked body 7 including the core 4, the trench layer 5 and the cladding layer 6 stacked concentrically flows from the third chamber 140 into the internal flow path through the inlet of the nozzle 150. The stacked body 7 is reduced in diameter through the internal flow path and is ejected from the ejection port of the nozzle 150 in a fiber shape.

[0202] The laminate 7 ejected from the ejection outlet of the nozzle 150 in a fibrous shape flows into the internal space 161 of the cooling pipe 160, is cooled while passing through the internal space 161, and is discharged from the opening to the outside of the cooling pipe 160. The laminate 7 discharged from the cooling pipe 160 passes between the two rollers 171 and 172 of the clamping roller 170, and further passes through the guide rollers 173 to 175, and is wound on the winding roller 176 as POF10. A displacement meter 180 for measuring the outer diameter of the POF10 may be further provided near the winding roller 176, for example, between the guide roller 175 and the winding roller 176.

[0203] The POF of this embodiment can also be applied to optical cables, active optical cables, and the like.

[0204] Figure 5 This is a schematic diagram showing an example of an optical cable including the POF 10 (or POF 20) according to the present embodiment. Figure 5 The optical cable 50 shown includes a cable 51 that accommodates the POF 10 (or POF 20 ) of the present embodiment, and a connector 52 attached to at least one end of the cable 51 .

[0205] Figure 6 This is a schematic diagram showing an example of an active optical cable including the POF 10 (or POF 20) according to the present embodiment. Figure 6 The active optical cable 60 shown includes a cable 61 that accommodates the POF10 (or POF20) of the present embodiment, a first connector 62 installed at the first end 61a of the cable 61 and including a first conversion unit (not shown) that converts an electrical signal into an optical signal, and a second connector 63 installed at the second end 61b of the cable 61 and including a second conversion unit (not shown) that converts an optical signal into an electrical signal.

[0206] Example

[0207] (Example 1)

[0208] [Preparation of the first fluorine-containing resin]

[0209] As the first fluorine-containing resin, a polymer of perfluoro-4-methyl-2-methylene-1,3-dioxolane (PFMMD) was prepared. Perfluoro-4-methyl-2-methylene-1,3-dioxolane is synthesized by first synthesizing 2-carboxymethyl-2-trifluoromethyl-4-methyl-1,3-dioxolane, fluorinating it, and separating the resulting carboxylate by decarbonation. In the polymerization of perfluoro-4-methyl-2-methylene-1,3-dioxolane, perfluorobenzoyl peroxide was used as a polymerization initiator.

[0210] The synthesis of 2-carboxymethyl-2-trifluoromethyl-4-methyl-1,3-dioxolane, the fluorination of 2-carboxymethyl-2-trifluoromethyl-4-methyl-1,3-dioxolane, the synthesis of perfluoro-4-methyl-2-methylene-1,3-dioxolane, and the polymerization of perfluoro-4-methyl-2-methylene-1,3-dioxolane are described in detail below.

[0211] <Synthesis of 2-carboxymethyl-2-trifluoromethyl-4-methyl-1,3-dioxolane>

[0212] Prepare a 3L three-necked flask with a water-cooled cooler, a thermometer, a magnetic stirrer and an isobaric dropping funnel, and put 139.4g (1.4 mol) of a mixture of 2-chloro-1-propanol and 1-chloro-2-propanol into the flask. Cool the flask to 0°C, slowly add methyl trifluoropyruvate thereto, and stir for 2 hours. Add 100mL of dimethyl sulfoxide (DMSO) and 194g of potassium carbonate thereto in 1 hour, and continue stirring for 8 hours to obtain a reaction mixture. The resulting reaction mixture is mixed with 1L of water, the aqueous phase is separated, and after further extraction with dichloromethane, the dichloromethane solution is mixed with the organic reaction mixture, and the solution is dried with magnesium sulfate. After removing the solvent, 245.5g of crude product is obtained. The crude product is fractionated under reduced pressure (12Torr) to obtain 230.9g of purified 2-carboxymethyl-2-trifluoromethyl-4-methyl-1,3-dioxolane. The boiling point of the purified product was 77-78°C and the yield was 77%. 19 FNMR confirmed that the obtained purified product was 2-carboxymethyl-2-trifluoromethyl-4-methyl-1,3-dioxolane.

