Copper paste for pressure bonding, semiconductor device, method for producing copper paste for pressure bonding, and method for producing semiconductor device
By using copper powder and solvent copper paste with different shapes and particle sizes, the problem of joint damage and unevenness during the joint process of thin or large-area semiconductor components in the existing technology is solved, high-strength and uniform jointing is achieved, and the efficiency is improved. The joint strength and reliability of the joint body.
Patent Information
- Application Number
- CN202380022055.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-02-28
- Publication Date
- 2024-10-01
AI Technical Summary
Existing pressure bonding compositions easily cause bonding damage and unevenness during the bonding process of thin or large-area semiconductor devices, making it difficult to ensure high strength and reliability.
Use a copper paste containing two or more copper powders with different shapes and/or particle sizes and a solvent. By adjusting the proportion, particle size and shape of the copper powder, the viscosity and the fluffiness of the dry coating film are controlled to ensure that the Achieve high strength and uniform bonding.
It achieves high-strength and uniform bonding in the case of thin or large-area semiconductor components, avoids uneven bonding and damage, and improves the bonding strength and reliability of the bonded body.
Smart Images

Figure BDA0004994865830000191 
Figure BDA0004994865830000201
Abstract
Description
Technical Field
[0001] The present invention relates to a copper paste for press bonding, a semiconductor device, a method for producing the copper paste for press bonding, and a method for producing a semiconductor device. Background Art
[0002] In recent years, electronic components called power modules have been used to achieve high efficiency and space saving of power semiconductor devices. A power module has multiple semiconductor elements mounted on one side of a substrate and cooling components such as a base plate and a heat sink mounted on the other side. The above components are connected by bonding materials, thermal conductive grease, etc. This power module requires long-term reliability, and as one of the methods to achieve long-term reliability, the use of sintered materials made by sintering metals such as silver and copper as bonding materials has attracted much attention. In order to obtain higher bonding reliability, a pressurization process is also used to bond the sintered materials.
[0003] On the other hand, semiconductor components are becoming thinner year by year. The thinning of semiconductor components may cause the semiconductor components to be damaged due to the pressurization process or the semiconductor components cannot be evenly bonded to the bonding material, resulting in uneven bonding. In addition, since the bonding area between the substrate on which the semiconductor chip is mounted and the base plate, heat sink, etc. is large, the above-mentioned bonding unevenness is easily generated.
[0004] In order to solve such a problem, the present applicant has previously proposed a pressurized bonding composition comprising metal powder and a solid reducing agent (see Patent Document 1). In this document, the compression rate ((AB) / A×100) calculated from the ratio of the thickness A of the coating obtained by drying the pressurized bonding composition in an atmospheric atmosphere to the thickness B of the sintered body obtained by calcining the composition in a nitrogen atmosphere is set within a specific range. This document states that, thereby, the conductors can be fully bonded to each other without being easily affected by the uneven thickness of the conductors to be bonded.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent document 1: EP3950185A1 Summary of the invention
[0008] In the field of power semiconductors, with the thinning and large-area of the above-mentioned joined bodies, it is more required than before to join these joined bodies with high reliability. In the joining process of the above-mentioned joined bodies, if the existing joining composition is used, the damage and uneven joining caused to the semiconductor element during joining will be more significant than before. For this reason, a joining composition with further improved joining performance compared to the joining composition described in the above-mentioned patent document 1 is required.
[0009] Therefore, an object of the present invention is to provide a copper paste for press bonding that can perform bonding with high strength and without causing bonding unevenness even when the bonded body is thin or has a large area.
[0010] The present invention provides a copper paste for press bonding, which contains at least two or more copper powders with different shapes and / or particle sizes and a solvent.
[0011] The copper paste has a viscosity at 25° C. of 10 Pa·s or more and 200 Pa·s or less,
[0012] The ratio of the total mass of the two or more copper powders to the mass of the copper paste is represented by A, the thickness of the coating film formed by applying the copper paste to the bonded body is represented by B,
[0013] The film thickness of the dried film formed by drying the coating film at 110° C. in an air atmosphere for 20 minutes is defined as C.
[0014] When the index H of bulkiness is set to H = C / (A×B),
[0015] A is 0.70 or more and less than 0.82, and H is 0.75 or more and 1.00 or less.
[0016] The present invention also provides a method for producing a copper paste for press bonding, comprising the steps of mixing two or more copper powders having different shapes and / or particle sizes with a solvent,
[0017] In the process, the shear rate of the copper paste is 10s -1 The viscosity value is adjusted to be 10 Pa·s or more and 200 Pa·s or less, and
[0018] The ratio of the total mass of the two or more copper powders having different shapes and / or particle sizes to the mass of the copper paste is defined as A.
[0019] The film thickness of the coating film formed by applying the copper paste to the bonded body is denoted as B.
[0020] The film thickness of the dried film formed by drying the coating film at 110° C. in an air atmosphere for 20 minutes is defined as C.
[0021] When the index H of bulkiness is set to H = C / (A×B),
[0022] A is adjusted to be greater than or equal to 0.70 and less than or equal to 0.82, and H is adjusted to be greater than or equal to 0.75 and less than or equal to 1.00. DETAILED DESCRIPTION
[0023] Hereinafter, the present invention will be described based on a preferred embodiment. The present invention relates to a copper paste for joining two joined bodies under a pressurized state. The "pressurization" described in this specification refers to intentionally applying a pressure of 0.001 MPa or more to the joined bodies from the outside of the parts. Therefore, pressurization consisting only of a pressure load caused by a change in atmospheric pressure or the dead weight of a part such as a joined body is not included in the "pressurization" described in this specification.
