Method for manufacturing printed circuit board

CN118743013APending Publication Date: 2024-10-01FUJIFILM CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202380022309.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-29
Filing Date
2023-03-07
Publication Date
2024-10-01

Smart Images

  • Figure CN118743013A_ABST
    Figure CN118743013A_ABST
Patent Text Reader

Abstract

Provided is a method for manufacturing a printed wiring board having excellent electromagnetic wave shielding layer coating properties and excellent electromagnetic shielding material characteristics. A method for manufacturing a printed wiring board, the printed wiring board having: a printed wiring board having a ground wire; at least one semiconductor device mounted in a region surrounded by the ground wire on the printed wiring board; an insulating layer that encloses at least one of the semiconductor devices, is disposed on the inside of the ground line, and has an inclined portion on the outer edge; and an electromagnetic wave shielding layer disposed on the insulating layer, the method including: performing a step of forming a layer by discharging insulating ink by inkjet multiple times on the printed wiring board on which the semiconductor device is mounted so as to laminate the layers; a step for forming a layer by stepwise reducing the outer edge of the discharge region of the insulating ink from the printed wiring board side so as to form the inclined portion, and forming an insulating layer having the inclined portion; and a step for forming an electromagnetic wave shielding layer by discharging a conductive ink on the insulating layer by inkjet.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a printed circuit board having a semiconductor device installed in an area surrounded by a grounding line on the printed circuit board, and more particularly, to a method for manufacturing a printed circuit board comprising: an insulating layer that embeds the semiconductor device and has an inclined portion; and an electromagnetic shielding layer that covers the insulating layer. Background Art

[0002] Semiconductor devices and the like may be prevented from operating normally due to electromagnetic interference, thereby causing failures. Furthermore, when semiconductor devices and the like generate electromagnetic waves, they may also cause electromagnetic interference to other semiconductor devices or electronic parts, thereby preventing normal operation.

[0003] Therefore, in order to avoid interference caused by electromagnetic waves from other electronic devices or to avoid electromagnetic interference to other electronic devices, it is necessary to shield electromagnetic waves. Usually, electromagnetic waves are shielded by covering the object to be shielded, such as semiconductor devices, with a shielding cover. The shielding cover has problems such as thick film thickness, heavy weight, and low degree of freedom in setting, and a technology to replace the shielding cover is required. For example, an electromagnetic shielding member is formed by stacking an insulating layer and an electromagnetic wave shielding layer on a printed circuit board on which a semiconductor device is mounted.

[0004] For example, Patent Document 1 describes a method for manufacturing a printed circuit board having an electromagnetically shielded track using an inkjet printer. In Patent Document 1, the method is implemented as follows: a printed circuit board having an electromagnetically shielded track is formed using a first inkjet print head and a second print head, an insulating resin ink forms a sleeve around the conductive track, a first metallic ink forms a shielding sleeve around the insulating resin sleeve, and / or a frame is formed around the conductive track, and the first metallic ink forms a shielding capsule around the insulating resin frame.

[0005] Previous technical literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2019-527463 Summary of the invention

[0008] Technical issues to be solved by the invention

[0009] In the method for producing a printed circuit board using an inkjet printer described in Patent Document 1, the covering property of the electromagnetic wave shielding layer is poor, and as a result, the electromagnetic shielding material characteristics are also poor, and improvement is required.

[0010] An object of the present invention is to solve the problems of the conventional techniques and to provide a method for producing a printed wiring board having excellent covering properties of an electromagnetic wave shielding layer and excellent electromagnetic shielding material characteristics.

[0011] Means for solving technical problems

[0012] In order to achieve the above-mentioned purpose, the invention [1] is a method for manufacturing a printed circuit board as follows, which comprises: a printed circuit board having a grounding wire; at least one semiconductor device mounted on an area of ​​the printed circuit board surrounded by the grounding wire; an insulating layer, which embeds at least one of the semiconductor devices, is arranged in the area surrounded by the grounding wire and has an inclined portion at the outer edge; and an electromagnetic wave shielding layer, which is arranged on the insulating layer, the method for manufacturing the printed circuit board comprising: a process of stacking layers by performing a process of forming layers by ejecting insulating ink by inkjet multiple times on a printed circuit board on which semiconductor devices are mounted, a process of forming an insulating layer having an inclined portion by gradually reducing the outer edge of the ejection area of ​​the insulating ink in a manner that forms an inclined portion; and a process of forming an electromagnetic wave shielding layer on the insulating layer by ejecting conductive ink by inkjet.

[0013] Invention [2] is a method for manufacturing a printed circuit board according to invention [1], wherein:

[0014] The shortest distance between the semiconductor device and the ground wire is 0.2 to 1.0 mm.

[0015] Invention [3] is a method for manufacturing a printed circuit board according to invention [1] or [2], wherein:

[0016] The maximum angle of the inclined portion is 85° or less.

[0017] Invention [4] is a method for manufacturing a printed wiring board according to any one of Inventions [1] to [3], wherein:

[0018] The maximum angle of the inclined portion is 75° or less.

[0019] Invention [5] is a method for manufacturing a printed circuit board according to any one of Inventions [1] to [4], wherein:

[0020] The semiconductor device has a side surface perpendicular to a surface of the printed wiring board, and has a height of 0.5 mm or more from the surface of the printed wiring board.

[0021] Effects of the Invention

[0022] According to the present invention, it is possible to provide a method for producing a printed wiring board having excellent covering properties of an electromagnetic wave shielding layer and excellent electromagnetic shielding material characteristics. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1This is a schematic plan view showing one step of the first example of the method for manufacturing a printed wiring board according to the embodiment of the present invention.

[0024] Figure 2 This is a schematic plan view showing one step of the first example of the method for manufacturing a printed wiring board according to the embodiment of the present invention.

[0025] Figure 3 This is a schematic plan view showing one step of the first example of the method for manufacturing a printed wiring board according to the embodiment of the present invention.

[0026] Figure 4 This is a schematic cross-sectional view showing one step of the first example of the method for manufacturing a printed wiring board according to the embodiment of the present invention.

[0027] Figure 5 This is a schematic cross-sectional view showing one step of the first example of the method for manufacturing a printed wiring board according to the embodiment of the present invention.

[0028] Figure 6 This is a schematic cross-sectional view showing one step of the first example of the method for manufacturing a printed wiring board according to the embodiment of the present invention.

[0029] Figure 7 This is a schematic perspective view showing an example of a printed image for forming an insulating layer in the method for manufacturing a printed wiring board according to the embodiment of the present invention.

[0030] Figure 8 This is a schematic cross-sectional view showing one step of an example of a method for forming an insulating layer in a method for manufacturing a printed wiring board according to an embodiment of the present invention.

[0031] Fig. 9 This is a schematic cross-sectional view showing one step of an example of a method for forming an insulating layer in a method for manufacturing a printed wiring board according to an embodiment of the present invention.

[0032] Fig.10 This is a schematic cross-sectional view showing one step of an example of a method for forming an insulating layer in a method for manufacturing a printed wiring board according to an embodiment of the present invention.

[0033] Fig.11 This is a schematic cross-sectional view showing one step of an example of a method for forming an insulating layer in a method for manufacturing a printed wiring board according to an embodiment of the present invention.

[0034] Fig.12 This is a schematic plan view showing one step of the second example of the method for manufacturing a printed wiring board according to the embodiment of the present invention.

[0035] Fig.13This is a schematic plan view showing one step of the second example of the method for manufacturing a printed wiring board according to the embodiment of the present invention.

[0036] Fig.14 This is a schematic plan view showing one step of the second example of the method for manufacturing a printed wiring board according to the embodiment of the present invention.

[0037] Fig.15 This is a schematic cross-sectional view showing one step of the second example of the method for manufacturing a printed wiring board according to the embodiment of the present invention.

[0038] Fig.16 This is a schematic cross-sectional view showing one step of the second example of the method for manufacturing a printed wiring board according to the embodiment of the present invention.

[0039] Fig.17 This is a schematic cross-sectional view showing one step of the second example of the method for manufacturing a printed wiring board according to the embodiment of the present invention.

[0040] Fig.18 It is a schematic diagram showing another example of the insulating layer structure of the printed wiring board according to the embodiment of the present invention. DETAILED DESCRIPTION

[0041] Hereinafter, a method for manufacturing a printed wiring board of the present invention will be described in detail based on preferred embodiments shown in the drawings.

[0042] In addition, the drawings described below are exemplary drawings for explaining the present invention, and the present invention is not limited to the drawings shown below.

[0043] In addition, the following "to" indicating a numerical range means that the numerical values ​​described on both sides are included. For example, ε is the numerical value ε. to the numerical value εβ means that the range of ε is a range including the numerical values ​​ε. and the numerical value εβ, and when expressed in mathematical notation, it is ε. ≤ε≤εβ.

[0044] “Angles expressed by specific numerical values,” “parallel,” “perpendicular,” and the like, unless otherwise specified, include an error range generally permitted in the relevant technical field.

[0045] Furthermore, unless otherwise specified, the temperature and time are within the error range generally allowed in the corresponding technical field.

[0046] "Process" includes not only independent processes but also processes that cannot be clearly distinguished from other processes as long as the process performs its intended function.

[0047] In the present specification, when a plurality of substances corresponding to each component are present in a composition, the amount of each component in the composition means the total amount of the plurality of substances present in the composition unless otherwise specified.

[0048] In addition, unless otherwise specified, inkjet refers to an inkjet recording method.

[0049] [First Example of Method for Manufacturing Printed Wiring Board]

[0050] Figures 1 to 3 It is a schematic plan view showing a first example of a method for manufacturing a printed wiring board according to an embodiment of the present invention in order of steps. Figures 4 to 6 It is a schematic cross-sectional view showing a first example of a method for manufacturing a printed wiring board according to an embodiment of the present invention in order of steps. Figure 1 and Figure 4 , Figure 2 and Figure 5 , Figure 3 and Figure 6 Indicates the same process.

[0051] exist Figures 1 to 6 In FIG. 1 , the ground line 12 is arranged in a quadrilateral shape on the surface 10a of the printed wiring board 10. Although the example in which one semiconductor device 14 is mounted in the region D surrounded by the ground line 12 is described, the present invention is not limited to this structure.

[0052] like Figure 1 and Figure 4 As shown, the printed wiring board 10 having the semiconductor device 14 mounted in the region D surrounded by the ground line 12 is also referred to as the processing substrate 11. Although not shown, in addition to the semiconductor device 14, various circuits, electronic parts, and electronic components are mounted on the printed wiring board 10.

[0053] Then, if Figure 2 and Figure 5 As shown, for Figure 1 and Figure 4 The illustrated processing substrate 11 has an insulating layer 16 that embeds a semiconductor device 14 and is disposed in a region D surrounded by a ground line 12 and has an inclined portion 16 b at an outer edge 16 c.

[0054] In the process of forming the insulating layer 16, a process of forming a layer (not shown) by ejecting insulating ink (not shown) by inkjet is performed multiple times on the surface 10a of the printed wiring board 10 on which the semiconductor device 14 is mounted, and when the layers are stacked, the outer edge of the ejection area of ​​the insulating ink is gradually reduced so as to form the inclined portion 16b, and the insulating layer 16 having the inclined portion 16b is formed. The process of forming the insulating layer 16 will be described in more detail below.

[0055] After forming the insulating layer 16 on the processing substrate 11, as shown in FIG. Figure 3 and Figure 6As shown, on the insulating layer 16 having the inclined portion 16b, an electromagnetic wave shielding layer 18 having conductivity is formed by ejecting a conductive ink (not shown) by inkjet. The electromagnetic wave shielding layer 18 covers the entire surface of the insulating layer 16 and is connected to the grounding line 12. The electromagnetic wave shielding layer 18 is in a state of being electrically connected to the grounding line 12. In this way, the printed circuit board 20 is manufactured.

[0056] The printed circuit board 20 comprises: a printed wiring board 10 having a grounding wire 12; a semiconductor device 14 mounted on the printed wiring board 10 in an area D surrounded by the grounding wire 12; an insulating layer 16 encapsulating the semiconductor device 14, arranged in the area D surrounded by the grounding wire 12, and having an inclined portion 16b at the outer edge 16c; and an electromagnetic wave shielding layer 18 arranged on the insulating layer 16.

[0057] In the method for manufacturing the printed circuit board 20, in a structure formed by stacking an insulating layer 16 and an electromagnetic wave shielding layer 18 in a region D surrounded by a ground line 12 on a surface 10a of the printed wiring board 10 on which a semiconductor device 14 is mounted, in order to improve electromagnetic wave shielding properties, the electromagnetic wave shielding layer 18 requires covering properties of the insulating layer 16 and needs to be attached to the side surfaces of the insulating layer 16. In an inkjet recording method for forming the electromagnetic wave shielding layer 18 by ejecting conductive ink from the upper portion of the insulating layer 16, in the case of an insulating layer that does not have an inclined portion and is configured in a thin manner to cover the semiconductor device 14, it is difficult to apply conductive ink to the side surfaces of the inclined portion that does not have the insulating layer.

[0058] If the side surface 14c of the semiconductor device 14 having a height is vertical, the conductive ink is not easy to adhere in the inkjet recording method, resulting in a decrease in electromagnetic wave shielding performance. By providing the insulating layer 16 with the inclined portion 16b to improve the adhesion of the conductive ink to the insulating layer 16, the formed electromagnetic wave shielding layer 18 can have excellent covering properties. As a result, the surface defects of the electromagnetic wave shielding layer 18 can be reduced, and the electromagnetic wave shielding performance can be improved.

[0059] (Method for Forming Insulating Layer)

[0060] Next, the process of forming the insulating layer 16 will be described in more detail.

[0061] As described above, the insulating layer 16 is formed by performing a process of forming a layer by ejecting insulating ink by inkjet multiple times, and has a multilayer structure in which multiple layers are stacked. When forming the insulating layer 16, multiple layers need to be set in advance. In addition, the number of layers used to form the insulating layer 16 is not particularly limited, and is, for example, 2 to 7 layers.

[0062] As a method of setting the above-mentioned multiple layers, for example, multiple layers are set by dividing the insulating layer 16 into multiple layers having thicknesses in a direction Y perpendicular to the surface 10a of the printed wiring board 10. Each layer is a layer obtained by cutting the insulating layer 16 along a direction X parallel to the surface 10a of the printed wiring board 10.

[0063] Regarding each layer, an image of the printed wiring board 10 representing each layer is set when viewed from the surface 10a side, and this image is used as a printed image. The image portion of the printed image is used as the ejection area, and each layer is formed by applying it using an insulating ink by inkjet. As described above, since each layer has a thickness along the direction Y, the layer is formed by using one printed image and repeating the process of applying the insulating ink multiple times. In addition, in the case where the insulating layer 16 is divided into a very large number of layers, it is necessary to prepare printed images divided into several parts. The more the number of divisions of the insulating layer 16 is, the more accurately the insulating layer 16 can be formed, but the number of image data required when forming the insulating layer 16 also increases by that amount. Therefore, considering the production time of the image data prepared when forming the insulating layer 16, the number of divisions of the insulating layer 16 is appropriately determined.

