Semiconductor device, display device, and method for manufacturing semiconductor device
By optimizing the design of the overlapping area of the metal oxide layer and the oxide semiconductor layer, combined with the etching process and heat treatment, the problem of reduced freedom in channel length design of the oxide semiconductor thin film transistor during size miniaturization is solved, and the electrical characteristics and Threshold voltage stability enables higher field-effect mobility.
Patent Information
- Application Number
- CN202410305656.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-18
- Publication Date
- 2024-10-01
AI Technical Summary
When the size of existing oxide semiconductor thin film transistors is miniaturized, the degree of freedom in channel length design is reduced, resulting in an increase in threshold voltage shift or deviation, which limits the use of the device.
Using a structural design including a metal oxide layer, an oxide semiconductor layer, a gate insulation layer and a gate wiring, through the optimization of the overlapping and non-overlapping areas of the metal oxide layer and the oxide semiconductor layer, combined with the etching process and heat treatment , control channel length and electrical characteristics.
The electrical characteristics of the oxide semiconductor device are improved, the offset and deviation of the threshold voltage are reduced, the size miniaturization capability and electrical stability of the device are enhanced, and a higher field effect mobility is achieved.
Smart Images

Figure CN118738136A_ABST
Abstract
Description
Technical Field
[0001] One embodiment of the present invention relates to a semiconductor device including an oxide semiconductor, a method for manufacturing the same, and a display device using the semiconductor device including an oxide semiconductor. Background Art
[0002] In recent years, oxide semiconductors have attracted attention as materials for semiconductor devices, replacing amorphous silicon, polycrystalline silicon, and single crystal silicon. In particular, as a semiconductor device including an oxide semiconductor, the development of thin film transistors using oxide semiconductors as channels has been continuously advancing (for example, Patent Documents 1 to 6). Thin film transistors using oxide semiconductors as channels can be formed by simple structures and low-temperature processes in the same way as semiconductor devices using amorphous silicon as channels. It is known that thin film transistors using oxide semiconductors as channels have higher field effect mobility than thin film transistors using amorphous silicon as channels.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2021-141338
[0006] Patent Document 2: Japanese Patent Application Publication No. 2014-099601
[0007] Patent Document 3: Japanese Patent Application Publication No. 2021-153196
[0008] Patent Document 4: Japanese Patent Application Publication No. 2018-006730
[0009] Patent Document 5: Japanese Patent Application Publication No. 2016-184771
[0010] Patent Document 6: Japanese Patent Application Publication No. 2021-108405 Summary of the invention
[0011] Problems to be solved by the invention
[0012] However, in the case of existing thin film transistors including oxide semiconductors, if the channel length is reduced, the threshold voltage representing the switching characteristics may shift in the negative direction, or the deviation of the threshold voltage may increase. Therefore, in the case of existing thin film transistors including oxide semiconductors, when the size is miniaturized, the design freedom of the channel length is reduced and the use is limited.
[0013] One of the objects of the present invention is to improve the electrical characteristics of a semiconductor device including an oxide semiconductor.
[0014] Means for solving problems
[0015] A semiconductor device according to one embodiment of the present invention includes: a metal oxide layer on an insulating surface; an oxide semiconductor layer on the metal oxide layer; a gate insulating layer on the oxide semiconductor layer; and a gate wiring on the gate insulating layer, wherein the metal oxide layer has a first region overlapping with the gate wiring and the oxide semiconductor layer, a second region overlapping with the oxide semiconductor layer and not overlapping with the gate wiring, and a third region overlapping with the gate wiring and not overlapping with the oxide semiconductor layer.
[0016] A method for manufacturing a semiconductor device involved in one embodiment of the present invention includes: forming a first metal oxide layer on an insulating surface; forming an oxide semiconductor layer having a pattern shape on the first metal oxide layer; forming a gate insulating layer on the oxide semiconductor layer; forming a gate wiring on the gate insulating layer; etching the gate insulating layer using the gate wiring as a mask; and etching the first metal oxide layer using the gate wiring and the oxide semiconductor layer as masks. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 It is a schematic cross-sectional view showing the structure of a semiconductor device in one embodiment of the present invention.
[0018] Figure 2 It is a schematic cross-sectional view showing the structure of a semiconductor device in one embodiment of the present invention.
[0019] Figure 3A It is a schematic plan view showing the structure of a semiconductor device in one embodiment of the present invention.
[0020] Figure 3B It is a schematic plan view showing the structure of a metal oxide layer in a semiconductor device according to one embodiment of the present invention.
[0021] Figure 4 It is a flowchart showing a method for manufacturing a semiconductor device in one embodiment of the present invention.
[0022] Figure 5 It is a cross-sectional view showing a method for manufacturing a semiconductor device in one embodiment of the present invention.
[0023] Figure 6 It is a cross-sectional view showing a method for manufacturing a semiconductor device in one embodiment of the present invention.
[0024] Figure 7 It is a cross-sectional view showing a method for manufacturing a semiconductor device in one embodiment of the present invention.
[0025] Figure 8 It is a cross-sectional view showing a method for manufacturing a semiconductor device in one embodiment of the present invention.
[0026] Fig. 9 It is a cross-sectional view showing a method for manufacturing a semiconductor device in one embodiment of the present invention.
[0027] Fig.10 It is a cross-sectional view showing a method for manufacturing a semiconductor device in one embodiment of the present invention.
[0028] Fig.11 It is a cross-sectional view showing a method for manufacturing a semiconductor device in one embodiment of the present invention.
[0029] Fig.12 It is a cross-sectional view showing a method for manufacturing a semiconductor device in one embodiment of the present invention.
[0030] Fig.13 It is a cross-sectional view showing a method for manufacturing a semiconductor device in one embodiment of the present invention.
[0031] Fig.14 It is a flowchart showing a method for manufacturing a semiconductor device in one embodiment of the present invention.
[0032] Fig.15 It is a plan view schematically showing a display device in one embodiment of the present invention.
[0033] Fig.16 This is a block diagram showing a circuit configuration of a display device in one embodiment of the present invention.
[0034] Fig.17 : is a circuit diagram showing a pixel circuit of a display device according to an embodiment of the present invention.
[0035] Fig.18 It is a cross-sectional view schematically showing a display device according to an embodiment of the present invention.
[0036] Fig.19 It is a plan view of a pixel electrode and a common electrode of a display device in one embodiment of the present invention.
[0037] Fig. 20 : is a circuit diagram showing a pixel circuit of a display device in one embodiment of the present invention.
[0038] Fig.21 It is a cross-sectional view schematically showing a display device in one embodiment of the present invention.
[0039] Fig.22A It is a diagram showing the electrical characteristics of the semiconductor device in one embodiment of the present invention.
[0040] Fig. 22B It is a graph showing the electrical characteristics of a semiconductor device in a comparative example.
[0041] Fig.23 This is a diagram illustrating the relationship between the channel resistance (R) of a transistor and the designed channel length (channel length on layout) (Lg) for different gate voltages (Vg).
[0042] Fig.24A This is a diagram showing the dependency of the threshold voltage on the channel length in the semiconductor device according to one embodiment of the present invention.
[0043] Fig. 24B This is a diagram showing the dependency of the threshold voltage on the channel length in a semiconductor device of a comparative example.
[0044] Description of Reference Numerals
[0045] 10, 10a…semiconductor device, 11…driving transistor, 12…selecting transistor, 20, 20a…display device, 22…liquid crystal region, 24…sealing region, 26…terminal region, 100…substrate, 105…conductive layer, 110…insulating layer, 120…insulating layer, 130…metal oxide layer, 140…oxide semiconductor layer, 141…upper surface, 142…lower surface, 143…side surface, 150…gate insulating layer, 160…gate wiring, 170…insulating layer, 171, 173…opening, 180…insulating layer, 190…metal oxide layer, 200…source / drain electrode, 201…source electrode, 203…drain electrode, 210…holding capacitor, 211…signal line, 212…gate line, 213…anode power line, 214…cathode power line, 300…array substrate, 301, 301a…pixel circuit, 302…source driver circuit, 303…gate driver circuit, 304…source wiring, 305…gate wiring, 306…terminal portion, 307, 308…connection wiring, 310…sealing portion, 311…liquid crystal element, 320…opposing substrate, 330…flexible printed circuit substrate, 340…chip, 350…holding capacitor, 360…insulating layer, 362…insulating layer, 363…opening, 370…common electrode, 380…insulating layer, 381…opening, 390…pixel electrode, 392…light-emitting layer, 394…common electrode DETAILED DESCRIPTION
[0046] Hereinafter, various embodiments of the present invention will be described with reference to the accompanying drawings. The following disclosure is only an example. The configuration that can be easily conceived by those skilled in the art by appropriately changing the configuration of the embodiment while maintaining the gist of the invention is of course included in the scope of the present invention. With respect to the accompanying drawings, in order to make the description clearer, the width, thickness, shape, etc. of each part are sometimes schematically indicated compared to the actual method. However, the shape shown in the figure is only an example and does not limit the interpretation of the present invention. In this specification and each figure, the same figure mark is marked for the same elements as those described in the accompanying drawings that have appeared, and the detailed description is sometimes appropriately omitted.
[0047] In each embodiment of the present invention, the direction from the substrate toward the oxide semiconductor layer is referred to as up or above. Conversely, the direction from the oxide semiconductor layer toward the substrate is referred to as down or below. Thus, for ease of explanation, the above or below phrases are used for explanation, but, for example, the up-and-down relationship between the substrate and the oxide semiconductor layer may be configured in a manner opposite to that shown in the figure. In the following description, for example, the expression "oxide semiconductor layer on the substrate" is only used to illustrate the up-and-down relationship between the substrate and the oxide semiconductor layer as described above, and other components may also be configured between the substrate and the oxide semiconductor layer. Above or below means the stacking order in a structure having multiple layers stacked. In the case of the expression "the pixel electrode above the transistor", it may also be a positional relationship in which the transistor and the pixel electrode do not overlap when viewed from above. On the other hand, in the case of the expression "the pixel electrode vertically above the transistor", it means a positional relationship in which the transistor and the pixel electrode overlap when viewed from above.