[0024] The copper powder contained in the copper paste of the present invention includes both pure copper powder and copper-based alloy powder. The copper powder contained in the copper paste may be pure copper powder only, copper-based alloy powder only, or a mixed powder of pure copper powder and copper-based alloy powder. In addition, the copper paste may contain a small amount of metal powder other than copper powder within a range that does not impair the effect of the present invention.
[0025] The copper paste of the present invention preferably contains two or more copper powders having different shapes and / or particle sizes. The shapes of the copper particles constituting the two or more copper powders are not particularly limited, and any spherical or non-spherical shape can be used.
[0026] It should be noted that, in the present invention, when two or more types of copper powders include two or more types of spherical copper particles, the D SEM50 In the case where the two or more copper powders include two or more non-spherical copper particles, the D 50 In addition, when two or more types of copper powders include spherical copper particles and non-spherical copper particles, the D SEM50 and the D of the non-spherical copper particles 50 It is preferably within the range described below.
[0027] The copper particles are spherical when the circularity coefficient measured by the following method is 0.85 or more. The circularity coefficient is calculated by the following method. That is, when a scanning electron microscope image of a copper particle of a primary particle is taken, and the area of the two-dimensional projection image of the copper particle is set to S and the perimeter length is set to L, the circularity coefficient is calculated by the formula 4πS / L 2 Calculate the circularity coefficient of the copper particles.
[0028] On the other hand, the copper particles being non-spherical means that the circularity coefficient is less than 0.85.
[0029] As a specific example of non-spherical, flat, hexahedral and octahedral polyhedral shapes, spindle-shaped, irregular shapes and the like can be listed. In the present invention, it is preferred that any one of the two or more copper powders is a flat copper particle, and it is more preferred that it contains flat copper particles and spherical copper particles as described below. It should be noted that in the present invention, flat refers to a shape having a pair of plate surfaces forming the main surface of the particles and side surfaces perpendicular to these plate surfaces, and the plate surface and the side surface can be independently a plane, a curved surface or a concave-convex surface.
[0030] By including flat copper particles as a material constituting two or more copper powders, cracks can be effectively suppressed in a dry coating or sintered body formed by the copper paste of the present invention. In addition, the bulkiness of the dry coating obtained when the copper paste of the present invention is applied to a body to be joined and dried can be increased. The advantages of increasing the bulkiness of the dry coating will be discussed later.
[0031] In addition, by including spherical copper particles as a material constituting two or more types of copper powder, the sinterability of the copper paste of the present invention can be improved.
[0032] When the copper powder is composed of spherical copper particles, the particle size of the copper powder is defined as the cumulative volume particle size D at a cumulative volume of 50% by volume obtained by the following measurement method: SEM50 That is, using an image observed by a scanning electron microscope in the range of 10,000 times or more and 150,000 times or less, 50 or more primary copper particles with clear outlines are selected and the Heywood diameter of each particle is measured. Next, the volume of the particle when it is assumed to be a sphere is calculated based on the obtained Heywood diameter, and the volume cumulative particle diameter D at 50% of the cumulative volume of the volume is calculated. SEM50 .
[0033] D of copper powder composed of spherical copper particles SEM50 It is preferably 60 nm or more and 300 nm or less. SEM50 Within the above range, excessive sintering of the copper paste and cracking of the sintered body are suppressed, and the strength and shape retention of the sintered body are improved. SEM50 The diameter is more preferably 70 nm or more and 270 nm or less, and still more preferably 80 nm or more and 250 nm or less.
[0034] It should be noted that when two or more copper powders contain two types of spherical copper particles, D SEM50 Small spherical copper particles D SEM50 Preferably, D SEM50 D of large spherical copper particles SEM50 It is preferably 1 μm or more and 10 μm or less.
[0035] When the copper powder is composed of non-spherical copper particles, the particle size of the copper powder is defined as the volume cumulative particle size D at a cumulative volume of 50% by volume determined by a laser diffraction scattering particle size distribution measurement method. 50 . For example, it can be performed by the following method. That is, 0.1 g of the test sample and the dispersant aqueous solution are mixed and dispersed for 1 minute using an ultrasonic homogenizer (US-300T manufactured by Nippon Seiki Co., Ltd.). Then, D is calculated by measuring the particle size distribution using, for example, MT3300 EXII manufactured by Microchip Biotech Co., Ltd. as a laser diffraction scattering particle size distribution measuring device. 50 .
[0036] D of copper powder composed of non-spherical copper particles 50 It is preferably 0.1 μm or more and 50 μm or less, more preferably 0.5 μm or more and 40 μm or less, and still more preferably 1 μm or more and 20 μm or less. 50 Within the above range, a dense sintered bonding layer can be easily obtained when the copper paste is formed into a coating film and then fired, and high bonding strength between bonded bodies and improved electrical conductivity reliability can be achieved.
[0037] It should be noted that, as described above, when two or more copper powders contain two or more non-spherical copper particles, the D 50 Preferably in the above D 50 The range is different.
[0038] When the non-spherical copper particles are flat copper particles, their shapes can also be quantitatively expressed by the following method.
[0039] That is, the ratio of the length of the major axis a to the length of the minor axis b of the flat copper particle (hereinafter also referred to as aspect ratio (a / b)) is preferably 2 or more, preferably 5 or more. The aspect ratio is preferably 80 or less, more preferably 40 or less.
[0040] In addition, the length of the major axis a of the flat copper particles is preferably 1 μm or more and 50 μm or less, more preferably 1.5 μm or more and 40 μm or less, and particularly preferably 2 μm or more and 30 μm or less. When the flat copper particles have the above-mentioned shape, it becomes easy to obtain a dense sintered bonding layer when the copper paste is formed into a coating film and baked, and it is possible to achieve high bonding strength between the bonded bodies and improve the reliability of the bonding portion.