[0064] Next, a method for obtaining a printed image of each layer constituting the insulating layer 16 is described. Figure 2 and Figure 5 The case of the insulating layer 16 shown will be described as an example.

[0065] First, the insulating layer 16 is formed. Figure 1 and Figure 4 The three-dimensional shape data of the processing substrate 11 is shown.

[0066] The method of acquiring the three-dimensional shape data is not particularly limited, and for example, a microscope or a three-dimensional scanner is used.

[0067] Next, slice data of the height of the printed wiring board 10 from the surface 10a in the direction Y is obtained from the three-dimensional shape data. At this time, the image is changed to a reverse image with the semiconductor device 14 as a white background. The above-mentioned process of changing to a reverse image as a white background is a process for removing the semiconductor device 14 from the discharge area of ​​the insulating ink.

[0068] When the insulating layer 16 is composed of four layers as described above, four printing images are required to set the ejection area of ​​the insulating ink ejected by the inkjet. Figure 7 The first image Im1 to the fourth image Im4 are shown.

[0069] When insulating layer 16 is composed of four layers, the four layers are the first layer, the second layer, the third layer, and the fourth layer from the printed wiring board 10 side.

[0070] in, Figure 7 This is a schematic perspective view showing an example of a printed image for forming an insulating layer in the method for manufacturing a printed wiring board according to the embodiment of the present invention.

[0071] The printed image representing the first layer in contact with the surface 10a of the printed wiring board 10 is set as the first image Im1 having an outer edge in contact with the ground line 12 (refer to Figure 7 ). The first image Im1 is not a solid image, but an image in which the semiconductor device 14 is a non-image portion NDm and the surroundings of the semiconductor device 14 are an image portion Dm. The image portion Dm of the first image Im1 is a discharge region of the insulating ink.

[0072] Next, a printed image representing the second layer is set on the first layer. The printed image representing the second layer is set as a second image Im2 (reference image Im2 ) whose outer edge is set closer to the side surface 14c of the semiconductor device 14 than the ground line 12. Figure 7 ). The second image Im2 is not a solid image like the first image Im1, but an image in which the semiconductor device 14 is a non-image portion NDm and the surrounding of the semiconductor device 14 is an image portion Dm. The outer edge of the second image Im2 is smaller than that of the first image Im1. That is, the outer edge of the image portion Dm is small, and the outer edge of the ejection area of ​​the insulating ink is smaller in the second image Im2 than in the first image Im1.

[0073] Next, a print image representing the third layer on the second layer is set. The print image representing the third layer is set as a third image Im3 (reference image Im3) whose outer edge is set closer to the side surface 14c of the semiconductor device 14 than the second image. Figure 7 ). The third image Im3 (reference Figure 7 ) is not a solid image like the first image Im1, but an image in which the semiconductor device 14 is a non-image portion NDm and the surrounding of the semiconductor device 14 is an image portion Dm. The outer edge of the third image Im3 is smaller than that of the second image Im2. That is, the outer edge of the image portion Dm is smaller, and the outer edge of the ejection area of ​​the insulating ink in the third image Im3 is smaller than that of the second image Im2.

[0074] Next, a printed image representing the fourth layer is set on the third layer. The fourth layer is a layer covering the upper surface 14a of the semiconductor device 14. The printed image representing the fourth layer is set as a fourth image Im4 (reference Figure 7). The fourth image is a solid image, and is an image in which the area covering the upper surface 14a of the semiconductor device 14 is set as the image portion Dm. The outer edge of the fourth image Im4 is smaller than that of the third image Im3. That is, the outer edge of the image portion Dm is small, and the outer edge of the ejection area of ​​the insulating ink is smaller in the fourth image Im4 than in the third image Im3.

[0075] In this way, the first image Im1 to the fourth image Im4 are set so that the outer edge of the discharge area of ​​the insulating ink is gradually reduced from the printed wiring board 10 side. In addition, the image portion Dm in the first image Im1 to the fourth image Im4 is set at Figure 1 Within the area D shown.

[0076] As mentioned above, Figure 7 The first to third images Im1 to Im3 shown have an image portion Dm which is a region where insulating ink is ejected and a non-image portion NDm which is a region where insulating ink is not ejected and corresponds to the semiconductor device 14 .

[0077] As described above, the fourth image Im4 is a solid image and is only the image portion Dm. The fourth image Im4 is used to discharge the insulating ink to the region covering the upper surface 14 a of the semiconductor device 14 .

[0078] The insulating layer 16 is formed using the image group 21 including the first image Im1 to the fourth image Im4 described above.

[0079] For use Figure 7 The steps of forming the insulating layer 16 in the first image Im1 to the fourth image Im4 shown will be described.

[0080] Figures 8 to 11 1 is a schematic cross-sectional view showing an example of a method for forming an insulating layer in a method for manufacturing a printed wiring board according to an embodiment of the present invention in order of steps. Figures 8 to 11 In, with Figures 1 to 6 The same structures as shown are denoted by the same symbols, and their detailed description is omitted.

[0081] First, an ejection area of ​​insulating ink by inkjet is set for each of the first image Im1 to the fourth image Im4. In addition, when forming the insulating layer and the electromagnetic wave shielding layer, the insulating ink and the conductive ink are ejected by inkjet using an inkjet recording device. The inkjet recording device stores the image information of the first image Im1 to the fourth image Im4 and sets the ejection position of the insulating ink for each image. In addition, the inkjet recording device also sets the ejection position of the conductive ink for the electromagnetic wave shielding layer in the same manner as the conductive layer.

[0082] Next, on the surface 10a of the printed wiring board 10, an insulating ink is ejected by inkjet in an ejection area corresponding to the image portion Dm of the first image Im1 to form Figure 8 The first layer 22 has a thickness in the direction Y. If the first layer 22 cannot be formed by applying the insulating ink only once based on the first image Im1, the application of the insulating ink by inkjet based on the first image Im1 is repeated until the thickness of the first layer 22 is reached.

[0083] After the first layer 22 is formed, insulating ink is ejected by inkjet to the ejection area corresponding to the image portion Dm of the second image Im2 on the surface 22a of the first layer 22, thereby forming Fig. 9 The second layer 24 is shown. The second layer 24 has a thickness in the direction Y similarly to the first layer 22. If the second layer 24 cannot be formed when the insulating ink is applied only once based on the second image Im2, the application of the insulating ink by inkjet based on the second image Im2 is repeated until the thickness of the second layer 24 is reached.

[0084] After the second layer 24 is formed, insulating ink is ejected by inkjet to the ejection area corresponding to the image portion of the third image Im3 on the surface 24a of the second layer 24, thereby forming Fig.10 The third layer 26. The third layer 26 has a thickness in the direction Y similarly to the first layer 22, and when the third layer 26 cannot be formed when the insulating ink is applied only once based on the third image Im3, the application of the insulating ink by inkjet based on the third image Im3 is repeatedly performed until the thickness of the third layer 26 is reached.

[0085] After the third layer 26 is formed, insulating ink is ejected by inkjet to the ejection area corresponding to the image portion Dm of the fourth image Im4 on the surface 26a of the third layer 26, thereby forming Fig.11 The fourth layer 28 is formed as described above. The fourth layer 28 has a thickness in the direction Y, similarly to the first layer 22. If the fourth layer 28 cannot be formed by applying the insulating ink only once based on the fourth image Im4, the application of the insulating ink by inkjet based on the fourth image Im4 is repeated until the thickness of the fourth layer 28 is reached. In addition, the fourth image Im4 is a solid image, and the fourth layer 28 is a solid film. In the above manner, the insulating layer 16 is formed.

[0086] The outer edge 22c of the first layer 22, the outer edge 24c of the second layer 24, the outer edge 26c of the third layer 26, and the outer edge 28c of the fourth layer 28 approach the side surface 14c of the semiconductor device 14, and the outer edge of the discharge area of ​​the insulating ink gradually decreases from the printed wiring board 10 side. That is, the first layer 22 to the fourth layer 28 are formed by gradually reducing the outer edges, thereby forming the insulating layer 16 with an inclined portion 16b.

[0087] Since the maximum angle of the inclined portion 16b of the insulating layer 16 is preferably 85° or less, and more preferably 75° or less, the position and thickness of the outer edge are preferably set so that the maximum angle of the inclined portion 16b is 85° or less. Based on the set first to fourth layers, the first to fourth images Im1 to Im4 are preferably set in the above-mentioned manner.

[0088] Furthermore, the length L of the inclined portion 16b of the insulating layer 16 (refer to Figure 5 ) relative to the thickness Tm of the insulating layer 16 (reference Figure 5 ) is preferably 1.004 to 2 times, more preferably 1.015 to 1.411 times, and further preferably 1.035 to 1.155 times.

[0089] In addition, the length L of the inclined portion 16b of the insulating layer 16 (refer to Figure 5 ) relative to the thickness Tm of the insulating layer 16 (reference Figure 5 ) and the angle θ of the inclined portion 16b are in the relationship L=Tm×cosecθ.

[0090] In order to form the insulating layer 16, the outer edge of the ejection area of ​​the insulating ink is gradually reduced to form each layer constituting the insulating layer, but the outer edge of the layer is gradually reduced from the printed wiring board side. In addition, the number of stages of the outer edge to be reduced can be 2 or more, preferably 3 or more, more preferably 4 or more, and further preferably 6 or more. If the number of stages of the outer edge of the layer to be reduced is large, the insulating layer 16 is formed using multiple layers, and the maximum angle of the inclined portion 16b of the formed insulating layer 16 can be reduced.

[0091] When the number of stages to be reduced is 2, for example, in the case of an insulating layer composed of 4 layers, after forming 2 layers of the same size, the outer edge of the ejection area of ​​the insulating ink can be reduced on the first 2 layers to form 2 layers of the same size. Also, after forming 3 layers of the same size, one layer can be formed on the first 2 layers by reducing the outer edge of the ejection area of ​​the insulating ink. Also, regarding the stage to be reduced, the outer edge of the ejection area of ​​the insulating ink can be reduced in sequence for each layer. For example, in the case of an insulating layer composed of 4 layers, the outer edge of the ejection area of ​​the insulating ink can be reduced for each layer.

[0092] [Second Example of Method for Manufacturing Printed Wiring Board]

[0093] Figures 12-14 It is a schematic plan view showing a second example of the method for manufacturing a printed wiring board according to an embodiment of the present invention in order of steps. Figure 15 to Figure 17 It is a schematic cross-sectional view showing a second example of the method for manufacturing a printed wiring board according to an embodiment of the present invention in order of steps. Figure 15 to Figure 17 Based on Figure 12 to Figure 14 The cross section of line AA. And, Fig.12 and Fig.15 , Fig.13 and Fig.16 , Fig.14 and Fig.17 They represent the same process.

[0094] In addition, Figure 12 to Figure 17 In, with Figures 1 to 6 The same structures as shown are denoted by the same symbols, and their detailed description is omitted.

[0095] Fig.12 The processing substrate 11 shown is Figure 1 The processing substrate 11 shown in FIG. 1 is different in the number of semiconductor devices mounted thereon, and the other structures are the same as those in FIG. Figure 1 The processing substrate 11 shown is the same.

[0096] exist Fig.12 In the illustrated processing substrate 11, a semiconductor device 15, a semiconductor device 17, a semiconductor device 30, and semiconductor devices 32a, 32b, and 32c are mounted in a region D on a surface 10a of a printed wiring board 10. In addition, although not shown in the figure, electronic components other than semiconductor components, such as capacitors, resistors, and coil components, are mounted in the region D. For example, the semiconductor device 15, the semiconductor device 17, the semiconductor device 30, and the semiconductor devices 32a, 32b, and 32c are different from each other, and a specific function is exerted by a plurality of semiconductor devices and electronic components.

[0097] In the semiconductor device 15 and the semiconductor device 17, as Fig.15 As shown, semiconductor device 17 is taller.

[0098] Then, if Fig.13 and Fig.16 As shown, a slanted portion 16b (reference Fig.16 ) insulating layer 16.

[0099] Since the method for forming the insulating layer 16 is as described above, its detailed description is omitted. Schematically, the data of the three-dimensional shape of the processing substrate 11 is acquired to obtain slice data. The number of layers for forming the insulating layer 16 and the thickness of each layer in the direction Y are set. A printed image of the set number of layers is obtained from the slice data. Based on the printed image representing each layer, each layer is formed by ejecting insulating ink by inkjet, thereby forming the insulating layer 16.

[0100] Then, if Fig.14 and Fig.17As shown, the electromagnetic shielding layer 18 is formed by ejecting conductive ink onto the insulating layer 16 by inkjet. The electromagnetic shielding layer 18 covers the entire surface of the insulating layer 16 and is electrically connected to the ground line 12. In this way, the printed circuit board 20 with a plurality of semiconductor devices mounted thereon is manufactured.

[0101] Next, a printed wiring board, a semiconductor device, an insulating layer, and an electromagnetic wave shielding layer constituting the printed wiring board will be described.

[0102] (Printed Circuit Board)

[0103] The printed wiring board is not particularly limited, and for example, a flexible printed circuit board, a rigid printed circuit board, and a rigid flexible circuit board can be used, and commercially available products can be used as appropriate. The printed wiring board may have a single-layer structure or a multi-layer structure.

[0104] Furthermore, the printed wiring board is made of, for example, glass epoxy, ceramic, polyimide, and polyethylene terephthalate.

[0105] The wiring (not shown) of the printed wiring board is not particularly limited, but is preferably copper wiring from the viewpoint of conductivity.

[0106] The printed wiring board is supplied with voltage or current from the outside to drive the circuit formed by the semiconductor device, etc. Furthermore, the printed wiring board may be configured to input a signal from the outside to the circuit formed by the semiconductor device, etc. or to output a signal from the circuit to the outside.

[0107] <Ground Wire>

[0108] The ground line 12 of the printed wiring board 10 is a wiring connected to the ground (GND) potential.

[0109] The ground line 12 is continuously arranged on the surface 10a of the printed wiring board 10 in a closed shape. Figure 1 and Figure 2 In the figure, when observing the surface 10a of the printed wiring board 10, the grounding wire 12 is arranged in a quadrilateral shape, but the arrangement of the grounding wire 12 is not limited thereto, and may be a triangle, a polygon with a pentagon or more, or a circle. The arrangement of the grounding wire 12 is determined according to the mounting position of the semiconductor device and the electronic component, etc. In the case where there are multiple semiconductor devices, the grounding wire 12 may be arranged to pass between the semiconductor devices.