[0048] A “display device” refers to a structure that uses an electro-optical layer to display an image. For example, a term such as a display device sometimes refers to a display panel that includes an electro-optical layer, or sometimes refers to a structure in which a display unit is equipped with other optical components (such as a polarization component, a backlight source, a touch panel, etc.). As long as no technical contradiction arises, the “electro-optical layer” can include a liquid crystal layer, an electroluminescent (EL) layer, an electrochromic (EC) layer, and an electrophoretic layer. Therefore, with respect to the embodiments described later, as display devices, a liquid crystal display device including a liquid crystal layer and an organic EL display device including an organic EL layer are exemplified for explanation, and the structure in this embodiment can be applied to a display device including the above-mentioned other electro-optical layers.
[0049] In this specification, unless otherwise specified, expressions such as “α includes A, B, or C”, “α includes any one of A, B, and C”, and “α includes one selected from the group consisting of A, B, and C” do not exclude the case where α includes a combination of multiple elements of A to C. In addition, the above expressions do not exclude the case where α includes other elements.
[0050] In this specification, "same" includes not only completely identical cases but also substantially identical cases. "Substantially identical" means that although not completely identical, they are within the range of slight differences that can be regarded as identical. For example, "substantially identical" means that the difference between two values is within the range of ±5% (preferably ±3%) error.
[0051] <First Embodiment>
[0052] use Figures 1 to 13 , a semiconductor device according to an embodiment of the present invention is described by taking a thin film transistor as an example. The semiconductor device according to the embodiment described below may be a thin film transistor used in a display device or may be a thin film transistor used in an integrated circuit (IC) such as a microprocessor (Micro-Processing Unit: MPU) or a memory circuit.
[0053] [Structure of semiconductor device]
[0054] The configuration of a semiconductor device 10 according to one embodiment of the present invention will be described. Figure 1 and Figure 2 It is a schematic cross-sectional view showing the structure of a semiconductor device 10 according to one embodiment of the present invention. Figure 3A It is a schematic plan view showing the structure of a semiconductor device 10 according to one embodiment of the present invention. Figure 3B It is a schematic plan view showing the structure of the metal oxide layer 130 in the semiconductor device 10 according to one embodiment of the present invention. Figure 1 Along with Figure 3A It corresponds to the cross-sectional view taken along the dashed line AA' shown in FIG. Figure 2 Along with Figure 3A It corresponds to the cross-sectional view taken along the dashed line BB' shown in FIG.
[0055] like Figure 1 and Figure 2 As shown, the semiconductor device 10 is disposed over a substrate 100. The semiconductor device 10 includes a conductive layer 105, insulating layers 110 and 120, a metal oxide layer 130, an oxide semiconductor layer 140, a gate insulating layer 150, a gate wiring 160, insulating layers 170 and 180, a source electrode 201, and a drain electrode 203.
[0056] The gate wiring includes a gate electrode. Specifically, a portion of the gate wiring that functions as a gate of the semiconductor device 10 is sometimes referred to as a gate electrode. When the source electrode 201 and the drain electrode 203 are not particularly distinguished, they are sometimes collectively referred to as a source / drain electrode 200 .
[0057] exist Figure 3A , the first direction is a direction connecting the source electrode 201 and the drain electrode 203, and corresponds to the direction in which carriers move. The length of the channel region CH in the oxide semiconductor layer 140 in the first direction (D1 direction) is the channel length (L), and the width of the channel region CH in the second direction (D2 direction) is the channel width (W).
[0058] The conductive layer 105 is provided on the substrate 100. The conductive layer 105 has a function as a light shielding film with respect to the oxide semiconductor layer 140. Figure 1 and Figure 3A As shown, in the first direction (direction D1), the width of the conductive layer 105 is larger than the width of the gate wiring 160. The reason for adopting such a structure is to effectively prevent the intrusion of external light into the channel region CH.
[0059] The insulating layers 110 and 120 are provided over the substrate 100 and the conductive layer 105. The insulating layer 110 has a function as a barrier film for blocking impurities diffusing from the substrate 100 toward the oxide semiconductor layer 140.
[0060] The metal oxide layer 130 is provided on the insulating layer 120. The metal oxide layer 130 is in contact with the insulating layer 120. The metal oxide layer 130 is a layer containing an oxide metal having aluminum as a main component, and has a function as a gas barrier film that blocks gases such as oxygen and hydrogen.
[0061] The oxide semiconductor layer 140 is provided on the metal oxide layer 130. The oxide semiconductor layer 140 is in contact with the metal oxide layer 130. The surface of the main surface of the oxide semiconductor layer 140 that is in contact with the metal oxide layer 130 is referred to as the lower surface 142. In this embodiment, a configuration in which the metal oxide layer 130 is in contact with the insulating layer 120 and the oxide semiconductor layer 140 is in contact with the metal oxide layer 130 is exemplified, but the present invention is not limited to this configuration. Other layers may also be provided between the metal oxide layer 130 and the oxide semiconductor layer 140. The oxide semiconductor layer 140 is patterned. For example, the oxide semiconductor layer 140 has an island-shaped pattern shape.
[0062] like Figure 1 As shown in FIG. 1 , in the first direction (direction D1), the ends of the metal oxide layer 130 and the oxide semiconductor layer 140 are substantially aligned. Figure 1In the embodiment, the side surface of the metal oxide layer 130 and the side surface of the oxide semiconductor layer 140 are arranged substantially in a straight line, but the present invention is not limited to this configuration. The angle of the side surface of the metal oxide layer 130 relative to the main surface of the substrate 100 may be different from the angle of the side surface 143 of the oxide semiconductor layer 140 relative to the main surface of the substrate 100. The cross-sectional shape of the side surface of at least one of the metal oxide layer 130 and the oxide semiconductor layer 140 may be curved. Figure 2 As shown, in the second direction (direction D2), the end of the metal oxide layer 130 is not consistent with the end of the oxide semiconductor layer 140. On the other hand, in the second direction, the end of the metal oxide layer 130 is roughly consistent with the ends of the gate insulating layer 150 and the gate wiring 160. The more specific structure of the metal oxide layer 130 will be described later.
[0063] The gate insulating layer 150 is provided on the oxide semiconductor layer 140. The gate insulating layer 150 is patterned into the same shape as the gate wiring 160. That is, the gate insulating layer 150 has the same pattern shape as the gate wiring 160. Therefore, a portion of the oxide semiconductor layer 140 (a region that does not overlap with the gate wiring 160) is not covered by the gate insulating layer 150. In other words, a portion of the oxide semiconductor layer 140 is exposed from the gate insulating layer 150. The gate insulating layer 150 has a function as a gate insulating layer relative to the top gate (gate wiring 160). The gate insulating layer 150 has a function of releasing oxygen by heat treatment in the manufacturing process.
[0064] The gate wiring 160 is opposite to the oxide semiconductor layer 140 via the gate insulating layer 150. The portion of the gate wiring 160 that is opposite to the oxide semiconductor layer 140 via the gate insulating layer 150 functions as a gate electrode. The gate insulating layer 150 is provided between the oxide semiconductor layer 140 and the gate wiring 160. The gate insulating layer 150 is in contact with the oxide semiconductor layer 140. The surface in contact with the gate insulating layer 150 among the main surfaces of the oxide semiconductor layer 140 is referred to as an upper surface 141. The surface between the upper surface 141 and the lower surface 142 is referred to as a side surface 143. The gate wiring 160 has the function of serving as a top gate of the semiconductor device 10 and a light shielding film relative to the oxide semiconductor layer 140.
[0065] The insulating layers 170 and 180 are provided on the gate insulating layer 150 and the gate wiring 160. In this embodiment, the stacked structure composed of the insulating layers 170 and 180 is sometimes referred to as a passivation layer. The insulating layers 170 and 180 insulate the gate wiring 160 from the source / drain electrode 200. By providing the insulating layers 170 and 180, the parasitic capacitance between the gate wiring 160 and the source / drain electrode 200 can be reduced.
[0066] In this embodiment, a silicon oxide layer is used as the insulating layer 170, and a silicon nitride layer is used as the insulating layer 180. The materials constituting the insulating layers 170 and 180 are not limited to this example, but as described later, it is desirable to have at least one insulating layer containing hydrogen. Figure 1 As shown, the insulating layer 170 constituting a part of the passivation layer is in contact with the gate wiring 160, the gate insulating layer 150 (specifically, the side surface of the gate insulating layer 150), and the oxide semiconductor layer 140. In addition, the insulating layers 170 and 180 are provided with openings 171 and 173 reaching the oxide semiconductor layer 140.
[0067] The source electrode 201 is provided inside the opening 171 provided in the insulating layers 170 and 180. The source electrode 201 is in contact with the oxide semiconductor layer 140 at the bottom of the opening 171. The drain electrode 203 is provided inside the opening 173 provided in the insulating layers 170 and 180. The drain electrode 203 is in contact with the oxide semiconductor layer 140 at the bottom of the opening 173.
[0068] exist Figure 3A , a configuration in which the source / drain electrode 200 does not overlap with the conductive layer 105 and the gate wiring 160 in a plan view is illustrated, but the present invention is not limited to this configuration. For example, the source / drain electrode 200 may overlap with at least one of the conductive layer 105 and the gate wiring 160 in a plan view. The above configuration is merely one embodiment, and the present invention is not limited to the above configuration.
[0069] The operation of the semiconductor device 10 is mainly controlled by the gate voltage supplied to the gate wiring 160. An auxiliary voltage may also be supplied to the conductive layer 105. That is, the conductive layer 105 may also function as a gate electrode by being supplied with an auxiliary voltage. However, this example is not limited thereto, and the conductive layer 105 may also be used as a simple light shielding film. In the case where the conductive layer 105 is used simply as a light shielding film, the conductive layer 105 may be set to a floating state without supplying a specific voltage.
[0070] In this embodiment, as the semiconductor device 10, a top-gate transistor in which a gate wiring 160 (i.e., a gate electrode) is provided above the oxide semiconductor layer 140 is exemplified, but the present invention is not limited to this configuration. For example, as the semiconductor device 10, a dual-gate transistor in which the conductive layer 105 is used as a gate electrode in addition to the gate wiring 160 may also be used. When the conductive layer 105 is used as a gate electrode, the insulating layers 110 and 120 function as gate insulating layers. However, the above configuration is only one embodiment, and the present invention is not limited to the above configuration.