[0041] The lengths of the major axis a and the minor axis b of the flat copper particles are obtained as follows. That is, a scanning electron microscope is used to obtain an observation image obtained in a range of 500 times or more and 50,000 times or less to obtain a photographic image of a flat copper particle with a clear outline, and the photographic image is analyzed. Specifically, when the imaginary circumscribed rectangle of each two-dimensional projection image is considered while rotating 360 degrees in a direction horizontal to the plate surface, the long side of the circumscribed rectangle where one side of the circumscribed rectangle reaches the maximum is set as the major axis a. On the other hand, when the particles of the measured object are rotated 360 degrees in a direction perpendicular to the plate surface while considering the imaginary circumscribed rectangle of each two-dimensional projection image, the short side of the circumscribed rectangle where one side of the circumscribed rectangle reaches the maximum is set as the short axis b. Similarly, more than 50 of the particles are randomly selected, and the major axis a and the minor axis b are measured respectively to obtain their arithmetic mean. Image analysis is performed, for example, using the image analysis particle size distribution software Mac-view manufactured by Mountech.
[0042] When the copper powder contained in the copper paste of the present invention comprises spherical copper particles and non-spherical copper particles, it is preferred that the copper powder is SEM50 The copper powder (first copper powder) having a diameter of 60 nm or more and 300 nm or less and D 50 It is composed of copper powder (second copper powder) having a particle size of 0.1 μm or more and 50 μm or less.
[0043] By including D SEM50 The first copper powder having a diameter of 60 nm or more and 300 nm or less suppresses over-sintering of the copper paste and cracking of the sintered body, and improves the strength and shape retention of the sintered body. 50 The second copper powder having a diameter of 0.1 μm or more and 50 μm or less can improve the sinterability of the copper paste and increase the strength of a sintered body obtained by firing.
[0044] In particular, the first copper powder is preferably composed of spherical copper particles and the second copper powder is preferably composed of flat copper particles because the sinterability of the copper paste can be further improved and the bonding strength between the sintered body obtained by firing and the bonded body can be further improved.
[0045] From the perspective of improving sinterability, the copper powder contained in the copper paste of the present invention preferably has controlled crystallinity. The degree of crystallinity of the copper powder can be evaluated using the crystallite size as a scale. Specifically, with respect to the crystallite size of the copper particles constituting the copper powder, the crystallite size of the (111) plane is preferably less than 100 nm, more preferably less than 70 nm, and further preferably less than 50 nm. By setting the crystallite size to this range, when the copper paste containing the copper powder is roasted, sintering can occur at a low temperature, and the bonding strength between the sintered body and the body to be bonded can be easily improved.
[0046] In at least one of the two or more copper powders contained in the copper paste of the present invention, when the crystallite size at 100°C measured by high temperature X-ray diffraction is set to D and the crystallite size at 300°C is set to E, E / D is preferably greater than 1.1, more preferably greater than 1.2.
[0047] When E / D is 1.1 or more, the sinterability of the copper particles during heat treatment becomes high, and the strength of the sintered body and the body to be joined can be sufficiently ensured.
[0048] The crystallite size of the copper particles is calculated using the Scherrer equation by analyzing an X-ray diffraction pattern obtained by XRD measurement based on a high temperature XRD (powder X-ray diffraction) method.
[0049] The high temperature XRD method is a method of placing a sample in a high temperature unit that can heat the sample to be measured, and performing XRD measurement while gradually heating it. XRD measurement is performed using a fully automatic horizontal multi-purpose X-ray diffraction device manufactured by Rigaku Corporation and a high-speed two-dimensional X-ray detector PILATUS100K / R manufactured by the same company as a detector. The measurement conditions of the X-ray diffraction pattern are as follows.
[0050] Optical system: parallel beam
[0051] X-ray source: CuKα rays
[0052] Measurement mode: Still mode 2θ = 42° fixed (using the above two-dimensional detector, the X-ray diffraction intensity equivalent to 2θ = 38 to 48° can be obtained)
[0053] Exposure time: 60 seconds
[0054] Collimator: Φ0.2mm
[0055] Measurement atmosphere: Nitrogen
[0056] Measuring temperature: 100, 300℃
[0057] Heating rate: 10℃ / min
[0058] During the XRD measurement at each measurement temperature (exposure time: 60 seconds), the measurement temperature was maintained without being increased.
[0059] Next, the crystallite size was calculated from the half-value width of the X-ray diffraction pattern of the crystal plane (111) of the copper particles obtained by the above XRD measurement using the following Scherrer equation.
[0060] Scherrer formula: D = Kλ / βcosθ
[0061] D: Crystallite size
[0062] K: Scherrer constant (0.94)
[0063] λ: wavelength of X-rays
[0064] β: Half-value width [rad]
[0065] θ: Bragg angle [rad]
[0066] When the two or more copper powders contained in the copper paste of the present invention include D SEM50 Spherical copper particles with a diameter of 60 nm or more and 300 nm or less and D 50 In the case of non-spherical copper particles having a diameter of 0.1 μm or more and 50 μm or less, at least one type of copper particles preferably satisfies the above E / D value, and two types of copper particles more preferably satisfy the above E / D value.
[0067] Examples of the copper powder having such crystallinity include CH-0200 and CH-0200L1 manufactured by Mitsui Mining & Smelting Co., Ltd.
[0068] An organic surface treatment agent may be applied to the surface of the copper particles constituting the copper powder contained in the copper paste. The organic surface treatment agent is a treatment agent for preventing excessive aggregation and oxidation of the copper particles. For this purpose, various fatty acids, aliphatic amines, and complexing agents having affinity for copper are preferably used in the present invention. In particular, from the perspective of preventing excessive aggregation of copper particles, it is preferred to use a saturated or unsaturated fatty acid or aliphatic amine having 6 to 18 carbon atoms, particularly 10 to 18 carbon atoms.