[0110] The grounding wire 12 is not limited to Figure 1 As shown, the ground wire 12 is continuously arranged on the surface 10a of the printed wiring board 10. For example, when observing the surface 10a of the printed wiring board 10, the ground wire 12 may be discontinuous as shown by the dotted line, or may be arranged in a closed shape such as a quadrilateral in a discontinuous manner.

[0111] And, if Figure 4 As shown, the grounding wire 12 is configured to be partially buried in the printed wiring board 10, but it is not limited to this. The grounding wire 12 may be formed on the surface 10a of the printed wiring board 10 without partially being buried in the printed wiring board 10. In addition, the grounding wire 12 may have a structure having a portion that penetrates the printed wiring board 10 along the direction Y.

[0112] (Insulation layer)

[0113] The insulating layer has electrical insulation properties. Figure 1 The semiconductor device and the like located in the area D surrounded by the ground line 12 are electrically insulated from the outside. Electrical insulation refers to a volume resistivity of 10 10 Ωcm or more.

[0114] The insulating layer has an inclined portion at the outer edge. The inclined portion is used to maintain the coating thickness of the conductive ink or improve the adhesion, and improve the electromagnetic wave shielding performance of the electromagnetic wave shielding layer. From the viewpoint of maintaining the coating thickness of the conductive ink or improving the adhesion, the maximum angle of the inclined portion is preferably 85° or less, more preferably 80° or less, further preferably 75° or less, and further preferably 70° or less. There is no particular restriction on the lower limit, but since it is limited to the configuration of a semiconductor device with thickness, it is preferably 60° or more, and more preferably 70° or more.

[0115] The maximum angle of the inclined portion of the insulating layer is measured as follows.

[0116] The three-dimensional shape of the insulating layer is measured using a laser microscope to obtain data on the three-dimensional shape of the insulating layer. Next, the angles formed between the surface of the printed wiring board 10 and the inner side of the inclined surface of the insulating layer are measured at 9 locations of the inclined portion formed between the semiconductor device and the ground line, and the largest angle among the 9 angles is taken as the maximum angle.

[0117] The above 9 measurement positions are basically random and vary according to the shape of the insulating layer. However, regarding the measurement position, it is preferred that the height of the insulating layer be greater than the distance Xm (reference Figure 1 ) is included in the measurement position. Furthermore, since the inclination angle of the inclined portion changes depending on the direction or the height of the surrounding components, the inclination angle is measured in a direction perpendicular to the outer frame of the insulating layer at the measured position, and not only one inclined portion but also a plurality of inclined portions are measured. With regard to the measurement position of the inclination angle, the measurement in a direction perpendicular to the outer frame of the insulating layer means, for example, Figure 2 As shown, the measurement is performed along the outer frame portion of the insulating layer 16 , that is, along a line Lm on the insulating layer 16 perpendicular to the ground line 12 .

[0118] When measuring the maximum angle of the inclined portion of the insulating layer, the three-dimensional shape of the insulating layer is measured using a laser microscope. The measurement magnification at this time is preferably 5 to 200 times, more preferably 50 to 200 times.

[0119] The insulating layer is formed by ejecting insulating ink by inkjet. The insulating layer is a cured film of the insulating ink. For example, the insulating layer is formed by applying the insulating ink and then irradiating active energy rays. The insulating ink will be described below.

[0120] in, Fig.18 Schematic diagram showing another example of the structure of the insulating layer of the printed circuit board according to the embodiment of the present invention. Fig.18 In, with Figures 1 to 6 The same structures as shown are denoted by the same symbols, and their detailed description is omitted.

[0121] exist Fig.18 In the embodiment, a grounding wire 40 is arranged in a pentagonal shape on the surface 10a of the printed wiring board 10. In addition, a grounding wire 42 is arranged to be orthogonal to two opposite sides of the grounding wire 40. The first area D1 surrounded by the grounding wire 40 is further divided into a second area D2 and a third area D3 by the grounding wire 42. A semiconductor device 44, electronic components 45a, 45b, a semiconductor device 46, and electronic parts 47a, 47b are mounted in the second area D2. A semiconductor device 48 is mounted in the third area D3.

[0122] In such Fig.18 In the mounted state of the semiconductor device shown, the insulating layer 16 can be formed over the entire first region D1 including the second region D2 and the third region D3. Alternatively, the insulating layer 16 can be formed separately in the second region D2 and the third region D3.

[0123] When forming the insulating layer 16, the data of the three-dimensional shape is acquired for each of the first region D1, the second region D2, and the third region D3 formed, and the slice data is obtained. The number of layers used to form the insulating layer 16 and the thickness of each layer in the direction Y are set for each of the first region D1, the second region D2, and the third region D3 formed. A printed image of the set number of layers is obtained from the slice data. Based on the printed image representing each layer, each layer is formed by ejecting insulating ink by inkjet, and the insulating layer 16 is formed for each of the first region D1, the second region D2, and the third region D3 formed. In this case, there is a case where the insulating layer 16 is formed in the first region D1 including the second region D2 and the third region D3, and a case where the insulating layer 16 is formed in each of the second region D2 and the third region D3.

[0124] The thickness of the insulating layer is preferably in the range of 30 to 3000 μm. That is, the thinnest part of the insulating layer is preferably 30 μm or more, and the thickest part of the insulating layer is preferably 3000 μm or less. If the thickness of the insulating layer is within the above range, it is easy to form a conductive ink, thereby improving the electromagnetic wave shielding property of the formed electromagnetic wave shielding layer.

[0125] Furthermore, the absolute value of the difference between the maximum value and the minimum value of the thickness of the insulating layer is preferably 30 μm or more, more preferably 100 μm or more, and the upper limit of the absolute value of the difference is not particularly limited.

[0126] When the absolute value of the difference between the maximum and minimum values ​​of the thickness of the insulating layer is 30 μm or more, the uppermost surface of the insulating layer can be easily flattened. The electromagnetic shielding layer can be easily uniformly formed by the conductive ink, thereby improving the electromagnetic shielding property.

[0127] In addition, the thickness of the insulating layer Tm (reference Figure 5 ) is the thickness measured based on the surface of a printed wiring board or the surface of an electronic component such as a semiconductor device in contact with the insulating layer. The thickness of the insulating layer is obtained by taking a cross-sectional image of the insulating layer, measuring the lengths of 10 locations corresponding to the thickness of the insulating layer, and taking the average value of the 10 lengths.

[0128] (Electromagnetic wave shielding layer)

[0129] The electromagnetic wave shielding layer shields electromagnetic waves from the outside to prevent them from reaching the semiconductor device embedded in the insulating layer. Furthermore, the electromagnetic wave shielding layer shields electromagnetic waves emitted from the semiconductor device embedded in the insulating layer to prevent them from being radiated to the outside. The electromagnetic wave shielding layer suppresses the influence of interference caused by electromagnetic waves from the outside on the semiconductor device, and suppresses the influence of electromagnetic waves emitted by the semiconductor device on other semiconductor devices or electronic devices.

[0130] like Figure 6 As shown, the electromagnetic wave shielding layer is electrically connected to the grounding wire 12, but when at least a portion of the electromagnetic wave shielding layer 18 is electrically connected to the grounding wire 12, the current generated by the electromagnetic wave incident on the electromagnetic wave shielding layer 18 flows to the ground, which can attenuate the electromagnetic wave. With respect to the electromagnetic wave shielding layer 18 and the grounding wire 12, when there are more electrically connected areas, the current generated by the electromagnetic wave incident on the electromagnetic wave shielding layer 18 is more likely to flow to the ground, which can further attenuate the electromagnetic wave. Furthermore, the number of electromagnetic waves passing through the discontinuous position of the grounding wire 12 in the continuous portion of the grounding wire 12 is reduced, so the more continuous portions of the grounding wire 12 are, the more electromagnetic waves can be attenuated. Therefore, for example, Figure 6 As shown, regarding the electromagnetic wave shielding layer 18 and the ground line 12, it is preferable that the areas to be electrically connected are large.

[0131] The electromagnetic wave shielding layer is formed by ejecting conductive ink on the insulating layer by inkjet. The electromagnetic wave shielding layer is a cured film of the conductive ink. The conductive ink will be described below.

[0132] The thickness of the electromagnetic wave shielding layer is preferably 0.1 μm to 100 μm, more preferably 1 μm to 50 μm.

[0133] The thickness of the electromagnetic shielding layer is determined by obtaining a cross-sectional image of the electromagnetic shielding layer, measuring the lengths at 10 locations corresponding to the thickness of the electromagnetic shielding layer, and taking the average value of the 10 lengths.

[0134] (Semiconductor devices)

[0135] The semiconductor device is not particularly limited, and examples thereof are shown below.

[0136] The semiconductor device is not particularly limited, and examples thereof include logic LSI (Large Scale Integration) (e.g., ASIC (Application Specific Integrated Circuit), FPGA (Field Programmable Gate Array), ASSP (Application Specific Standard Product), etc.), microprocessor (e.g., CPU (Central Processing Unit), GPU (Graphics Processing Unit), etc.), memory (e.g., DRAM (Dynamic Random Access Memory), HMC (Hybrid Memory Cube), MRAM (Magnetic RAM) and PCM (Phase-Change Memory), ReRAM (Resistive RAM), FeRAM (Ferroelectric RAM), flash memory (NAND (Not AND) flash), etc.), power / element, analog IC (Integrated Circuit) (e.g., DC (Direct Current)-DC (Direct Current) Current (DC) converters, insulated gate bipolar transistors (IGBT), etc.), A / D converters, MEMS (MicroElectro Mechanical Systems) (e.g., accelerometers, pressure sensors, vibrators, gyro sensors, etc.), power amplifiers, wireless (e.g.,GPS (Global Positioning System), FM (Frequency Modulation), NFC (Nearfield communication), RFEM (RF Expansion Module), MMIC (Monolithic Microwave Integrated Circuit), WLAN (Wireless Local Area Network), etc.), discrete components, BSI (Back Side Illumination), CIS (Contact Image Sensor), passive devices, bandpass filters, SAW (Surface Acoustic Wave) filters, RF (Radio Frequency) filters, RFIPD (Radio Frequency Integrated Passive Devices), BB (Broadband), stacked capacitors and crystal resonators, etc.

[0137] In addition, semiconductor devices can be passive components or active components. In addition to the above, semiconductor devices also include switches and phase shifters, etc., and also include balun transformers for changing or modulating sensors and high-frequency signals.

[0138] For example, Fig.11 As shown, the semiconductor device 14 has a side surface 14c perpendicular to the surface 10a of the printed wiring board 10, and the height H from the surface 10a of the printed wiring board 10 is greater than 0.5 mm. When the height H of the semiconductor device 14 is greater than 0.5 mm, it becomes difficult to make the insulating ink adhere to the side surface of the semiconductor device 14, but according to the manufacturing method of the printed circuit board, an electromagnetic wave shielding layer with excellent coating and excellent electromagnetic shielding characteristics can be formed.

[0139] In addition, if the height H of the semiconductor device 14 is 3 mm or less, the distance between the inkjet head and the substrate surface becomes narrower, so the influence of the sprayed ink mist or the bending of the ink becomes smaller. Therefore, when printing a layer at the same height as the substrate, the reduction in printing quality is suppressed, and the ink is attached to an unintended position, or the occurrence of ink loss, short circuit, or shielding reduction is suppressed. Therefore, the height H of the semiconductor device 14 is preferably 3 mm or less.

[0140] Height H of semiconductor device 14 is obtained by measuring the length from surface 10a of printed wiring board 10 to a point on surface 10a of printed wiring board 10 farthest from semiconductor device 14 using a microscope while semiconductor device 14 is mounted on printed wiring board 10 .

[0141] The shortest distance between the semiconductor device and the ground wire is, for example, 0.2 to 1.0 mm. When the shortest distance is 0.2 to 1.0 mm, it becomes difficult to attach the insulating ink to the side of the semiconductor device, but according to the manufacturing method of the printed circuit board, an insulating layer having an inclined portion can be formed, and an electromagnetic wave shielding layer having excellent covering properties and excellent electromagnetic shielding properties can be formed.

[0142] Regarding the above shortest distance, Figure 1 In the embodiment, the distances between the side surfaces of the semiconductor device 14 and the ground line 12 are measured in a state where the semiconductor device 14 is mounted on the printed wiring board 10, and the shortest distance Xm is the shortest distance.

[0143] The distance between each side surface of the semiconductor device 14 and the ground line 12 was measured using a microscope.

[0144] Hereinafter, insulating ink and conductive ink will be described.

[0145] (Insulation ink)

[0146] Insulating ink is an ink used to form an insulating layer with electrical insulation properties. Electrical insulation properties refer to a volume resistivity of 10 10 Properties above Ωcm.

[0147] Hereinafter, the description common to the first insulating ink and the second insulating ink will be simply described as “insulating ink”.

[0148] The insulating ink is preferably an active energy ray-curable ink.

[0149] The insulating ink preferably contains a polymerizable monomer and a polymerization initiator.

[0150] -Polymerizable Monomer-

[0151] A polymerizable monomer refers to a monomer having at least one polymerizable group in one molecule. The polymerizable group in the polymerizable monomer may be a cationic polymerizable group or a free radical polymerizable group, and from the viewpoint of curability, a free radical polymerizable group is preferably a free radical polymerizable group. Furthermore, from the viewpoint of curability, the free radical polymerizable group is preferably an ethylenically unsaturated group.

[0152] A monomer refers to a compound having a molecular weight of not more than 1000. The molecular weight can be calculated from the types and numbers of atoms constituting the compound.

[0153] The polymerizable monomer may be a monofunctional polymerizable monomer having one polymerizable group, or may be a polyfunctional polymerizable monomer having two or more polymerizable groups.

[0154] The monofunctional polymerizable monomer is not particularly limited as long as it is a monomer having one polymerizable group.

[0155] From the viewpoint of curability, the monofunctional polymerizable monomer is preferably a monofunctional radical polymerizable monomer, and more preferably a monofunctional ethylenically unsaturated monomer.

[0156] Examples of the monofunctional ethylenically unsaturated monomer include monofunctional (meth)acrylates, monofunctional (meth)acrylamides, monofunctional aromatic vinyl compounds, monofunctional vinyl ethers, and monofunctional N-vinyl compounds.