[0213] HNMR (ppm): 4.2-4.6, 3.8-3.6 (CHCH2, multiplet, 3H), 3.85-3.88 (COOCH3, multiplet, 3H), 1.36-1.43 (CCH3, multiplet, 3H) 19 FNMR (ppm): -81.3 (CF3, s, 3F)

[0214] <Fluorinated 2-carboxymethyl-2-trifluoromethyl-4-methyl-1,3-dioxolane>

[0215] Inject 4L of 1,1,2-trichlorotrifluoroethane into a 10L stirred reaction tank. In the stirred reaction tank, nitrogen is circulated at a flow rate of 1340cc / min, and fluorine is circulated at a flow rate of 580cc / min, and the atmosphere is set to nitrogen / fluorine. After 5 minutes, 290g of the previously prepared 2-carboxymethyl-2-trifluoromethyl-4-methyl-1,3-dioxolane is dissolved in 750mL of 1,1,2-trichlorotrifluoroethane solution, and the solution is added to the reaction tank at a rate of 0.5ml / min. The reaction tank is cooled to 0°C. After all the dioxolanes are added within 24 hours, the fluorine gas flow is stopped. After purging nitrogen, potassium hydroxide aqueous solution is added until it becomes weakly alkaline.

[0216] After removing the volatile matter under reduced pressure, the surrounding of the reaction tank was cooled, and then dried under reduced pressure at 70°C for 48 hours to obtain a solid reaction product. The solid reaction product was dissolved in 500 mL of water and separated into an organic phase and an aqueous phase by adding excess hydrochloric acid. The organic phase was separated and distilled under reduced pressure to obtain perfluoro-2,4-dimethyl-1,3-dioxolane-2-carboxylic acid. The boiling point of the main distillate was 103-106°C / 100 mmHg. The yield of fluorination was 85%.

[0217] <Synthesis of perfluoro-4-methyl-2-methylene-1,3-dioxolane>

[0218] The above distillate was neutralized with an aqueous potassium hydroxide solution to obtain perfluoro-2,4-dimethyl-2-formyl potassium-1,3-dioxolane. The potassium salt was vacuum dried at 70°C for 1 day. The salt was decomposed at 250°C to 280°C in a nitrogen or argon atmosphere. The product was cooled to -78°C using a cooling trap to obtain perfluoro-4-methyl-2-methylene-1,3-dioxolane in a yield of 82%. The boiling point of the product is 45°C / 760 mmHg. Use 1 The product was identified by 9F NMR and GC-MS.

[0219] 1 9FNMR: -84ppm (3F, CF3), -129ppm (2F, =CF2) GC-MS: m / e244 (Molecular ion) 225, 197, 169, 150, 131, 100, 75, 50.

[0220] <Polymerization of perfluoro-4-methyl-2-methylene-1,3-dioxolane>

[0221] 100 g of perfluoro-4-methyl-2-methylene-1,3-dioxolane and 1 g of perfluorobenzoyl peroxide obtained by the above method were sealed in a glass tube. The glass tube was deoxygenated by freeze degassing, then filled with argon and heated at 50° C. for several hours. The contents became solid, but when further heated at 70° C. overnight, 100 g of a transparent rod-like object was obtained.

[0222] The obtained transparent rod-like substance was dissolved in Fluorinert FC-75 (manufactured by Sumitomo 3M Co.), and the obtained solution was injected into a glass plate to obtain a thin film of the polymer. The obtained polymer had a glass transition temperature of 117 and was completely amorphous. The transparent rod-like substance was dissolved in hexafluorobenzene, and chloroform was added thereto to precipitate it, thereby purifying the product. The glass transition temperature of the purified polymer was about 131°C. This polymer was used as the first fluorine-containing resin.

[0223] [Refractive index adjusting agent]

[0224] As a refractive index adjuster, chlorotrifluoroethylene oligomer (molecular weight 585) was used. Specifically, "DAIFLOIL#10" manufactured by DAIKIN INDUSTRIES was distilled to separate and obtain only a component with a molecular weight of 585. The separated component with a molecular weight of 585 was filtered with a filter "DFA1ANDESW44" (manufactured by PALL) with a pore size of 40 nm to obtain a refractive index adjuster.