[0069] Specific examples of such fatty acids or aliphatic amines include benzoic acid, valeric acid, caproic acid, caprylic acid, nonanoic acid, capric acid, lauric acid, palmitic acid, oleic acid, stearic acid, amylamine, hexylamine, octylamine, decylamine, laurylamine, oleylamine, stearylamine, etc. In addition, as complexing agents having affinity for copper, for example, amino acids such as glycine and dimethylglyoxime, etc., can be listed. These fatty acids, aliphatic amines and complexing agents can be used alone or in combination of two or more.
[0070] The mass ratio A of the total mass of the two or more copper powders of the present invention to the mass of the copper paste is preferably 0.60 or more and less than 0.82, more preferably 0.65 or more and 0.80 or less, and further preferably 0.70 or more and 0.78 or less. By setting A to 0.60 or more, the viscosity required when the copper paste is applied to the body to be joined can be ensured, and the shape of the coating film after application can be properly maintained. In addition, by setting A to less than 0.82, it can work together with the index H of the bulkiness described later to achieve high strength and uneven joining.
[0071] The copper powder contained in the copper paste can be produced by various methods known in the art. For example, the copper powder can be produced by a wet reduction method, an atomization method, an electrolysis method, etc. The method to be used can be appropriately selected according to the particle size and shape of the copper powder.
[0072] Next, the solvent contained in the copper paste of the present invention is described. As a solvent, solvents similar to those used so far in the technical field of conductive compositions containing metal powders can be used without particular limitation. As such solvents, for example, monohydric alcohols, polyols, polyol alkyl ethers, polyol aryl ethers, polyethers, esters, nitrogen-containing heterocyclic compounds, amides, amines, terpene alcohols, ketones and saturated hydrocarbons can be listed. These solvents can be used alone or in combination of two or more. Among them, from the perspective of low reactivity and difficulty in side reactions during roasting and the perspective of well dissolving other components described later, polyols such as polyethers such as polyethylene glycol and polypropylene glycol, ethylene glycol, propylene glycol, and hexylene glycol are preferably used. From the same perspective, when polyethylene glycol is used as a solvent, its number average molecular weight is preferably 600 or less.
[0073] The boiling point of the solvent is preferably 180°C or more and 300°C or less, more preferably 185°C or more and 290°C or less, and particularly preferably 190°C or more and 280°C or less. By having a boiling point of 180°C or more, when the copper paste of the present invention is applied to the body to be joined, the solvent can remain on the body to be joined for a sufficient time. Thus, the index H of the fluffiness described later can be easily set to an appropriate value. On the other hand, by having a boiling point of 300°C or less, after the copper paste of the present invention is applied to the body to be joined, the solvent can be easily removed by heating and drying.
[0074] In addition to the above-mentioned two or more copper powders and solvents, other ingredients may be mixed in the copper paste of the present invention. As such ingredients, for example, a binder component, a surface tension adjuster, a defoamer, a viscoelasticity adjuster, a reducing agent, etc. may be listed. The proportion of other ingredients is preferably such that the total amount thereof is 0.01 mass parts or more and 10 mass parts or less relative to 100 mass parts of copper powder, and more preferably 0.1 mass parts or more and 8 mass parts or less.
[0075] As the reducing agent, a reducing agent that promotes the sintering of copper particles is preferred, and examples thereof include monohydric alcohols, polyhydric alcohols, amino alcohols, citric acid, oxalic acid, formic acid, ascorbic acid, aldehydes, hydrazine and its derivatives, hydroxylamine and its derivatives, dithiothreitol, phosphites, dihydrogen phosphates, phosphorous acid and its derivatives, and the like.
[0076] The viscosity of the copper paste for press bonding can be measured using a rheometer MARSIII manufactured by Thermo Scientific. From the perspective of improving the coating and printing properties of the copper paste for press bonding, the shear rate is 10 s-1 The viscosity value at the time of φ is preferably 10 Pa·s or more and 200 Pa·s or less, and more preferably 15 Pa·s or more and 200 Pa·s or less. The measurement conditions of the viscosity of the copper paste for press bonding are as follows.
[0077] Measurement mode: Shear rate dependent measurement
[0078] Sensor: Parallel type (Φ20mm)
[0079] Measurement temperature: 25℃
[0080] Gap: 0.300mm
[0081] Shear speed: 0.05~120.0s -1
[0082] Measurement time: 2 minutes
[0083] In order to set the shear rate of the copper paste for press bonding within the above range, the particle size of each copper powder, the concentration of the copper powder, the type of the solvent, etc. may be adjusted in the step of mixing the copper powder and the solvent.
[0084] One of the characteristics of the copper paste for press bonding of the present invention is that the content of two or more copper powders contained in the copper paste, the film thickness of the coating formed by applying the copper paste to the body to be bonded, and the film thickness of the dry coating formed by drying the coating have a prescribed relationship. Specifically, the ratio of the total mass of the two or more copper powders to the mass of the copper paste is set to A, the film thickness of the coating formed by applying the copper paste for press bonding containing at least two or more copper powders and a solvent to the body to be bonded is set to B (μm), the film thickness of the dry coating formed by drying the coating at 110°C for 20 minutes in an atmospheric atmosphere is set to C (μm), and the index H of the bulkiness is set to H = C / (A×B). At this time, H is preferably greater than 0.75 and less than 1.00.
[0085] Since the copper paste for press-bonding of the present invention has the above-mentioned physical properties, the dry coating formed by applying the copper paste for press-bonding to the substrate or other body to be bonded and then drying it becomes a layer like a cushioning material with a fluffy structure. By press-bonding the bodies to be bonded to each other through such a dry coating, the bodies to be bonded can be fully bonded to each other without being easily affected by the uneven thickness of the bonding object, i.e., the body to be bonded. As a result, for example, even when the area of the body to be bonded is large or when press-bonding is performed on a thin body to be bonded such as a semiconductor element, the bodies to be bonded can be bonded to each other with high adhesion and stability without damaging the body to be bonded, and the bonding strength is high.
