Method for correcting thickness of piezoelectric layer

Through measurement and numerical model optimization, combined with ion beam grinding technology, the problem of uneven thickness of the piezoelectric layer was solved, the uniform distribution of characteristic parameters in the radio frequency device was achieved, and the device performance was improved.

CN118743330APending Publication Date: 2024-10-01SOITEC SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380022992.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-08
Filing Date
2023-03-07
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In RF devices, the thickness non-uniformity of the piezoelectric layer causes significant changes in the electromechanical coupling coefficient, sound wave propagation velocity and frequency temperature coefficient, affecting the performance of the device.

Method used

By measuring the thickness of the intermediate layer and the piezoelectric layer, a numerical model is used to calculate the target thickness, and ion beam milling technology is used to adjust the thickness of the piezoelectric layer in a morphological identification manner to ensure uniform distribution of its characteristics.

Benefits of technology

The uniform distribution of the thickness of the piezoelectric layer is achieved, which improves the performance stability and characteristic consistency of the radio frequency device and meets the needs of different application parameters.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118743330A_ABST
    Figure CN118743330A_ABST
Patent Text Reader

Abstract

The invention relates to a method for correcting the thickness of a piezoelectric layer (3) arranged on a piezoelectric substrate on insulator, comprising the following steps: measuring the thickness of at least one intermediate layer (2) located between the piezoelectric layer (3) and a carrier substrate (1); measuring the thickness of the piezoelectric layer (3); calculating a thickness correction of the piezoelectric layer (3) on the basis of a measurement of the thickness of the at least one intermediate layer (2) and of the piezoelectric layer (3) and on the basis of a numerical model of at least one property of the plurality of paired piezoelectric layers (3) as a function of the thickness of the piezoelectric layer (3) and of the at least one intermediate layer (2), in order to obtain a target value for each property; the thickness of the piezoelectric layer (3) is corrected in a topographical manner by means of a grinding process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for correcting the thickness of a piezoelectric layer and to a piezoelectric-on-insulator substrate whose thickness is corrected using said method. The present invention is particularly suitable for the manufacture of radio frequency devices such as resonators or filters. Background Art

[0002] It is known to manufacture radio frequency (RF) devices, such as resonators or filters, on a substrate which comprises, from bottom to surface, a carrier substrate, usually made of a semiconductor such as silicon, one or more intermediate layers, and a piezoelectric layer.

[0003] The piezoelectric layer is usually formed by using Smart Cut TM The process is obtained by transferring a thick substrate of piezoelectric material (obtained, for example, by slicing an ingot) to a carrier substrate. The carrier substrate is typically a silicon substrate, which may optionally include one or more layers of one or more other materials.

[0004] Transfer of the piezoelectric layer requires bonding a thick piezoelectric substrate to a carrier substrate and subsequently thinning the thick piezoelectric substrate, leaving only a thin piezoelectric layer of the thickness required to fabricate the RF device on the carrier substrate.

[0005] In order to obtain good adhesion of the piezoelectric substrate to the carrier substrate, an oxide layer (eg silicon oxide SiO 2 ) is usually deposited on each of the two substrates and the substrates are joined via the oxide layers.

[0006] The properties of the piezoelectric layer, such as the electromechanical coupling coefficient, the propagation speed of the acoustic wave, and the frequency temperature coefficient, depend on the thickness of the piezoelectric layer.

[0007] It is known to locally adjust the thickness of a piezoelectric layer by milling with an ion beam (for example argon ions) scanned over the surface of the piezoelectric layer, thereby improving the uniformity of this thickness. This adjustment process is called trimming.

[0008] However, because the piezoelectric layer is very thin, irregularities in the thickness of one or more layers underlying the piezoelectric layer may cause significant variations in these characteristics. Summary of the invention

[0009] An object of the present invention is to provide a method capable of obtaining a uniform distribution of at least one of the following parameters of a piezoelectric layer: electromechanical coupling coefficient, propagation speed of acoustic waves and frequency temperature coefficient.