[0225] [First core material]

[0226] The first fluorine-containing resin prepared by the above method is dissolved in Vertrel XF-UP (manufactured by Chemours-Mitsui Fluoroproducts) as a solvent. The solution is filtered twice with a filter "LPJ-CTA-001-N3" (manufactured by ROKI TECHNO) with a pore size of 100 nm, and the filtrate is dripped into a container made of Hastelloy heated to 260°C to evaporate the solvent and dry it. The filtered fluorine-containing resin obtained after drying and the above refractive index adjuster are melt-mixed at 260°C to prepare a resin composition. The concentration of the refractive index adjuster in the obtained resin composition is 12% by mass. The resin composition is used as the first core material.

[0227] [Second core material]

[0228] The first fluorine-containing resin prepared by the above method is filtered by the same method as the filtration of the fluorine-containing resin in the preparation of the first core material to obtain a filtered fluorine-containing resin. The filtered fluorine-containing resin is used as the second core material.

[0229] [Trench layer material]

[0230] Prepare a second fluorine-containing resin as a groove layer material. Dissolve "Teflon AF1600" (manufactured by Chemours-Mitsui Fluoroproducts) as the second fluorine-containing resin and "Fomblin YR" (manufactured by Solvay) as a viscosity adjuster in Vertrel XF-UP (manufactured by Chemours-Mitsui Fluoroproducts) as a solvent. It should be noted that the mixing ratio of "Teflon AF1600" and "Fomblin YR" is set to "Teflon AF1600": "Fomblin YR" = 7:3 in terms of mass ratio. Filter the obtained solution with a filter "LPA-SLF-003-N2" (manufactured by ROKITECHNO) with a pore size of 300nm, and add the filtrate dropwise to a Hastelloy container heated to 260°C to evaporate the solvent and dry it. The resin composition obtained after drying is used as a groove layer material.

[0231] [Coating material]

[0232] As the covering layer material, Xylex (manufactured by SABIC, glass transition temperature: 113° C.) was used.

[0233] [Production of POF]

[0234] Using the first core material, the second core material, the trench layer material, and the cladding layer material prepared by the above method, a fiber having the same Figure 3 The POF 20 shown in the figure has the same structure as the POF. In this embodiment, Figure 4 The manufacturing apparatus shown is used for manufacturing POF.

[0235] In this embodiment, the inner diameter (diameter) of the diffusion tube 120 is 6.3 mm. The length of the diffusion tube 120 is set so that the diffusion time becomes 120 minutes.

[0236] In this embodiment, the melting temperature of the first core material is 250°C, the melting temperature of the second core material is 255°C, the melting temperature of the groove layer material is 260°C, and the melting temperature of the cladding layer material is 240°C. In addition, the temperature of the diffusion tube 120 is set to 275°C. The first core material and the second core material form a core. The draw-down temperature of the stacked body 7 composed of the core, the groove layer, and the cladding layer is 240°C.

[0237] The melt extrusion was performed at a volume ratio of 1.04 for the second core material, 0.705 for the trench layer material, and 40.438 for the cladding layer material relative to the first core material 1.

[0238] exist Figure 4 In the first chamber 110 shown in FIG. 1 , the temperature of the confluence die used when the inner layer of the core formed of the first core material is covered with the second core material is set to 260° C. Figure 4 In the second chamber 130 shown, the temperature of the confluence die used when coating the core with the groove layer material is set to 205°C. Figure 4 In the third chamber 140 shown, the temperature of the confluence die used when coating the surface of the stacked body composed of the core and the trench layer with the coating material was set to 250°C.

[0239] Regarding the POF produced in Example 1, the core diameter (outer diameter of the core) measured by the method described later is 50μm, the thickness of the second region of the core is 2.85μm, the outer diameter of the groove layer is 58μm (that is, the thickness of the groove layer is 4μm), and the outer diameter of the coating layer is 230μm.

[0240] (Example 2)

[0241] In the production of POF, the POF of Example 2 was produced in the same manner as Example 1 except that the volume ratio of each material ejected was changed to 1 for the first core material, 1.441 for the second core material, 1.559 for the groove layer material, and 47.660 for the coating layer material.