[0086] The coating method of the copper paste for press bonding of the present invention is not particularly limited, and examples thereof include screen printing, gravure printing, dispenser printing, reverse coating, and doctor blade methods.
[0087] The film thicknesses B and C of the coating film before and after drying can be measured by the following method.
[0088] The film thickness B and C can be measured in a non-contact state without being affected by the change in film thickness caused by the contact of the probe, for example, by using an interference microscope. Specifically, the copper paste for press bonding is applied to the center of a flat substrate (thickness 2 mm) to form a coating film of a size of 6 mm square. The film thickness B of the formed coating film is not particularly limited, and is usually set to 15 μm or more and 800 μm or less, more preferably 15 μm or more and 300 μm or less, and particularly preferably 15 μm or more and 150 μm or less.
[0089] For a substrate having a coating formed on one side, a non-contact surface profiler is used to scan from the substrate surface to the maximum height of the coating, and line profile analysis is performed on the scanning result to measure the film thickness B and C of the coating. The detailed measurement method is described in the following examples.
[0090] As a method for adjusting the index H of bulkiness, for example, there can be cited the appropriate selection of the type of copper particles. Specifically, when the copper paste contains flat copper particles and the aspect ratio of the flat copper particles is further increased, the index H of bulkiness tends to increase. In addition, even if the type of solvent is changed, the index H of bulkiness can be increased by intentionally agglomerating the copper particles contained.
[0091] The film thickness C of the dried coating is preferably 5 μm or more and 500 μm or less, more preferably 10 μm or more and 400 μm or less, further preferably 15 μm or more and 300 μm or less, and particularly preferably 15 μm or more and 130 μm or less, provided that it is less than the film thickness B of the coating before drying. The film thickness of the coating before and after drying can be appropriately adjusted according to, for example, the shape and content of the copper powder contained in the composition for forming these films, the type and content of the solvent, or the type and content of other components.
[0092] It should be noted that, when calculating the index H of bulkiness, the drying conditions of the coating film were 110° C. and 20 minutes in order to effectively volatilize the solvent while suppressing oxidation of the body to be joined.
[0093] The copper paste for pressurized bonding of the present invention can be used for bonding a body to be bonded with another body to be bonded. In particular, due to the high bonding strength obtained by using the copper paste for pressurized bonding of the present invention, it can be suitable for bonding a large-area body to be bonded or a thin body to be bonded. For example, it can be used for bonding a body to be bonded having a thickness of less than 10 times the film thickness C of the dry coating. In order to make better use of the feature that the copper paste for pressurized bonding of the present invention can be applied to bonding thin bodies to be bonded, the thickness of the body to be bonded is more preferably less than 10 times the film thickness C of the dry coating, and particularly preferably less than 8 times. In addition, in order to ensure sufficient bonding strength, it is preferably used for bonding a body to be bonded having a thickness of more than 1 times the film thickness C of the dry coating.
[0094] In a bonded body, a semiconductor element is bonded to a substrate by using the copper paste for press bonding of the present invention, i.e., a semiconductor device can be made by chip bonding. In a method for manufacturing a semiconductor device, a laminated body formed with a bonded body, the copper paste for press bonding of the present invention, and another bonded body is prepared in sequence, and the copper paste for press bonding is baked under a pressure of 0.1 MPa or more. In this manufacturing method, at least one of the bonded bodies includes a semiconductor element. For example, one of the bonded bodies is a semiconductor element, and the other is a substrate.
[0095] In particular, as described above, the copper paste for press bonding of the present invention is suitable for bonding thin bodies to be bonded, so the thickness of the semiconductor element bonded to the substrate is preferably 0.25 mm or less, more preferably 0.23 mm or less, and particularly preferably 0.20 mm or less. On the other hand, in order to ensure sufficient bonding strength, the thickness of the semiconductor element bonded to the substrate is preferably 0.03 mm or more.
[0096] Since the copper paste for press bonding of the present invention is suitable for bonding a large area of a bonded body, the paste of the present invention can be used, for example, for bonding substrates. Specifically, the copper paste for press bonding of the present invention can be used to bond a first substrate and a second substrate to form a semiconductor device, wherein the first substrate is provided with a substrate having a thickness greater than 25 mm. 2 From the perspective of the feature that the copper paste for press bonding of the present invention can be suitably used for bonding a large-area bonded body, the area of the semiconductor element mounted on the first substrate is more preferably larger than 30 mm. 2 .
[0097] The types of the first substrate and the second substrate are not particularly limited. Generally, it is preferred that the surfaces to be joined of the first substrate and the second substrate both contain metal. For example, a component having a surface composed of metal can be used as at least one of the first substrate and the second substrate. It should be noted that the "metal" here refers to a metal single substance that does not form a compound with other elements or an alloy of two or more metals. Examples of such metals include copper, silver, gold, aluminum, palladium, nickel, or an alloy composed of a combination of two or more of them.
[0098] When at least one of the first substrate and the second substrate is a component having a surface composed of metal, the surface composed of metal may be composed of one metal, or may be composed of two or more metals. When composed of two or more metals, the surface may be an alloy. The surface composed of metal is usually preferably a plane, but may sometimes be a curved surface.
[0099] Examples of the first substrate and the second substrate include an insulating substrate having a metal layer such as copper on the surface of a ceramic or aluminum nitride plate, etc. The second substrate may be a heat sink, and is preferably a heat sink.
[0100] The conditions for joining two objects to be joined using the copper paste of the present invention are, for example, as follows.
