Asymmetric UPE filter membrane and preparation process thereof

Through the non-directional tortuous path and the structural design of the loose area and dense area of ​​the asymmetric UPE filter membrane, the problem of high retention and high flux of the existing UPE porous membrane is solved, and the filtration effect of high load capacity and high flux is achieved. , suitable for liquid and gas sterilization fields.

CN118743931APending Publication Date: 2024-10-08HANGZHOU COBETTER FILTRATION EQUIPMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410945287.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

When balancing high retention capacity and high flux, it is difficult for existing UPE porous membranes to balance high loading capacity, and the flux is easily attenuated due to clogging of small pores.

Method used

It adopts an asymmetric UPE filter membrane design, with a non-directional tortuous path and a loose zone and dense zone structure. The average pore size of the loose zone is larger than that of the dense zone, and the thickness of the dense zone is not higher than 15%, ensuring high flux and high loading capacity of the filter membrane. At the same time, the interception capacity is improved through appropriate pore size distribution and structural design.

Benefits of technology

It is possible to significantly increase the flux and capacity of the filter membrane without reducing the retention capacity, ensuring high-efficiency filtration performance under different working conditions, including liquid and gas sterilization applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118743931A_ABST
    Figure CN118743931A_ABST
Patent Text Reader

Abstract

The invention relates to an asymmetric UPE filter membrane and a preparation process thereof, the filter membrane comprises a porous main body, a non-directional zigzag passage is arranged in the porous main body, and the PMI average pore size of the filter membrane is 0.08-0.7 [mu] m; in the thickness direction of the porous main body, the porous main body comprises a large-thickness loose layer (accounting for at least 85% of the total thickness of the filter membrane) and a small-thickness compact layer (accounting for not higher than 15% of the thickness of the porous main body), the resistance of the filter membrane to feed liquid is greatly reduced due to the special morphology structure, the flux of the filter membrane is remarkably improved, and meanwhile, the performance of the filter membrane is improved. The large-thickness loose layer provides enough accommodating space for large-particle impurities, the loading capacity of the filter membrane is remarkably improved, further, the large-thickness and low-density loose layer makes up for the loss of the interception capability of the filter membrane due to the small-thickness compact layer, and it is guaranteed that the final filter membrane has good bacterium interception capability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of membrane separation technology, and more particularly to an asymmetric UPE filter membrane and a preparation process thereof. Background Art

[0002] Polymer filter membrane is a thin film made of organic high molecular polymer, which mainly plays the role of filtering and separating impurities. According to the different high molecular polymers, polymer filter membranes can be divided into cellulose polymer filter membranes, polyamide polymer filter membranes, polysulfone polymer filter membranes, polyester polymer filter membranes, polyolefin polymer filter membranes, etc.

[0003] Among them, polyolefin polymer porous membranes, especially UPE filter membranes, do not contain fluorine (Europe, the United States, etc. have successively proposed the ban on perfluoro / polyfluoroalkyl substances), and have excellent advantages such as resistance to low temperatures, chemical corrosion, impact resistance, wear resistance, and resistance to gamma-ray irradiation. Therefore, they play a very important role in more complex fields such as semiconductors, batteries, and biopharmaceuticals.

[0004] For example, the Chinese invention patent application document CN113694745A (Hangzhou Longze Filter Equipment Co., Ltd.) discloses a UPE porous membrane with a high specific surface area and a preparation method and use thereof. The UPE porous membrane is a symmetrical membrane with a thickness of 1-30 μm (preferably 5-20 μm), a pore size of the first porous outer surface and a pore size of the second porous outer surface are both 1-150 nm, and the specific surface area of ​​the UPE porous membrane is not less than 35 m 2 / g, the higher specific surface area allows the filter membrane to have more contact with the liquid to be filtered. Under the effect of the relatively higher specific surface area and the relatively ideal pore size, the thin-film UPE membrane has a higher retention capacity. At the same time, since the filter membrane is a symmetrical membrane, any outer surface of the membrane can be used as the first surface in actual use, making the assembly of the membrane and other related processes simpler.

[0005] The above-mentioned UPE porous membrane has a high interception efficiency and a low assembly difficulty, however, the above-mentioned filter membrane still has certain shortcomings. First, the UPE porous membrane is a symmetrical membrane. In order to ensure the interception capacity of the filter membrane, the size of its membrane pore structure should not be too large. However, a filter membrane with a relatively small membrane pore size often means that it has a relatively large resistance to the feed liquid, and the flux of the filter membrane is relatively low, that is, it is difficult to have both high flux and high interception. Secondly, the relatively small membrane pore structure is more easily blocked by impurity particles, and once the particulate impurities block the relatively small membrane pores, it will cause the flux of the filter membrane to be greatly attenuated, that is, it is difficult to have both high flux and high loading of the filter membrane.