[0242] Regarding the POF produced in Example 2, the core diameter (outer diameter of the core) measured by the method described later is 50μm, the thickness of the second region of the core is 4.01μm, the outer diameter of the groove layer is 64μm (that is, the thickness of the groove layer is 7μm), and the outer diameter of the coating layer is 230μm.

[0243] (Example 3)

[0244] In the production of POF, the POF of Example 3 was produced in the same manner as Example 1 except that the volume ratio of each material ejected was changed to 1 for the first core material, 1.602 for the second core material, 1.661 for the groove layer material, and 50.785 for the coating layer material.

[0245] Regarding the POF produced in Example 3, the core diameter (outer diameter of the core) measured by the method described later is 50μm, the thickness of the second region of the core is 4.53μm, the outer diameter of the groove layer is 64μm (that is, the thickness of the groove layer is 7μm), and the outer diameter of the coating layer is 230μm.

[0246] (Example 4)

[0247] In the production of POF, the POF of Example 4 was produced in the same manner as Example 1 except that the volume ratio of each material ejected was changed to 1 for the first core material, 1.74 for the second core material, 1.47 for the groove layer material, and 53.787 for the coating layer material.

[0248] Regarding the POF produced in Example 4, the core diameter (outer diameter of the core) measured by the method described later is 50μm, the thickness of the second region of the core is 4.96μm, the outer diameter of the groove layer is 62μm (that is, the thickness of the groove layer is 6μm), and the outer diameter of the coating layer is 230μm.

[0249] (Example 5)

[0250] In the production of POF, the POF of Example 5 was produced in the same manner as Example 1 except that the volume ratio of each material ejected was changed to 1 for the first core material, 1.100 for the second core material, 0.726 for the groove layer material, and 41.618 for the coating layer material.

[0251] Regarding the POF produced in Example 5, the core diameter (outer diameter of the core) measured by the method described later is 50μm, the thickness of the second region of the core is 2.89μm, the outer diameter of the groove layer is 58μm (that is, the thickness of the groove layer is 4μm), and the outer diameter of the coating layer is 230μm.

[0252] (Comparative Example 1)

[0253] FONTEX (manufactured by AGC Corporation) was prepared as the POF of Comparative Example 1. Regarding the POF of Comparative Example 1, the core diameter (outer diameter of the core) measured by the method described later was 55 μm, the thickness of the second region of the core was 0 μm, the outer diameter of the groove layer was 65 μm (that is, the thickness of the groove layer was 5 μm), and the outer diameter of the coating layer was 490 μm.

[0254] (Comparative Example 2)

[0255] In the production of POF, the POF of Comparative Example 2 was produced in the same manner as Example 1 except that the volume ratio of each material ejected was changed to 1 for the first core material, 1.815 for the second core material, 1.513 for the groove layer material, and 55.241 for the coating layer material.

[0256] Regarding the POF produced in Comparative Example 2, the core diameter (outer diameter of the core) measured by the method described later is 50μm, the thickness of the second region of the core is 5.00μm, the outer diameter of the groove layer is 62μm (i.e., the thickness of the groove layer is 6μm), and the outer diameter of the coating layer is 230μm.

[0257] (Comparative Example 3)

[0258] In the production of POF, the POF of Comparative Example 3 was produced in the same manner as Example 1 except that the volume ratio of each material ejected was changed to 1 for the first core material, 1.873 for the second core material, 1.544 for the groove layer material, and 56.370 for the cladding layer material.

[0259] Regarding the POF produced in Comparative Example 3, the core diameter (outer diameter of the core) measured by the method described later is 50 μm, the thickness of the second region of the core is 5.12 μm, the outer diameter of the groove layer is 62 μm (i.e., the thickness of the groove layer is 6 μm), and the outer diameter of the coating layer is 230 μm.

[0260] (Comparative Example 4)

[0261] In the production of POF, the POF of Comparative Example 4 was produced in the same manner as Example 1 except that the volume ratio of each material ejected was changed to 1 for the first core material, 1.973 for the second core material, 1.898 for the groove layer material, and 58.031 for the coating layer material.

[0262] Regarding the POF produced in Comparative Example 4, the core diameter (outer diameter of the core) measured by the method described later is 50 μm, the thickness of the second region of the core is 5.22 μm, the outer diameter of the groove layer is 64 μm (i.e., the thickness of the groove layer is 7 μm), and the outer diameter of the coating layer is 230 μm.