[0101] The heating temperature is preferably 200°C or higher and 350°C or lower, more preferably 210°C or higher and 330°C or lower, and further preferably 220°C or higher and 300°C or lower.
[0102] The pressure is preferably 0.1 MPa to 30 MPa, more preferably 1 MPa to 25 MPa, and even more preferably 3 MPa to 20 MPa.
[0103] The atmosphere may be an inert atmosphere, a reducing atmosphere or an oxidizing atmosphere. Examples of the inert atmosphere include nitrogen atmosphere, rare gas atmospheres such as argon or neon. From the perspective of economy, a nitrogen atmosphere is preferably used. Examples of the reducing atmosphere include hydrogen atmosphere, hydrogen atmosphere diluted with an inert gas, and the like. Examples of the oxidizing atmosphere include air atmosphere, and the like.
[0104] The heating time also depends on the application state of the pressure, but is preferably 0.5 minutes to 20 minutes, more preferably 1 minute to 15 minutes. In addition, the pressurization time is preferably 0.5 minutes to 20 minutes, more preferably 1 minute to 15 minutes.
[0105] In a bonded body obtained by using the copper paste of the present invention, for example, the above-mentioned semiconductor device, the bonding strength between two bonded bodies is sufficiently high, and the occurrence of bonding unevenness is suppressed.
[0106] Regarding the above-mentioned embodiment, the present invention further discloses the following copper paste for press bonding, semiconductor device, method for manufacturing the copper paste for press bonding, and method for manufacturing the semiconductor device.
[0107] [1] A copper paste for press bonding, comprising at least two or more copper powders having different shapes and / or particle sizes and a solvent.
[0108] The copper paste has a viscosity at 25° C. of 10 Pa·s or more and 200 Pa·s or less,
[0109] The ratio of the total mass of the two or more copper powders to the mass of the copper paste is represented by A, the thickness of the coating film formed by applying the copper paste to the bonded body is represented by B,
[0110] The film thickness of the dried film formed by drying the coating film at 110° C. in an air atmosphere for 20 minutes is defined as C.
[0111] When the index H of bulkiness is set to H = C / (A×B),
[0112] A is 0.60 or more and less than 0.82, and H is 0.75 or more and 1.00 or less.
[0113] [2] The copper paste for press bonding according to [1], wherein the two or more copper powders having different shapes and / or particle sizes include spherical copper particles and non-spherical copper particles,
[0114] The volume cumulative particle size D of the spherical copper particles at a cumulative volume of 50% by volume measured by image analysis using a scanning electron microscope SEM50 is greater than 60nm and less than 300nm,
[0115] The volume cumulative particle diameter D of the non-spherical copper particles at a cumulative volume of 50% by volume determined by laser diffraction scattering particle size distribution measurement method is: 50 It is not less than 0.1 μm and not more than 50 μm.
[0116] [3] The copper paste for press bonding according to [2], wherein the non-spherical copper particles are flat copper particles.
[0117] The length of the major axis a of the flat copper particles measured by image analysis using a scanning electron microscope is 1 μm or more and 50 μm or less.
[0118] [4] The copper paste for press bonding according to [2] or [3], wherein the non-spherical copper particles are flat copper particles.
[0119] The aspect ratio of the flat copper particles is 2 or more and 80 or less.
[0120] [5] A copper paste for press bonding according to any one of [1] to [4], wherein, in at least one of the two or more copper powders, when the crystallite size at 100°C measured by high temperature X-ray diffraction is set to D and the crystallite size at 300°C is set to E, E / D is greater than 1.1.
[0121] [6] The copper paste for press bonding according to any one of [1] to [5], which is used for bonding a body to be bonded having a thickness of 10 times or less of a film thickness C of the dry coating film.
[0122] [7] The copper paste for press bonding according to any one of [1] to [6], wherein the boiling point of the solvent is 180° C. or higher.
[0123] [8] A semiconductor device formed by bonding a semiconductor element having a thickness of 0.25 mm or less to a substrate using the copper paste for press bonding according to any one of [1] to [7].
[0124] [9] A semiconductor device, wherein a first substrate and a second substrate are bonded together using the copper paste for press bonding described in any one of [1] to [7], wherein the first substrate is provided with a 2 area of semiconductor components.
[0125]
[10] A method for manufacturing a semiconductor device, comprising the steps of: preparing a laminated body having a body to be bonded, the copper paste for press bonding according to any one of [1] to [7], and another body to be bonded formed in this order, and baking the copper paste for press bonding under a pressure of 0.1 MPa or more.
[0126] At least one of the bonded bodies includes a semiconductor element.
[0127]
[11] A method for producing a copper paste for press bonding, comprising the steps of mixing two or more copper powders having different shapes and / or particle sizes with a solvent,
[0128] In the process, the shear rate of the copper paste is 10s -1 The viscosity value is adjusted to be 10 Pa·s or more and 200 Pa·s or less, and
[0129] The ratio of the total mass of the two or more copper powders having different shapes and / or particle sizes to the mass of the copper paste is defined as A.
[0130] The thickness of the coating formed by applying the copper paste on the bonded body is B, the thickness of the dried coating formed by drying the coating at 110° C. for 20 minutes in an air atmosphere is C, and
[0131] When the index H of bulkiness is set to H = C / (A×B),
[0132] A is adjusted to be greater than or equal to 0.70 and less than or equal to 0.82, and H is adjusted to be greater than or equal to 0.75 and less than or equal to 1.00.
[0133] Example
[0134] Hereinafter, the present invention will be further described in detail by way of examples, but the scope of the present invention is not limited to these examples.