[0006] In summary, how to prepare a UPE filter membrane with high retention capacity, high flux and high loading capacity is an urgent problem to be solved by those skilled in the art. Summary of the invention

[0007] In view of the shortcomings of the prior art, the present invention aims to provide an asymmetric UPE filter membrane and a preparation process thereof, which has high loading capacity, high flux and high retention capacity, and is particularly suitable for liquid sterilization or gas sterilization. To achieve the above purpose, the present invention provides the following technical solutions:

[0008] In a first aspect, the present application provides an asymmetric UPE filter membrane, which adopts the following technical solution:

[0009] An asymmetric UPE filter membrane comprises a porous body, wherein the porous body has a non-directional tortuous passage, the porous body has a first surface for fluid to flow in and a second surface for fluid to flow out, and the PMI average pore size of the UPE filter membrane is 0.08-0.7 μm; along the thickness direction of the porous body, the porous body comprises a loose area and a dense area, the loose area and the dense area are continuously transitioned, one side surface of the loose area is the first surface, and one side surface of the dense area is the second surface, the average pore size of the loose area is greater than the average pore size of the dense area, the thickness of the porous body is 60-140 μm, and the thickness of the dense area in the porous body accounts for no more than 15%.

[0010] By adopting the above technical scheme, the main body of the UPE filter membrane of the present application has a non-directional tortuous path, which refers to a randomly oriented groove structure and / or a discretely distributed hole structure, and each non-directional tortuous path is interconnected. The filter membrane in the present application has an asymmetric membrane structure. Along its thickness direction, loose areas and dense areas can be seen in turn, and the two transition continuously. "Continuous" means that basically all the entity parts are connected to each other as a whole, such as being formed as one piece, without the need to use additional adhesives to connect them to each other. Unless torn by external force, the network-like fibers cannot be separated from each other. The PMI average pore size of the filter membrane of the present application is 0.08-0.7μm. Under the synergistic effect of the appropriate PMI average pore size and the non-directional tortuous path, the retention performance of the UPE filter membrane of the present application is ensured, especially the good filtration effect on bacteria.

[0011] The present application provides an "asymmetric" UPE filter membrane, wherein "asymmetry" specifically refers to that the membrane pore structure of the UPE filter membrane changes with the pore depth, and the structures of the porous bodies on the two side surfaces and their vicinities are different, that is, the porous bodies on the two side surfaces and their vicinities form pore structures of different sizes. Among them, the porous bodies on the first surface and its vicinity form a loose area with relatively low density of the filter membrane of the present application (the density of the loose area specifically refers to the ratio of the volume of the solid part of the loose area to the volume of the entire loose area), and the porous bodies on the second surface and its vicinity form a dense area with relatively high density of the filter membrane of the present application. Figure 1 In this application, the dense area and the loose area of ​​the filter membrane can be distinguished by the following method: the cross section of the filter membrane is characterized by scanning electron microscopy ( Figure 1 The magnification is 500 times, of course, a larger or smaller magnification can also be used, subject to the ability to clearly distinguish the overall structure of the filter membrane cross section), and the corresponding SEM image is obtained. Along the thickness direction of the filter membrane, the area where the pore structure can be clearly observed is considered to be the relatively "loose" part in the SEM image of the filter membrane. This area is the loose area of ​​the filter membrane of the present application. Conversely, along the thickness direction of the filter membrane, the area where the pore structure cannot be clearly observed is the dense area of ​​the filter membrane of the present application.

[0012] It is generally believed that the pressure bearing capacity of the porous body on the first surface and its vicinity of the filter membrane with a large thickness ratio in the loose area is relatively insufficient. Under high pressure, the porous body on the first surface and its vicinity will often deform and collapse to a certain extent, thereby affecting the performance of the membrane (including the flux, load and retention performance of the filter membrane). Therefore, the loose area with a large thickness ratio is often a discarded technical means. However, the inventors of this application found that the performance of the filter membrane with a large thickness ratio in the loose area (small thickness ratio in the dense area) has not decreased, and in particular, under certain working conditions, the performance of the filter membrane has been significantly improved, which is quite unexpected.