[0071] [Material of each layer of semiconductor device]
[0072] The substrate 100 can support each layer constituting the semiconductor device 10. As the substrate 100, for example, a glass substrate, a quartz substrate, a sapphire substrate or other light-transmitting rigid substrate can be used. In addition, as the substrate, a silicon substrate or other non-light-transmitting rigid substrate can be used. In addition, as the substrate, a polyimide resin substrate, an acrylic resin substrate, a siloxane resin substrate or a fluororesin substrate or other light-transmitting flexible substrate can be used. In order to improve the heat resistance of the substrate 100, impurities can also be introduced into the above-mentioned resin substrate. A substrate having a silicon oxide film or a silicon nitride film formed on the above-mentioned rigid substrate or flexible substrate can also be used as the substrate 100.
[0073] The conductive layer 105 can reflect or absorb external light. As described above, the conductive layer 105 has an area larger than the channel region CH of the oxide semiconductor layer 140, and therefore can block external light incident on the channel region CH. As the conductive layer 105, for example, aluminum (Al), copper (Cu), titanium (Ti), molybdenum (Mo) or tungsten (W), or their alloys or compounds can be used. When conductivity is not required, a resin layer composed of a black resin or the like can be used instead of the conductive layer 105. The conductive layer 105 can be a single-layer structure or a stacked structure.
[0074] The insulating layers 110, 120, 170, and 180 have a function of preventing impurities from diffusing into the oxide semiconductor layer 140. The insulating layers 110, 120, 170, and 180 may have a single-layer structure or a stacked structure. As the insulating layers 110, 120, 170, and 180, for example, silicon oxide (SiOx), silicon oxynitride (SiOxNy), silicon nitride (SiNx), silicon nitride oxide (SiNxOy), aluminum oxide (AlOx), aluminum oxynitride (AlOxNy), aluminum nitride oxide (AlNxOy), aluminum nitride (AlNx), etc. may be used. Here, silicon oxynitride (SiOxNy) and aluminum oxynitride (AlOxNy) are silicon compounds and aluminum compounds, respectively, containing nitrogen (N) at a ratio (x>y) less than oxygen (O). Silicon nitride oxide (SiNxOy) and aluminum nitride oxide (AlNxOy) are silicon compounds and aluminum compounds containing oxygen at a ratio (x>y) less than nitrogen. In this embodiment, silicon nitride (SiNx) is used as the insulating layers 110 and 180, and silicon oxide (SiOx) is used as the insulating layers 120 and 170.
[0075] As the metal oxide layer 130, an oxide metal containing aluminum as a main component is used. For example, as the metal oxide layer 130, aluminum oxide (AlOx), aluminum oxynitride (AlOxNy), aluminum nitride oxide (AlNxOy), aluminum nitride ... x) or the like. “A metal oxide layer having aluminum as a main component” means that the ratio of aluminum contained in the metal oxide layer 130 is greater than 1% of the entire metal oxide layer 130. The ratio of aluminum contained in the metal oxide layer 130 may also be greater than 5% and less than 70%, greater than 10% and less than 60%, or greater than 30% and less than 50% of the entire metal oxide layer 130. The above ratio may be a mass ratio or a weight ratio.
[0076] In this embodiment, the oxide semiconductor layer 140 has a polycrystalline structure. That is, the oxide semiconductor layer 140 of this embodiment is composed of an oxide semiconductor formed using Poly-OS technology. Poly-OS technology refers to a technology for forming an oxide semiconductor layer having a polycrystalline structure. As the oxide semiconductor layer 140, a metal oxide having semiconductor properties can be used. For example, as the oxide semiconductor layer 140, an oxide semiconductor containing two or more metals including indium (In) is used. The ratio of indium to the overall oxide semiconductor layer 140 is 50% or more. As the oxide semiconductor layer 140, in addition to indium, gallium (Ga), zinc (Zn), aluminum (Al), hafnium (Hf), yttrium (Y), zirconium oxide (Zr), and lanthanide elements are used. As the oxide semiconductor layer 140, other elements other than the above may also be used.
[0077] In the oxide semiconductor layer 140 of this embodiment, since the ratio of indium is 50% or more, oxygen deficiency is easily formed. On the other hand, it is difficult for a crystalline oxide semiconductor to form oxygen deficiency compared with an amorphous oxide semiconductor. Therefore, the oxide semiconductor layer 140 has an advantage that it is difficult to form oxygen deficiency even if the ratio of indium is 50% or more.
[0078] The gate insulating layer 150 includes an insulating oxide. Specifically, as the gate insulating layer 150, silicon oxide (SiOx), silicon oxynitride (SiOxNy), aluminum oxide (AlOx), aluminum oxynitride (AlOxNy), etc. can be used. The gate insulating layer 150 preferably has a composition close to a stoichiometric ratio. In addition, the gate insulating layer 150 preferably has few defects. For example, as the gate insulating layer 150, an oxide in which no defects are observed when evaluated by electron spin resonance (ESR) can also be used.
[0079] The gate wiring 160, the source electrode 201, and the drain electrode 203 are conductive. For example, copper (Cu), aluminum (Al), titanium (Ti), chromium (Cr), cobalt (Co), nickel (Ni), molybdenum (Mo), hafnium (Hf), tantalum (Ta), tungsten (W), or bismuth (Bi), or alloys or compounds thereof can be used as the gate wiring 160, the source electrode 201, and the drain electrode 203. The gate wiring 160, the source electrode 201, and the drain electrode 203 can each have a single-layer structure or a stacked structure.
[0080] (Composition of Metal Oxide Layer)
[0081] exist Figure 1 and Figure 3A In the embodiment, the metal oxide layer 130 is in contact with the entire lower surface 142 of the oxide semiconductor layer 140. In other words, when viewed from above, the metal oxide layer 130 overlaps the entire oxide semiconductor layer 140. However, the present invention is not limited to this example, and the metal oxide layer 130 may not be in contact with the entire or a portion of the lower surface 142 of the oxide semiconductor layer 140. For example, the metal oxide layer 130 may be in contact with the channel region CH and not in contact with the source region S and the drain region D. Conversely, the metal oxide layer 130 may be in contact with the source region S and the drain region D and not in contact with the channel region CH.
[0082] exist Figure 2 and Figure 3A In the embodiment, the metal oxide layer 130 overlaps with the gate insulating layer 150 and the gate wiring 160. Specifically, the end of the metal oxide layer 130, the end of the gate insulating layer 150 and the end of the gate wiring 160 are substantially consistent with each other. In other words, when viewed from above, the metal oxide layer 130 and the gate wiring 160 overlap as a whole.
[0083] As described later, the method for manufacturing the semiconductor device 10 of the present embodiment includes a process of etching the metal oxide layer 130 using the gate wiring 160 and the oxide semiconductor layer 140 as masks. Therefore, the metal oxide layer 130 is patterned in a self-aligned manner using the gate wiring 160 and the oxide semiconductor layer 140 as masks. As a result, the metal oxide layer 130 has a pattern shape that is the same as the union of the pattern shape of the gate wiring 160 and the pattern shape of the oxide semiconductor layer 140. The union of the pattern shape of the gate wiring 160 and the pattern shape of the oxide semiconductor layer 140 is as follows: Figure 3B The pattern 130 a derived from the pattern shape of the gate wiring 160 and the pattern 130 b derived from the pattern shape of the oxide semiconductor layer 140 are integrated into one another.
[0084] according to Figure 1 , Figure 2, Figure 3A and Figure 3B It is clear that the metal oxide layer 130 has a first region overlapping with the gate wiring 160 and the oxide semiconductor layer 140, a second region overlapping with the oxide semiconductor layer 140 and not overlapping with the gate wiring 160, and a third region overlapping with the gate wiring 160 and not overlapping with the oxide semiconductor layer 140. Figure 1 and Figure 3A In the embodiment, the first region corresponds to a region connected to the channel region CH and two overlapping regions OL described later. Figure 1 and Figure 3A In the embodiment, the second region corresponds to the region connected to the region obtained by removing the overlapping region OL close to the source region S from the source region S and the region obtained by removing the overlapping region OL close to the drain region D from the drain region D. The third region is Figure 2 The region corresponds to a region overlapping with the gate wiring 160 and not overlapping with the oxide semiconductor layer 140 .
[0085] like Figure 1 As shown in FIG. 1 , the insulating layer 170 is in contact with the side surface of the second region in the metal oxide layer 130. Figure 2 As shown, the insulating layer 170 is connected to the side of the third region in the metal oxide layer 130. Figure 1 and Figure 2 It is clear that the insulating layer 170 is not in contact with the first region of the metal oxide layer 130 .
[0086] (Configuration of Oxide Semiconductor Layer)
[0087] The oxide semiconductor layer 140 is divided into a source region S, a drain region D, and a channel region CH. The channel region CH is a region of the oxide semiconductor layer 140 that is located vertically below the gate wiring 160 and in contact with the gate insulating layer 150. The source region S is a region of the oxide semiconductor layer 140 that is in contact with the insulating layer 170 and is closer to the source electrode 201 than the channel region CH. The drain region D is a region of the oxide semiconductor layer 140 that is in contact with the insulating layer 170 and is closer to the drain electrode 203 than the channel region CH. The source region S and the drain region D are formed by reducing the resistance of a portion of the pattern formed by the oxide semiconductor layer. That is, in Figure 3A In the first direction (direction D1 ) shown, the channel region CH, the source region S, and the drain region D are continuous with each other.
[0088] The oxide semiconductor layer 140 in the channel region CH has physical properties as a semiconductor. The oxide semiconductor layer 140 in the source region S and the drain region D has physical properties as a conductor. That is, the source region S and the drain region D can also be said to be regions with lower resistance than the channel region CH. In other words, the conductivity of the source region S and the drain region D is greater than the conductivity of the channel region CH. The source electrode 201 and the drain electrode 203 are respectively connected to the source region S and the drain region D and are electrically connected to the oxide semiconductor layer 140. The oxide semiconductor layer 140 can be a single-layer structure or a stacked structure.