[0135] [Example 1]
[0136] (Preparation of copper paste)
[0137] Copper powder 1 (made by D SEM50 Copper powder composed of spherical copper particles with a diameter of 0.14 μm) and copper powder 2 (composed of D 50 A copper paste is prepared by mixing a copper powder mixture (copper powder 1: copper powder 2 = 70:30 (mass ratio) with a copper powder consisting of flat copper particles with a diameter of 7.1 μm, a length of the major axis a of 6.2 μm, and an aspect ratio of 22), a reducing agent (bis(2-hydroxyethyl)iminotris(hydroxymethyl)methane as an amino alcohol (hereinafter also referred to as "BIS-TRIS")) and a solvent (polyethylene glycol 300 and hexylene glycol). The mixing ratio of each component is shown in Table 1. The E / D of copper powder 1 is 1.1. The E / D of copper powder 2 is 1.0.
[0138] In the prepared copper paste, the mass ratio A of the copper powder mixture to the mass of the copper paste is 0.76. In addition, the shear rate is 10s -1 The viscosity of the copper paste at 25° C. is 33 Pa·s.
[0139] (Manufacture of bonding structure)
[0140] The copper paste was applied to the center of the copper substrate for packaging (thickness 2 mm) by screen printing to form a 6 mm square printed coating (hereinafter, also referred to as a "printed coating formed body"). The coating was dried at 110° C. for 20 minutes in an air atmosphere to remove the liquid medium to obtain a dried coating (hereinafter, also referred to as a "dried coating formed body").
[0141] Next, a silicon wafer (5 mm×5 mm, 0.2 mm thick, with a silver-plated layer as the surface to which the copper paste adheres) was placed on the dried coating film, and a pressure of 15 MPa was applied in this state, and baking was performed at 300°C for 10 minutes in a nitrogen atmosphere to produce a bonding structure.
[0142] [Example 2]
[0143] Use by D50 Copper powder 2 is composed of flat copper particles with a diameter of 4.9 μm, a length of the major axis a of 4.5 μm, and an aspect ratio of 13. The E / D of copper powder 2 is 1.0. In addition, diethylene glycol dibutyl ether is added to the solvent, and the content ratio of each solvent relative to 100 parts by mass of the mixture of copper powder is shown in Table 1. A copper paste is prepared in the same manner as in Example 1 except for the above. Shear rate 10 s -1 The viscosity of the copper paste at 25° C. was 19 Pa·s. A dried coating film was prepared under the same conditions as in Example 1, and a joint structure was prepared under the same conditions as in Example 1.
[0144] [Comparative Example 1]
[0145] Change copper powder 2 to D 50 The copper powder was composed of flat copper particles with a length of 4.9 μm, a length of the major axis a of 4.5 μm, and an aspect ratio of 13, and the content ratio of each solvent to 100 parts by mass of the copper powder mixture was set as shown in Table 1. A copper paste was prepared in the same manner as in Example 1. The ratio A of the mass of the copper powder mixture to the mass of the copper paste was 0.82, and the shear rate was 10 s -1 The viscosity of the copper paste for press bonding at 25° C. was 28 Pa·s. A dried coating film was prepared under the same conditions as in Example 1, and a bonded structure was prepared under the same conditions as in Example 1.
[0146] [Comparative Example 2]
[0147] In addition to changing copper powder 2 to D 50 A copper paste was prepared in the same manner as in Example 1 except that the copper powder was composed of flat copper particles having a diameter of 4.9 μm, a length of the major axis a of 4.5 μm, and an aspect ratio of 13. Shear rate 10 s -1 The viscosity of the copper paste for press bonding at 25° C. was 10 Pa·s. A dried coating film was prepared under the same conditions as in Example 1, and a bonded structure was prepared under the same conditions as in Example 1.
[0148] (Evaluation of Fluffiness)
[0149] For each example and each comparative example, a non-contact surface profiler (Zegage Pro manufactured by Zygo Corporation) was used to measure the film thickness B of the printed coating film and the film thickness C of the dried coating film. Using a 1.4x objective lens and a 1.0x zoom lens, observation was performed within a measurement field of 13.9 mm × 10.4 mm, and the film thickness of each coating film was measured based on the height difference between the surface of each coating film and the surface of the substrate.
[0150] That is, after selecting the measurement mode and placing the object to be measured (printed coating film formation and dried coating film formation of the embodiment and comparative example) on the stage, the vertical and horizontal directions are adjusted so that the coating film is in a roughly central position, and then the objective lens is moved in the height direction to focus on the substrate surface. The scanning start position in the height direction is set to Bottom, the scanning length is set to 500 μm, and the measurement is performed in the horizontal direction at a pitch of 6.3 μm in the vertical and horizontal directions.
[0151] The obtained measurement results are subjected to line profile analysis. Draw a line on the diagonal line of the coating film so that both ends of the line respectively include about 1 mm of the substrate surface (area where the coating film is not formed). By processing to make the heights of both ends of the line consistent, parallel correction of the substrate surface is performed. The film thickness of the coating film is obtained based on the height difference between the coating film surface and the substrate surface. The height measurement position of the substrate surface is set to a position 0.5 mm away from the edge of the coating film. The height measurement position of the coating film surface is set to the center point of the coating film, and the center point is set to the intersection of the two diagonal lines drawn on the square coating film. Using the following formula, the index H of fluffiness is calculated from the film thickness B of the obtained printed coating film, the film thickness C of the dried coating film, and the ratio A of the total mass of copper powder in the copper paste.
[0152] H=C / (A×B)
[0153] Table 2 shows the film thickness B, C and the value of the index H of bulkiness obtained in each Example and each Comparative Example.
