Multi-component nano probe, preparation method and application

By developing Au@Cu2-xSe@Pt multi-component nanoprobes, the problem of sensitivity and resolution in the diagnosis and treatment of deep tumors has been solved, precise diagnosis and treatment of tumors has been achieved, and efficient deep tissue penetration and high space have been provided. resolution solution.

CN118743753APending Publication Date: 2024-10-08HUNAN UNIV OF ARTS & SCI
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410651403.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-24
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Existing deep tumor diagnosis and treatment methods have problems such as low sensitivity, poor resolution, many radiation side effects, and separation of diagnosis and treatment. It is difficult for a single treatment method to completely eliminate tumors and solve the problem of cancer cell metastasis.

Method used

Develop a multi-component nanoprobe, including an Au@Cu2-xSe@Pt structure. By wrapping Cu2-xSe on the Au nanosphere and growing Pt in an island shape on its surface, combined with PEG modification, a multi-component near-infrared region is formed. Meta-nanomaterials for photothermal therapy, chemokinetic therapy, and photoacoustic imaging.

Benefits of technology

It improves the photothermal stability and surface plasmon capabilities of precious metals, enhances the light absorption and charge separation of metal-semiconductor heterostructures, achieves deep tissue penetration capabilities, high spatial resolution and sensitivity, and solves the problem of tumor diagnosis and treatment. The integrated problem provides accurate diagnosis and treatment of deep tumors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118743753A_ABST
    Figure CN118743753A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of nano medicines, and particularly relates to a multi-component nano probe, a preparation method and application, the multi-component nano probe comprises Au-coated Cu2-xSe-coated Pt and PEG modified on the surface of Au-coated Cu2-xSe-coated Pt, the Au-coated Cu2-xSe-coated Pt comprises Au nanospheres, Cu2-xSe coated on the Au nanospheres and Pt growing on the surface of Cu2-xSe in an island shape, the system has the advantages of deep tissue penetrating power, high spatial resolution and sensitivity, high maximum allowable exposure intensity, multiple treatment and imaging modes and other tumor diagnosis and treatment integration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of nanomedicine, and in particular relates to a multi-component nanoprobe, a preparation method and an application thereof. Background Art

[0002] At present, the clinical methods used for deep tumor diagnosis include positron emission tomography (PET), X-ray computed tomography (CT), ultrasound and magnetic resonance imaging (MRI). Although these methods have their own advantages, they all have obvious disadvantages, such as low sensitivity, poor resolution, many radiation side effects and expensive instruments. More importantly, these methods separate diagnosis and treatment, which is not conducive to real-time and precise treatment. New optical diagnosis and treatment methods for tumors, such as chemodynamic therapy (CDT), sonodynamic therapy (SDT), photodynamic therapy (PDT) and photothermal therapy (PTT), have greatly improved the effectiveness of tumor treatment, and have the advantages of non-invasiveness, high specificity, high spatial resolution, low side effects, high sensitivity and high controllability. So far, various photofunctional materials have been developed, such as organic molecular materials, semiconductor quantum dots, polymer materials, etc. However, the problems of photobleaching, low photothermal stability, poor water solubility and lack of multifunctionality of these photofunctional materials limit their wide application in optical diagnosis and treatment.

[0003] Due to the heterogeneity, complexity and diversity of tumors, a single treatment method may not be able to eliminate the entire tumor, and it is also unable to solve the problem of cancer cell metastasis. Therefore, the use of two or more treatment forms of combined therapy is considered to be one of the best means to effectively solve this problem.

[0004] Application publication number CN 117414445 A discloses a medical multifunctional optical probe and its preparation method and application in surgical navigation, wherein the multifunctional optical probe is a Raman molecule-encoded gold nanostar embedded with doped Gd 3+ Au@Cu with near-infrared second-region plasmon effect is further modified with polyethylene glycol on the surface of magnetic silica shell. 2-x Se core-shell nanoparticle modification. Although it solves the problem of difficulty in depicting the complete outline of the tumor during surgical navigation treatment, it cannot completely eradicate highly invasive tumor lesions and tumor metastases in unknown locations. The nanoprobes have low enrichment rates in tumor sites and their uneven spatial distribution, resulting in poor spatial accuracy of imaging. At the same time, the tumors treated are superficial tumors, such as deep tumors (gliomas), which cannot achieve complete removal of tumor tissue, and the treatment methods are single, such as photothermal therapy. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a multi-component nanoprobe, a preparation method and an application thereof, so as to improve the effect of treating and / or diagnosing tumors.

[0006] The embodiment of the present invention provides a multi-component nanoprobe, comprising Au@Cu 2-x Se@Pt and modified Au@Cu 2- x PEG on the Se@Pt surface, the Au@Cu 2-x Se@Pt is Au nanospheres, and Cu 2-x Se, and islands grown on Cu 2-x Pt on Se surface.

[0007] The embodiment of the present invention provides a method for preparing the multi-component nanoprobe, comprising the following steps: Chloroplatinic acid solution and Au@Cu 2-x Se solution, add reducing agent, react, centrifuge, wash, and obtain Au@Cu 2- x Se@Pt, then Au@Cu 2-x The Se@Pt solution and methoxypolyethylene glycol-thiol are mixed and reacted to obtain a multi-component nanoprobe.