[0263] (Comparative Example 5)

[0264] As the POF of Comparative Example 5, Giga-POF-50SR (manufactured by Chromis) was prepared. Regarding the POF of Comparative Example 5, the core diameter (outer diameter of the core) measured by the method described later was 50 μm, the thickness of the second region of the core was 0 μm, and the outer diameter of the coating layer was 490 μm. It should be noted that the groove layer was not provided in the POF of Comparative Example 5.

[0265] (POF's review)

[0266] [Measurement of the core diameter, the thickness of the second region of the core, and the outer diameter of the trench layer]

[0267] The core diameter, the thickness of the second region of the core, and the outer diameter of the groove layer are obtained by the NFP method using light of a wavelength of 850nm in accordance with the method of IEC60793-1-20 and IEC60793-2-40subcategory A4h. Specifically, the outer edge 11b of the core 11 and the outer edge of the groove layer are determined by using the surface distribution of the POF emitted light intensity, and the core diameter and the outer diameter of the groove layer are obtained. It should be noted that the outer edge 11b of the core 11 is equivalent to the interface between the core 11 and the groove layer 12 (core / groove layer interface). In addition, using the surface distribution of the emitted light intensity of the POF, the surface distribution is differentiated to obtain the inflection point, thereby distinguishing the first region 111 having a refractive index distribution and the second region 112 having a constant refractive index, and determining the outer diameter of the first region 111. The outer edge of the second region 112 is the outer edge 11b of the core 11 (i.e., the core / trench layer interface), so the core / trench layer interface determined by the NFP method is determined as the outer edge of the second region 112. The thickness of the second region 112 is calculated from the outer diameters of the determined regions.

[0268] [Measurement of outer diameter of coating layer]

[0269] The POF was cut into 2 cm pieces and placed so that the axis of the POF was perpendicular to the sample stage of a digital microscope: VHX-950F manufactured by KEYENCE Co., Ltd. The light source attached to the microscope was irradiated to one end of the POF, and the transmitted light emitted from the other end was observed to measure the coating layer of the POF.

[0270] [Measurement of refractive index]

[0271] The refractive index n1 of the first region of the core, the second refractive index n2 of the second region of the core, and the refractive index n3 of the groove layer were measured at room temperature (about 23°C) using a prism coupler (model 2010 / M) manufactured by Metricon. Specifically, the materials of the core and the groove layer were hot stamped at about 210°C to obtain a sheet with a thickness of about 100 μm. Next, the obtained sheet was introduced into a prism coupler (model 2010 / M) manufactured by Metricon to determine the refractive index. In addition, the opening angle was measured by the far-field pattern method to determine the refractive index difference between the core and the groove layer. Finally, referring to 2.4 of the paper (Tachibana Mitsuhiro, "Measurement of Refractive Index Distribution of Optical Fibers", Applied Physics Vol. 48, No. 8), the refractive index n1 of the first region of the core, the refractive index n2 of the second region of the core, and the refractive index n3 of the groove layer 12 were calculated. This method confirmed that the POFs of Examples 1 to 5 satisfied the refractive index relationship of n1≥n2>n3. It should be noted that the POFs of Comparative Examples 2 to 4 also satisfied the refractive index relationship of n1≥n2>n3 by the same method.

[0272] [Evaluation of Frequency Band]

[0273] The frequency bands of 5 m of the POFs of Examples 1 to 5 and Comparative Examples 1 to 5 were measured by the pulse method in the method based on IEC60793-1-41. However, in order to measure the frequency band of a POF over a very short distance of 5 m, as the optical pulse generator, a device capable of generating ultra-high-speed pulses was used, and as the photoreceiver, a device capable of performing image recognition in a short time was used. Specifically, the frequency band was measured by the following method.

[0274] As the optical pulse generator, InSightX3+ manufactured by SpectraPhisics Co., Ltd. was used. Using this optical pulse generator, a laser with a wavelength of 850 nm was generated. The generated laser was combined with an OM1 fiber (manufactured by THORLABS, "M31L01-OM1, 0.275 NA, Graded-Index Patch Cable") through a lens, and mode scrambling (Japanese original: モ一ドスクラソブル) was applied using an FM-1 manufactured by Newport Corporation. The outgoing side was connected to an OM1 fiber with a 2-m band mode filter (test reference code MRC-625-EFC-SCFC manufactured by FLUKE Networks Co., Ltd.), and the POF to be measured was connected to the outgoing side of this OM1 fiber.