[0089] like Figure 1 As shown, in the semiconductor device 10 of the present embodiment, a portion of the source region S and the drain region D overlap with the gate wiring 160. Specifically, the end of the source region S on the side close to the channel region CH and the end of the drain region D on the side close to the channel region CH overlap with the gate wiring 160. In other words, the end of the source region S on the side close to the channel region CH and the end of the drain region D on the side close to the channel region CH are respectively connected to the gate insulating layer 150. That is, the source region S and the drain region D are connected to both the gate insulating layer 150 and the insulating layer 170. Here, the area where the source region S (or the drain region D) overlaps with the gate wiring 160 is referred to as the "overlapping area OL". As shown Figure 1 As shown, the width of the overlapping area OL in the first direction is represented by ΔL / 2.
[0090] The semiconductor device 10 of the present embodiment has a symmetrical structure in the first direction (D1 direction), and is a structure in which both the source region S and the drain region D intrude below the gate wiring 160. Therefore, the end of the channel region CH in the first direction does not coincide with the end of the gate wiring 160. Specifically, the end of the channel region CH connected to the source region S and the end of the channel region CH connected to the drain region D are respectively located directly below the gate wiring 160. That is, in the first direction, the width of the channel region CH is narrower than the width of the gate wiring 160. This means that the designed channel length (hereinafter referred to as the "designed channel length") is narrower than the designed value by the amount of the overlapping region OL.
[0091] Generally, the designed channel length in a top-gate transistor is determined by the width of the gate electrode overlapping the semiconductor layer. That is, in the case of the semiconductor device 10 of this embodiment, the width of the gate wiring 160 in the first direction is equivalent to the designed channel length. Figure 1As shown in FIG. 1 , the width of the channel region CH is narrower than the width of the gate wiring 160. That is, the effective channel length corresponding to the width of the channel region CH (hereinafter referred to as “effective channel length”) is shorter than the designed channel length corresponding to the width of the gate wiring 160. Specifically, the difference between the designed channel length (Lg) and the effective channel length (L eff ), L eff =Lg-ΔL, such a relationship holds true.
[0092] In the present embodiment, when forming the source region S and the drain region D, the diffusion of hydrogen from the insulating layers 170 and 180 to the oxide semiconductor layer 140 is utilized. In this case, since hydrogen also diffuses into the oxide semiconductor layer 140 directly below the gate wiring 160 in terms of structure, an overlapping region OL is formed. The overlapping region OL is a region formed by the intrusion of hydrogen into the oxide semiconductor layer 140 directly below the gate wiring 160. However, in the present embodiment, by reducing the amount of hydrogen diffused directly below the gate wiring 160, the range of the overlapping region OL can be suppressed. Specifically, the semiconductor device 10 of the present embodiment is controlled so that the width (ΔL / 2) of the overlapping region OL is less than 1 μm.
[0093] The width of the overlap region OL being 1 μm or less means that, for example, even if the designed channel length is 4 μm, an effective channel length of at least 2 μm can be ensured. According to the present embodiment, the designed channel length (the width of the gate wiring in the first direction) of the semiconductor device 10 can be set to 4 μm or less (preferably 3 μm or less). However, in order to ensure an effective channel length of at least 1 μm, the designed channel length of the semiconductor device 10 is preferably 1 μm or more greater than twice the width of the overlap region OL (2×ΔL / 2=ΔL).
[0094] As described above, in the semiconductor device 10 of the present embodiment, since the gate insulating layer 150 has the same pattern shape as the gate wiring 160, a portion of the oxide semiconductor layer 140 is in contact with the insulating layer 170. Therefore, the semiconductor device 10 has a structure in which a portion of the source region S and the drain region D extend below the gate wiring 160 under the influence of hydrogen diffused from the insulating layers 170 and 180. However, according to the present embodiment, since the width of the overlapping region OL where the source region S and the drain region D overlap with the gate wiring 160 can be suppressed to 1 μm or less, the deviation between the designed channel length and the effective channel length can be suppressed.
[0095] [Method for manufacturing semiconductor device]
[0096] use Figures 4 to 13 A method for manufacturing the semiconductor device 10 according to one embodiment of the present invention will be described. Figure 4It is a sequence diagram showing a method for manufacturing the semiconductor device 10 according to one embodiment of the present invention. Figure 5 to Figure 13 It is a cross-sectional view showing a method for manufacturing the semiconductor device 10 according to one embodiment of the present invention.
[0097] like Figure 4 and Figure 5 As shown, a conductive layer 105 is formed on the substrate 100 as a light shielding layer, and insulating layers 110 and 120 are formed on the conductive layer 105 ( Figure 4 As the insulating layer 110, for example, silicon nitride is formed. As the insulating layer 120, for example, silicon oxide is formed. The insulating layers 110 and 120 are formed by CVD (Chemical Vapor Deposition). In this specification, the case of forming a film on a substrate by a sputtering method, a CVD method, etc. is described as "forming a thin film", which is used in the same meaning as the expression "forming a thin film".
[0098] By using silicon nitride as the insulating layer 110, the insulating layer 110 can block, for example, impurities diffusing from the substrate 100 toward the oxide semiconductor layer 140. Silicon oxide used as the insulating layer 120 has a property of releasing oxygen when subjected to heat treatment.
[0099] In this embodiment, when the insulating layers 110 and 120 are formed, the film forming temperature is set to 350°C. In particular, for the insulating layer 120 (i.e., the silicon oxide layer), the oxygen content can be increased by setting the film forming temperature relatively low. As described later, by increasing the amount of oxygen contained in the insulating layer 120, the amount of hydrogen diffused into the oxide semiconductor layer 140 can be reduced. The film forming temperature of the insulating layers 110 and 120 can be set to 250°C to 500°C (preferably 300°C to 450°C, more preferably 325°C to 400°C).
[0100] Then, if Figure 4 and Figure 6 As shown, a metal oxide layer 130 and an oxide semiconductor layer 140 are formed on the insulating layer 120 ( Figure 4 In the present embodiment, the metal oxide layer 130 and the oxide semiconductor layer 140 are formed by sputtering. In particular, the oxide semiconductor layer 140 is formed by sputtering using a target formed of a crystalline oxide semiconductor.
[0101] The thickness of the metal oxide layer 130 is, for example, 1 nm to 10 nm, 1 nm to 4 nm, or 1 nm to 3 nm. In the present embodiment, the thickness of the metal oxide layer 130 is set to 3 nm. In the present embodiment, an oxide having aluminum as a main component (specifically, aluminum oxide) is used as the metal oxide layer 130. Aluminum oxide has a high barrier property against gases.
[0102] In this embodiment, aluminum oxide used as the metal oxide layer 130 blocks hydrogen and oxygen released from the insulating layer 120 and prevents the released hydrogen and oxygen from reaching the oxide semiconductor layer 140 .
[0103] In the oxide semiconductor layer 140 of this embodiment, the ratio of indium is 50% or more as described above, so a semiconductor device 10 with high mobility can be realized, but on the other hand, oxygen is easily reduced and oxygen defects are easily formed in the layer. Therefore, from the perspective of suppressing the reduction of the oxide semiconductor layer 140, it is preferable to use the metal oxide layer 130 to block hydrogen released from the insulating layer 120.
[0104] In addition, after the oxide semiconductor layer 140 is formed, more oxygen defects are formed on the upper side of the oxide semiconductor layer 140 than on the lower side during various manufacturing processes (patterning process or etching process). That is, the oxygen defects in the oxide semiconductor layer 140 exist in an uneven distribution in the thickness direction. In this case, if a sufficient amount of oxygen is supplied to repair the oxygen defects formed on the upper side of the oxide semiconductor layer 140, oxygen will be excessively supplied to the lower side of the oxide semiconductor layer 140. As a result, defect energy levels different from those of the oxygen defects are formed due to the excessive supply of oxygen, which sometimes leads to characteristics changes in reliability tests or a decrease in field effect mobility. Therefore, it can be said that from the perspective of suppressing the excessive supply of oxygen to the lower side of the oxide semiconductor layer 140, it is also preferable to use the metal oxide layer 130 to block the oxygen released from the insulating layer 120.
[0105] The thickness of the oxide semiconductor layer 140 is, for example, 10 nm to 100 nm, 15 nm to 70 nm, or 15 nm to 40 nm. The oxide semiconductor layer 140 is in an amorphous state before heat treatment (OS annealing) described below.
[0106] When the oxide semiconductor layer 140 is to be crystallized by OS annealing described later, it is preferred that the oxide semiconductor layer 140 is in an amorphous state (a state in which the crystal component of the oxide semiconductor is small) from the formation based on the sputtering method to the implementation of the OS annealing. That is, it is preferred that the formation conditions of the oxide semiconductor layer 140 are conditions that do not crystallize the oxide semiconductor layer 140 immediately after formation as much as possible. For example, in the case of forming the oxide semiconductor layer 140 by sputtering, it is desirable to form the oxide semiconductor layer 140 while controlling the temperature of the object to be formed (including the substrate 100 and the structure formed thereon). It should be noted that although the object to be temperature controlled is actually the object to be formed, since the structure formed on the substrate 100 is very thin, it can also be regarded as substantially controlling the temperature of the substrate 100. Therefore, in the following description, the object to be formed is sometimes referred to as a "substrate".
[0107] When a thin film is formed on a substrate by sputtering, ions generated in plasma and atoms recoiled from a sputtering target collide with an object to be formed (specifically, a structure formed on the substrate 100), so the temperature of the substrate rises during the thin film formation process. If the temperature of the substrate rises during the thin film formation process, the oxide semiconductor layer 140 contains microcrystals in a state immediately after formation, which hinders crystallization by OS annealing thereafter.
[0108] In order to control the temperature of the substrate (i.e., the film forming temperature) when the oxide semiconductor layer 140 is formed, for example, the thin film can be formed while the substrate is cooled. For example, the substrate can be cooled from the surface opposite to the formed surface in such a manner that the film forming temperature is below 100°C, below 70°C, below 50°C, or below 30°C. In particular, the film forming temperature of the oxide semiconductor layer 140 of the present embodiment is preferably below 50°C. In the present embodiment, the oxide semiconductor layer 140 is formed at a film forming temperature below 50°C, and the OS annealing described later is performed at a heating temperature above 400°C. Thus, in the present embodiment, the difference between the temperature when the oxide semiconductor layer 140 is formed and the temperature when the oxide semiconductor layer 140 is OS annealed is preferably 350°C or more. By forming the oxide semiconductor layer 140 while cooling the substrate, an oxide semiconductor layer 140 having a small crystal component in the state just after formation can be obtained.