[0008] In one embodiment, the reducing agent is ascorbic acid.

[0009] In one embodiment, the Au@Cu 2-x The preparation method of Se is as follows: mixing an aqueous solution of chloroauric acid and an aqueous solution of sodium citrate, boiling to obtain gold seeds, then lowering the temperature to 85-95°C, sequentially adding an aqueous solution of sodium citrate and an aqueous solution of chloroauric acid, reacting, cooling, centrifuging, washing and purifying to obtain Au nanospheres; sequentially adding an aqueous solution of selenium oxide and an aqueous solution of ascorbic acid to an aqueous solution of Au nanospheres, then adding a mixture of an aqueous solution of copper sulfate and an aqueous solution of ascorbic acid, reacting, centrifuging, and obtaining Au@Cu 2-x Se.

[0010] In one embodiment, the temperature is lowered to 90° C., and an aqueous sodium citrate solution and an aqueous chloroauric acid solution are added in sequence.

[0011] In one embodiment, the water washing purification is performed using an aqueous solution containing PVP.

[0012] In one embodiment, the sodium citrate aqueous solution and the chloroauric acid aqueous solution are added more than once.

[0013] In one embodiment, the molar concentration of the aqueous solution of chloroauric acid is 50 mM.

[0014] In one embodiment, the mass concentration of the sodium citrate aqueous solution is 0.0006 g / mL.

[0015] An embodiment of the present invention provides an application of the multi-component nanoprobe for preparing drugs for treating and / or diagnosing tumors.

[0016] The beneficial effect of the present invention is that the present invention combines precious metal (Au, Pd, Pt, etc.) nanomaterials and copper sulfide compounds (Cu 2-x E, X>0, E=S, Se, Te) into a system, preferably with Au as the core, Cu 2-x Se is the middle wrapping layer, and finally Pt is attached to the outside. Pt grows in the form of islands on Cu 2-x Se surface, forming a multi-heterogeneous nanostructure, can effectively improve the photothermal stability of precious metals under near-infrared light. At the same time, the unique surface plasmon enhancement ability of precious metals can enhance the light absorption and charge separation at the interface of metal-semiconductor heterostructures, especially Pt with nanozyme-like catalytic activity. They achieve deep tissue penetration ability, high spatial resolution and sensitivity, and high maximum allowable exposure intensity.

[0017] The present invention is Au@Cu 2-x Se is externally linked with Pt nanoparticles, and the Pt nanoparticles are distributed in the Au@Cu 2-x Se, relative to Au@Cu 2-x Se externally links to other metals such as Au@Cu 2-x Se@Au, or other distributions on Au@Cu relative to Pt nanoparticles 2-x Se structure, has a better effect.

[0018] The present invention uses sodium citrate as a reducing agent to reduce HAuCl4 to obtain gold nanospheres. Compared with strong reducing agents such as sodium borohydride or ascorbic acid, the gold nanoparticles obtained are larger and more stable and less likely to agglomerate. Large and stable gold nanoparticles can keep the final multi-component nanomaterials at a relatively suitable size (~100 nm), increase the long-term circulation in the body, and the penetration retention effect of tumor tissues, thereby achieving better deep tissue penetration, high spatial resolution and sensitivity, and high maximum allowable exposure intensity.

[0019] The present invention realizes the integration of tumor diagnosis and treatment, which can effectively solve the current problem of separation of clinical diagnosis and treatment, and provides a new idea for the precise diagnosis and treatment of various deep tumors.

[0020] The present invention is a near-infrared second region (NIR-II) multi-component nanomaterial, namely, gold / cuprous selenide / platinum (Au@Cu 2-x Se@Pt) multi-component nanomaterials are used to realize the integration of tumor diagnosis and treatment such as photothermal therapy, chemodynamic therapy, Pt nanozyme catalytic therapy, photoacoustic imaging, and photothermal imaging in the near-infrared region. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The Au@Cu provided in the embodiment of the present invention 2-x Se@Pt multi-component nanoflower materials and Au@Pt@Cu 2-x Schematic diagram of the preparation process of Se core-shell nanomaterials.

[0022] Figure 2 The Au nanospheres and Au@Cu provided in the embodiments of the present invention 2-x Se core-shell nanostructures, Au@Cu 2-x UV-visible absorption spectrum of Se@Pt nanoflower material.

[0023] Figure 3 The Au@Cu modified with different amounts of Pt provided in the embodiments of the present invention 2-x UV-visible absorption spectrum of Se@Pt nanoflower material.

[0024] Figure 4 (a) shows Au@Cu grown with 0.3 mL, 0.4 mL, and 0.5 mL chloroplatinic acid provided in an embodiment of the present invention. 2- x Transmission electron microscopy image of Se@Pt nanoflower material.

[0025] Figure 4(b) is a transmission electron micrograph of gold nanoparticles grown when reduced with sodium borohydride.

[0026] Figure 5 The Au nanospheres and Au@Cu provided in the embodiments of the present invention 2-x Se core-shell nanostructures, Au@Cu 2-x Transmission electron microscopy image of Se@Pt nanoflower material.