[0010] To this end, the present invention provides a method for correcting the thickness of a piezoelectric layer disposed on a piezoelectric substrate on an insulator, comprising the following steps:

[0011] measuring the thickness of at least one intermediate layer located between the piezoelectric layer and the carrier substrate,

[0012] Measure the thickness of the piezoelectric layer,

[0013] calculating a thickness correction for the piezoelectric layer based on said measurements of the thickness of at least one intermediate layer and of the piezoelectric layer and based on a numerical model of at least one property of a plurality of pairs of piezoelectric layers as a function of the thickness of the piezoelectric layer and of said at least one intermediate layer in order to obtain a target value for the respective property,

[0014] • Utilize the grinding process to apply thickness correction to the piezoelectric layer in a topography-sensitive manner.

[0015] Advantageously, said property of the piezoelectric layer is selected from the group consisting of an electromechanical coupling coefficient, a wave propagation speed and / or a frequency temperature coefficient.

[0016] One or more properties of the piezoelectric layer may be selected depending on the intended application of the substrate. A single property may be selected so as to obtain a very uniform distribution of that property across the substrate, or a compromise between two or three parameters may be selected so that each parameter is as uniform as possible without creating substantial inhomogeneities in the other corresponding parameters.

[0017] Preferably, the thickness of at least one intermediate layer and the piezoelectric layer is measured locally at a plurality of measuring points, the method further comprising a step of linear interpolation of the thickness of the respective layers between at least two measuring points.The grid of measuring points may be selected depending on the measuring technique and the desired accuracy.

[0018] Advantageously, the milling process is an ion beam etching process. The method may comprise a step of scanning the ion beam along two axes of the main plane of the piezoelectric layer, in which the duration of the irradiation of the ion beam at various locations is adjusted according to the thickness of the piezoelectric layer to be obtained.

[0019] Advantageously, the intermediate layer comprises a dielectric layer, a stack of a plurality of dielectric layers, a metal layer and / or a layer for trapping charges.

[0020] Preferably, the thickness of the piezoelectric layer and / or the intermediate layer is measured by ellipsometry and / or reflectometry.The use of these techniques allows the thickness of multiple superimposed layers to be measured simultaneously.

[0021] The present invention also relates to a method for manufacturing a piezoelectric substrate on insulator, comprising the following steps:

[0022] Providing a carrier substrate,

[0023] Providing a piezoelectric donor substrate,

[0024] bonding the donor substrate to the carrier substrate, providing an intermediate layer at the interface between the donor substrate and the carrier substrate,

[0025] thinning a donor substrate to transfer the piezoelectric layer from said donor substrate to a carrier substrate,

[0026] • Correct the thickness of the piezoelectric layer using the method described above.

[0027] Preferably, thinning the donor substrate comprises forming a weakened region prior to bonding so as to define the piezoelectric layer to be transferred, and separating the donor substrate along the weakened region after bonding.

[0028] In some embodiments, the thickness of the at least one intermediate layer is measured after the piezoelectric layer is transferred to the carrier substrate.

[0029] In other embodiments, the thickness of at least one intermediate layer is measured before the donor substrate is bonded to the carrier substrate.The method is also capable of measuring the thickness of opaque layers.

[0030] Advantageously, the at least one intermediate layer comprises: a metal layer, a dielectric layer, a stack of a plurality of dielectric layers, and / or a layer for trapping charges.

[0031] Another subject of the present invention relates to a piezoelectric substrate on an insulator, which comprises, in sequence, a piezoelectric layer, an intermediate layer and a carrier substrate, characterised in that, according to the method as described above, the local thickness of the piezoelectric layer is adjusted according to the local thickness of the intermediate layer by grinding the piezoelectric layer in a morphologically discriminating manner based on a numerical model of at least one characteristic of a plurality of paired piezoelectric layers according to the thickness of the piezoelectric layer and the at least one intermediate layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Other features and advantages of the present invention will become apparent from the following detailed description with reference to the accompanying drawings, in which:

[0033] Figure 1 A piezoelectric-on-insulator (POI) substrate including a base substrate, an intermediate layer, and a piezoelectric layer is shown.

[0034] FIG. 2A to FIG. 2E The steps of a method according to the invention for manufacturing a POI substrate are shown, the method comprising the adjustment of the thickness of the piezoelectric layer.

[0035] Figure 3 A grid of measurement points of the thickness of the intermediate layer is shown.

[0036] Figure 4 is a diagram of a POI substrate showing the thickness of the LiTaO3 layer.

[0037] Figure 5 is an example of reflection measurements taken at two different angles from a POI substrate comprising a transparent intermediate layer.