[0109] Then, if Figure 4 and Figure 7 As shown, a pattern (OS pattern) composed of the oxide semiconductor layer 140 is formed ( Figure 4Step S1003). Although not shown in the figure, a resist mask is formed on the oxide semiconductor layer 140, and the oxide semiconductor layer 140 is etched using the resist mask patterned by photolithography. The etching of the oxide semiconductor layer 140 can be wet etching or dry etching. In wet etching, for example, an acidic etchant can be used. Specifically, oxalic acid or hydrofluoric acid can be used as the etchant.
[0110] After the patterning of the oxide semiconductor layer 140, the oxide semiconductor layer 140 is subjected to a heat treatment (OS annealing) ( Figure 4 Step S1004). In the OS annealing, the oxide semiconductor layer 140 is heat-treated in an air atmosphere at a temperature of 250°C to 500°C (preferably 300°C to 500°C, more preferably 350°C to 450°C), thereby crystallizing the amorphous oxide semiconductor layer 140. The heating atmosphere is not limited to the air atmosphere, and is preferably an oxidizing atmosphere (an atmosphere containing oxygen). More preferably, the oxidizing atmosphere is a humid atmosphere (specifically, a humid air atmosphere). The treatment time of the heat treatment can also be 15 minutes to 120 minutes, or 30 minutes to 60 minutes after reaching the specified temperature. In this embodiment, the temperature of the OS annealing is set to 350°C.
[0111] In the present embodiment, a substrate having a patterned oxide semiconductor layer 140 is placed in a heating furnace having a heating medium (e.g., a support plate) which is maintained at a set temperature in advance (250° C. to 500° C., 350° C. in the present embodiment). The support plate as a heating medium has the function of supporting the substrate and heating the substrate and the coating (including the oxide semiconductor layer 140) formed on the substrate. When the substrate having the oxide semiconductor layer 140 is placed on the support plate, the oxide semiconductor layer 140 is rapidly heated. When the substrate is placed in the heating furnace, it is desirable to suppress the temperature drop of the support plate to within 15%, within 10%, or within 5% of the set temperature. That is, it is preferred to control the temperature of the support plate in such a way that the oxide semiconductor layer 140 reaches the set temperature in a very short time.
[0112] It should be noted that, in this embodiment, an example of performing OS annealing after forming an OS pattern is illustrated, but the present invention is not limited to this example, and OS annealing may be performed on the oxide semiconductor layer 140 before forming an OS pattern. In this case, since the crystallized oxide semiconductor layer 140 is etched to form the OS pattern, dry etching is preferably used for the etching process.
[0113] Then, if Figure 4 and Figure 8As shown, a gate insulating layer 150 ( Figure 4 Step S1005). As the gate insulating layer 150, for example, a silicon oxide layer is formed. The gate insulating layer 150 is formed by a CVD method. As the gate insulating layer 150, it is desirable to form an insulating layer with as few defects as possible. In this embodiment, the film forming temperature of the gate insulating layer 150 is set to 350° C. The thickness of the gate insulating layer 150 is, for example, 50 nm to 300 nm, 60 nm to 200 nm, or 70 nm to 150 nm.
[0114] Next, in this embodiment, after the gate insulating layer 150 is formed, a metal oxide layer 190 ( Figure 4 The metal oxide layer 190 is formed by sputtering. By using the sputtering method in the film formation of the metal oxide layer 190, oxygen is injected into the gate insulating layer 150 when the metal oxide layer 190 is formed. Therefore, a large amount of oxygen is contained in the gate insulating layer 150 after the metal oxide layer 190 is formed.
[0115] The thickness of the metal oxide layer 190 is, for example, 5 nm to 100 nm, 5 nm to 50 nm, 5 nm to 30 nm, or 7 nm to 15 nm. In this embodiment, aluminum oxide is used as the metal oxide layer 190. As described above, aluminum oxide has a high barrier property against gas, and therefore, during the heat treatment described later, it is possible to suppress the upward diffusion of oxygen injected into the gate insulating layer 150.
[0116] When the metal oxide layer 190 is formed by sputtering, the process gas used for sputtering may remain in the film of the metal oxide layer 190. For example, when Ar is used as the process gas for sputtering, Ar may remain in the film of the metal oxide layer 190. The remaining Ar can be detected by performing SIMS (Secondary Ion Mass Spectrometry) analysis on the metal oxide layer 190, etc.
[0117] Next, in a state where the metal oxide layer 190 is formed on the gate insulating layer 150, a heat treatment (oxidation annealing) is performed to supply oxygen to the oxide semiconductor layer 140 ( Figure 4Step S1007). In other words, the patterned metal oxide layer 130 and the oxide semiconductor layer 140 are subjected to heat treatment (oxidation annealing). In the process from the formation of the oxide semiconductor layer 140 to the formation of the gate insulating layer 150 on the oxide semiconductor layer 140, oxygen defects are generated on the upper surface 141 and the side surface 143 of the oxide semiconductor layer 140. The oxygen released from the insulating layer 120 and the gate insulating layer 150 by the oxidation annealing is supplied to the oxide semiconductor layer 140 to repair the oxygen defects. The oxidation annealing can be performed at a temperature of 250°C to 500°C (preferably 300°C to 500°C, more preferably 350°C to 450°C). In this embodiment, the oxidation annealing is performed at a temperature of 350°C.
[0118] Oxygen released from the insulating layer 120 by the oxidation annealing is blocked by the metal oxide layer 130, so it is difficult to supply oxygen to the lower surface 142 of the oxide semiconductor layer 140. Oxygen released from the insulating layer 120 diffuses from the region where the metal oxide layer 130 is not formed to the gate insulating layer 150, and reaches the oxide semiconductor layer 140 via the gate insulating layer 150. As a result, oxygen released from the insulating layer 120 is not easily supplied to the lower surface 142 of the oxide semiconductor layer 140, but is mainly supplied to the side surface 143 and the upper surface 141 of the oxide semiconductor layer 140. In addition, oxygen released from the gate insulating layer 150 by the oxidation annealing is supplied to the upper surface 141 and the side surface 143 of the oxide semiconductor layer 140. Hydrogen is sometimes released from the insulating layer 110 by the above-mentioned oxidation annealing. However, the hydrogen is captured by the oxygen contained in the insulating layer 120 or blocked by the metal oxide layer 130 before reaching the oxide semiconductor layer 140.
[0119] As described above, by oxidation annealing, it is possible to suppress the supply of oxygen to the lower surface 142 of the oxide semiconductor layer 140 having a small amount of oxygen defects, and it is possible to supply oxygen to the upper surface 141 and the side surface 143 of the oxide semiconductor layer 140 having a relatively large amount of oxygen defects. Similarly, during oxidation annealing, the upward diffusion of oxygen injected into the gate insulating layer 150 is blocked by the metal oxide layer 190, thereby suppressing the release of oxygen into the atmosphere. Therefore, during oxidation annealing, oxygen can be efficiently supplied to the oxide semiconductor layer 140.
[0120] Then, if Figure 4 and Fig. 9 As shown, after the oxidation annealing, the metal oxide layer 190 is etched to remove ( Figure 4 The etching of the metal oxide layer 190 may be wet etching or dry etching. In wet etching, for example, diluted hydrofluoric acid (DHF) is used. The entire metal oxide layer 190 is removed by the etching process of step S1008.
[0121] Then, if Figure 4 and Fig.10 As shown, a gate wiring 160 is formed on the gate insulating layer 150, and then the gate insulating layer 150 is etched ( Figure 4 The gate wiring 160 is formed by patterning the metal layer formed by sputtering or atomic layer deposition and then performing dry etching. The gate insulating layer 150 is etched by further continuing dry etching after forming the gate wiring 160. That is, the gate insulating layer 150 is etched using the gate wiring 160 as a mask. In this way, in this embodiment, the metal layer and the gate insulating layer 150 are etched together, thereby forming a patterned gate insulating layer 150 and gate wiring 160.
[0122] In this embodiment, the gate insulating layer 150 is etched using the gate wiring 160 as a mask, thereby exposing a portion of the oxide semiconductor layer 140 (a region to be a source region S and a drain region D described later). In addition, since the etching process is performed using the gate wiring 160 as a mask, the gate insulating layer 150 and the gate wiring 160 have the same pattern shape.
[0123] like Fig.10 As shown, when the gate insulating layer 150 is etched until the oxide semiconductor layer 140 is exposed, not only the upper surface 141 of the oxide semiconductor layer 140 is exposed, but also the side surface 143 of the oxide semiconductor layer 140 and the upper surface of the metal oxide layer 130 are exposed. At this time, in this embodiment, since the metal oxide layer 130 is not patterned, the insulating layer 120 disposed under the metal oxide layer 130 is not exposed. That is, the insulating layer 120 does not need to be exposed to the environment in which the gate insulating layer 150 is etched.
[0124] The insulating layer 120 is composed of a silicon oxide layer like the gate insulating layer 150, so if it is exposed to an environment in which the gate insulating layer 150 is etched, it will be etched at a substantially equal speed. That is, if the insulating layer 120 is exposed from the metal oxide layer 130, the insulating layer 120 will be deeply etched in the case of over-etching, and a large step difference may be generated between the end of the metal oxide layer 130 (or the end of the oxide semiconductor layer 140) and the upper surface of the insulating layer 120. Such a step difference sometimes has a bad effect on the electrical characteristics of the semiconductor device 10 (for example, an increase in leakage current, etc.). On the contrary, if the etching time is insufficient, the gate insulating layer 150 remains on the oxide semiconductor layer 140, which sometimes has a bad effect on the electrical characteristics of the semiconductor device 10 (for example, a shift of the threshold voltage in the negative direction, etc.).