[0027] Figure 6 The amount of Au@Cu added to 0.4 mL of chloroplatinic acid in the present invention is 2-x STEM image of Se@Pt multi-component core-shell nanoflower material and distribution diagram of Au, Pt, Cu and Se elements.

[0028] Figure 7 For the present embodiment, chloroplatinic acid and Cu 2-x The Au@Pt core-shell spiny nanostructures and Au@Pt@Cu 2-x Transmission electron microscopy image of Se core-shell nanomaterials.

[0029] Figure 8 This is the Au@Pt@Cu embodiment of the present invention. 2-x STEM image of Se core-shell nanomaterials and elemental distribution of Au, Pt, Cu, and Se.

[0030] Fig. 9 The Cu provided in the embodiment of the present invention 2-x Se nanospheres, Cu 2-x Transmission electron microscopy image of Se@Au nanomaterials.

[0031] Fig.10 The Au@Cu provided in the embodiment of the present invention 2-x Se and Au@Cu 2-x ESR spectrum of Se@Pt nanoflower material. Fig.10 (a) ESR spectrum of ·OH detected using DMPO as a capture probe; Fig.10 (b) Detection using TEMP as capture probe 1 ESR spectrum of O2.

[0032] Fig.11 The Cu provided in the embodiment of the present invention 2-x ESR spectrum of Se@Au nanomaterials. Fig.11 (a) ESR spectrum of ·OH detected using DMPO as a capture probe; Fig.11 (b) Detection using TEMP as capture probe 1 ESR spectrum of O2.

[0033] Fig.12 The Au nanospheres and Au@Cu provided in the embodiments of the present invention 2-x Se core-shell nanostructures, Au@Cu 2-x Zeta potential and hydrated particle size changes of Se@Pt nanoflower materials.

[0034] Fig.13 The Au@Cu provided in the embodiment of the present invention 2-x Se core-shell nanostructures, Au@Cu 2-x XRD spectrum of Se@Pt nanoflower material.

[0035] Fig.14 The Au@Cu provided in the embodiment of the present invention 2-x Graph showing changes in the photothermal properties of Se@Pt nanoflower materials. Fig.14 (a) Temperature-time variation curves at different concentrations, Fig.14 (b) Curves of six consecutive laser on / off cycles.

[0036] Fig.15 The Au@Cu with different concentrations provided in the embodiment of the present invention 2-xRelationship diagram between Se@Pt nanoflower material and photoacoustic signal intensity.

[0037] Fig.16 The Au@Cu provided in the embodiment of the present invention 2-x Cytotoxicity of Se@Pt nanoflower materials. Fig.16 (a) Cell viability of L-02 cells treated with different concentrations. Fig.16 (b) Cell viability of U87 after different treatment conditions.

[0038] Fig.17 The Au@Cu provided in the embodiment of the present invention 2-x In vivo photothermal properties of Se@Pt nanoflower materials. Fig.17 (a) is an infrared thermal image. Fig.17 (b) is the corresponding temperature change curve.

[0039] Fig.18 The Au@Cu provided in the embodiment of the present invention 2-x Antitumor therapeutic properties and histological analysis of Se@Pt nanoflower materials. Fig.18 (a) is the weight change curve of tumor-bearing mice. Fig.18 (b) is the change of tumor volume. Fig.18 (c) H&E staining photograph of tumor sections. DETAILED DESCRIPTION

[0040] Example 1 Au@Cu 2-x Se@Pt multi-component nanoflower structure: (1) Preparation of Au nanospheres: First, under vigorous stirring, 0.25 mL of 50 mM HAuCl4 aqueous solution was added to 75 mL of aqueous solution containing 0.045 g of sodium citrate, the solution was boiled, and the reaction was continued for 15 min to synthesize gold seeds. When the temperature dropped to 90°C, 0.5 mL of aqueous solution containing 0.062 g of sodium citrate and 0.25 mL of 50 mM HAuCl4 solution were added in sequence, and the reaction was continued at 90°C for 30 min. This process was repeated three times, and the reaction solution was cooled to room temperature. Purification was performed by centrifugation at 10,000 rpm and washing with PVP (i.e., an aqueous solution of PVP with a concentration of 10 mg / mL), and finally 200 µg / mL 30mL of PVP-modified PVP-Au gold nanosphere aqueous solution was obtained.

[0041] (2) Au@Cu 2-xPreparation of Se nanocore-shell structure: At room temperature, 0.1 mL of 50 mM SeO2 aqueous solution and 0.2 mL of 200 mM AA (ascorbic acid) aqueous solution were added to the 2 mL aqueous solution of PVP-Au nanospheres obtained above. After 15 minutes of reaction, a solution of Au-Se nanospheres was obtained; then a mixture of 0.1 mL of 100 mM CuSO4·5H2O aqueous solution and 0.4 mL of 100 mM AA aqueous solution was added to the solution of Au-Se nanospheres. The reaction was allowed to proceed overnight until the solution turned dark green. Subsequently, the excess PVP ligands were removed by multiple centrifugation at 8000 rpm, and finally the obtained Au@Cu 2-x The Se nanocore-shell structures were stored in water at a concentration of 200 µg / mL for further use.