[0275] The core diameter of the incident light incident on the POF to be measured was 57.3 μm, and the numerical aperture (N.A.) was 0.26, which were respectively confirmed to be larger than the core diameter and numerical aperture (N.A.) of the POF to be measured. That is, incident overflow light was used to measure the frequency band of the POF.

[0276] As the photoreceiver, a general-purpose streak camera C10910 series manufactured by Hamamatsu Photonics Co., Ltd. was used. The pulse waveform was obtained using this photoreceiver.

[0277] The measurement at a distance of 5 m was carried out by the following method. First, a 7-m long POF was prepared, an optical pulse was incident from one end, and the optical pulse of the outgoing light 7 m ahead was measured. Then, the POF was cut to a length of 2 m, and an optical pulse was similarly incident, and the outgoing pulse was measured. The transfer function was obtained by performing the Fourier transform specified in IEC60793-1-41 on the two outgoing pulses, and the frequency at which the optical power was -1.5 dB was obtained. The results are shown in Table 1. It should be noted that Table 1 shows both the measurement results of the frequency band (unit: GHz) obtained when measuring at a distance of 5 m and the results converted to the unit "MHz·km". In addition, the "frequency band value at 5 m" shown in Table 1 refers to the value of the frequency band obtained through the evaluation of the frequency band.

[0278] [Evaluation of Bending Loss]

[0279] Prepare POF with a length of 5 m. Figure 7 Schematic diagram of a measuring system for measuring the bending loss of POF in the embodiment and the comparative example. In the measuring system 70, FOLS-01 (wavelength 850nm LED) manufactured by Sawaki Kobo Co., Ltd. is connected to the incident side 71a of POF 71 as a light source 72. An optical power meter 8230E manufactured by ADCMT Co., Ltd. is connected to the light receiving side 71b of POF 70 as an optical power meter 73. The 1m portion of the incident side is wound 10 times on a φ12.5mm cylinder to remove the cladding mode, and the central portion (2.5m portion) of the POF is set at Figure 7 The POF was bent by using a plate 74 with a U-shaped groove having a bending radius R as shown in the figure. In this way, the change in insertion loss from the straight state to the bent state was confirmed, and the optical loss was calculated. In this embodiment and the comparative example, the optical loss (first optical loss) when the U-shaped shape was bent with a bending radius R = 1.5 mm and the optical loss (second optical loss) when the U-shaped shape was bent with a bending radius R = 2.0 mm were calculated. The results are shown in Table 1.

[0280] [Evaluation of Numerical Aperture (NA)]

[0281] In the method based on IEC60793-1-43 and IEC60793-2-40 sub-category A4h, the numerical aperture (NA) is measured by the FFP method (Far Field Pattern) using light with a wavelength of 850nm. A POF with a length of 6m is prepared, and 850nm LED light is incident from one end. The light intensity distribution relative to the angular position of the emitted light 6m ahead is measured, and the numerical aperture (NA) is calculated.

[0282]

Table 1

[0283]

[0284] As shown in Table 1, the POF of Examples 1 to 5 having a groove layer and a core having a second region with a thickness of 2 μm or more and less than 5 μm can suppress the bending loss to a small level and achieve a high frequency band of 40 MHz·km or more in a short distance of 5 m. In contrast, in Comparative Example 1 in which a groove layer is provided but a second region is not provided, the frequency band value is low because the frequency band is reduced by light reflected in the groove layer. On the other hand, in Comparative Examples 2 to 4 in which a groove layer is provided but the thickness of the second region is 5 μm or more, the frequency band value is reduced due to reflection of light incident on the second region because the second region is thick, so although the frequency band value is higher than that of Comparative Example 1, the frequency band value is lower than that of the embodiment. The POF of Comparative Example 5 has a high frequency band value because a groove layer is not provided, but the bending loss is large and the numerical aperture (NA) is also small.

[0285] [Note]

[0286] In summary, one embodiment of the present invention is as follows.

[0287] (1) A plastic optical fiber comprising:

[0288] a fiber core; and

[0289] A groove layer is arranged on the outer periphery of the core.