[0125] Thus, when the insulating layer 120 is exposed from the metal oxide layer 130, it is necessary to accurately grasp the etching time required until the upper surface of the oxide semiconductor layer 140 is exposed so as to perform etching control such as minimizing over-etching. In contrast, according to the manufacturing method of this embodiment, the metal oxide layer 130 functions as an etching stopper when etching the gate insulating layer 150, so that even if over-etching is performed, the insulating layer 120 is not etched. That is, according to the manufacturing method of this embodiment, the process margin when etching the gate insulating layer 150 can be greatly improved.
[0126] Then, if Figure 4 and Fig.11 As shown, a pattern (AlOx pattern) consisting of a metal oxide layer 130 is formed ( Figure 4 Step S1010). The crystallized oxide semiconductor layer 140 has etching resistance against hydrofluoric acid. Therefore, the metal oxide layer 130 of this embodiment is etched using the patterned oxide semiconductor layer 140 as a mask. The etching of the metal oxide layer 130 can use wet etching or dry etching. In wet etching, for example, diluted hydrofluoric acid (DHF) is used. By using the oxide semiconductor layer 140 as a mask to etch the metal oxide layer 130, the photolithography process can be omitted.
[0127] Then, if Figure 4 and Fig.12 As shown, insulating layers 170 and 180 are formed on the gate insulating layer 150 and the gate wiring 160 as passivation layers ( Figure 4 Step S1011). The insulating layers 170 and 180 are formed by a CVD method. In the present embodiment, a silicon oxide layer is formed as the insulating layer 170, and a silicon nitride layer is formed as the insulating layer 180. The film forming temperature of the insulating layers 170 and 180 is preferably set to be not less than 250°C and not more than 500°C (preferably not less than 300°C and not more than 450°C, more preferably not less than 325°C and not more than 400°C). In the present embodiment, the film forming temperature of the insulating layers 170 and 180 is set to 350°C. In addition, the thickness of the insulating layers 170 and 180 can be set to be not less than 50nm and not more than 500nm. In the present embodiment, the thickness of the insulating layer 170 is set to 100nm, and the thickness of the insulating layer 180 is set to 300nm.
[0128] The insulating layers 170 and 180 function as a passivation layer (protective layer) for preventing gas and moisture from entering from the outside. In addition, as described above, they also have the function of insulating and separating the gate wiring 160 from the source / drain electrode 200. In addition, in this embodiment, by forming the insulating layers 170 and 180 (especially the insulating layer 180), the source region S and the drain region D are formed in the oxide semiconductor layer 140.
[0129] The insulating layer 180 of the present embodiment is composed of silicon nitride. When the insulating layer 180 is formed by the CVD method, ammonia is used as the raw material gas, so the insulating layer 180 contains a large amount of hydrogen. Therefore, when the insulating layer 180 is formed and after the insulating layer 180 is formed, hydrogen is diffused from the insulating layer 180 by heating the insulating layer 180. The diffused hydrogen reaches the oxide semiconductor layer 140 via the insulating layer 170. At this time, the oxygen contained in the region of the oxide semiconductor layer 140 that is in contact with the insulating layer 170 is reduced to form an oxygen defect. Hydrogen is captured in the formed oxygen defect to form a donor level. As a result, a portion of the oxide semiconductor layer 140 supplied with hydrogen is reduced in resistance and functions as a source region S and a drain region D. In contrast, the oxide semiconductor layer 140 located directly below the gate wiring 160 is not reduced in resistance because no hydrogen reaches it, and functions as a channel region CH.
[0130] In the semiconductor device 10 of this embodiment, since the gate insulating layer 150 has the same pattern shape as the gate wiring 160, the oxide semiconductor layer 140 exposed from the gate insulating layer 150 is directly in contact with the insulating layer 170. Therefore, compared with a structure in which the oxide semiconductor layer 140 is covered by the gate insulating layer 150, hydrogen is easily diffused under the gate wiring 160. Fig.12 As shown, a portion of the region that should have been the channel region CH is also reduced in resistance by hydrogen diffused below the gate wiring 160. That is, the source region S and the drain region D extend toward the channel region CH to form an overlapping region OL.
[0131] As described above, in this embodiment, the width (ΔL) of the overlap region OL in the first direction (channel length direction) can be suppressed to less than 1 μm. By suppressing the width of the overlap region OL to less than 1 μm, the deviation between the designed channel length and the effective channel length can be suppressed. As a result, in the semiconductor device 10 of this embodiment, even if the channel length is less than 4 μm, stable electrical characteristics can be obtained.
[0132] The reason why the width (ΔL) of the overlapping region OL can be suppressed to 1 μm or less is that a large amount of oxygen is contained in the insulating layer 120 (silicon oxide layer in this embodiment) provided under the oxide semiconductor layer 140 .
[0133] In a plan view, the insulating layer 120 containing a large amount of oxygen is directly in contact with the insulating layer 170 around the oxide semiconductor layer 140. Therefore, most of the hydrogen diffused from the insulating layers 170 and 180 is captured by the insulating layer 120, and the amount of hydrogen diffused toward the oxide semiconductor layer 140 is suppressed. At this time, the source region S and the drain region D of the oxide semiconductor layer 140 are directly in contact with the insulating layer 170, so even if the amount of diffused hydrogen is small, the resistance is sufficiently low, but the amount of hydrogen diffused toward the bottom of the gate wiring 160 is reduced. As a result, it is considered that in this embodiment, the width of the overlapping region OL (that is, the diffusion length of hydrogen) is shortened.
[0134] In order to increase the oxygen content of the insulating layer 120, it is preferable to set the film forming temperature of the insulating layer 120 relatively low. In this embodiment, it is set to 350°C, but it can be within the range of 250°C to 500°C (preferably 300°C to 500°C, more preferably 350°C to 450°C).
[0135] In addition, in this embodiment, a process of forming the metal oxide layer 130 on the insulating layer 120 is included, and this process also contributes to increasing the oxygen content of the insulating layer 120. Specifically, when aluminum oxide is formed as the metal oxide layer 130 by sputtering, oxygen is injected into the insulating layer 120. Thus, oxygen is further injected into the insulating layer 120 whose oxygen content increases at the above-mentioned film formation temperature, so that the total amount of oxygen in the insulating layer 120 can be increased.
[0136] As described above, in the semiconductor device 10 of the present embodiment, the gate insulating layer 150 is processed into the same pattern shape as the gate wiring 160, so that the oxide semiconductor layer 140 and the insulating layer 170 are directly connected. As a result, the resistance of a part of the oxide semiconductor layer 140 can be reduced using hydrogen diffused from the insulating layers 170 and 180, thereby forming the source region S and the drain region D. In addition, at this time, since a large amount of oxygen is contained in the insulating layer 120 that becomes the base of the oxide semiconductor layer 140, the amount of hydrogen used for reducing the resistance of the oxide semiconductor layer 140 can be reduced. As a result, the diffusion of hydrogen directly below the gate wiring 160 can be suppressed, and the width of the overlapping region OL can be shortened.
[0137] Then, if Figure 4 and Fig.13 As shown, openings 171 and 173 are formed in the insulating layers 170 and 180 ( Figure 4The opening 171 exposes the oxide semiconductor layer 140 in the source region S. The opening 173 exposes the oxide semiconductor layer 140 in the drain region D. The source / drain electrode 200 ( Figure 4 Step S1013), thereby completing Figure 1 A semiconductor device 10 is shown.
[0138] In the semiconductor device 10 manufactured by the manufacturing method of this embodiment, when the channel length L of the channel region CH is within the range of 2 μm to 4 μm and the channel width of the channel region CH is within the range of 2 μm to 25 μm, a field effect mobility of 30 cm 2 / Vs or above, 35cm 2 / Vs or above or 40cm 2 The "field effect mobility" in this embodiment refers to the field effect mobility in the saturation region of the semiconductor device 10, which means the maximum value of the field effect mobility in the region where the potential difference (Vd) between the source electrode and the drain electrode is greater than the value (Vg-Vth) obtained by subtracting the threshold voltage (Vth) of the semiconductor device 10 from the voltage (Vg) supplied to the gate wiring.
[0139] <Second Embodiment>
[0140] In this embodiment, a semiconductor device manufactured by a method different from that of the first embodiment is described. The structure of the semiconductor device 10 of this embodiment is similar to the semiconductor device 10 described in the first embodiment in appearance. In this embodiment, the description is focused on the points different from the first embodiment.
[0141] Fig.14 FIG. 1 is a flowchart showing a method for manufacturing a semiconductor device 10 according to an embodiment of the present invention. Fig.14 As shown, in this embodiment, the Figure 4 The two steps of step S1006 (AlOx formation) and S1008 (AlOx removal) are shown. That is, in this embodiment, after the gate insulating layer 150 is formed, oxidation annealing is performed in this state. Through this oxidation annealing, oxygen released from the gate insulating layer 150 is supplied to the oxide semiconductor layer 140, and oxygen defects contained in the oxide semiconductor layer 140 are repaired. The role of the metal oxide layer 130 at this time is the same as that of the first embodiment, so the description here is omitted.
[0142] In the semiconductor device 10 manufactured by the manufacturing method of this embodiment, when the channel length L of the channel region CH is within the range of 2 μm to 4 μm and the channel width W of the channel region CH is within the range of 2 μm to 25 μm, a mobility of 30 cm 2 / Vs or above, 35cm 2 / Vs or above or 40cm 2 The definition of field effect mobility in this embodiment is the same as that in the first embodiment.
[0143] <Third Embodiment>
[0144] use Figure 15 to Figure 19 A display device using a semiconductor device according to an embodiment of the present invention will be described. In the following embodiments, a circuit configuration in which each semiconductor device described in the first embodiment and the second embodiment is applied to a liquid crystal display device will be described.
[0145] [Overview of Display Device]
[0146] Fig.15 FIG. 2 is a top view showing an overview of a display device 20 in one embodiment of the present invention. Fig.15 As shown, the display device 20 includes an array substrate 300, a sealing portion 310, an opposing substrate 320, a flexible printed circuit substrate 330 (FPC 330), and an IC chip 340. The array substrate 300 and the opposing substrate 320 are bonded together by the sealing portion 310. A plurality of pixel circuits 301 are arranged in a matrix in a liquid crystal region 22 surrounded by the sealing portion 310. The liquid crystal region 22 is a region that overlaps with a liquid crystal element 311 described later in a plan view.