[0042] (3) Au@Cu 2-x Preparation of Se@Pt nanoflower structure: Different volumes of 0.05 mL, 0.1 mL, 0.2 mL, 0.3 mL, 0.4 mL, and 0.5 mL of 10 mM chloroplatinic acid solution were quickly added to 5 mL of 200 µg / mL Au@Cu 2-x Se solution, then add 1 mL of 200 mM AA solution, stir vigorously for 2 min, place it in a 40 ℃ oven, react for 12 hours, centrifuge it at 5000 rpm for 10 min, discard the supernatant, wash it twice with deionized water, and finally disperse it in deionized water at a concentration of 200 µg / mL for later use.

[0043] (4) mPEG-modified Au@Cu 2-x Preparation of Se@Pt nanoflowers: Au@Cu grown in 0.5 mL 10 mM chloroplatinic acid 2-x Se@Pt nanoflowers were used as an example to prepare 5 mL of 50 µg / mL PVP-modified Au@Cu 2-x mPEG-SH was added to the Se@Pt nanoflower solution to make it 30 μg / mL and stirred for 15 min. It was then placed at 4 °C for 24 h. Finally, it was centrifuged at 5000 rpm and dispersed in PBS solution for later use.

[0044] Au@Cu 2-x The synthesis process of Se@Pt multi-component nanoflower materials is as follows Figure 1 (1) as shown.

[0045] Comparative Example 1 The Cu 2-x The order of Se and Pt raw materials was adjusted to obtain Au@Pt@Cu 2-x Se multi-component core-shell structure: (1) Preparation of Au nanospheres: First, under vigorous stirring, 0.25 mL of 50 mM HAuCl4 aqueous solution was added to 75 mL of aqueous solution containing 0.045 g of sodium citrate, the solution was boiled, and the reaction was continued for 15 min to synthesize gold seeds. When the temperature dropped to 90 °C, 0.5 mL of aqueous solution containing 0.062 g of sodium citrate and 0.25 mL of 50 mM HAuCl4 solution were added in sequence, and the reaction was continued at 90 °C for 30 min. This process was repeated three times, and the reaction solution was cooled to room temperature. The solution was purified by centrifugation at 10,000 rpm and washing with PVP to obtain 200 µg / mL 30 mL of PVP-modified PVP-Au gold nanosphere aqueous solution.

[0046] (2) Preparation of Au@Pt nanocore-shell structure: Different volumes of 0.05 mL, 0.1 mL, 0.2 mL, 0.3 mL, 0.4 mL, and 0.5 mL of 10 mM chloroplatinic acid solution were quickly added to 5 mL of 200 µg / mL PVP-Au gold nanosphere aqueous solution, followed by 2 mL of 200 mM AA solution and vigorous stirring for 2 min. After being placed in a 40 °C oven for 12 hours, the mixture was centrifuged at 5000 rpm for 10 min, the supernatant was discarded, and the mixture was washed twice with deionized water, and finally dispersed in deionized water at a concentration of 200 µg / mL for later use.

[0047] (3) Au@Pt@Cu 2-x Se multi-component core-shell structure: At room temperature, 0.1 mL of 50 mM SeO2 aqueous solution and 0.2 mL of 200 mM AA aqueous solution were added to the aqueous solution of the Au@Pt nanocore-shell structure obtained above, in which 0.5 mL of 10 mM chloroplatinic acid solution was added. After 15 minutes of reaction, a mixture of 0.1 mL of 100 mM CuSO4·5H2O aqueous solution and 0.4 mL of 100 mM AA aqueous solution was added to the solution of Au@Pt-Se nanospheres. The reaction was allowed to proceed overnight, and then the excess PVP ligand was removed by multiple centrifugation at 5000 rpm. Finally, the obtained Au@Pt@Cu 2-x The Se multicomponent core-shell nanostructures are stored in water for further use.

[0048] Au@Pt@Cu 2-x The synthesis process of Se multi-component core-shell nanomaterials is shown in Figure (2).

[0049] Comparative Example 2 Cu 2-xSe@Au nanostructure: 200 µL of 0.1 M AA solution was added to 10 mL of 10 mg / mL PVP aqueous solution, followed by 0.1 mL of 50 mM SeO2 aqueous solution. After stirring for 10 minutes, the solution slowly changed from colorless to orange, indicating the formation of selenium nanospheres. 0.1 mL of the pre-prepared 0.1 M CuSO4·5H2O and 0.2 mL of 0.1 M AA mixed solution was added to the selenium nanosphere solution and stirred for 12 h. The solution gradually changed from gray to dark green, indicating the formation of Cu 2-x Then, 0.5 mL of 200 mM AA aqueous solution was added to the Cu 2-x Se aqueous solution, and then 0.4 mL 1 mM HAuCl4 aqueous solution was quickly injected under vigorous stirring. After reacting at room temperature for 30 minutes, Cu 2-x The Se@Au nanostructures were then purified by centrifugation at 8000 rpm and washed with water. 2-x The Se@Au meta-nanostructures were stored in water for further use.