[0038] Figure 6The variation of the frequency temperature coefficient of POI substrates with different thicknesses of the intermediate LiTaO3 layer is shown.

[0039] Figure 7 The changes in the electromechanical coupling coefficient and the propagation velocity of acoustic waves of POI substrates with different thicknesses of the intermediate LiTaO3 layer are shown.

[0040] For the sake of legibility of the drawings, various elements are not necessarily shown to scale. In particular, variations in thickness of various layers of the piezoelectric-on-insulator substrate may have been exaggerated. DETAILED DESCRIPTION

[0041] Figure 1 A substrate for an RF device is shown, comprising a carrier substrate 1, typically made of a semiconductor such as silicon, at least one intermediate layer 2 disposed on the carrier substrate, and a piezoelectric layer 3 disposed on the intermediate layer. In some cases, multiple intermediate layers are disposed between the carrier substrate and the piezoelectric layer.

[0042] The term "on" denotes the relative position of the layers taking into account the plurality of layers from the back side of the substrate, ie the free side of the carrier substrate, to the front side, ie the free side of the piezoelectric layer.

[0043] Although the intermediate layer 2 and the piezoelectric layer 3 are shown to have constant thickness, the layers generally exhibit Figure 1 Thickness variation not shown in .

[0044] The method for manufacturing such a substrate includes:

[0045] one or more steps of forming a substrate, which may include steps of depositing, bonding and / or transferring layers,

[0046] one or more steps of measuring the thickness of one or more intermediate layers,

[0047] a step to calculate a thickness correction for the piezoelectric layer, and

[0048] • The correction is applied to the piezoelectric layer using a grinding process.

[0049] Each of these steps will now be described in detail.

[0050] Substrate formation

[0051] Formation of the substrate typically includes bonding a carrier substrate to a piezoelectric donor substrate via at least one intermediate layer and then transferring the piezoelectric layer from the donor substrate to the carrier substrate.

[0052] Prior to the bonding step, at least one intermediate layer is formed on the carrier substrate and / or the donor substrate. Said layer may be present on one or both of the substrates used or may be deposited during the process for manufacturing the piezoelectric-on-insulator substrate.

[0053] refer to Figure 2A , an intermediate layer 2 is deposited on a carrier substrate 1. Illustratively and not restrictively, such an intermediate layer may be a dielectric layer, such as an oxide layer. Figure 2A A single intermediate layer 2 is shown in the figure, but two or more intermediate layers may be deposited on the carrier substrate. In some embodiments, these layers may take the form of a stack of multiple superimposed dielectric layers, such as at least one oxide (e.g. SiO2) layer, at least one nitride (e.g. SiN) layer and / or at least one oxynitride (e.g. SiON) layer. In some embodiments, which may differ from or be combined with the aforementioned embodiments, at least one metallic intermediate layer and / or at least one intermediate layer for trapping charges (made of, for example, polysilicon) is deposited.

[0054] Alternatively (not shown), at least one intermediate layer as described above is deposited on the piezoelectric donor substrate. The deposition is performed such that the intermediate layer is located on the side of the donor substrate that is to be joined to the carrier substrate.

[0055] In some embodiments (not shown), at least a first intermediate layer is deposited on a carrier substrate and at least a second intermediate layer is deposited on a piezoelectric donor substrate such that the first intermediate layer and the second intermediate layer are located at a bonding interface of the donor substrate on the carrier substrate.

[0056] Typically, the number of the intermediate layers is between one and three, but the present invention is not limited thereto.

[0057] like Figure 2A As schematically shown in FIG. 1 , each intermediate layer 2 exhibits some variation in its thickness over the entire area of ​​the intermediate layer 2. Illustratively and non-limitingly, the thickness variation of each intermediate layer is between 5% and 30%.

[0058] Advantageously, Smart Cut TM The piezoelectric layer is transferred to the carrier substrate by a process. Figure 2B , a weakened region 31 is formed in the donor substrate 30 , thereby defining the piezoelectric layer 3 .

[0059] The weakened region 31 is formed in the donor substrate 30 at a predetermined depth, which corresponds approximately to the thickness of the piezoelectric layer 3 to be transferred. The piezoelectric layer 3 typically has a thickness between 100 nm and 15 μm. Preferably, the weakened region 31 is produced by implanting hydrogen and / or helium atoms into the donor substrate 30.