[0290] The above-mentioned fiber core has:

[0291] a first region having a refractive index n1 that decreases in a direction from the center toward the outer edge; and

[0292] a second region, which is located at the periphery of the first region, includes the outer edge of the core, and has a constant refractive index n2,

[0293] The refractive index n2 of the second region is less than the refractive index n1 of the first region,

[0294] The thickness of the second region is greater than or equal to 2 μm and less than 5 μm.

[0295] A refractive index n3 of the trench layer is lower than the refractive index n2 of the second region.

[0296] (2) The plastic optical fiber according to (1) above, wherein the -1.5 dB band value when overflow light is incident at a distance of 5 m is 40 MHz·km or more.

[0297] (3) The plastic optical fiber according to (1) or (2) above, wherein the first optical loss when the plastic optical fiber is bent into a U-shape with a bending radius of 1.5 mm is 3.0 dB or less.

[0298] (4) The plastic optical fiber according to (3) above, wherein the first optical loss is 1.0 dB or less.

[0299] (5) The plastic optical fiber according to any one of (1) to (4) above, wherein the second optical loss when the plastic optical fiber is bent into a U-shape with a bending radius of 2.0 mm is 0.5 dB or less.

[0300] (6) The plastic optical fiber according to any one of (1) to (5) above, wherein the thickness of the second region is not less than 2.9 μm and not more than 4.8 μm.

[0301] (7) The plastic optical fiber according to (6) above, wherein the thickness of the second region is not less than 2.9 μm and not more than 4.5 μm.

[0302] (8) The plastic optical fiber according to (7) above, wherein the thickness of the second region is not less than 3.5 μm and not more than 4.4 μm.

[0303] (9) The plastic optical fiber according to any one of (1) to (8) above, wherein the numerical aperture (NA) of the plastic optical fiber is not less than 0.190 and not more than 0.235.

[0304] (10) An optical cable comprising the plastic optical fiber according to any one of (1) to (9) above.

[0305] (11) An active optical cable comprising the optical cable described in (10) above and an optoelectronic hybrid module.

[0306] Industrial Applicability

[0307] The POF of the present disclosure can suppress bending loss to a small level and can realize a high frequency band within a short distance. Therefore, the POF of the present disclosure is suitable for use in short-distance signal transmission such as within a home.

Claims

1. A plastic optical fiber, comprising: a fiber core; and a groove layer disposed on the outer periphery of the core, The fiber core has: a first region having a refractive index n1 that decreases in a direction from the center toward the outer edge; and a second region, which is located at the periphery of the first region, includes the outer edge of the core, and has a constant refractive index n2, The refractive index n2 of the second region is less than the refractive index n1 of the first region, The thickness of the second region is greater than or equal to 2 μm and less than 5 μm, A refractive index n3 of the trench layer is lower than the refractive index n2 of the second region. 2 . The plastic optical fiber according to claim 1 , wherein the −1.5 dB band value when overflow light is incident on the plastic optical fiber at a distance of 5 m is 40 MHz·km or more.

3. The plastic optical fiber according to claim 1, wherein: When the plastic optical fiber is bent into a U-shape with a bending radius of 1.5 mm, the first optical loss is 3.0 dB or less.

4. The plastic optical fiber according to claim 3, wherein: The first optical loss is less than 1.0 dB.

5. The plastic optical fiber according to claim 1, wherein: When the plastic optical fiber is bent into a U-shape with a bending radius of 2.0 mm, the second optical loss is 0.5 dB or less.

6. The plastic optical fiber according to claim 1, wherein: The thickness of the second region is greater than or equal to 2.9 μm and less than or equal to 4.8 μm.

7. The plastic optical fiber according to claim 6, wherein: The thickness of the second region is greater than or equal to 2.9 μm and less than or equal to 4.5 μm.

8. The plastic optical fiber according to claim 7, wherein: The thickness of the second region is greater than or equal to 3.5 μm and less than or equal to 4.4 μm.

9. The plastic optical fiber according to claim 1, wherein: The plastic optical fiber has a numerical aperture (NA) of 0.190 or more and 0.235 or less. 10 . An optical cable comprising the plastic optical fiber according to claim 1 .

11. An active optical cable comprising the optical cable according to claim 10 and an optoelectronic hybrid module.