[0050] Example 2 Performance Testing UV-visible absorption spectra: The obtained Au nanospheres and Au@Cu 2-x Se core-shell nanostructures, Au@Cu 2- x Se@Pt multi-component nanoflowers were added to a cuvette containing 2 mL of water and tested for UV-visible absorption spectroscopy. The results are shown in Figure 2 and Figure 3 shown.

[0051] from Figure 2 It can be seen that Cu 2-x The coating of Se on the surface of Au nanospheres caused the absorption peak of gold nanospheres to red-shift from 525 nm to 612 nm, and Cu 2-x The absorption peak of Se is 1132 nm.

[0052] Au@Cu grown in 0.4 mL 0.5 mL 10 mM chloroplatinic acid 2-x Se@Pt nanoflowers are taken as an example. Pt is further deposited on Au@Cu 2-x Se nanostructures grow on the surface, which increases the absorption intensity of the entire nanostructure and makes the gold nanospheres and Cu 2-x The absorption peak of Se is blue-shifted.

[0053] from Figure 3It can be seen that with the increase of the volume addition of 0.05 mL, 0.1 mL, 0.2 mL, 0.3 mL, 0.4 mL, 0.5 mL and 0.5 mL 10 mM chloroplatinic acid, the corresponding absorption peak in the second near-infrared region red-shifts from 1072 nm to 1168 nm, and the intensity increases from 0.50 to 0.95, while the corresponding absorption peak in the infrared region red-shifts from 591 nm to 598 nm, and the overall intensity in the entire wavelength range increases.

[0054] Morphology observation: Au nanospheres and Au@Cu 2-x Se nanocore-shell structure, Au@Cu 2-x Se@Pt multi-component nanoflowers, Au@Pt@Cu 2-x Se, Cu 2-x Se, Cu 2-x Se@Au nanostructures were dropped onto a 230-mesh copper grid, dried in an oven, and observed using a transmission electron microscope. The results are shown in Figure 4. Figure 5 , Figure 6 , Figure 7 , Figure 8 , Fig. 9 shown.

[0055] As can be seen from Figure 4 (a), the Au@Cu 2-x Se@Pt multi-component nanoflower material, with Au nanospheres as cores, the size is about 30 nm, Cu 2-x Se is the shell, the shell thickness is about 20 nm, and the Pt islands grow in the shape of petals. The morphology and size of the entire nanostructure are uniform. Figure 4 (b) shows the gold nanoparticles grown when reduced with sodium borohydride. They are small (about 5-6 nm in size) and unstable, and are prone to agglomeration. The preparation method of the Au nanospheres in Figure 4 (b) is as follows: First, under vigorous stirring, 0.25 mL of 50 mM HAuCl4 aqueous solution is added to 75 mL of aqueous solution containing 0.045 g of sodium borohydride, and the reaction is carried out for 15 minutes to synthesize gold seeds. 0.5 mL of aqueous solution containing 0.062 g of sodium borohydride and 0.25 mL of 50 mM HAuCl4 solution are added in sequence, and the reaction is continued for 15 minutes. Repeat this process three times, and the reaction solution is cooled to room temperature. The mixture was purified by centrifugation at 15,000 rpm and washing with PVP-containing water (i.e., an aqueous solution of PVP with a concentration of 10 mg / mL), and finally 200 µg / mL 30mL of PVP-modified PVP-Au gold nanosphere aqueous solution was obtained.

[0056] from Figure 5 It can be seen that when the volume of chloroplatinic acid added was 0.3 mL, a small amount of Pt nanoparticles were deposited on the Au@Cu 2-xA small amount of individual Pt nanoparticles were generated on the surface of Se core-shell nanoparticles. As the amount of chloroplatinic acid added was 0.5 mL, a large number of small Pt particles were deposited on the Au@Cu 2-x The surface of Se core-shell nanoparticles has some Cu 2-x Se will undergo a substitution reaction with Pt to generate a cavity structure, and the other part will self-nucleate to generate separate Pt nanoparticles. 2-x Relatively large Pt nanoflowers are generated on the surface of Se core-shell nanoparticles, while relatively few free Pt nanoparticles are generated.

[0057] from Figure 6 As can be seen, the STEM-EDX distribution map clearly proves that Au@Cu 2-x Se@Pt multi-component nanoflower structure, the brighter center and petals are Au and Pt, while the relatively darker in the middle is Cu 2-x Se shell structure, STEM-EDX elemental analysis further confirmed the Au@Cu 2-x Successful synthesis of Se@Pt multi-component nanoflower structure.

[0058] from Figure 7 It can be seen that the above Cu 2-x The order of Se and Pt raw materials was adjusted to obtain Au@Cu 2-x Se@Pt multi-component core-shell structure. In the presence of PVP and AA, Pt grows in islands on the gold nanospheres by reducing H2PtCl6 in the solution. This is because there is a large lattice mismatch between gold and palladium. The Pt multi-thorny structure grows more on the gold nanospheres. Pt basically completely covers the nanospheres, forming a thorny core-shell coating. 2-x Se is continuously deposited on its surface, Cu 2-x Se is interspersed in the gaps of the prickly Pt, Cu 2-x Se forms a uniform core-shell coating structure on the Au@Pt nanospiny surface.