[0060] Alternatively, a treatment may be performed on the surface of the donor substrate to prepare the surface for direct bonding. By way of illustrative, but not limiting, example, the treatment may include chemical cleaning or plasma activation. In some embodiments, after forming the weakened region and / or optionally treating the surface of the donor substrate, one or more intermediate layers are deposited on the donor substrate.

[0061] refer to Figure 2C , the donor substrate 30 is then bonded to the carrier substrate 1 . Thus, one or more intermediate layers 2 are provided at the bonding interface between the carrier substrate 1 and the donor substrate 30 .

[0062] The donor substrate is separated along the weakened region 31, thereby transferring the piezoelectric layer 3 to the carrier substrate 1, between which one or more intermediate layers are arranged (see Figure 2D ). One or more intermediate layers 2 and the piezoelectric layer 3 are arranged to be in direct contact across their interface.

[0063] As Smart Cut TM Alternatively to the process, the piezoelectric layer and / or one or more intermediate layers may be transferred using other techniques that do not produce weakened areas. For example, the piezoelectric layer may be transferred by thinning from the back side of the donor substrate.

[0064] The thickness of the piezoelectric layer transferred to the carrier substrate is greater than that required for the intended application, so that its thickness can be adjusted in a subsequent step by grinding, as described below. By initially providing a sufficiently thick layer of piezoelectric material, a margin is obtained that allows local optimization.

[0065] Thickness measurement

[0066] refer to Figure 2E , non-destructive measurement of the thickness of one or more intermediate layers 2 and the piezoelectric layer 3 is performed to generate a map of the thickness of one or more intermediate layers 2.

[0067] When the substrate includes a plurality of intermediate layers 2A and 2B, refer to Figure 2F , the measurement of the thickness of the first intermediate layer 2A and the measurement of the thickness of the second intermediate layer 2B can be performed continuously or simultaneously to generate a map of the thickness of the individual intermediate layers and the piezoelectric layer 3. In other cases, only the thickness of the piezoelectric layer 3 and the top intermediate layer 2B is determined, and the thickness of any lower intermediate layer 2A is not measured.

[0068] The thickness of one or more intermediate layers is advantageously measured using an optical measuring device. Such a device is preferably an ellipsometric device or a reflectometric device. One advantage of these optical techniques is that they can measure the thickness of multiple superimposed layers, such as Figure 2FThis optical technique is particularly suitable for piezoelectric layers (e.g. LiTaO3) and intermediate layers made of oxides (e.g. SiO2) because these materials are optically transparent in the wavelength ranges conventionally used in the semiconductor field (e.g., 360nm to 900nm or 190nm to 1700nm). Stacks of these materials also have a high refractive index contrast between the respective layers, which facilitates the measurement of the stack of layers by optical means.

[0069] However, the invention is not limited to these measurement techniques. The thickness of the intermediate layer may be determined by any other means capable of non-destructively measuring the thickness of a layer arranged below the piezoelectric layer 3 .

[0070] In some embodiments, the thickness of one or more intermediate layers is measured prior to transferring the piezoelectric layer.This technique is particularly useful in the case of an opaque upper layer whose thickness cannot be determined by optical means through the opaque upper layer.

[0071] For example, the thickness of an opaque layer or another layer located below the opaque layer may be measured by picosecond ultrasound or by wavelength dispersive X-ray fluorescence (WDXRF).

[0072] Advantageously, the measuring device is configured to perform a series of automatic thickness measurements at a grid of measuring points distributed over the substrate surface. Figure 3 A grid of such measurement points is shown in .

[0073] In such a grid, the measurement points 5 are typically located in an (X, Y) plane parallel to the surface of the substrate. Each measurement point is associated with a pair of X, Y coordinates in this plane. Illustratively and not by way of limitation, the measurement points are located on straight lines to make it easier to guide the measuring device. These lines may be radial with respect to the center of the substrate. Alternatively, the measurement points may be located on a rectangular grid or evenly distributed over the surface of the substrate. If in a particular area (e.g. the middle or reference area) the measurement points are located on a rectangular grid, the measurement points may be located on a rectangular grid or evenly distributed over the surface of the substrate. Figure 3 If greater thickness variations are to be expected near the edge of the substrate, it may be chosen to make the measurement points 5 more densely packed in this area.