[0157] Examples of the monofunctional (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, tert-octyl (meth)acrylate, isoamyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, cyclohexyl (meth)acrylate, 4-n-butylcyclohexyl (meth)acrylate, 4-tert-butylcyclohexyl (meth)acrylate, bornyl (meth)acrylate, isobornyl (meth)acrylate, and 1,2-dimethylbenzene (meth)acrylate. Acid ester, 2-ethylhexyl diethylene glycol (meth)acrylate, butoxy (meth)acrylate ethyl, 2-chloro (meth)acrylate ethyl, 4-bromo (meth)acrylate butyl, cyano (meth)acrylate ethyl, benzyl (meth)acrylate, butoxy (meth)acrylate methyl, 3-methoxy (meth)acrylate butyl, 2-(2-methoxyethoxy) (meth)acrylate ethyl, 2-(2-butoxyethoxy) ethyl (meth)acrylate, 2,2,2-tetrafluoro (meth)acrylate ethyl, 1H,1H,2H,2H-perfluoro (meth)acrylate decyl, 4-butylphenyl (meth)acrylate, phenyl (meth)acrylate, 2,4,5-Tetramethylphenyl (meth)acrylate, 4-chlorophenyl (meth)acrylate, 2-phenoxy (meth)acrylate methyl, 2-phenoxy (meth)acrylate ethyl, glycidyl (meth)acrylate, glycidyloxybutyl (meth)acrylate, glycidyloxyethyl (meth)acrylate, glycidyloxypropyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl 4-Hydroxybutyl (meth)acrylate, cyclotrimethylolpropane formal (meth)acrylate, phenyl glycidyl ether (meth)acrylate, ethyl dimethylamino (meth)acrylate, ethyl diethylamino (meth)acrylate, propyl dimethylamino (meth)acrylate, propyl diethylamino (meth)acrylate, trimethoxysilyl (meth)acrylate, trimethylsilyl (meth)acrylate, polyethylene oxide monomethyl ether (meth)acrylate, polyethylene oxide (meth)acrylate, polyethylene oxide monoalkyl ether (meth)acrylate 2-Methacryloyloxyethyl succinate, 2-methacryloyloxyhexahydrophthalate, 2-methacryloyloxyethyl-2-hydroxypropyl phthalate, ethoxydiethylene glycol (meth)acrylate, butoxydiethylene glycol (meth)acrylate, trifluoroethyl (meth)acrylate, perfluorooctylethyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, ethylene oxide (E0) modified phenol (meth)acrylate, Acrylate, E0 modified cresol (meth) acrylate, E0 modified nonylphenol (meth) acrylate, propylene oxide (P0) modified nonylphenol (meth) acrylate, E0 modified-2-ethylhexyl (meth) acrylate, dicyclopentenyl (meth) acrylate, dicyclopentenyloxyethyl (meth) acrylate, dicyclopentyl (meth) acrylate, (3-ethyl-3-oxetanemethyl) (meth) acrylate, phenoxyethylene glycol (meth) acrylate, 2-carboxyethyl (meth) acrylate and 2-(meth)acryloyloxyethyl succinate. ,

[0158] Among them, from the viewpoint of improving heat resistance, the monofunctional (meth)acrylate is preferably a monofunctional (meth)acrylate having an aromatic ring or an aliphatic ring, and more preferably isobornyl (meth)acrylate, 4-tert-butyl cyclohexyl (meth)acrylate, dicyclopentenyl (meth)acrylate, or dicyclopentanyl (meth)acrylate.

[0159] Examples of the monofunctional (meth)acrylamide include (meth)acrylamide, N-methyl (meth)acrylamide, N-ethyl (meth)acrylamide, N-propyl (meth)acrylamide, N-n-butyl (meth)acrylamide, N-tert-butyl (meth)acrylamide, N-butoxymethyl (meth)acrylamide, N-isopropyl (meth)acrylamide, N-methylol (meth)acrylamide, N,N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide and (meth)methacryloyl morpholine.

[0160] Examples of the monofunctional aromatic vinyl compound include styrene, dimethylstyrene, trimethylstyrene, isopropylstyrene, chloromethylstyrene, methoxystyrene, acetoxystyrene, chlorostyrene, dichlorostyrene, bromostyrene, methyl vinylbenzoate, 3-methylstyrene, 4-methylstyrene, 3-ethylstyrene, 4-ethylstyrene, 3-propylstyrene, 4-propylstyrene, 3-butylstyrene, 4-butylstyrene, 3-hexylstyrene, 4-hexylstyrene, 3-octylstyrene, 4-octylstyrene, 3-(2-ethylhexyl)styrene, 4-(2-ethylhexyl)styrene, allylstyrene, isopropenylstyrene, butenylstyrene, octenylstyrene, 4-tert-butoxycarbonylstyrene and 4-tert-butoxystyrene.

[0161] Examples of the monofunctional vinyl ether include methyl vinyl ether, ethyl vinyl ether, propyl vinyl ether, n-butyl vinyl ether, tert-butyl vinyl ether, 2-ethylhexyl vinyl ether, n-nonyl vinyl ether, lauryl vinyl ether, cyclohexyl vinyl ether, cyclohexyl methyl vinyl ether, 4-methylcyclohexyl methyl vinyl ether, benzyl vinyl ether, dicyclopentenyl vinyl ether, 2-dicyclopentenyloxyethyl vinyl ether, methoxyethyl vinyl ether, ethoxyethyl vinyl ether, butoxyethyl vinyl ether, methoxyethoxyethyl vinyl ether, ethoxyethoxyethyl vinyl ether, methoxypolyethylene glycol vinyl ether, tetrahydrofurfuryl vinyl ether, 2-hydroxyethyl vinyl ether, 2-hydroxypropyl vinyl ether, 4-hydroxybutyl vinyl ether, 4-hydroxymethylcyclohexyl methyl vinyl ether, diethylene glycol monovinyl ether, polyethylene glycol vinyl ether, chloroethyl vinyl ether, chlorobutyl vinyl ether, chloroethoxyethyl vinyl ether, phenethyl vinyl ether, and phenoxypolyethylene glycol vinyl ether.

[0162] Examples of the monofunctional N-vinyl compound include N-vinyl-ε-caprolactam and N-vinyl pyrrolidone.

[0163] The polyfunctional polymerizable monomer is not particularly limited as long as it is a monomer having two or more polymerizable groups. From the viewpoint of curability, the polyfunctional polymerizable monomer is preferably a polyfunctional radical polymerizable monomer, and more preferably a polyfunctional ethylenically unsaturated monomer.

[0164] Examples of the polyfunctional ethylenically unsaturated monomer include polyfunctional (meth)acrylate compounds and polyfunctional vinyl ethers.

[0165] Examples of the multifunctional (meth)acrylate include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, butylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, Acid ester, pentaerythritol di(meth)acrylate, 3-methyl-1,5-pentanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, heptanediol di(meth)acrylate, EO-modified pentaerythritol di(meth)acrylate, PO-modified pentaerythritol di(meth)acrylate, EO-modified hexanediol di(meth)acrylate, PO-modified hexanediol di(meth)acrylate, octanediol alcohol di(meth)acrylate, nonanediol di(meth)acrylate, decanediol di(meth)acrylate, dodecanediol di(meth)acrylate, glycerol di(meth)acrylate, pentaerythritol di(meth)acrylate, ethylene glycol diglycidyl ether di(meth)acrylate, diethylene glycol diglycidyl ether di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, trimethylolethane tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolpropane EO addition tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tri(meth)acryloyloxyethoxy trimethylolpropane, glycerol polyglycidyl ether poly(meth)acrylate, and tris(2-acryloyloxyethyl)isocyanurate.

[0166] Examples of the polyfunctional vinyl ethers include 1,4-butanediol divinyl ether, ethylene glycol divinyl ether, diethylene glycol divinyl ether, triethylene glycol divinyl ether, polyethylene glycol divinyl ether, propylene glycol divinyl ether, butylene glycol divinyl ether, hexanediol divinyl ether, 1,4-cyclohexanedimethanol divinyl ether, bisphenol A epoxy alkyl divinyl ether, bisphenol F epoxy alkyl divinyl ether, trimethylolethane trivinyl ether, trimethylolpropane trivinyl ether, ditrimethylolpropane trivinyl ether, and the like. alkyl tetravinyl ether, glycerol trivinyl ether, pentaerythritol tetravinyl ether, dipentaerythritol pentavinyl ether, dipentaerythritol hexavinyl ether, EO addition trimethylolpropane trivinyl ether, PO addition trimethylolpropane trivinyl ether, EO addition ditrimethylolpropane tetravinyl ether, PO addition ditrimethylolpropane tetravinyl ether, EO addition pentaerythritol tetravinyl ether, PO addition pentaerythritol tetravinyl ether, EO addition dipentaerythritol hexavinyl ether and PO addition dipentaerythritol hexavinyl ether.

[0167] Among them, from the viewpoint of curability, the polyfunctional polymerizable monomer is preferably a monomer having 3 to 11 carbon atoms in the part other than the (meth)acryloyl group. As the monomer having 3 to 11 carbon atoms in the part other than the (meth)acryloyl group, more preferably, specifically, 1,6-hexanediol di(meth)acrylate, dipropylene glycol di(meth)acrylate, PO-modified pentaerythritol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 3-methyl-1,5-pentanediol di(meth)acrylate, polyethylene glycol di(meth)acrylate (EO chain n=4) or 1,10-decanediol di(meth)acrylate.

[0168] The content of the polymerizable monomer is preferably 10% by mass to 98% by mass, and more preferably 50% by mass to 98% by mass, based on the total mass of the insulating ink.

[0169] -Polymerization initiator-

[0170] Examples of the polymerization initiator contained in the insulating ink include oxime compounds, alkylphenone compounds, acylphosphine compounds, aromatic onium salt compounds, organic peroxides, sulfur compounds, hexaarylbisimidazole compounds, borate compounds, azinium compounds, titanocene compounds, active ester compounds, compounds having a carbon-halogen bond, and alkylamines.

[0171] Among them, from the viewpoint of further improving the conductivity, the polymerization initiator contained in the insulating ink is preferably at least one selected from the group consisting of oxime compounds, alkylphenone compounds and titanocene compounds, more preferably an alkylphenone compound, and further preferably at least one selected from the group consisting of α-aminoalkylphenyl ketone compounds and benzyl ketal alkylphenone compounds.

[0172] The content of the polymerization initiator is preferably 0.5% by mass to 20% by mass, more preferably 2% by mass to 10% by mass, based on the total mass of the insulating ink.

[0173] The insulating ink may contain other components besides the polymerization initiator and the polymerizable monomer. Examples of other components include a chain transfer agent, a polymerization inhibitor, a sensitizer, a surfactant, and an additive.

[0174] -Chain transfer agent-

[0175] The insulating ink may contain at least one chain transfer agent.

[0176] From the viewpoint of improving the reactivity of the photopolymerization reaction, the chain transfer agent is preferably a polyfunctional thiol.

[0177] Examples of the polyfunctional thiol include aliphatic thiols such as hexane-1,6-dithiol, decane-1,10-dithiol, dithiol diethyl ether, and dithiol diethyl sulfide; and aromatic thiols such as xylene dithiol, 4,4′-dithiol diphenyl sulfide and 1,4-phenyl dithiol.

[0178] Poly(thioglycolate) of polyols such as ethylene glycol bis(thioglycolate), polyethylene glycol bis(thioglycolate), propylene glycol bis(thioglycolate), glycerol tri(thioglycolate), trimethylolethane tri(thioglycolate), trimethylolpropane tri(thioglycolate), pentaerythritol tetra(thioglycolate), dipentaerythritol hexa(thioglycolate);

[0179] Poly(3-mercaptopropionate) of polyols such as ethylene glycol bis(3-mercaptopropionate), polyethylene glycol bis(3-mercaptopropionate), propylene glycol bis(3-mercaptopropionate), glycerol tris(3-mercaptopropionate), trimethylolethane tris(mercaptopropionate), trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptopropionate), and dipentaerythritol hexa(3-mercaptopropionate); and

[0180] Poly(mercaptobutyrate) such as 1,4-bis(3-mercaptobutyryloxy)butane, 1,3,5-tris(3-mercaptobutoxyethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione and pentaerythritol tetrakis(3-mercaptobutyrate).

[0181] -Inhibitors-

[0182] The insulating ink may contain at least one polymerization inhibitor.

[0183] Examples of the polymerization inhibitor include p-methoxyphenol, quinones (e.g., hydroquinone, benzoquinone, methoxybenzoquinone, etc.), phenothiazines, catechols, alkylphenols (e.g., butylhydroxytoluene (BHT)), alkylbisphenols, zinc dimethyldithiocarbamate, copper dimethyldithiocarbamate, copper dibutyldithiocarbamate, copper salicylate, thiodipropionates, mercaptobenzimidazole, phosphites, 2,2,6,6-tetramethylpiperidin-1-oxyl (TEMPO), 2,2,6,6-tetramethyl-4-hydroxypiperidin-1-oxyl (TEMPOL), and tris(N-nitroso-N-phenylhydroxylamine)aluminum salt (also known as cupferroin Al).

[0184] Among them, the inhibitor is preferably at least one selected from p-methoxyphenol, catechols, quinones, alkylphenols, TEMPO, TEMPOL and tris(N-nitroso-N-phenylhydroxylamine)aluminum salt, and more preferably at least one selected from p-methoxyphenol, hydroquinone, benzoquinone, BHT, TEMPO, TEMPOL and tris(N-nitroso-N-phenylhydroxylamine)aluminum salt.

[0185] When the ink contains a polymerization inhibitor, the content of the polymerization inhibitor is preferably 0.01 to 2.0% by mass, more preferably 0.02 to 1.0% by mass, and further preferably 0.03 to 0.5% by mass, based on the total mass of the ink.

[0186] -Sensitizer-

[0187] The insulating ink may contain at least one sensitizer.

[0188] As the sensitizer, for example, polynuclear aromatic compounds (for example, pyrene, perylene, triphenylene and 2-ethyl-9,10-dimethoxyanthracene), xanthene compounds (for example, fluorescein, eosin, erythrosine, rhodamine B and rose bengal), cyanine compounds (for example, thiacarbocyanine and oxacarbocyanine), merocyanine compounds (for example, merocyanidin and carbomerocyanidin), thiazine compounds (for example, thiazine, methylene blue and toluidine blue), acridine compounds (for example, acridine orange, chloroflavin and acriflavin), anthraquinones (for example, anthraquinone), squarylium compounds (for example, squarylium), coumarin compounds (for example, 7-diethylamino-4-methylcoumarin), thioxanthone compounds (for example, isopropylthioxanthone) and dihydrochromanone compounds (for example, dihydrochromanone). Among them, the sensitizer is preferably a thioxanthone compound.

[0189] When the insulating ink contains a sensitizer, the content of the sensitizer is not particularly limited, but is preferably 1.0% by mass to 15.0% by mass, and more preferably 1.5% by mass to 5.0% by mass, based on the total mass of the insulating ink.

[0190] -Surfactant-

[0191] The insulating ink may contain at least one surfactant.