[0147] The sealing region 24 provided with the sealing portion 310 is the region around the liquid crystal region 22. The FPC 330 is provided in the terminal region 26. The terminal region 26 is the region exposed from the counter substrate 320 in the array substrate 300 and is provided outside the sealing region 24. The outside of the sealing region 24 refers to the region provided with the sealing portion 310 and the outside of the region surrounded by the sealing portion 310. The IC chip 340 is provided on the FPC 330. The IC chip 340 supplies a signal for driving each pixel circuit 301.
[0148] [Circuit Configuration of Display Device]
[0149] Fig.16 1 is a block diagram showing a circuit configuration of a display device 20 in one embodiment of the present invention. Fig.16As shown in FIG. 1 , a source driving circuit 302 is provided at a position adjacent to the liquid crystal region 22 where the pixel circuit 301 is arranged in the Y direction (column direction). In addition, a gate driving circuit 303 is provided at a position adjacent to the liquid crystal region 22 in the X direction (row direction). The source driving circuit 302 and the gate driving circuit 303 are provided in the above-mentioned sealing region 24. However, the region where the source driving circuit 302 and the gate driving circuit 303 are provided is not limited to the sealing region 24, and may be any region as long as it is outside the region where the pixel circuit 301 is provided.
[0150] The source wiring 304 extends from the source driving circuit 302 in the Y direction and is connected to the plurality of pixel circuits 301 arranged in the Y direction. The gate wiring 305 extends from the gate driving circuit 303 in the X direction and is connected to the plurality of pixel circuits 301 arranged in the X direction.
[0151] The terminal region 26 is provided with a terminal portion 306. The terminal portion 306 and the source driver circuit 302 are connected via a connection wiring 307. Similarly, the terminal portion 306 and the gate driver circuit 303 are connected via a connection wiring 308. By connecting the FPC 330 and the terminal portion 306, an external device is connected to the display device 20 via the FPC 330. Each pixel circuit 301 provided in the display device 20 is driven by a signal from an external device input via the FPC 330.
[0152] The semiconductor device 10 described in the first embodiment and the second embodiment is used as a transistor included in the pixel circuit 301 , the source driver circuit 302 , and the gate driver circuit 303 .
[0153] [Pixel circuit of display device]
[0154] Fig.17 is a circuit diagram showing a pixel circuit 301 of a display device 20 in one embodiment of the present invention. Fig.17 As shown, the pixel circuit 301 includes elements such as the semiconductor device 10, a storage capacitor 350, and a liquid crystal element 311.
[0155] The semiconductor device 10 includes a gate wiring 160, a source electrode 201, and a drain electrode 203. The gate wiring 160 is connected to the gate wiring 305. The source electrode 201 is connected to the source wiring 304. The drain electrode 203 is connected to the storage capacitor 350 and the liquid crystal element 311. The source electrode 201 and the drain electrode 203 may switch roles depending on the relationship between the voltage supplied to the source wiring 304 and the voltage accumulated in the storage capacitor 350. That is, there is a case where the source electrode 201 functions as a drain electrode and the drain electrode 203 functions as a source electrode.
[0156] [Cross-sectional structure of display device]
[0157] Fig.18 2 is a cross-sectional view showing an overview of a display device 20 in one embodiment of the present invention. Fig.18 As shown in FIG. 1 , the display device 20 is a display device using the semiconductor device 10. In this embodiment, the semiconductor device 10 is used in the pixel circuit 301, but the semiconductor device 10 can also be used in peripheral circuits including the source driver circuit 302 and the gate driver circuit 303. In the following description, the configuration of the semiconductor device 10 is similar to that of the semiconductor device 10. Figure 1 The semiconductor device 10 shown is the same, so the detailed description is omitted.
[0158] An insulating layer 360 is provided on the source electrode 201 and the drain electrode 203. A common electrode 370 provided in common to a plurality of pixels is provided on the insulating layer 360. An insulating layer 380 is provided on the common electrode 370. An opening 381 is provided on the insulating layers 360 and 380. A pixel electrode 390 is provided on the insulating layer 380 and inside the opening 381. The pixel electrode 390 is connected to the drain electrode 203.
[0159] Fig.19 FIG. 2 is a top view of a pixel electrode 390 and a common electrode 370 of a display device 20 in one embodiment of the present invention. Fig.19 As shown, the common electrode 370 is composed of a flat conductive layer. The pixel electrode 390 is composed of a comb-shaped conductive layer composed of a portion extending along the X direction and a portion extending along the Y direction. The portion extending along the Y direction is composed of a plurality of linear electrodes, which are respectively connected to the portion extending along the X direction.
[0160] The common electrode 370 has an overlapping region that overlaps with the pixel electrode 390 in a plan view and a non-overlapping region that does not overlap with the pixel electrode 390. When a voltage is supplied between the pixel electrode 390 and the common electrode 370, a transverse electric field is formed from the pixel electrode 390 in the overlapping region toward the common electrode 370 in the non-overlapping region. The liquid crystal molecules contained in the liquid crystal element 311 are moved by the transverse electric field, thereby determining the grayscale of the pixel.
[0161] <Fourth Embodiment>
[0162] use Fig. 20 and Fig.21 A display device using a semiconductor device in one embodiment of the present invention will be described. In the following embodiment, the configuration of a circuit in which each semiconductor device described in the first embodiment and the second embodiment is applied to an organic EL display device will be described. Fig.15 and Fig.16The situation shown is the same, so the description here is omitted.
[0163] [Pixel circuit of display device]
[0164] Fig. 20 2 is a circuit diagram showing a pixel circuit 301a of a display device 20a according to an embodiment of the present invention. Fig. 20 As shown, the pixel circuit 301a includes components such as a driving transistor 11, a selection transistor 12, a holding capacitor 210 and a light-emitting element DO.
[0165] The driving transistor 11 and the selecting transistor 12 have the same structure as the semiconductor device 10. The source electrode of the selecting transistor 12 is connected to the signal line 211, and the gate wiring of the selecting transistor 12 is connected to the gate line 212. The source electrode of the driving transistor 11 is connected to the anode power line 213, and the drain electrode of the driving transistor 11 is connected to one end of the light emitting element DO. The other end of the light emitting element DO is connected to the cathode power line 214. The gate wiring of the driving transistor 11 is connected to the drain electrode of the selecting transistor 12. The holding capacitor 210 is connected to the gate wiring and the drain electrode of the driving transistor 11. A grayscale signal that determines the light intensity of the light emitting element DO is supplied to the signal line 211. A signal for selecting a pixel row to which the grayscale signal is to be written is supplied to the gate line 212.
[0166] [Cross-sectional structure of display device]
[0167] Fig.21 It is a cross-sectional view schematically showing a display device 20 a in one embodiment of the present invention. Fig.21 The display device 20a shown in FIG. Fig.18 The display device 20 shown in FIG. 2 is similar to the display device 20 shown in FIG. 20 , but the structure above the insulating layer 360 in the display device 20 and the display device 20a is different. Fig.21 The display device 20a shown in FIG. Fig.18 Description of the same configurations as the display device 20 shown will be omitted, and differences between the two will be described.
[0168] like Fig.21As shown, the display device 20a has a pixel electrode 390, a light-emitting layer 392 and a common electrode 394 above the insulating layer 360. The light-emitting element DO is composed of the pixel electrode 390, the light-emitting layer 392 and the common electrode 394. The pixel electrode 390 is arranged on the insulating layer 360 and inside the opening 381. Here, the insulating layer 362 is called a bank, a rib, etc., and has the function of defining the light-emitting area. The insulating layer 362 is arranged on the pixel electrode 390. An opening 363 is provided in the insulating layer 362. The opening 363 corresponds to the light-emitting area. The light-emitting layer 392 and the common electrode 394 are arranged on the pixel electrode 390 exposed by the opening 363. The pixel electrode 390 and the light-emitting layer 392 are respectively provided for each pixel. On the other hand, the common electrode 394 is provided in common with respect to multiple pixels. Different materials are used for the light-emitting layer 392 according to the display color of the pixel.
[0169] In the third embodiment and the fourth embodiment, the semiconductor device described in the first embodiment and the second embodiment is applied to the configuration of a liquid crystal display device and an organic EL display device, respectively. However, the semiconductor device described in the first embodiment and the second embodiment can also be applied to display devices other than the above-mentioned display devices (for example, self-luminous display devices other than organic EL display devices or electronic paper type display devices). In addition, the above-mentioned semiconductor devices can be applied to display devices ranging from small and medium-sized display devices to large display devices without special limitations.
[0170] <Example>
[0171] [Electrical Characteristics of Semiconductor Devices]
[0172] Fig.22A It is a diagram showing the electrical characteristics of the semiconductor device 10 according to one embodiment of the present invention. Fig. 22B is a graph showing the electrical characteristics of a semiconductor device in a comparative example. Specifically, Fig. 22B With Figure 1 The electrical characteristics of the semiconductor device 10 shown correspond to those of the semiconductor device having a structure in which the metal oxide layer 130 is omitted. Fig.22A and Fig. 22B A plurality of electrical characteristics obtained by measuring a plurality of semiconductor devices are shown respectively.
[0173] Fig.22A and Fig. 22B The measurement conditions of the electrical characteristics shown are as follows.
[0174] ·Size of channel region CH: W / L=4.5μm / 3.0μm
[0175] Source-drain voltage: 0.1V, 10V
[0176] ·Gate voltage: -15V~+15V
[0177] ·Measurement environment: room temperature, dark room
[0178] exist Fig.22A and Fig. 22B In FIG. 1 , as electrical characteristics of the semiconductor device, the Id-Vg characteristics and the field effect mobility (μsat) in the saturation region are shown. Fig.22A and Fig. 22B As shown by an arrow in the graph of , the vertical axis representing the drain current (Id) is shown on the left side of the graph. In addition, the vertical axis representing the field effect mobility calculated based on the drain current is shown on the right side of the graph. The horizontal axis is the gate voltage supplied to each semiconductor device.