[0074] The grid, density and position of the measuring points can be selected depending on the measuring technique, the thickness variation of the intermediate layer and the piezoelectric layer and depending on the required accuracy.

[0075] Figure 4 A thickness map on a grid of measurement points is shown, i.e. a spatial representation of the thicknesses measured on a grid of measurement points as described above. Each measurement point is associated with a measurement value or, in the case of a plurality of superimposed intermediate layers, with a set of measurement values, the respective value of each measurement value corresponding to a respective intermediate layer. For example, each thickness range can be associated with a predefined hue or color on the map.

[0076] Optical reflectance measurements involve measuring how the intensity of a beam of light reflected from a surface or interface varies relative to the intensity of the incident beam as a function of the wavelength of the beam (this ratio is called reflectivity).

[0077] refer to Figure 5 , the measured values ​​of the reflection measurement at different incident angles provide a spectrum of the reflected intensity expressed as a percentage of the incident intensity according to the wavelength λ (in nanometers) of the incident light beam. The spectrum drawn with a solid line corresponds to a reflection angle of 70°, and the spectrum drawn with a dashed line corresponds to a reflection angle of 6.5°. Other incident angles and / or a greater number of different angles may be used.

[0078] The intensity of the reflection depends on the wavelength of the light and on the thickness of each layer that the incident and reflected light beams pass through. The intensity of the reflection also depends on the optical properties of each layer, which are known for the materials used. The variation of the intensity with the wavelength is different for each reflection angle. Therefore, individual spectra recorded at different reflection angles can provide additional information about the thickness of each layer in a stack of multiple superimposed layers.

[0079] The thickness of a set of n layers can be calculated from n reflection measurement spectra at various angles, n being an integer. The roughness of the layer can be used as an additional fitting parameter or can be considered constant.

[0080] Ellipsometry is a characterization technique based on the change in the polarization state of light when it is reflected from a surface or interface. Thus, an ellipsometric spectrum (not shown) describes the change in polarization according to the wavelength of the incident beam. The change in polarization also depends on the thickness of each layer traversed by the incident and reflected beams and the reflection angle of the beams. Similar to a set of reflectometry spectra, the corresponding thickness of a set of n layers can be calculated from n ellipsometric spectra at various angles, n being an integer.

[0081] Likewise, the ellipsometry spectrum can be combined with the reflectance spectrum to calculate the corresponding thicknesses of a set of intermediate layers at various points on a selected grid.

[0082] Next, a thickness interpolation step between the measurement points is performed to obtain a thickness map for the entire substrate. Advantageously, linear interpolation is used, since this type of interpolation is fast and easy to implement.

[0083] Numerical model

[0084] The piezoelectric layer has a number of parameters depending on the thickness of the piezoelectric layer and the thickness of one or more intermediate layers. These parameters are, for example, the electromechanical coupling coefficient, the propagation speed of the acoustic wave, and the frequency temperature coefficient.

[0085] Each of these parameters may depend differently on the thickness of the respective intermediate layers, depending on the mechanical, electrical and / or thermal properties of the respective layers.

[0086] When one or more of the intermediate layers exhibit variations in thickness, each of these parameters is obtained as a function of the variation in the respective thickness of the respective intermediate layer.

[0087] After obtaining a map of the piezoelectric layer of at least one intermediate layer, the local thickness and its location on the substrate are taken into account in a numerical model of at least one property of the piezoelectric layer. Such a numerical model comprises a data matrix of one or more parameters of the piezoelectric layer. In this matrix, the model associates the individual values ​​of the corresponding parameters with all combinations of thicknesses of the layers in the stack superimposed on the substrate, and vice versa.

[0088] Based on the target values ​​of such parameters and the thicknesses of the individual intermediate layers involved, a target thickness of the piezoelectric layer can therefore be determined.

[0089] In order to improve the uniformity of such a parameter across the substrate, a target value for the parameter may be selected that corresponds to the indicated thickness of each respective intermediate layer present in the substrate. Since the thickness of one or more intermediate layers is not modified during the process, it is advantageous to select a target value that remains compatible with all thicknesses of the intermediate layers present in the substrate.

[0090] In some cases, a target value is selected that corresponds to an indicated thickness that is close to the average thickness of the respective intermediate layers. In other cases, it may prove necessary to use a maximum or minimum indicated thickness so that the target value for all thicknesses of one or more intermediate layers present in the substrate can be achieved.