[0192] As the surfactant, there can be mentioned the surfactants described in Japanese Patent Application Laid-Open No. 62-173463 and Japanese Patent Application Laid-Open No. 62-183457. Also, as the surfactant, for example, there can be mentioned anionic surfactants such as dialkyl sulfosuccinates, alkylnaphthalene sulfonates, fatty acid salts, etc.; nonionic surfactants such as polyoxyethylene alkyl ethers, polyoxyethylene alkyl allyl ethers, acetylene glycol, polyoxyethylene·polyoxypropylene block copolymers, etc.; and cationic surfactants such as alkylamine salts and quaternary ammonium salts. Also, the surfactant can be a fluorine-based surfactant or a silicone-based surfactant.

[0193] When the insulating ink contains a surfactant, the content of the surfactant is preferably 0.5% by mass or less, and more preferably 0.1% by mass or less, based on the total mass of the insulating ink. The lower limit of the content of the surfactant is not particularly limited.

[0194] When the content of the surfactant is 0.5 mass % or less, the insulating ink is less likely to spread after being applied to the insulating ink, thereby suppressing the outflow of the insulating ink and improving the electromagnetic wave shielding property.

[0195] -Organic Solvents-

[0196] The insulating ink may contain at least one organic solvent.

[0197] Examples of the organic solvent include (poly)alkylene glycol monoalkyl ethers such as ethylene glycol monoethyl ether, diethylene glycol monoethyl ether, triethylene glycol monomethyl ether, propylene glycol monomethyl ether (PGME), dipropylene glycol monomethyl ether, and tripropylene glycol monomethyl ether;

[0198] (Poly)alkylene glycol dialkyl ethers such as ethylene glycol dibutyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, dipropylene glycol diethyl ether and tetraethylene glycol dimethyl ether;

[0199] (Poly)alkylene glycol acetates such as diethylene glycol acetate;

[0200] (Poly)alkylene glycol diacetates such as ethylene glycol diacetate and propylene glycol diacetate;

[0201] (Poly)alkylene glycol monoalkyl ether acetates such as ethylene glycol monobutyl ether acetate and propylene glycol monomethyl ether acetate, ketones such as methyl ethyl ketone and cyclohexanone;

[0202] Lactones such as γ-butyrolactone;

[0203] Esters such as ethyl acetate, propyl acetate, butyl acetate, 3-methoxybutyl acetate (MBA), methyl propionate, and ethyl propionate;

[0204] Cyclic ethers such as tetrahydrofuran and dioxane; and

[0205] Amides such as dimethylformamide and dimethylacetamide.

[0206] When the insulating ink contains an organic solvent, the content of the organic solvent is preferably 70% by mass or less, and more preferably 50% by mass or less, relative to the total mass of the insulating ink. The lower limit of the content of the organic solvent is not particularly limited.

[0207] -additive-

[0208] The insulating ink may contain additives such as a co-sensitizer, an ultraviolet absorber, an antioxidant, an anti-fading agent, and an alkaline compound as needed.

[0209] -Physical properties-

[0210] From the viewpoint of improving discharge stability when imparting by inkjet recording, the pH (hydrogen ion concentration) of the insulating ink is preferably 7 to 10, more preferably 7.5 to 9.5. The pH is measured at 25° C. using a pH meter, for example, a pH meter manufactured by DKK-TOA CORPORATION (model “HM-31”).

[0211] The viscosity of the insulating ink is preferably 0.5 to 60 mPa·s, more preferably 2 to 40 mPa·s. The viscosity is measured at 25° C. using a viscometer, for example, a TV-22 viscometer manufactured by TOKI SANGYO CO., LTD.

[0212] The surface tension of the insulating ink is preferably 60 mN / m or less, more preferably 20 mN / m to 50 mN / m, and further preferably 25 mN / m to 45 mN / m. The surface tension is measured at 25° C. using a surface tensiometer, for example, an automatic surface tensiometer manufactured by Kyowa Interface Science Co., Ltd. (product name “CBVP-Z”), and measured by a plate method.

[0213] (Provision of insulating ink)

[0214] The insulating ink is applied by inkjet recording. The inkjet recording method can make the thickness of the formed insulating layer thin by ejecting a small amount of insulating ink once. In addition, the inkjet recording method can form a film of any thickness by further printing on the printed material so that multiple layers are overlapped.

[0215] The inkjet recording method can be any of a charge control method that utilizes electrostatic induction force to discharge ink, an on-demand ejection method (pressure pulse method) that utilizes the vibration pressure of a piezoelectric element, an acoustic inkjet method that converts an electrical signal into a sound beam and irradiates the ink and discharges the ink using radiation pressure, and a thermal inkjet (Bubble jet (registered trademark)) method that forms bubbles by heating the ink and utilizes the generated pressure.

[0216] Inkjet recording methods can be particularly effective in utilizing the method described in Japanese Patent Application Laid-Open No. 54-059936, in which ink undergoes a dramatic volume change due to thermal energy and the ink is ejected from a nozzle by the force caused by the state change.

[0217] In addition, regarding the inkjet recording method, the method described in paragraphs 0093 to 0105 of Japanese Patent Application Laid-Open No. 2003-306623 can also be referred to.

[0218] There is no particular limitation on the inkjet head used in the inkjet recording method, and examples include a shuttle scanning method that uses a short serial head to record while scanning the head along the width direction of the electronic substrate, and a line method that uses a line head in which recording elements are arranged corresponding to the entire area of ​​one side of the electronic substrate.

[0219] The ejection amount of the insulating ink ejected from the inkjet head is preferably 1 pL (picoliter) to 100 pL, more preferably 3 pL to 80 pL, and even more preferably 3 pL to 20 pL.

[0220] (Formation of Insulating Layer)

[0221] When forming the insulating layer, it is preferred that the insulating ink is applied before irradiation with active energy rays. In particular, it is preferred that the steps of applying the insulating ink and irradiating with active energy rays are repeated.

[0222] Examples of active energy rays include ultraviolet rays, visible rays, and electron beams, and among these, ultraviolet rays (hereinafter also referred to as “UV”) are preferred.

[0223] The peak wavelength of ultraviolet rays is preferably 200 nm to 405 nm, more preferably 250 nm to 400 nm, and further preferably 300 nm to 400 nm.

[0224] From the viewpoint of further suppressing the generation of wrinkles in the insulating layer, the illuminance during irradiation with active energy rays is more preferably 2 W / cm 2 More preferably, 4W / cm 2 The upper limit of the illumination is not particularly limited, but is, for example, 20 W / cm 2 .

[0225] The exposure time in the semi-curing treatment and curing step is preferably 0.1 seconds or longer, and more preferably 0.5 seconds or longer from the viewpoint of achieving a more excellent effect of the present invention. The upper limit may be 30 seconds or shorter, and preferably 10 seconds or shorter.

[0226] The exposure dose when irradiating with active energy rays is preferably 100 mJ / cm 2 ~10000mJ / cm 2 , more preferably 500 mJ / cm 2 ~7500mJ / cm 2 In addition, when the application of the insulating ink and the irradiation of the active energy ray are regarded as one cycle, the exposure amount mentioned here means the exposure amount of the active energy ray in one cycle.

[0227] As a light source for ultraviolet irradiation, a mercury lamp, a gas laser, and a solid-state laser are mainly used, and the most well-known ones are a mercury lamp, a metal halide lamp, and an ultraviolet fluorescent lamp.

[0228] In addition, UV-LED (light emitting diode) and UV-LD (laser diode) are small, long-life, highly efficient and low-cost, and are expected to be used as light sources for ultraviolet irradiation. Among them, the ultraviolet irradiation light source is preferably a metal halide lamp, a high-pressure mercury lamp, a medium-pressure mercury lamp, a pressure mercury lamp or a UV-LED.

[0229] (Conductive Ink)

[0230] Conductive ink refers to ink used to form an electromagnetic wave shielding layer.

[0231] The conductive ink is preferably an ink containing metal particles (hereinafter also referred to as "metal particle ink"), an ink containing a metal complex (hereinafter also referred to as "metal complex ink") or an ink containing a metal salt (hereinafter also referred to as "metal salt ink"), and is more preferably a metal salt ink or a metal complex ink.

[0232] From the viewpoint of improving electromagnetic wave shielding properties, the conductive ink preferably contains silver, and more preferably is an ink containing a silver salt or an ink containing a silver complex.

[0233] <<Metallic Particle Ink>>

[0234] The metal particle ink is, for example, an ink composition in which metal particles are dispersed in a dispersion medium.

[0235] -Metal particles-

[0236] As the metal constituting the metal particles, for example, particles of base metals and noble metals can be cited. As the base metal, for example, nickel, titanium, cobalt, copper, chromium, manganese, iron, zirconium, tin, tungsten, molybdenum and vanadium can be cited. As the noble metal, for example, gold, silver, platinum, palladium, iridium, osmium, ruthenium, rhodium, rhenium and alloys containing these metals can be cited. Among them, from the viewpoint of conductivity, the metal constituting the metal particles preferably includes at least one selected from the group consisting of silver, gold, platinum, nickel, palladium and copper, and more preferably includes silver.

[0237] The average particle size of the metal particles is not particularly limited, preferably 10nm to 500nm, more preferably 10nm to 200nm. If the average particle size is within the above range, the calcination temperature of the metal particles is reduced, and the process suitability of the electromagnetic wave shielding layer is improved. In particular, when the metal particle ink is imparted by an inkjet recording method, there is a tendency to improve the ejection property, and to improve the uniformity of the pattern formation and the film thickness of the electromagnetic wave shielding layer. The average particle size mentioned here refers to the average value of the primary particle size of the metal particles (average primary particle size).

[0238] The average particle size of the metal particles is measured by a laser diffraction / scattering method. The average particle size of the metal particles is, for example, a value obtained by measuring the 50% volume cumulative diameter (D50) three times and calculating the average value of the values ​​measured three times, and can be measured using a laser diffraction / scattering type particle size distribution measuring device (product name "LA-960", manufactured by HORIBA, Ltd.).

[0239] Furthermore, the metal particle ink may contain metal particles having an average particle size of 500 nm or more as required. When metal particles having an average particle size of 500 nm or more are contained, the nm-sized metal particles can bond to each other by lowering the melting point around the μm-sized metal particles.

[0240] In the metal particle ink, the content of the metal particles is preferably 10% to 90% by mass, and more preferably 20% to 50% by mass, relative to the total mass of the metal particle ink. If the content of the metal particles is 10% by mass or more, the surface resistivity of the electromagnetic wave shielding layer is further reduced. If the content of the metal particles is 90% by mass or less, the ejection property is improved when the metal particle ink is applied by inkjet recording.

[0241] The metal particle ink may contain, in addition to the metal particles, for example, a dispersant, a resin, a dispersion medium, a thickener, and a surface tension adjuster.

[0242] -Dispersant-

[0243] The metal particle ink may contain a dispersant attached to at least a portion of the surface of the metal particles. The dispersant substantially constitutes metal colloid particles together with the metal particles. The dispersant has the function of coating the metal particles to improve the dispersibility of the metal particles and prevent aggregation. The dispersant is preferably an organic compound capable of forming metal colloid particles. From the viewpoint of conductivity and dispersion stability, the dispersant is preferably an amine, a carboxylic acid or a salt thereof, an alcohol or a resin dispersant.

[0244] The dispersant contained in the metal particle ink may be one kind or two or more kinds.

[0245] Examples of the amine include aliphatic amines and aromatic amines.

[0246] The aliphatic amine may be saturated or unsaturated. Among them, the aliphatic amine is preferably an aliphatic amine having 4 to 8 carbon atoms. The aliphatic amine having 4 to 8 carbon atoms may be linear or branched, and may have a ring structure.

[0247] Examples of the aliphatic amine include butylamine, n-pentylamine, iso-pentylamine, hexylamine, 2-ethylhexylamine, and octylamine.

[0248] Examples of the amine having an alicyclic structure include cycloalkylamines such as cyclopentylamine and cyclohexylamine.

[0249] Examples of the aromatic amine include aniline.

[0250] Ammonia may have a functional group other than an amino group. Examples of the functional group other than an amino group include a hydroxyl group, a carboxyl group, an alkoxy group, a carbonyl group, an ester group, and a mercapto group.

[0251] Examples of the carboxylic acid include formic acid, oxalic acid, acetic acid, hexanoic acid, acrylic acid, octanoic acid, oleic acid, tauric acid, ricinoleic acid, gallic acid, and salicylic acid.

[0252] Examples of the carboxylate salt include metal salts of carboxylic acids. The metal ions forming the metal salt of carboxylic acids may be one type or two or more types.

[0253] The carboxylic acid and the carboxylate may have a functional group other than the carboxyl group. Examples of the functional group other than the carboxyl group include an amino group, a hydroxyl group, an alkoxy group, a carbonyl group, an ester group, and a mercapto group.

[0254] Examples of the alcohol include terpene alcohol, allyl alcohol, and oleyl alcohol. Alcohols are easily coordinated to the surface of metal particles and can suppress aggregation of metal particles.

[0255] As the resin dispersant, for example, there can be mentioned a dispersant having a nonionic group as a hydrophilic group and being uniformly soluble in a solvent. As the resin dispersant, for example, there can be mentioned polyvinyl pyrrolidone, polyethylene glycol, polyethylene glycol-polypropylene glycol copolymer, polyvinyl alcohol, polyallylamine and polyvinyl alcohol-polyvinyl acetate copolymer.

[0256] The weight average molecular weight of the resin dispersant is preferably 1,000 to 50,000, more preferably 1,000 to 30,000.

[0257] In the metal particle ink, the content of the dispersant is preferably 0.5% by mass to 50% by mass, and more preferably 1% by mass to 30% by mass, relative to the total mass of the metal particle ink.

[0258] -Dispersion medium-

[0259] The metal particle ink preferably contains a dispersion medium. The type of the dispersion medium is not particularly limited, and examples thereof include hydrocarbons, alcohols, and water.

[0260] The dispersion medium contained in the metal particle ink may be one kind or two or more kinds.

[0261] The dispersion medium contained in the metal particle ink is preferably volatile. The boiling point of the dispersion medium is preferably 50°C to 250°C, more preferably 70°C to 220°C, and further preferably 80°C to 200°C. If the boiling point of the dispersion medium is 50°C to 250°C, there is a tendency that both the stability and calcinability of the metal particle ink can be achieved.

[0262] In this specification, unless otherwise specified, the boiling point means the standard boiling point.

[0263] Examples of the hydrocarbons include aliphatic hydrocarbons and aromatic hydrocarbons.

[0264] Examples of the aliphatic hydrocarbons include saturated aliphatic hydrocarbons or unsaturated aliphatic hydrocarbons such as tetradecane, octadecane, heptamethylnonane, tetramethylpentadecane, hexane, heptane, octane, nonane, decane, tridecane, methylpentane, normal paraffins, and isoparaffins.

[0265] Examples of the aromatic hydrocarbon include toluene and xylene.