[0179] like Fig.22A As shown, the Id-Vg characteristics of the semiconductor device 10 of the first embodiment show a so-called normally off characteristic in which the drain current Id starts to flow when the gate voltage Vg is approximately 0V. Regardless of whether the source-drain voltage is 0.1V or 10V, the deviation of the drain current is small and very stable. The average value of the threshold voltage (Vth) obtained from the multiple Id-Vg characteristics is 0.16V. In addition, the average value of the intrinsic mobility obtained from the multiple Id-Vg characteristics is 24.8cm 2 / Vs, the average field effect mobility is 39.3cm 2 / Vs.
[0180] In contrast, Fig. 22B As shown, the Id-Vg characteristics of the semiconductor device of the comparative example show the so-called normally on characteristics in which the threshold voltage is shifted in the negative direction and the drain current Id begins to flow when the gate voltage Vg is below 0V. The average value of the threshold voltage obtained from multiple Id-Vg characteristics is -3.59V. In addition, although some deviations are observed in the drain current, it shows an average high value, and no major problems are seen in the switching characteristics. The average value of the intrinsic mobility obtained from multiple Id-Vg characteristics is 19.5cm 2 / Vs, the average field effect mobility is 30.8cm 2 / Vs.
[0181] Here, the average value of the width (ΔL / 2) of the overlap region OL in the semiconductor device 10 of the first embodiment is 0.82 μm, and the average value of the width of the overlap region OL in the semiconductor device of the comparative example is 1.50 μm. Figure 1The width of the overlap region OL differs by nearly 2 times depending on the presence or absence of the metal oxide layer 130. That is, it is found that providing the metal oxide layer 130 is very effective in reducing the width of the overlap region OL.
[0182] In the semiconductor device of the comparative example, the designed channel length is 3.0 μm and the width of the overlap region OL is 1.5 μm, so the channel region CH does not appear to exist in calculation. However, in reality, there is an error in the designed channel length, and the width of the overlap region OL is only an average value, so in reality, the channel region CH does not completely disappear.
[0183] The width of the overlap region OL can be obtained by various methods. In this embodiment, an example of obtaining the overlap region OL based on the relationship between the designed channel length and the channel resistance R of the transistor when different gate voltages are applied is described.
[0184] Fig.23 is a diagram illustrating the relationship between the channel resistance (R) in a transistor and the designed channel length (channel length on layout) (Lg) for different gate voltages (Vg). Fig.23 In the figure, the horizontal axis is the designed channel length (Lg) and the vertical axis is the channel resistance (R). Fig.23 , the channel resistance (R) of each transistor with a designed channel length (Lg) of L1, L2 or L3 is shown when 1V, 2V or 3V is applied as the gate voltage (Vg). Fig.23 As shown, at each gate voltage (Vg), the designed channel length (Lg) and the channel resistance (R) are linearly related.
[0185] Here, when the straight lines representing the linear relationships are extrapolated in the direction in which Lg decreases, a point where the extrapolated lines intersect appears. This intersection point is the effective channel length (L eff ) becomes zero. At this time, if the X coordinate of the intersection is ΔL and the Y coordinate is R0, ΔL is equivalent to the width of the overlapping area OL, and R0 is equivalent to the series resistance generated by the overlapping area OL. eff ) and the designed channel length (Lg), L eff =Lg-ΔL. Figure 1 As shown, when the transistor is symmetrical with respect to the first direction (direction D1), the overlapping area OL on the source side S The overlap area OL with the drain side D The sum of ΔL is the overlap area OL on the source side. S The overlap area OL with the drain side D Between, OL S =OLD =ΔL / 2 holds true.
[0186] then, Fig.24A This is a diagram showing the dependency of the threshold voltage on the channel length in the semiconductor device 10 according to one embodiment of the present invention. Fig. 24B Graph showing the dependency of the threshold voltage on the channel length in the semiconductor device of the above-mentioned comparative example. Here, the channel width (W) of each semiconductor device is set to 4.5 μm.
[0187] like Fig.24A As shown, it can be seen that in the semiconductor device 10 of the present embodiment, the threshold voltage hardly changes within the range of the channel length being 4 μm to 20 μm, and exhibits stable switching characteristics. In addition, it can be seen that even within the range of the channel length being 4 μm or less (for example, 2.5 μm to 4 μm), a threshold voltage of -0.4 V or more can be ensured. That is, the semiconductor device 10 of the present embodiment can obtain a stable threshold voltage independent of the channel length, and even if the channel length is 4 μm or less, the threshold voltage will not shift significantly in the negative direction. In contrast, Fig. 24B As shown, it is observed that the threshold voltage of the semiconductor device of the comparative example shifts in the negative direction within the range of the channel length being 10 μm or less.
[0188] Think in Fig.24A and Fig. 24B The difference in electrical characteristics observed in the embodiment is due to the width of the overlap region OL (ΔL / 2). That is, since the width of the overlap region OL can be suppressed to less than 1 μm, the channel length (Lg) and the effective channel (L eff ) is small. Therefore, the dependence of the threshold voltage on the channel length shows a trend close to the dependence of the threshold voltage on the designed channel length. On the other hand, the width of the overlapping region OL in the semiconductor device of the comparative example is longer than that of the present embodiment. Therefore, the shorter the designed channel length, the more significant the influence brought by the width of the overlapping region OL.
[0189] As described above, it can be said that setting the width of the overlapping region OL to 1 μm or less is important in suppressing the degradation of the electrical characteristics of the semiconductor device, especially suppressing the shift of the threshold voltage in the negative direction. In addition, in order to suppress the width of the overlapping region OL to 1 μm or less, it is effective to increase the oxygen content of the insulating layer 120, which is the layer that serves as the base of the oxide semiconductor layer 140. In addition, it is desirable to provide a metal oxide layer 130 between the insulating layer 120 and the oxide semiconductor layer 140 in addition to increasing the oxygen content of the insulating layer 120.
[0190] The various embodiments described above as embodiments of the present invention can be appropriately combined and implemented as long as they do not contradict each other. In addition, solutions obtained by adding, deleting or designing components appropriately based on the various embodiments, or solutions obtained by adding, omitting or changing conditions of processes, as long as they have the gist of the present invention, are also included in the scope of the present invention.
[0191] Even if there are other effects different from the effects brought about by the schemes of the above-mentioned embodiments, if they are clearly known from the description of this specification or can be easily predicted by those skilled in the art, they can of course be understood as the effects brought about by the present invention.
Claims
1. A semiconductor device comprising: a metal oxide layer above an insulating surface; an oxide semiconductor layer on the metal oxide layer; a gate insulating layer on the oxide semiconductor layer; and a gate wiring on the gate insulating layer, The metal oxide layer has a first region overlapping the gate wiring and the oxide semiconductor layer, a second region overlapping the oxide semiconductor layer and not overlapping the gate wiring, and a third region overlapping the gate wiring and not overlapping the oxide semiconductor layer.
2. The semiconductor device according to claim 1, wherein The metal oxide layer has a pattern shape that is the same as a union of a pattern shape of the gate wiring and a pattern shape of the oxide semiconductor layer in a plan view.
3. The semiconductor device according to claim 1, wherein The gate insulating layer has the same pattern shape as the gate wiring in a plan view.
4. The semiconductor device according to claim 1, further comprising an insulating layer over the gate wiring, The first region is not in contact with the insulating layer, A side surface of the second region and a side surface of the third region are in contact with the insulating layer.
5. The semiconductor device according to claim 4, wherein: The insulating layer is in contact with the gate wiring, the gate insulating layer, and the oxide semiconductor layer.
6. The semiconductor device according to claim 4, wherein: The insulating layer has a stacked structure including a silicon nitride layer and a silicon oxide layer.
7. The semiconductor device according to claim 1, wherein The oxide semiconductor layer contains two or more metals including indium, and a ratio of indium in the two or more metals is 50% or more.
8. The semiconductor device according to claim 1, wherein The first region is connected to the channel region, The second region is connected to the source region or the drain region.
9. The semiconductor device according to claim 8, wherein: The channel region is continuous with the source region or the drain region in a first direction, A portion of the source region or the drain region that is in contact with the gate insulating layer has a width in the first direction of 1 μm or less.
10. The semiconductor device according to claim 9, wherein In the first direction, the width of the gate wiring is 4 μm or less.
11. The semiconductor device according to claim 9, wherein In the first direction, the width of the gate wiring is greater than twice the width of a portion of the source region or the drain region in contact with the gate insulating layer in the first direction by 1 μm or more.
12. A display device, wherein: Each pixel includes the semiconductor device according to any one of claims 1 to 11.
13. A method for manufacturing a semiconductor device, comprising: forming a first metal oxide layer over the insulating surface; forming an oxide semiconductor layer having a pattern shape on the first metal oxide layer; forming a gate insulating layer on the oxide semiconductor layer; forming a gate wiring on the gate insulating layer; Using the gate wiring as a mask to etch the gate insulating layer; The first metal oxide layer is etched using the gate wiring and the oxide semiconductor layer as masks.
14. The method for manufacturing a semiconductor device according to claim 13, wherein: The etching of the gate insulating layer is performed by dry etching, The etching of the first metal oxide layer is performed by wet etching.
15. The method for manufacturing a semiconductor device according to claim 13, wherein: The formation of the gate wiring and the etching of the gate insulating layer are performed simultaneously by dry etching.
16. The method for manufacturing a semiconductor device according to claim 13, comprising: After the oxide semiconductor layer is formed, the oxide semiconductor layer is made into a polycrystalline structure by a first annealing treatment.
17. The method for manufacturing a semiconductor device according to claim 16, wherein: The first metal oxide layer is formed on the first insulating layer, The manufacturing method further includes, after etching the first metal oxide layer, forming a second insulating layer including a silicon nitride layer.
18. The method for manufacturing a semiconductor device according to claim 17, comprising: After forming the gate insulating layer, forming a second metal oxide layer on the gate insulating layer; After forming the second metal oxide layer, performing a second annealing process; and After the second annealing process, the second metal oxide layer is removed.
19. The method for manufacturing a semiconductor device according to claim 18, wherein: The formation of the first insulating layer, the formation of the gate insulating layer, the formation of the second insulating layer, the first annealing process, and the second annealing process are performed at a temperature of 250° C. or more and 500° C. or less.