[0091] Then, the target thickness value of the piezoelectric layer at each position on the entire substrate is calculated based on the thickness of the corresponding intermediate layer below the corresponding piezoelectric layer at the same position on the substrate. The target thickness of the piezoelectric layer at each point on the substrate is obtained so that the selected parameter has a target value corresponding to the pre-selected indicated value, regardless of the actual value of one or more intermediate layers at each corresponding position. Therefore, after obtaining the target thickness of each corresponding position on the piezoelectric layer, a parameter that is very uniform over the entire substrate can be selected for the piezoelectric layer.

[0092] In the case where the selected parameters exhibit maximum and / or minimum values ​​according to the thickness of the piezoelectric layer, multiple target thicknesses are feasible. In this case, the target thickness that minimizes the thickness variation across the substrate can be selected, or the target thicknesses can be selected based on other parameters to make them as uniform as possible across the substrate.

[0093] Alternatively, two or three different piezoelectric layer parameters can be selected and a target piezoelectric layer value calculated for each of the two or three corresponding parameters. Typically, these target values ​​are not the same for each corresponding parameter at each location across the substrate. Therefore, for each location on the substrate, an average value is calculated that represents a compromise between two or three parameters so that each parameter is as uniform as possible across the substrate without creating excessive non-uniformities in other corresponding parameters. The thickness of the piezoelectric layer is selected based on the thickness of the intermediate layer at each location on the substrate surface.

[0094] Thus, the thickness of the piezoelectric layer can be adjusted to take into account the effect of the thickness of the intermediate layer on a specific parameter, or to obtain a compromise of a set of parameters. The parameters to be optimized are typically selected based on the intended application of the substrate.

[0095] The most relevant piezoelectric layer parameters are the electromechanical coupling coefficient, the propagation speed of the acoustic waves and the frequency temperature coefficient. However, other piezoelectric layer parameters can be adjusted using the method of the invention.

[0096] Commercially available software packages use a model based on the Fresnel coefficients of thin-film multilayers and the transfer matrix method. This model allows for a fast and reliable determination of thickness.

[0097] Figure 6 Displays the sound wave v in m / s I or v f The propagation speed of sound waves on a free surface, v m The propagation velocity on the metallized surface, and the coupling coefficient k s These parameters are shown as the product d*f (in m.GHz or km / s) of the thickness d of the piezoelectric layer made of lithium tantalate (LiTaO3) and the frequency f.

[0098] Typically, the frequencies employed in applications are between 500 MHz and 3000 MHz. The representation of the parameter in terms of thickness-frequency product enables an easy assessment of the required piezoelectric layer thickness for a given application frequency.

[0099] The parameters of various thicknesses (100 nm, 500 nm and 900 nm) of an intermediate layer made of silicon oxide (SiO2) have been measured. Lithium tantalate and silicon oxide are optically transparent and there is a high contrast between the refractive indices of the corresponding layers, which makes it easier to perform optical measurements on the stack of these layers.

[0100] For this configuration of a piezoelectric layer made of LiTaO3 and an intermediate layer made of SiO2, if one wishes to optimize the electromechanical coupling coefficient, a value of 500 nm can be chosen for an intermediate layer with a thickness-frequency product greater than or equal to 1 km / s, or a value of 100 nm for smaller thickness-frequency product values. When the thickness of the layer is 500 nm, at 2 km / s, an electromechanical coupling coefficient squared of about 8.5% is obtained. The same value is obtained for a 100 nm layer at 2.3 km / s and a 900 nm layer at 1.8 km / s ( Figure 6 ).

[0101] For the same configuration, in order to increase the wave propagation speed v on the metallized surface equal to the product of the piezoelectric layer thickness multiplied by the frequency to 1 km / s m To ensure uniformity, a thickness of 500nm (approximately 4100m / s) can be selected as the target value.

[0102] In the region where the thickness of the SiO2 layer is thin (equal to 100 nm), the thickness of the piezoelectric layer multiplied by the frequency must be adjusted to about 3 km / s. In the region where the thickness of the SiO2 layer is 900 nm, this product must be increased to 3 to obtain the same wave propagation speed, or reduced to about 0.4 km / s. If it is desired to simultaneously maintain a certain uniformity of the electromechanical coupling coefficient, a value of 3 km / s will be chosen, since the coupling coefficient shows a significant variation for a thickness-frequency product of 0.4 km / s.