[0266] Examples of the alcohol include aliphatic alcohols and alicyclic alcohols. When an alcohol is used as the dispersion medium, the dispersant is preferably an amine or a carboxylic acid or a salt thereof.

[0267] Examples of the aliphatic alcohol include aliphatic alcohols having 6 to 20 carbon atoms which may contain an ether bond in a saturated or unsaturated chain, such as heptanol, octanol (e.g., 1-octanol, 2-octanol, 3-octanol, etc.), decanol (e.g., 1-decanol, etc.), lauryl alcohol, tetradecyl alcohol, hexadecanol, 2-ethyl-1-hexanol, octadecyl alcohol, hexadecanol, and oleyl alcohol.

[0268] Examples of the alicyclic alcohol include cycloalkanols such as cyclohexanol; terpene alcohols such as terpineol (including α, β, γ isomers or any mixture thereof) and dihydroterpineol; myrtenol, sobretol, menthol, carveol, perillyl alcohol, carveol, sobretol and verbenol.

[0269] The dispersion medium may be water. From the viewpoint of adjusting physical properties such as viscosity, surface tension, volatility, etc., the dispersion medium may be a mixed solvent of water and other solvents.

[0270] The other solvent miscible with water is preferably an alcohol or a glycol ether. The alcohol or glycol ether used together with water is preferably an alcohol or glycol ether miscible with water and having a boiling point of 130° C. or less.

[0271] Specific examples of the alcohol include 1-propanol, 2-propanol, 1-butanol, 2-butanol, tert-butanol, and 1-pentanol.

[0272] Specific examples of the glycol ether include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, and propylene glycol monomethyl ether.

[0273] In the metal particle ink, the content of the dispersion medium is preferably 1 to 50% by mass, more preferably 10 to 45% by mass, and further preferably 20 to 40% by mass relative to the total mass of the metal particle ink. If the content of the dispersion medium is 1 to 50% by mass, sufficient conductivity can be obtained as a conductive ink.

[0274] -Resin-

[0275] The metal particle ink may contain a resin. Examples of the resin include polyester, polyurethane, melamine resin, acrylic resin, styrene resin, polyether, and terpene resin.

[0276] The metal particle ink may contain one type of resin or two or more types of resin.

[0277] In the metal particle ink, the content of the resin is preferably 0.1% by mass to 5% by mass based on the total amount of the metal particle ink.

[0278] -Thickener-

[0279] The metal particle ink may contain a thickener. Examples of the thickener include clay minerals such as clay, bentonite, and swellite; cellulose derivatives such as methyl cellulose, carboxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, and hydroxypropyl methyl cellulose; and polysaccharides such as xanthan gum and guar gum.

[0280] The thickener contained in the metal particle ink may be one kind or two or more kinds.

[0281] In the metal particle ink, the content of the thickener is preferably 0.1% by mass to 5% by mass relative to the total mass of the metal particle ink.

[0282] -Surfactant-

[0283] The metal particle ink may contain a surfactant. If the metal particle ink contains a surfactant, a uniform electromagnetic wave shielding layer can be easily formed.

[0284] The surfactant may be any of anionic surfactants, cationic surfactants and nonionic surfactants. Among them, the surfactant is preferably a fluorine-based surfactant from the viewpoint of being able to adjust the surface tension with a small amount of content. In addition, the surfactant is preferably a compound having a boiling point exceeding 250°C.

[0285] -Physical properties of metal particle ink-

[0286] The viscosity of the metal particle ink is preferably 1 mPa·s to 100 mPa·s, more preferably 2 mPa·s to 50 mPa·s, and even more preferably 3 mPa·s to 30 mPa·s.

[0287] The viscosity of the metal particle ink is a value measured using a viscometer at 25° C. For example, the viscosity is measured using a VISCOMETER TV-22 type viscometer (manufactured by TOKI SANGYO CO., LTD.).

[0288] The surface tension of the metal particle ink is not particularly limited, but is preferably 20 mN / m to 45 mN / m, and more preferably 25 mN / m to 40 mN / m.

[0289] The surface tension is a value measured at 25°C using a surface tensiometer.

[0290] For example, the surface tension of the metal particle ink is measured using DY-700 (manufactured by Kyowa Interface Science Co., Ltd.).

[0291] -Method for producing metal particles-

[0292] The metal particles can be commercially available or can be manufactured by a known method. As a method for manufacturing metal particles, for example, a wet reduction method, a gas phase method and a plasma method can be cited. As a preferred method for manufacturing metal particles, a wet reduction method that can manufacture metal particles with an average particle size of less than 200 nm into a narrow particle size distribution can be cited. Regarding the method for manufacturing metal particles based on the wet reduction method, for example, a method including the following steps can be cited: a step of mixing a metal salt and a reducing agent described in Japanese Patent Publication No. 2017-37761, International Publication No. 2014-57633, etc. to obtain a complex reaction solution; and a step of reducing the metal ions in the complex reaction solution by heating the complex reaction solution to obtain a slurry of metal nanoparticles.

[0293] In the process of manufacturing the metal particle ink, a heat treatment may be performed in order to adjust the content of each component contained in the metal particle ink to a predetermined range. The heat treatment may be performed under reduced pressure or under normal pressure. Furthermore, when the heat treatment is performed under normal pressure, it may be performed in the air or under an inert gas environment.

[0294] <<Metal Complex Ink>>

[0295] The metal complex ink is, for example, an ink composition in which a metal complex is dissolved in a solvent.

[0296] -Metal Complex-

[0297] Examples of the metal constituting the metal complex include silver, copper, gold, aluminum, magnesium, tungsten, molybdenum, zinc, nickel, iron, platinum, tin, copper, and lead. From the viewpoint of conductivity, the metal constituting the metal complex preferably includes at least one selected from the group consisting of silver, gold, platinum, nickel, palladium, and copper, and more preferably includes silver.

[0298] The content of the metal contained in the metal complex ink is preferably 1 to 40% by mass, more preferably 5 to 30% by mass, and even more preferably 7 to 20% by mass, based on the total mass of the metal complex ink in terms of metal element.

[0299] The metal complex is obtained, for example, by reacting a metal salt with a complexing agent. As a method for producing the metal complex, for example, a method in which a metal salt and a complexing agent are added to an organic solvent and stirred for a predetermined time can be cited. The stirring method is not particularly limited and can be appropriately selected from known methods such as a method using a stirrer, a stirring blade or a mixer to stir, and a method of applying ultrasonic waves.

[0300] Examples of the metal salt include metal oxides, thiocyanates, sulfides, chlorides, cyanides, nitrites, carbonates, acetates, nitrates, nitrites, sulfates, phosphates, perchlorates, tetrafluoroborate, acetylacetonate and carboxylates.

[0301] Examples of the complexing agent include amines, ammonium carbamate compounds, ammonium carbonate compounds, ammonium bicarbonate compounds, and carboxylic acids. From the viewpoint of conductivity and stability of the metal complex, the complexing agent preferably includes at least one selected from the group consisting of ammonium carbamate compounds, ammonium carbonate compounds, amines, and carboxylic acids having 8 to 20 carbon atoms.

[0302] The metal complex has a structure derived from a complexing agent, preferably a metal complex having a structure derived from at least one of the group consisting of ammonium carbamate compounds, ammonium carbonate compounds, amines, and carboxylic acids having 8 to 20 carbon atoms.

[0303] Examples of the amine as the complexing agent include ammonia, primary amines, secondary amines, tertiary amines, and polyamines.

[0304] Examples of the primary amine having a linear alkyl group include methylamine, ethylamine, 1-propylamine, n-butylamine, n-pentylamine, n-hexylamine, heptylamine, octylamine, nonylamine, n-decylamine, undecylamine, dodecylamine, tridecylamine, tetradecylamine, pentadecylamine, hexadecylamine, heptadecylamine and octadecylamine.

[0305] Examples of the primary amine having a branched alkyl group include isopropylamine, sec-butylamine, tert-butylamine, isopentylamine, 2-ethylhexylamine, and tert-octylamine.

[0306] Examples of the primary amine having an alicyclic structure include cyclohexylamine and dicyclohexylamine.

[0307] Examples of the primary amine having a hydroxyalkyl group include ethanolamine, diethanolamine, triethanolamine, N-methylethanolamine, propanolamine, isopropanolamine, dipropanolamine, diisopropanolamine, tripropanolamine, and triisopropanolamine.

[0308] Examples of the primary amine having an aromatic ring include benzylamine, N,N-dimethylbenzylamine, phenylamine, diphenylamine, triphenylamine, aniline, N,N-dimethylaniline, N,N-dimethyl-p-toluidine, 4-aminopyridine, and 4-dimethylaminopyridine.

[0309] Examples of the secondary amine include dimethylamine, diethylamine, dipropylamine, dibutylamine, diphenylamine, dicyclopentylamine, and methylbutylamine.

[0310] Examples of the tertiary amine include trimethylamine, triethylamine, tripropylamine and triphenylamine.

[0311] Examples of the polyamine include ethylenediamine, 1,3-diaminopropane, diethylenetriamine, triethylenetetramine, tetramethylenepentamine, hexamethylenediamine, tetraethylenepentamine, and combinations thereof.

[0312] The amine is preferably an alkylamine, more preferably an alkylamine having 3 to 10 carbon atoms, and still more preferably a primary alkylamine having 4 to 10 carbon atoms.

[0313] The amines constituting the metal complex may be one type or two or more types.

[0314] When the metal salt and the amine are reacted, the ratio of the amount of the amine to the amount of the metal salt is preferably 1 to 15 times, more preferably 1.5 to 6 times. When the ratio is within the above range, the complex formation reaction is completed and a transparent solution can be obtained.

[0315] As the ammonium carbamate compound of the complexing agent, there can be mentioned ammonium carbamate, methylammonium methylcarbamate, ethylammonium ethylcarbamate, 1-propylammonium 1-propylcarbamic acid, isopropylammonium isopropylcarbamate, butylammonium butylcarbamate, isobutylammonium isobutylcarbamate, pentylaminopentylammoniumcarbamate, hexylaminohexylammoniumcarbamate, heptylaminoheptylammoniumcarbamate, octylaminooctylammoniumcarbamate, 2-ethylhexylammonium 2-ethylhexylcarbamic acid, nonylaminononylammoniumcarbamate and decylaminodecylammoniumcarbamate.

[0316] Examples of ammonium carbonate compounds as complexing agents include ammonium carbonate, methylammonium carbonate, ethylammonium carbonate, 1-propylammonium carbonate, isopropylammonium carbonate, butylammonium carbonate, isobutylammonium carbonate, pentylammonium carbonate, hexylammonium carbonate, heptylammonium carbonate, octylammonium carbonate, 2-ethylhexylammonium carbonate, nonylammonium carbonate and decylammonium carbonate.

[0317] Examples of the ammonium bicarbonate compound as the complexing agent include ammonium bicarbonate, methylammonium bicarbonate, ethylammonium bicarbonate, 1-propylammonium bicarbonate, isopropylammonium bicarbonate, butylammonium bicarbonate, isobutylammonium bicarbonate, pentylammonium bicarbonate, hexylammonium bicarbonate, heptylammonium bicarbonate, octylammonium bicarbonate, 2-ethylhexylammonium bicarbonate, nonylammonium bicarbonate and decylammonium bicarbonate.

[0318] When the metal salt reacts with an ammonium carbamate compound, an ammonium carbonate compound or an ammonium bicarbonate compound, the ratio of the amount of the ammonium carbamate compound, the ammonium carbonate compound or the ammonium bicarbonate compound to the amount of the metal salt is preferably 0.01 to 1 times, more preferably 0.05 to 0.6 times.

[0319] Examples of the carboxylic acid of the complexing agent include caproic acid, caprylic acid, nonanoic acid, 2-ethylhexanoic acid, caprylic acid, neodecanoic acid, undecanoic acid, lauric acid, myristic acid, palmitic acid, stearic acid, palmitic acid, oleic acid, linoleic acid, and linolenic acid. Among them, the carboxylic acid is preferably a carboxylic acid having 8 to 20 carbon atoms, and more preferably a carboxylic acid having 10 to 16 carbon atoms.

[0320] In the metal complex ink, the content of the metal complex is preferably 10% to 90% by mass, more preferably 10% to 40% by mass, relative to the total mass of the metal complex ink. If the content of the metal complex is 10% by mass or more, the surface resistivity is further reduced. If the content of the metal complex is 90% by mass or less, the ejection property is improved when the metal complex ink is applied using an inkjet recording method.

[0321] -Solvents-

[0322] The metal complex ink preferably contains a solvent. The solvent is not particularly limited as long as it can dissolve the components contained in the metal complex ink such as the metal complex. From the viewpoint of ease of production, the boiling point of the solvent is preferably 30°C to 300°C, more preferably 50°C to 200°C, and even more preferably 50°C to 150°C.

[0323] The solvent is preferably contained in the metal complex ink in such a manner that the concentration of metal ions relative to the metal complex (the amount of metal present as free ions in 1 g of the metal complex) is 0.01 mmol / g to 3.6 mmol / g, and more preferably contained in the metal complex ink in such a manner that the concentration of metal ions relative to the metal complex (the amount of metal present as free ions in 1 g of the metal complex) is 0.05 mmol / g to 2 mmol / g. When the concentration of metal ions is within the above range, the metal complex ink has excellent fluidity and can obtain conductivity.

[0324] Examples of the solvent include hydrocarbons, cyclic hydrocarbons, aromatic hydrocarbons, carbamates, olefins, amides, ethers, esters, alcohols, thiols, thioethers, phosphines, and water. The metal complex ink may contain only one type of solvent or two or more types of solvents.

[0325] The hydrocarbon is preferably a linear or branched hydrocarbon having a carbon number of 6 to 20. Examples of the hydrocarbon include pentane, hexane, heptane, octane, nonane, decane, undecane, dodecane, tridecane, tetradecane, pentadecane, hexadecane, octadecane, nonadecane and eicosane.

[0326] The cyclic hydrocarbon is preferably a cyclic hydrocarbon having a carbon number of 6 to 20. Examples of the cyclic hydrocarbon include cyclohexane, cycloheptane, cyclooctane, cyclononane, cyclodecane, and decalin.

[0327] Examples of the aromatic hydrocarbon include benzene, toluene, xylene, and tetralin.

[0328] The ether may be any of a linear ether, a branched ether and a cyclic ether. Examples of the ether include diethyl ether, dipropyl ether, dibutyl ether, methyl-tert-butyl ether, tetrahydrofuran, tetrahydropyran, dihydropyran and 1,4-dioxane.

[0329] The alcohol may be any of a primary alcohol, a secondary alcohol and a tertiary alcohol.