[0154] (Evaluation of the bonding rate between sintered copper and chip)
[0155] For the bonding structure manufactured in each embodiment and each comparative example, a probe with a frequency of 75 MHz of an ultrasonic imaging device (FineSAT FS300 III manufactured by Hitachi High-Technologies) was used, and the bonding interface between the chip and the sintered copper was analyzed in the horizontal direction at a spacing of 20 μm in the vertical and horizontal directions by the reflection method to obtain an ultrasonic flaw detection image (SAT image). When observing the peeling state of the bonding layer, the gain value is set to a value of 25 to 35 dB, and then the delay and width of the S gate are adjusted so that the peak position of the S gate is on the surface of the copper substrate. In order to specify the observation range of the bonding layer, the delay of the F gate is adjusted and the width is set to a peak width corresponding to 1.5 wavelengths. The Z-axis coordinate of the probe is adjusted so that the amplitude of the observed peak is maximized for observation. The contrast of the observed image is adjusted using the automatic function.
[0156] In the obtained SAT image, the chip bonding area is binarized using image processing software (Image J), and the black area ratio (bonding rate; %) in the observed area is calculated. That is, after starting Image-J, select Analyze-Set measurement, and check Area, Area fraction, and Limit to Threshold. Then, select File-Open, open the image data for calculating the bonding rate, and specify the range (A) of the silicon chip mounting part in the image. Next, select Edit-Copy to system, copy the specified range (A), and select File-New-System clipboard to paste the image of the specified range (A). Then, in order to clarify the bonding part, select Image-Type-8bit, convert the image, and select Image-Adjust-Threshold to adjust the image threshold to 100. In addition, specify the black range (B) existing in the range (A) of the silicon chip mounting part in the adjusted image. The black range (B) is a range with a threshold value of less than 100 and can be regarded as a silicon chip bonding part. The bonding rate (%) is calculated by the area of (B) / the area of (A)×100. Table 2 shows the bonding ratio (%) obtained in each Example and each Comparative Example.
[0157] [Table 1]
[0158]
[0159] [Table 2]
[0160]
[0161] As can be seen from the results shown in Table 2, the bonded bodies produced using the copper pastes obtained in the examples can be bonded with high strength even when the bonded bodies are thin or have a large area.
[0162] Industrial Applicability
[0163] According to the present invention, there is provided a copper paste for press bonding that can perform bonding with high strength and without causing bonding unevenness even when the bonded body is thin or has a large area.
Claims
1. A copper paste for press bonding, comprising at least two or more copper powders having different shapes and / or particle sizes and a solvent, The copper paste has a viscosity at 25° C. of 10 Pa·s or more and 200 Pa·s or less, The ratio of the total mass of the two or more copper powders to the mass of the copper paste is defined as A. The film thickness of the coating film formed by applying the copper paste to the bonded body is denoted as B. The film thickness of the dried film formed by drying the coating film at 110° C. in an air atmosphere for 20 minutes is defined as C. When the index H of bulkiness is set to H = C / (A×B), A is 0.60 or more and less than 0.82, and H is 0.75 or more and 1.00 or less.
2. The copper paste for press bonding according to claim 1, wherein The two or more copper powders having different shapes and / or particle sizes include spherical copper particles and non-spherical copper particles. The volume cumulative particle size D of the spherical copper particles at a cumulative volume of 50% by volume measured by image analysis using a scanning electron microscope SEM50 is greater than 60nm and less than 300nm, The volume cumulative particle diameter D of the non-spherical copper particles at a cumulative volume of 50% by volume determined by laser diffraction scattering particle size distribution measurement method is: 50 It is not less than 0.1 μm and not more than 50 μm.
3. The copper paste for press bonding according to claim 2, wherein The non-spherical copper particles are flat copper particles. The length of the major axis a of the flat copper particles measured by image analysis using a scanning electron microscope is 1 μm or more and 50 μm or less.
4. The copper paste for press bonding according to claim 2 or 3, wherein The non-spherical copper particles are flat copper particles. The aspect ratio of the flat copper particles is 2 or more and 80 or less.
5. The copper paste for press bonding according to any one of claims 1 to 3, wherein In at least one of the two or more copper powders, when D is the crystallite size at 100° C. and E is the crystallite size at 300° C. measured by high temperature X-ray diffraction, E / D is 1.1 or more. 6 . The copper paste for press bonding according to claim 1 , which is used for bonding a body to be bonded having a thickness of 10 times or less of a film thickness C of the dry coating film.
7. The copper paste for press bonding according to any one of claims 1 to 3, wherein The boiling point of the solvent is 180° C. or higher. 8 . A semiconductor device, wherein a semiconductor element having a thickness of 0.25 mm or less and a substrate are bonded together using the copper paste for press bonding according to claim 1 .
9. A semiconductor device, wherein a first substrate and a second substrate are bonded together using the copper paste for press bonding according to any one of claims 1 to 3, wherein the first substrate is provided with a 2 area of semiconductor components.
10. A method for manufacturing a semiconductor device, comprising the steps of: preparing a laminated body in which a body to be bonded, the copper paste for press bonding according to any one of claims 1 to 3, and another body to be bonded are sequentially formed, and baking the copper paste for press bonding under a pressure of 0.1 MPa or more. At least one of the bonded bodies includes a semiconductor element.
11. A method for producing a copper paste for press bonding, comprising the steps of mixing two or more copper powders having different shapes and / or particle sizes with a solvent, In the process, the shear rate of the copper paste is 10s -1 The viscosity value is adjusted to be 10 Pa·s or more and 200 Pa·s or less, and The ratio of the total mass of the two or more copper powders having different shapes and / or particle sizes to the mass of the copper paste is defined as A. The film thickness of the coating film formed by applying the copper paste to the bonded body is denoted as B. The film thickness of the dried film formed by drying the coating film at 110° C. in an air atmosphere for 20 minutes is defined as C. When the index H of bulkiness is set to H = C / (A×B), A is adjusted to be greater than or equal to 0.60 and less than 0.82, and H is adjusted to be greater than or equal to 0.75 and less than or equal to 1.00.