[0103] As dielectric layers are added, the maximum value of the coupling coefficient k moves to lower frequencies. Therefore, the thickness profile will be chosen depending on the frequencies used in the application of the substrate.

[0104] Figure 7 The frequency temperature coefficient FTC is shown as a function of the product d*f (in m.GHz or km / s) of the thickness d of a piezoelectric layer made of lithium tantalate (LiTaO3) and the frequency f. The frequency temperature coefficient increases with increasing dielectric layer thickness d. At the same time, the maximum value of this coefficient shifts to higher frequencies for thicker piezoelectric layers. When it is desired to improve the uniformity of this parameter over the entire substrate, it is also recommended to select the desired thickness depending on the frequency of the target application.

[0105] For example, for a 500 nm layer and a thickness-frequency product of 1 km / s, this parameter can be adjusted starting from a value of about 9 ppm / K. For a 100 nm piezoelectric layer, a thickness-frequency product of about 0.6 km / s is obtained, for a 200 nm layer, a thickness-frequency product of about 0.8 km / s is obtained, for a 700 nm layer, a thickness-frequency product of 1.1 km / s is obtained, and for a 900 nm thick layer, a thickness-frequency product of 1.2 km / s is obtained.

[0106] Grinding of piezoelectric layer

[0107] Based on the target value of the piezoelectric layer thickness determined by the above calculation, the piezoelectric layer is then partially ground. Figure 2G , which enables the thickness of the piezoelectric layer to be adjusted according to the parameters considered in the calculation.

[0108] The grinding process is usually an etching process using an ion beam, usually an ion beam composed of argon ions. The ions hit the sample surface at a very high speed, thereby tearing the material from the target area. Illustratively and not by way of limitation, the ion beam is scanned along two axes of the main plane of the piezoelectric layer, thereby etching the piezoelectric layer over the entire range of the substrate. This process enables the thickness of the piezoelectric layer to be precisely adjusted at various locations across the substrate by continuously scanning the surface. Therefore, the thickness variation matches the desired parameters everywhere over the entire surface. The grinding process may further include etching using a chemical etchant, usually a reactive gas.

[0109] The local thickness removed is determined by the dwell time of the ion beam at each location on the surface of the piezoelectric layer. This dwell time is calculated by an algorithm to match the scanning process to the desired thickness uniformity.

[0110] In some grinding tools, the ion beam can be adjusted to the hardness of the material by varying the energy and current of the ion beam to obtain the appropriate flow rate without excessively affecting the final roughness of the surface.

[0111] The nature of the ion species used for the ion beam can also result in a chemical reaction with the etched material, which can speed up the etching process or smooth the surface of the piezoelectric layer.

[0112] Correction of the thickness of the intermediate layer

[0113] The same method can be used to correct the thickness of the intermediate layer (e.g., a dielectric layer such as SiO2, SiON or SiN) arranged below the piezoelectric layer in a step after the intermediate layer is deposited on the donor substrate or carrier substrate and before the piezoelectric layer is transferred to the carrier substrate. This can advantageously produce a very uniform dielectric layer, which also has a beneficial effect on the uniformity of the electromechanical coupling coefficient over the entire substrate. The steps to be performed in order to obtain a substrate whose thickness of the dielectric layer has been corrected as described above will now be described.

[0114] First, a SiO2 layer is deposited on a base substrate, preferably made of Si. The base substrate may comprise a stack of one or more layers on its surface, which typically comprises a layer made of polysilicon rich in charge carrier traps. The stack may further comprise a layer made of silicon oxide, a layer made of silicon oxynitride, a layer made of silicon nitride, a layer made of aluminum oxide, a layer made of tantalum nitride, or a combination of said layers, other layers made of dielectric materials or stacks of layers.

[0115] Next, in the same way as described above for the intermediate layer below the piezoelectric layer, a local thickness profile of the dielectric layer is generated by ellipsometric and / or reflectometric measurements of at least the SiO2 dielectric material and the underlying layer over a grid of measurement points.

[0116] Subsequently, the map of the local thickness of the corresponding layer is injected into the numerical model, which includes data of the parameter to be optimized according to the thickness. Preferably, the map is injected in the form of values ​​related to the X, Y coordinates of the measurement points used. Interpolation is also performed between the measurement points, preferably linear interpolation.