[0330] Examples of the alcohol include ethanol, 1-propanol, 2-propanol, 1-methoxy-2-propanol, 1-butanol, 2-butanol, 1-pentanol, 2-pentanol, 3-pentanol, 1-hexanol, 2-hexanol, 3-hexanol, 1-octanol, 2-octanol, 3-octanol, tetrahydrofurfuryl alcohol, cyclopentanol, terpineol, decanol, isodecanol, lauryl alcohol, isolauryl alcohol, myristyl alcohol, isomyristyl alcohol, cetyl alcohol (cetyl alcohol), isohexadecanol, stearyl alcohol, isostearyl alcohol, oleyl alcohol, isooleyl alcohol, linoleyl alcohol, isolinoleyl alcohol, palmityl alcohol, isopalmityl alcohol, eicosanol, and isoeicosanol.

[0331] Examples of the ketone include acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone.

[0332] Examples of the esters include methyl acetate, ethyl acetate, isopropyl acetate, butyl acetate, isobutyl acetate, sec-butyl acetate, methoxybutyl acetate, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol monobutyl ether acetate, dipropylene glycol monomethyl ether acetate, dipropylene glycol monoethyl ether acetate, dipropylene glycol monobutyl ether acetate and 3-methoxybutyl acetate.

[0333] -reducing agent-

[0334] The metal complex ink may contain a reducing agent. If the metal complex ink contains a reducing agent, the reduction of the metal complex to the metal is promoted.

[0335] Examples of the reducing agent include metal borohydride salts, aluminum hydride salts, amines, alcohols, organic acids, reducing sugars, sugar alcohols, sodium sulfite, hydrazine compounds, dextrin, hydroquinone, hydroxylamine, ethylene glycol, glutathione, and oxime compounds.

[0336] The reducing agent may be an oxime compound described in Japanese Patent Application No. 2014-516463. Examples of the oxime compound include acetone oxime, cyclohexanone oxime, 2-butanone oxime, 2,3-butanedione monoxime, dimethylglyoxime, methyl acetoacetate monoxime, methyl pyruvate monoxime, benzaldehyde oxime, 1-indanone oxime, 2-adamantanone oxime, 2-methylbenzamide oxime, 3-methylbenzamide oxime, 4-methylbenzamide oxime, 3-aminobenzamide oxime, 4-aminobenzamide oxime, acetophenone oxime, benzamide oxime, and tert-butyl ethyl ketone oxime.

[0337] The reducing agent contained in the metal complex ink may be one kind or two or more kinds.

[0338] The content of the reducing agent in the metal complex ink is not particularly limited, but is preferably 0.1 to 20% by mass, more preferably 0.3 to 10% by mass, and further preferably 1 to 5% by mass, based on the total mass of the metal complex ink.

[0339] -Resin-

[0340] The metal complex ink may contain a resin. If the metal complex ink contains a resin, the adhesion of the metal complex ink to the electronic substrate is improved.

[0341] Examples of the resin include polyester, polyethylene, polypropylene, polyacetal, polyolefin, polycarbonate, polyamide, fluororesin, silicone resin, ethyl cellulose, hydroxyethyl cellulose, rosin, acrylic resin, polyvinyl chloride, polysulfone, polyvinyl pyrrolidone, polyvinyl alcohol, polyethylene resin, polyacrylonitrile, polysulfide, polyamideimide, polyether, polyarylate, polyetheretherketone, polyurethane, epoxy resin, vinyl ester resin, phenolic resin, melamine resin and urea resin.

[0342] The resin contained in the metal complex ink may be one kind or two or more kinds.

[0343] -additive-

[0344] The metal complex ink may further contain inorganic salts, organic salts, inorganic oxides such as silicon dioxide, surface conditioners, wetting agents, crosslinking agents, antioxidants, rust inhibitors, heat stabilizers, surfactants, plasticizers, curing agents, thickeners, silane coupling agents and other additives within the range that does not impair the coating property or electromagnetic wave shielding property. The total content of the additives in the metal complex ink is preferably 20% by mass or less relative to the total mass of the metal complex ink.

[0345] The viscosity of the metal complex ink is preferably 1 mPa·s to 100 mPa·s, more preferably 2 mPa·s to 50 mPa·s, and even more preferably 3 mPa·s to 30 mPa·s.

[0346] The viscosity of the metal complex ink is a value measured using a viscometer at 25° C. For example, the viscosity is measured using a VISCOMETER TV-22 viscometer (manufactured by TOKI SANGYO CO., LTD.).

[0347] The surface tension of the metal complex ink is not particularly limited, but is preferably 20 mN / m to 45 mN / m, and more preferably 25 mN / m to 35 mN / m. The surface tension is a value measured at 25°C using a surface tensiometer.

[0348] The surface tension of the metal complex ink is measured using, for example, DY-700 (manufactured by Kyowa Interface Science Co., Ltd.).

[0349] <<Metal Salt Ink>>

[0350] The metal salt ink is, for example, an ink composition in which a metal salt is dissolved in a solvent.

[0351] -Metal Salts-

[0352] Examples of the metal constituting the metal salt include silver, copper, gold, aluminum, magnesium, tungsten, molybdenum, zinc, nickel, iron, platinum, tin, copper, and lead. From the viewpoint of conductivity, the metal constituting the metal salt preferably includes at least one selected from the group consisting of silver, gold, platinum, nickel, palladium, and copper, and more preferably includes silver.

[0353] The content of the metal contained in the metal salt ink is preferably 1 to 40% by mass, more preferably 5 to 30% by mass, and even more preferably 7 to 20% by mass, based on the total mass of the metal salt ink in terms of metal element.

[0354] The content of the metal salt in the metal salt ink is preferably 10% to 90% by mass, more preferably 10% to 40% by mass, relative to the total mass of the metal salt ink. If the content of the metal salt is 10% by mass or more, the surface resistivity is further reduced. If the content of the metal salt is 90% by mass or less, the ejection property is improved when the metal salt ink is applied using an inkjet recording method.

[0355] Examples of the metal salt include benzoates, halides, carbonates, citrates, iodides, nitrites, nitrates, acetates, phosphates, sulfates, sulfides, trifluoroacetates, and carboxylates of metals. Two or more salts may be used in combination.

[0356] From the viewpoint of conductivity and storage stability, the metal salt is preferably a metal carboxylate. The carboxylic acid forming the metal carboxylate is preferably at least one selected from the group consisting of formic acid and carboxylic acids having 1 to 30 carbon atoms, more preferably a carboxylic acid having 8 to 20 carbon atoms, and further preferably a fatty acid having 8 to 20 carbon atoms. The fatty acid may be linear or branched, and may have a substituent.

[0357] Examples of the straight-chain fatty acid include acetic acid, propionic acid, butyric acid, valeric acid, pentanoic acid, hexanoic acid, heptanoic acid, behenic acid, oleic acid, octanoic acid, nonanoic acid, decanoic acid, hexanoic acid, heptanoic acid, octanoic acid, n-nonanoic acid, caprylic acid, and undecanoic acid.

[0358] Examples of the branched fatty acid include isobutyric acid, isovaleric acid, ethylhexanoic acid, neodecanoic acid, trimethylacetic acid, 2-methylpentanoic acid, 3-methylpentanoic acid, 4-methylpentanoic acid, 2,2-dimethylbutyric acid, 2,3-dimethylbutyric acid, 3,3-dimethylbutyric acid, and 2-ethylbutyric acid.

[0359] Examples of the carboxylic acid having a substituent include hexafluoroacetylacetonic acid, 3-hydroxybutyric acid, 2-methyl-3-hydroxybutyric acid, 3-methoxybutyric acid, acetone dicarboxylic acid, 3-hydroxyglutaric acid, 2-methyl-3-hydroxyglutaric acid, and 2,2,4,4-hydroxyglutaric acid.

[0360] The metal salt may be a commercially available product or may be produced by a known method. The silver salt may be produced, for example, by the following method.

[0361] First, a silver compound (e.g., silver acetate) serving as a silver supply source and an amount of formic acid or a fatty acid having 1 to 30 carbon atoms equal to the molar equivalent of the silver compound are added to an organic solvent such as ethanol. The mixture is stirred for a predetermined time using an ultrasonic stirrer, and the resulting precipitate is washed with ethanol for decantation. All of these steps can be performed at room temperature (25° C.). The mixing ratio of the silver compound to formic acid or a fatty acid having 1 to 30 carbon atoms is preferably 1:2 to 2:1, more preferably 1:1, in terms of molar ratio.

[0362] -Other ingredients-

[0363] The metal salt ink may contain a solvent, a reducing agent, a resin, and an additive. Preferred embodiments of the solvent, the reducing agent, the resin, and the additive are the same as those that may be contained in the metal complex ink.

[0364] -Physical properties of metal salt inks-

[0365] The viscosity of the metal salt ink is preferably 1 mPa·s to 100 mPa·s, more preferably 2 mPa·s to 50 mPa·s, and even more preferably 3 mPa·s to 30 mPa·s.

[0366] The viscosity of the metal salt ink is a value measured using a viscometer at 25° C. For example, the viscosity is measured using a VISCOMETER TV-22 type viscometer (manufactured by TOKI SANGYO CO., LTD.).

[0367] The surface tension of the metal salt ink is not particularly limited, but is preferably 20 mN / m to 45 mN / m, and more preferably 25 mN / m to 35 mN / m. The surface tension is a value measured at 25°C using a surface tensiometer.

[0368] The surface tension of the metal salt ink is measured using, for example, DY-700 (manufactured by Kyowa Interface Science Co., Ltd.).

[0369] (Provision of conductive ink)

[0370] The conductive ink is applied by the inkjet recording method, which is the same as the insulating ink. In the inkjet recording method, a small amount of conductive ink is ejected, so that the thickness of the electromagnetic wave shielding layer formed by applying once can be made thin.

[0371] Since a preferred embodiment of the inkjet recording method is the same as a preferred embodiment of the inkjet recording method when the insulating ink is applied, a detailed description thereof will be omitted.

[0372] Before applying the conductive ink, it is preferred to preheat the printed wiring board having the insulating layer formed thereon. The temperature of the printed wiring board when applying the conductive ink is preferably 20°C to 120°C, more preferably 40°C to 100°C.

[0373] As described above, when forming the electromagnetic wave shielding layer, the conductive ink is applied to at least a portion of the insulating layer and the grounding line to form a cured film of the conductive ink, namely, the electromagnetic wave shielding layer.

[0374] As described above, the electromagnetic wave shielding layer is formed by ejecting insulating ink onto the insulating layer by inkjet. At this time, the electromagnetic wave shielding layer is formed in a manner of contacting at least a portion of the grounding wire. As a result, the current generated by the electromagnetic wave incident on the electromagnetic wave shielding layer flows into the ground, which can attenuate the electromagnetic wave.

[0375] When forming an electromagnetic wave shielding layer, for example, the position and arrangement shape of the grounding wire forming the insulating layer are measured in advance with a microscope to obtain the arrangement information of the grounding wire. Preferably, the area to apply the conductive ink and the number of times the conductive ink is applied are set based on the arrangement information.

[0376] When forming the electromagnetic wave shielding layer, for example, the three-dimensional shape data of the processing substrate 11 can also be used. In this case, the three-dimensional shape data of the processing substrate 11 can be used. Figure 7The first image Im1 shown is a solid image composed entirely of image parts and is used as a printed image for the electromagnetic wave shielding layer. After forming the insulating layer, the electromagnetic wave shielding layer can be formed by ejecting conductive ink on the insulating layer using the printed image for the electromagnetic wave shielding layer.

[0377] (Formation of electromagnetic wave shielding layer)

[0378] After the conductive ink is applied to the insulating layer, it is preferred to cure the conductive ink using heat or light.

[0379] When curing is performed using heat, the calcination temperature is 250° C. or less, and the calcination time is preferably 1 minute to 120 minutes. If the calcination temperature and the calcination time are within the above ranges, damage to the electronic substrate is suppressed.

[0380] The calcination temperature is more preferably 80° C. to 250° C., and even more preferably 100° C. to 200° C. Furthermore, the calcination time is preferably 1 minute to 60 minutes.

[0381] The calcination method is not particularly limited, and can be performed by a generally known method.

[0382] The time from the time when the conductive ink is applied to the time when the calcination starts is preferably 60 seconds or less. The lower limit of the time is not particularly limited, and is, for example, 20 seconds. If the time is 60 seconds or less, the conductivity is improved.

[0383] In addition, “the time point at which the application of the conductive ink is completed” means the time point at which all ink drops of the conductive ink land on the insulating layer.

[0384] When curing is performed using light, examples of the light include ultraviolet rays and infrared rays.

[0385] The peak wavelength of ultraviolet rays is preferably 200 nm to 405 nm, more preferably 250 nm to 400 nm, and further preferably 300 nm to 400 nm.

[0386] The exposure amount during irradiation is preferably 100 mJ / cm 2 ~10000mJ / cm 2 , more preferably 500 mJ / cm 2 ~7500mJ / cm 2 .

[0387] The present invention is basically configured as described above. The method for manufacturing a printed wiring board of the present invention has been described in detail above, but the present invention is not limited to the above-described embodiment, and various improvements or changes can be made without departing from the spirit of the present invention.

[0388] Example

[0389] Below, enumerate embodiment, feature of the present invention is described in more detail.Material, reagent, amount of substance and its ratio and operation etc. shown in following example, as long as do not depart from the purpose of the present invention, just can change suitably.Thereby, the scope of the present invention is not limited to following example.

[0390] In this example, an insulating layer and an electromagnetic wave shielding layer were formed on a printed wiring board A having a semiconductor device mounted thereon as shown below, and surface coating defects and electromagnetic wave shielding properties of the electromagnetic wave shielding layer were evaluated.

[0391] The printed wiring board A uses an LTE (Long Term Evolution) substrate BG96 (product name) manufactured by Quectel Wireless Solutions. The printed wiring board A has an area surrounded by a ground line.

[0392] There are a plurality of semiconductor devices, among which there are semiconductor devices having a vertical surface perpendicular to the surface of the printed wiring board A. The semiconductor devices include a stacked capacitor, a crystal resonator, and an integrated circuit. Among the semiconductor devices, there is a semiconductor device with a height of 0.9 mm.

[0393] Furthermore, the semiconductor device is mounted in an area surrounded by the ground line. The shortest distance between the ground line and the semiconductor device of the printed wiring board A is 0.3 mm.

[0394] The printed wiring board A is a communication module on which a semiconductor device having a height of 0.9 mm is mounted, and is connected to a circuit and an antenna for driving the communication module during communication.

[0395] Hereinafter, the insulating ink 1 used for forming the insulating layer and the conductive inks 1 and 2 used for forming the electromagnetic wave shielding layer will be described.