[0059] from Figure 8 It can be seen from the STEM-EDX distribution diagram that Pt, Cu and Se elements are distributed in the outer layer, Au element is distributed in the inner core, and Pt, Cu and Se overlap with each other. The distribution once again confirms the Au@Pt@Cu 2-x Se nested sandwich nanostructure formation: Au@Pt@Cu 2-x Se multi-component core-shell structure.

[0060] from Fig. 9 It can be seen that the Cu grown directly using PVP as a surfactant 2-xSe nanospheres grew uniformly and were about 40 nm in size. Then, under the action of HAuCl4 and AA, Au nanospheres were deposited on Cu 2-x Se process island growth, and no free Au nanospheres appeared, successfully preparing Cu 2-x Se@Au nanostructures.

[0061] Hydroxyl radical ·OH generation and singlet oxygen 1 O2 generation: Au@Cu measured by electron spin resonance (ESR) 2-x Se and Au@Cu 2-x Se@Pt、Cu 2-x Se@Au catalyzes the production of ·OH and 1 O2 capacity, and 5,5-dimethyl-1-pyrroline-N-oxide (DMPO) as ·OH scavenger, 2,2,6,6-tetramethylpiperidine (TEMP) as 1 The O2 capture agent was irradiated with 1064 nm laser. Fig.10 and Fig.11 shown.

[0062] from Fig.10 It can be seen that when there is no Au@Cu 2-x In the case of Se@Pt, no obvious ESR signal was detected. 2-x In the ESR spectra of Se@Pt and H2O2 solutions, four characteristic peaks with a peak intensity ratio of 1:2:2:1 and three characteristic peaks with a peak intensity ratio of 1:1:1 are clearly seen, indicating that . OH and 1 When irradiated with 1064 nm laser, the ESR signal of ·OH is significantly enhanced. 1 The signal intensity of O2 also increases, which is due to the laser-induced Au@Cu 2-x As the temperature of Se@Pt nanoparticles increases, more ·OH and 1 O2. From Fig.10 and Fig.11 In comparison, only Au@Cu 2-x Se or Cu 2-x When Se@Au is used, ·OH can be generated, but not 1 O2, indicating that only Pt in Au@Cu 2-x Se or Cu 2-x The island growth of Se shell can catalyze the production of H2O2 1 O2. This further confirmed that Au@Cu 2-x Se@Pt multi-component core-shell nanoflower structure simultaneously catalyzes H2O2 to produce ·OH and 1 O2.

[0063] Potential and particle size: Au nanospheres, Au@Cu 2-x Se nanocore-shell structure, Au@Cu 2-x Se@Pt nanoflowers and Au@Cu 2-x Se@Pt-PEG nanoflowers were added into 1.5 mL of deionized water to test the changes of particle size and potential. The results are shown in Fig.12 shown.

[0064] from Fig.12 As can be seen from the figure, the synthesized Au nanospheres, Au@Cu 2-x Se nanocore-shell structure, Au@Cu 2-x Se@Pt nanoflowers and Au@Cu 2-x The hydrated particle sizes of Se@Pt-PEG nanoflowers are 51.23±5.71 nm, 89.53±6.83 nm, 110.62±8.96 nm, and 121.34±10.72 nm, respectively. The hydrated particle sizes of the nanoparticles gradually increase, which is due to the gradual deposition of Cu on the basis of Au nanospheres. 2-x Se, Pt and PEG modified to increase biocompatibility. The surface potential of Au nanospheres is -22.46±4.46 mV. 2-x After Se shell wrapping, Au@Cu 2-x The surface potential of Se decreased to -18.54±3.54 mV, and further Pt 2-x The surface potential of Se islands became less negative and was -14.62±3.62 mV. In order to increase biocompatibility and reduce biotoxicity, the potential was finally -10.72±2.72 mV after PEG modification.

[0065] XRD spectrum: Au nanospheres, Au@Cu 2-x Se core-shell nanostructures, Au@Cu 2-x Se@Pt nanoflowers and Au@Cu 2-x Se@Pt-PEG nanoflowers were added repeatedly onto the silicon diffraction plate and then dried. Fig.13 shown.

[0066] from Fig.13 It can be seen that Au@Cu 2-x Se core-shell structure, Au@Cu 2-x The XRD spectra of the two nanostructures of Se@Pt nanoflowers show that all the diffraction peaks of the two prepared structures are consistent with the cubic crystal structure of Au (JCPDS#01-1172) and Cu 2-xThe standard data of cubic crystal structure of Se (JCPDS#06-0680) and cubic phase of Pt (JCPDS#04-0802) correspond perfectly, indicating that Au@Cu with good crystallinity has been successfully prepared. 2-x Se@Pt nanoflowers. and Au@Cu 2-x Compared with the characteristic diffraction peak of Se, the characteristic diffraction peak of Pt appears at 39.763 o ,46.232 o The corresponding (111) and (200) crystal planes indicate that Pt is successfully deposited on Au@Cu 2- x Se is deposited on the core-shell structure.