[0117] The thickness of the dielectric layer is locally adjusted using a milling process (eg, an ion beam milling process). The value of the thickness after milling is based on the local target value determined above.

[0118] By initially providing a sufficiently thick layer of dielectric material, a margin sufficient to allow such local optimization is obtained.

[0119] A piezoelectric layer can then be deposited on the dielectric layer and the thickness of the piezoelectric layer can be readjusted using the method according to the invention. A piezoelectric layer is thereby obtained whose thickness is fine-tuned to optimize one or more parameters of the piezoelectric layer.

Claims

1. A method for correcting the thickness of a piezoelectric layer (3) arranged on a piezoelectric substrate on an insulator, comprising the following steps: measuring the thickness of at least one intermediate layer (2) located between the piezoelectric layer (3) and the carrier substrate (1), · measuring the thickness of the piezoelectric layer (3), calculating a thickness correction of the piezoelectric layer (3) based on said measurements of the thickness of at least one intermediate layer (2) and of the piezoelectric layer (3) and based on a numerical model of at least one property of a plurality of paired piezoelectric layers (3) as a function of the thickness of the piezoelectric layer (3) and of said at least one intermediate layer (2) in order to obtain a target value for the respective property, • Utilizing the grinding process to apply thickness correction to the piezoelectric layer (3) in a topographically sensitive manner.

2. The method according to claim 1, wherein: The property of the piezoelectric layer is selected from the group consisting of an electromechanical coupling coefficient, a wave propagation speed and / or a frequency temperature coefficient.

3. The method according to claim 1 or claim 2, wherein: The thickness of at least one intermediate layer (2) and the piezoelectric layer is measured locally at a plurality of measuring points, the method further comprising a step of linear interpolation of the thickness of the individual layers between at least two measuring points.

4. A method according to any one of the preceding claims, wherein: The milling process is an ion beam milling process.

5. The method according to claim 4 comprises a step of scanning the ion beam along two axes of the main plane of the piezoelectric layer (3), in which step the duration of the ion beam radiation at each position is adjusted according to the thickness of the piezoelectric layer (3) to be obtained.

6. A method according to any one of the preceding claims, wherein: The intermediate layer includes a dielectric layer, a stack of a plurality of dielectric layers, a metal layer and / or a layer for trapping charges.

7. A method according to any one of the preceding claims, wherein: The thickness of the piezoelectric layer (3) and / or the intermediate layer (2) is measured by ellipsometry and / or reflectometry.

8. A method for manufacturing a piezoelectric substrate on insulator, comprising the following steps: Providing a carrier substrate (1), Providing a piezoelectric donor substrate (30), bonding a donor substrate (30) to a carrier substrate (1), providing an intermediate layer (2) at the interface between the donor substrate and the carrier substrate, thinning the donor substrate to transfer the piezoelectric layer (3) from said donor substrate to a carrier substrate, The thickness of the piezoelectric layer (3) is corrected using a method according to any one of claims 1 to 7.

9. The method according to claim 8, wherein: Thinning the donor substrate (30) includes forming a weakened region (31) before bonding, thereby defining the piezoelectric layer (3) to be transferred, and separating the donor substrate along the weakened region (31) after bonding.

10. The method according to any one of claims 8 and 9, wherein: The thickness of at least one intermediate layer (2) is measured after the piezoelectric layer (3) has been transferred to the carrier substrate (1).

11. The method according to any one of claims 8 and 9, wherein: The thickness of at least one intermediate layer (2) is measured before the donor substrate (30) is bonded to the carrier substrate (1).

12. The method according to any one of claims 8 to 11, wherein: The at least one intermediate layer (2) comprises: a metal layer, a dielectric layer, a stack of a plurality of dielectric layers, and / or a layer for trapping charges.

13. A piezoelectric substrate on insulator, comprising a piezoelectric layer (3), an intermediate layer (2) and a carrier substrate (1) in sequence, characterized in that: According to the method described in any one of claims 1 to 12, the local thickness of the piezoelectric layer is adjusted according to the local thickness of the intermediate layer (2) by grinding the piezoelectric layer in a morphologically discriminating manner based on a numerical model of at least one characteristic of multiple paired piezoelectric layers (3) according to the thickness of the piezoelectric layer (3) and the at least one intermediate layer (2).