[0396] <Insulation ink 1>

[0397] In a 300 mL resin beaker, 4.0 g of 2-(dimethylamino)-2-(4-methylbenzyl)-1-(4-morpholinophenyl)-butan-1-one (product name "Omnirad 379", manufactured by IGM Resins BV Company), 2.0 g of 2-isopropylthioxanthone (product name "SPEEDCURE ITX", manufactured by Lambson Ltd.), 30.0 g of isobornyl acrylate (manufactured by FUJIFILM Wako Pure Chemical Corporation), 20.0 g of N-vinyl caprolactam, 10.0 g of 1,6-hexanediol diacrylate, cyclohexanedimethanol diacrylate (manufactured by Tokyo Chemical Industry Co., Ltd.) and 9.0 g of trimethylolpropane triacrylate (manufactured by FUJIFILM Wako Pure Chemical Corporation) were added and the mixture was stirred using a mixer (product name "L4R", Silverson Machines). Ltd.), and stirred at 25° C. and 5000 rpm for 20 minutes to obtain insulating ink 1.

[0398] <Conductive ink 1>

[0399] 6.08 g of isobutylammonium carbonate and 15.0 g of isopropyl alcohol were added to a 50 mL three-necked flask and dissolved. Next, 2.0 g of silver oxide was added and reacted at room temperature for 2 hours to obtain a uniform solution. In addition, 0.3 g of 2-hydroxy-2-methylpropylamine was added and stirred to obtain a solution containing a silver complex. The solution was filtered using a PTFE (polytetrafluoroethylene) membrane filter with a pore size of 0.45 μm to obtain a conductive ink 1. The conductive ink is a silver complex ink.

[0400] <Conductive Ink 2>

[0401] (Silver particle ink)

[0402] -Preparation of Silver Particle Dispersion Liquid 1-

[0403] As a dispersant, a solution a was prepared by dissolving 6.8 g of polyvinyl pyrrolidone (weight average molecular weight 3000, manufactured by Sigma-Aldrich) in 100 mL of water. In addition, a solution b was prepared by dissolving 50.00 g of silver nitrate in 200 mL of water. In the mixed solution obtained by mixing and stirring solution a and solution b, 78.71 g of an 85% by mass aqueous solution of N, N-diethylhydroxylamine was added dropwise at room temperature, and a solution obtained by dissolving 6.8 g of polyvinyl pyrrolidone in 1000 mL of water was further added dropwise at room temperature. The obtained suspension was passed through an ultrafiltration unit (Vivaflow50 manufactured by Sartorius Stedim Japan Co., Ltd., fractional molecular weight: 100,000, number of units: 4), and purified water was passed through until about 5 L of exudate was exuded from the ultrafiltration unit and purified. The supply of purified water was stopped and concentrated to obtain 30 g of silver particle dispersion 1. The solid content in the silver particle dispersion 1 was 50% by mass. The silver content in the solid content was measured by TG-DTA (differential thermal thermogravimetric simultaneous measurement) (manufactured by Hitachi High-Tech Corporation, model: STA7000 series), and the result was 96.0% by mass. The obtained silver particle dispersion 1 was diluted 20 times with ion exchange water, and measured using a particle size analyzer FPAR-1000 (manufactured by Otsuka Flectronics Co., Ltd.) to obtain the volume average particle size of the silver particles. The volume average particle size of the silver particles contained in the silver particle dispersion 1 was 60 nm.

[0404] - Adjustment of silver particle ink -

[0405] To 10 g of the silver particle dispersion 1, 2 g of 2-propanol and 0.1 g of OLFINE E-1010 (manufactured by Nissin Chemical Industry Co., Ltd.) as a surfactant were added, and water was added until the silver concentration became 40% by mass to obtain a silver particle ink as conductive ink 2. Conductive ink 2 was a silver nano ink.

[0406] <Production of Printed Images>

[0407] The three-dimensional shape of printed circuit board A was photographed using a microscope VHX-7000 (KEYENCE CORPORATION). Slice data of 0.3mm, 0.6mm, and 0.9mm heights were output from the substrate and changed to a reverse image with the portion containing the semiconductor device as a white background. The outer edge of the image with a height of 0.3mm was aligned with the inside of the ground wire (image 1). The image with a height of 0.6mm was set to reduce the outer edge by 0.1mm from the inside of the ground to the inside (image 2). The image with a height of 0.9mm was set to reduce the outer edge by 0.2mm to the inside (image 3). In addition, as an image of the printed surface, a solid image with the outer edge set 0.3mm inside from the ground was produced (image 4).

[0408] As the printed image of the electromagnetic wave shielding layer, a solid image (image 5) was prepared in which the entire inner side was printed from the outer periphery of the ground wire.

[0409] As the images at a height of 0.6 to 0.9 mm and the upper portion of the printed image of the insulating layer, images 6, 7, and 8 were prepared by aligning the outer edges with the inner sides of the ground wires.

[0410] Table 1 below shows the relationship between the distance from the ground line and the height from the surface of the printed wiring board of the produced printed image.

[0411] [Table 1]

[0412] 0 0.05 0.1 0.15 0.2 0.25 0.3 Height 0.3mm Image 1 - - - - - - Height 0.45mm - Image 12 Image 13 - - - - Height 0.6mm Image 6 Image 9 Image 2 Image 18 - - - Height 0.75mm Image 14 - - Image 17 Image 15 - - Height 0.9mm Image 7 - - Image 10 Image 3 Image 16 - Solid Image Image 8 - - - Image 19 Image 11 Image 4

[0413] Hereinafter, Examples 1 to 7 and Comparative Examples 1 and 2 will be described.

[0414] (Example 1)

[0415] <Formation of Insulating Layer>

[0416] On a printed wiring board A on which a semiconductor device is mounted, an insulating layer is formed using the insulating ink 1 based on the images 1 to 4 described above.

[0417] The insulating ink 1 (insulating active energy curing ink) mentioned above was filled in an ink cartridge (for 10 picoliters) for an inkjet recording device (product name "DMP-2850", manufactured by FUJIFILM Dimatix, Inc.). The image recording conditions were set as follows: resolution 2510 dpi (dots per inch), ejection volume 10 picoliters per dot, ejection frequency 16 kHz, and ejection temperature 45°C. Next to the head of the inkjet recording device, UVspot cur Omni Cure S2000 (manufactured by Lumen Dynamics) was installed 7 cm away from the inkjet nozzle position. After the position of the printed circuit board A was adjusted to correspond to the position of the printed image, printing was performed. During printing, the power was set at 4 W / cm 2 The ink was cured by exposing to UV light at an illumination of 1.5 seconds. 16 layers of each of image 1, image 2, image 3 and image 4 were printed to form an insulating layer. In addition, it was confirmed that the insulating layer was formed inside the ground wire, and all the semiconductor devices inside the ground wire were buried in the insulating layer.

[0418] For images 1 to 19 shown in Table 1, 16 layers were printed by inkjet printing to form a layer with a height of 0.3 mm. Therefore, if there are 8 layers, a layer with a height of 0.15 mm is formed, and if there are 24 layers, a layer with a height of 0.45 mm is formed.

[0419] <Formation of Electromagnetic Wave Shielding Layer>

[0420] Conductive ink 1 is filled in an ink cartridge for an inkjet recording device for forming the above-mentioned insulating layer. The image recording conditions are set as follows: a resolution of 2510 dpi (dots per inch), a jetting amount of 10 picoliters per dot, a discharge frequency of 4 kHz, and a head temperature of 30°C. The printed circuit board A formed with an insulating layer is heated by setting the platen temperature to 60°C. The printing origin is aligned with the upper left end of the ground wire on the frame, and a printed pattern of a solid image having the same size as the outer edge of the ground wire is printed on the ground wire and the insulating layer by inkjet. After printing, the printed circuit board is placed in an oven at a temperature of 160°C and heated for 30 minutes. An electromagnetic wave shielding layer is formed by heating the printed circuit board.

[0421] (Examples 2 to 7, and Comparative Examples 1 and 2)

[0422] Compared with Example 1, Examples 2 to 7 and Comparative Examples 1 and 2 used the insulating ink and conductive ink shown in Table 2 below when forming the insulating layer and the electromagnetic wave shielding layer. In addition, when forming the insulating layer, the image of the insulating layer column shown in Table 2 below was used, and a printed circuit board was produced in the same manner as Example 1 except for the number of printed layers and printed dots recorded in parentheses for each image. In addition, the number of layers in parentheses in Table 2 below indicates the number of printed layers for one printed image. The number of printed layers indicates the number of printing repetitions for one printed image.

[0423] In Comparative Examples 1 and 2, the insulating layer was not formed by reducing the outer edge of the discharge region of the insulating ink in a stepwise manner.

[0424] The maximum angle of the inclined portion, the surface coating defects of the electromagnetic shielding layer, and the electromagnetic shielding properties were evaluated for Examples 1 to 7 and Comparative Examples 1 and 2. The results are shown in Table 2 below.

[0425] <Maximum Angle of Inclined Part>

[0426] The three-dimensional shape of the manufactured printed circuit board was measured using a laser microscope VK-X1000 (manufactured by KEYENCE CORPORATION, magnification 100 times, 3D connection mode). The angles between the inclined portion of the insulating layer formed between the semiconductor device and the ground line and the printed circuit board were measured at 9 locations, and the maximum value was taken as the maximum angle of the inclined portion.

[0427] There is no rule for the measurement positions of the above 9 points. Regarding the measurement positions, the height value of the insulating layer is equal to the distance Xm between the measurement position and the grounding wire (reference Figure 1 ) is included in the measurement position. In addition, since the inclination angle of the inclined portion changes depending on the direction or the height of the surrounding components, the inclination angle is measured in a direction perpendicular to the outer frame of the insulating layer at the measured position, and not only one inclined portion but multiple inclined portions are measured. In the printed wiring board A on which the above-mentioned semiconductor device is mounted, the maximum inclination is achieved between the crystal resonator or the integrated circuit and the ground.

[0428] <Defects of Surface Coating>

[0429] For the electromagnetic wave shielding layer of the produced printed circuit board, a magnified image of the entire printed circuit board A (communication module) was obtained using a microscope VHX-7000 (manufactured by KEYENCE CORPORATION, magnification 100 times, 3D connection mode), and among the defects of the surface coating of the electromagnetic wave shielding layer, a printed circuit board with a length of 0.1 to 1.0 mm was used as the evaluation object. The number of defects that became the evaluation object was evaluated using the following evaluation criteria. In the following evaluation criteria, the most excellent level in the evaluation of surface coating defects is 5.

[0430] -Evaluation criteria for surface coating defects-

[0431] 5: The number of defects that are subject to evaluation is 0 (no defects)

[0432] 4: The number of defects that are subject to evaluation is 1

[0433] 3: The number of defects that are subject to evaluation is 2

[0434] 2: The number of defects to be evaluated is 3 or more and less than 5

[0435] 1: The number of defects to be evaluated is 5 or more, or there is a crack larger than 1.0 mm

[0436] <Electromagnetic wave shielding properties>

[0437] The printed circuit board was made to communicate using LTE BAND13, and a near magnetic field measurement device (product name "SmartScan550", manufactured by API) was used to perform near magnetic field measurement at a frequency of 777MHz. The noise suppression level (unit: dB) in the near magnetic field measurement was measured, and the electromagnetic wave shielding properties were evaluated based on the obtained noise suppression level using the following evaluation criteria. In the following evaluation criteria, the most excellent level of electromagnetic wave shielding properties is 5.

[0438] -Evaluation criteria for electromagnetic shielding properties-

[0439] 5: Noise suppression level is below -40dB

[0440] 4: Noise suppression level exceeds -40dB and is below -30dB

[0441] 3: Noise suppression level exceeds 30dB and is below -20dB

[0442] 2: Noise suppression level exceeds -20dB and is below -10dB

[0443] 1: Noise suppression level exceeds -10dB

[0444]

[0445] As shown in Table 2, in Examples 1 to 7, compared with Comparative Examples 1 and 2, an insulating layer is formed by gradually reducing the outer edge of the discharge area of ​​the insulating ink in a manner that forms an inclined portion, and the electromagnetic wave shielding layer has excellent covering properties, few surface defects, and excellent electromagnetic wave shielding properties.

[0446] In Examples 1 to 7, when the maximum angle of the inclined portion was 75° or less, there were few defects in the surface coating and excellent electromagnetic wave shielding properties.

[0447] Explanation of symbols

[0448] 10-printed circuit board, 10a, 22a, 24a, 26a-surface, 11-processing substrate, 12-grounding wire, 14-semiconductor device, 14a-upper surface, 14c-side surface, 15-semiconductor device, 16-insulating layer, 16b-inclined portion, 6c, 22c, 24c, 26c, 28c-outer edge, 17-semiconductor device, 18-electromagnetic wave shielding layer, 20-printed circuit board, 21-image group, 22-first layer, 24-second layer, 26-third layer, 28-fourth layer, 30 , 32a, 32b, 32c-semiconductor devices, 40, 42-ground wires, 44, 46, 48-semiconductor devices, 45a, 45b, 47a, 47b-electronic parts, D-area, D1-first area, D2-second area, D3-third area, Dm-image part, H-height, Im1-first image, Im2-second image, Im3-third image, Im4-fourth image, L-length, NDm-non-image part, Tm-thickness, X-direction, Xm-distance, Y-direction.

Claims

1. A method for manufacturing a printed circuit board, the printed circuit board comprising: A printed circuit board having a ground line; at least one semiconductor device mounted on the printed circuit board in an area surrounded by the ground line; an insulating layer, embedding at least one of the semiconductor devices, arranged in the region surrounded by the ground line, and having an inclined portion at an outer edge; and an electromagnetic wave shielding layer, disposed on the insulating layer, The method for manufacturing the printed circuit board comprises: On the printed circuit board on which the semiconductor device is mounted, when the process of forming the layer by ejecting the insulating ink by inkjet is performed multiple times to stack the layer, the outer edge of the ejection area of ​​the insulating ink is gradually reduced in a manner to form the inclined portion to form the layer, and the insulating layer having the inclined portion is formed; and A step of forming the electromagnetic wave shielding layer on the insulating layer by ejecting conductive ink by inkjet.

2. The method for manufacturing a printed circuit board according to claim 1, wherein: The shortest distance between the semiconductor device and the ground wire is 0.2-1.0 mm.

3. The method for manufacturing a printed circuit board according to claim 1 or 2, wherein: The maximum angle of the inclined portion is less than 85°.

4. The method for manufacturing a printed circuit board according to claim 1 or 2, wherein: The maximum angle of the inclined portion is less than 75°.

5. The method for manufacturing a printed circuit board according to claim 1 or 2, wherein: The semiconductor device has a side surface perpendicular to a surface of the printed wiring board, and has a height of 0.5 mm or more from the surface of the printed wiring board.

Citation Information

Patent Citations

  • Aqueous ink

    JP2003306623A

  • Silver ink composition

    JP2014516463A

  • Fabrication of PCBs and FPCs with shielded tracks and / or components using 3D inkjet printing

    JP2019527463A

  • Bonding composition

    WO2014057633A1