[0067] Photothermal performance testing: The obtained Au@Cu 2-x Se@Pt nanoflower materials were prepared into solutions of different concentrations of 12.5 μg / mL, 25.0 μg / mL, 50.0 μg / mL, 75.0 μg / mL, 100.0 μg / mL, and 125.0 μg / mL and placed in centrifuge tubes. A solution with a concentration of 125.0 μg / mL was selected to test the photothermal stability of the solution. The light was measured at 1064 nm, 1 W / cm 2 The laser irradiates the solution with a laser power of 10 times and switches on and off. The thermal imager collects and analyzes the data. The results are shown in the figure below. Fig.14 shown.

[0068] from Fig.14 It can be seen that at 1.0 W / cm 2 After 10 min of 1064 nm laser irradiation, the steady-state temperature of the solution increases with the Au@Cu 2-x The concentration of Se@Pt gradually increased with the increase of concentration. 2-x The temperature of Se@Pt aqueous solution increased by about 42 ºC compared with the initial temperature, which was significantly higher than that of 12.5 μg / mL Au@Cu under the same conditions. 2-x Temperature difference of Se@Pt aqueous solution in water (12ºC). In order to investigate the photothermal stability of the material, 125 μg / mL Au@Cu 2-x Se@Pt aqueous solution was placed at 1 W / cm 2 The Au@Cu@C was irradiated with 1064 nm laser for 10 min and then turned off the laser and cooled to room temperature. 2- x The photothermal performance of Se@Pt did not show a significant decrease, indicating good photothermal stability.

[0069] Photoacoustic imaging performance: Obtained Au@Cu 2-xSe@Pt nanoflower materials were prepared into solutions with a certain concentration gradient, such as 0 µg / mL, 25 µg / mL, 50 µg / mL, 75 µg / mL, 100 µg / mL, 125 µg / mL, and 150 µg / mL, and placed in a 500 µL centrifuge tube for in vitro photoacoustic performance testing. The results are shown in Figure 2. Fig.15 As shown; Depend on Fig.15 It can be seen that with the Au@Cu 2-x As the concentration of Se@Pt nanoflower material increases, the photoacoustic signal intensity increases, and the concentration and signal intensity are proportional. When the concentration is 150 µg / mL, the photoacoustic intensity is as high as 1600, which is very suitable for in vivo photoacoustic imaging.

[0070] Cytotoxicity analysis: U87 cells and L-02 cells in logarithmic growth period were collected and cultured at 8×10 3 The cells were seeded at a density of 100 cells / well in a 96-well plate and incubated with different concentrations (0, 25, 50, 100, 125, and 150 μg / mL) of Au@Cu 2-x Se@Pt nanoflowers were co-cultured with cells for 24 h and illuminated with a 1064 nm laser (1.0 W / cm 2 ) for 5 min. Then, the cells were cultured in an incubator for 4 h, the culture medium was aspirated, and the cell viability test was performed using the CCK-8 assay to evaluate the Au@Cu 2-x The cytotoxicity of Se@Pt nanoflowers to U87 cells is shown in the following table. Fig.16 shown.

[0071] In in vitro experiments, Au@Cu 2-x Se@Pt promotes the generation of H2O2·OH and 1 O2 has excellent ability, so we further studied it at the cellular level using U87 brain glioma cells and L-02 human normal liver cells. Fig.16 As can be seen in (a), when using 150 μg / mL Au@Cu 2-x After Se@Pt-PEG treatment, more than 80% of L-02 cells were still alive, indicating that Au@Cu 2-x Se@Pt-PEG nanomaterials have good biocompatibility with L-02 cells. Fig.16 (b) As shown, Au@Cu 2-x The activity of Se@Pt-PEG on U87 cells decreased with the increase of nanomaterial dosage. 2-x Compared with Se@Pt-PEG nanoflower materials, Au@Cu 2-xThe Se@Pt-PEG+1064 nm treatment caused more U87 cell death, which is due to the higher H2O2 level in cancer cells than in normal cells. After 1064 nm laser irradiation, almost all cancer cells were effectively killed, which was much higher than that without laser irradiation. The photocatalytic reaction induced by the light-enhanced Fenton-like reaction and surface plasmon holes in cancer cells promoted the release of ·OH and 1 O2 is produced, leading to increased cell apoptosis. Au@Pt@Cu 2-x In vitro cytotoxicity of Se-PEG on U87 and L-02 cells.

[0072] In vivo photothermal antitumor performance: 100 μL U87 cells (5×10 6 The breast tumor model was established by subcutaneously injecting 100 cells into the right armpit of nude mice. 3 The mice were used for in vivo experiments. U87 tumor-bearing mice were randomly divided into 4 groups (n=5) for in vivo anticancer studies and intravenously injected with PBS (200 μL, PBS, pH=7.4) (Group 1), PBS (200 μL, PBS, pH=7.4) + 1064 laser (Group 2), and Au@Cu 2-x Se@Pt (200 µL, 10 mg / kg) (Group 3), Au@Cu 2-x Se@Pt (200 µL, 10 mg / kg) + 1064 laser (Group 4). The power density of 1064 nm laser was 1 W / cm 2 , the irradiation time is 10 min, such as Fig.17 Laser irradiation was performed 12 h after injection. After treatment, the body weight and tumor volume of each mouse were measured every other day. Fig.18 (a) and Fig.18 (b) As shown. On day 14 after treatment, the mice were sacrificed and the tumors were collected for histopathological analysis. Fig.18 (c) shown.

[0073] from Fig.17 As can be seen in Figure 1, 12 hours after intravenous injection, laser irradiation (1 W / cm 2 , 10 min), we can clearly see that Au@Cu 2-x The tumor temperature of Se@Pt-treated mice irradiated with 1064 nm laser increased to 56.0 °C, which was sufficient to effectively kill cancer cells through PTT; in contrast, the tumor steady-state temperature of Group 2 was only 37.5 °C.

[0074] from Fig.18As can be seen in (a), no obvious weight change was observed, only a slight increase, indicating that Au@Cu 2-x Se@Pt has no systemic toxicity. Fig.18 As can be seen in (b), tumor growth was not inhibited in mice treated with PBS or +1064 nm laser. 2-x The mice treated with Se@Pt and +1064 nm laser completely inhibited tumor growth, and the therapeutic effect was far better than that of Au@Cu alone. 2-x Se@Pt treated mice (Group 3), which was mainly attributed to the +1064 nm laser-induced Au@Cu 2-x Se@Pt produces toxic substances OH, 1 O2 and thermal effects. Whether it is PBS alone (Group 1) or PBS plus +1064 nm laser irradiation (Group 2), due to the lack of Au@Cu 2-x Se@Pt, did not show effective tumor growth inhibition. These results confirm the multifunctional Au@Cu 2-x Se@Pt has anticancer effects, and +1064 nm laser-triggered synergistic therapy significantly improves the therapeutic effect.

[0075] from Fig.18 (c) After 14 days of various treatments, the tumor sections collected from U87 tumor-bearing mice were subjected to histological analysis. Hematoxylin and eosin (H&E) staining further confirmed that the light-enhanced CDT / PCT / PTT combined treatment caused severe damage to tumor tissue and could effectively inhibit the proliferation of tumor cells. 2-x Se@Pt exhibited the best therapeutic effect, Au@Cu 2-x The cell apoptosis or necrosis in the tumor tissue irradiated by Se@Pt+1064 nm laser was more serious than that in other groups, which was attributed to the superior photothermal performance, ·OH and 1 O2 generation capacity.

[0076] A person skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of protection of the present application is limited to these examples. In line with the concept of the present application, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of different aspects of one or more embodiments of the present application as described above, which are not provided in detail for the sake of simplicity.

[0077] One or more embodiments of the present application are intended to cover all such substitutions, modifications and variations that fall within the broad scope of the present application. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of one or more embodiments of the present application should be included in the protection scope of the present application.

Claims

1. A multi-component nanoprobe, characterized in that it comprises Au@Cu 2-x Se@Pt and modified Au@Cu 2-x PEG on the Se@Pt surface, the Au@Cu 2-x Se@Pt is Au nanospheres, and Cu 2-x Se, and islands grown on Cu 2-x Pt on Se surface.

2. A method for preparing a multi-component nanoprobe as claimed in claim 1, characterized in that: The following steps are included: Chloroplatinic acid solution and Au@Cu 2-x Se solution, add reducing agent, react, centrifuge, wash, and obtain Au@Cu 2-x Se@Pt, then Au@Cu 2-x The Se@Pt solution and methoxypolyethylene glycol-thiol are mixed and reacted to obtain a multi-component nanoprobe.

3. The preparation method according to claim 2, characterized in that: The reducing agent is ascorbic acid.

4. The preparation method according to claim 2, characterized in that: The Au@Cu 2-x The preparation method of Se is as follows: mixing an aqueous solution of chloroauric acid and an aqueous solution of sodium citrate, boiling to obtain gold seeds, then lowering the temperature to 85-95°C, sequentially adding an aqueous solution of sodium citrate and an aqueous solution of chloroauric acid, reacting, cooling, centrifuging, washing and purifying to obtain Au nanospheres; sequentially adding an aqueous solution of selenium oxide and an aqueous solution of ascorbic acid to an aqueous solution of Au nanospheres, then adding a mixture of an aqueous solution of copper sulfate and an aqueous solution of ascorbic acid, reacting, centrifuging, and obtaining Au@Cu 2-x Se.

5. The preparation method according to claim 4, characterized in that: The temperature was lowered to 90°C, and aqueous sodium citrate solution and aqueous chloroauric acid solution were added in sequence.

6. The preparation method according to claim 4, characterized in that: During the water washing and purification, an aqueous solution containing PVP is used for water washing and purification.

7. The preparation method according to claim 4, characterized in that: The sodium citrate aqueous solution and the chloroauric acid aqueous solution are added once or more.

8. The preparation method according to claim 4, characterized in that: The molar concentration of the chloroauric acid aqueous solution is 50 mM.

9. The preparation method according to claim 4, characterized in that: The mass concentration of the sodium citrate aqueous solution is 0.0006 g / mL.

10. A use of the multi-component nanoprobe as claimed in claim 1, characterized in that: Used for preparing drugs for treating and / or diagnosing tumors.

Citation Information

Patent Citations

  • Medical multifunctional optical probe, preparation method thereof and application of medical multifunctional optical probe in surgical navigation

    CN117414445A