[0013] This may be because, firstly, the filter membrane of the present application has a relatively thick thickness (60-140μm), which ensures that the filter membrane of the present application itself has relatively good self-supporting performance (relatively good pressure resistance). Even in the face of relatively high-pressure working conditions, the overall deformation of the filter membrane of the present application (especially the first surface and the porous body near it) is relatively limited. Secondly, the thickness of the dense area of ​​the filter membrane of the present application accounts for no more than 15% of the thickness of the porous body, that is, along the thickness direction of the filter membrane, the thickness of the loose area accounts for at least 85% of the total thickness of the filter membrane. The loose area with large thickness and low density, on the one hand, greatly reduces the overall resistance of the filter membrane to materials (including liquid materials and gas materials), and ensures that the porous body on the first surface of the filter membrane and the vicinity has a relatively sufficient effective flow area for the feed liquid to enter. Under the combined effect of the two, the flux of the filter membrane is significantly improved; on the other hand, it ensures that the first surface and the vicinity of the porous body have relatively sufficient pollution-receiving space, which can pre-intercept and accommodate large particles of impurities in the feed liquid, greatly reducing the possibility of large particles of impurities clogging the membrane pore structure, that is, significantly improving the load capacity of the filter membrane. Although the pore size of the loose zone is relatively large, the loose zone with great thickness, through the continuous stacking of membrane pores and membrane pores in the direction of membrane thickness, makes the retention effect of the loose zone smaller than the size of its actual pore structure, that is, the loose zone with great thickness and low density plays a partial pre-retention role. Furthermore, with the continuous interception of the loose zone (including pre-retention of bacteria and retention of large particle impurities), the pore size of the loose zone continues to decrease, and the retention capacity of the loose zone for bacteria is further improved. That is, although the thickness of the dense zone of the present application is relatively small, the loose zone with great thickness and low density makes up for the loss of the retention capacity of the filter membrane of the present application, thereby ensuring that the final filter membrane's bacteria retention capacity still meets actual needs. That is, the filter membrane of the present application has an appropriate thickness, which first ensures that the filter membrane of the present application has a relatively high pressure resistance in actual use and ensures the integrity of the overall membrane pore structure of the filter membrane. At the same time, the filter membrane of the present application has an appropriate thickness ratio of loose areas and dense areas. Under the synergistic effect of the appropriate thickness, although the filter membrane thickness is relatively thick, the overall resistance of the filter membrane to the fluid is still relatively small, the overall flux of the filter membrane is still relatively high, and the large thickness of the loose area ensures the overall load capacity of the filter membrane. At the same time, the overall filter membrane's ability to retain bacteria still meets actual needs.

[0014] Further, under certain specific working conditions, the research and development personnel of this application hope that the filter membrane will be deformed to a certain extent to further ensure the performance of the filter membrane. For example, in the field of gas sterilization, especially for closed containers such as fermentation tanks, with the fermentation process of fermentation bacteria (such as yeast), temperature and other influences, the air pressure inside the fermentation tank is not stable. For example, in the early stage of fermentation, with the increase of yeast activity and the production of carbon dioxide, the pressure in the fermentation tank will gradually increase. As the fermentation proceeds, the pressure in the fermentation tank will gradually stabilize and begin to decline when the fermentation is close to the end. For this working condition, under a certain pressure, the UPE filter membrane in this application, the loose layer with a large thickness ratio, has a process of adaptive adjustment. In the early stage of fermentation, when the air pressure in the fermentation tank is relatively high, the porous body of the first surface of the filter membrane and its vicinity shrinks to a certain extent under the influence of air pressure, and the density of the porous body of the first surface of the filter membrane and its vicinity rises relatively, thereby ensuring the pressure-bearing performance of the filter membrane as a whole, and then ensuring the high flux of the membrane (under high air pressure, the filtration driving force of the membrane is originally large, and the flux of the membrane is relatively large). At the same time, under high pressure, the driving force of the airflow is relatively large, and the bacteria in the airflow can easily penetrate the filter membrane under the influence of the airflow with excessive flow rate, while the filter membrane with increased density can appropriately reduce the flow rate of the airflow, thereby increasing the probability of bacteria in the airflow directly colliding with the solid part of the filter membrane, that is, solving the problem that the risk of filter membrane leakage is relatively high under high pressure conditions due to the fast flow rate of the airflow. Of course, since the filter membrane of the present application has a relatively suitable thickness, it itself has a relatively ideal self-supporting performance. Therefore, the deformation degree of the filter membrane as a whole (especially the first surface and the porous body near it) will not be too large, that is, the filter membrane will not be blocked by air pressure, which will eventually affect the performance of the filter membrane.

[0015] Different from liquid filtration, the filter membrane for gas filtration is not limited to the particle size exclusion type screening and interception. The small impurities in the membrane often perform irregular Brownian motion. The impurity particles that perform irregular Brownian motion often collide with the entity part in the membrane and are thus intercepted. The smaller the particle size of the impurity particles, the more violent their irregular motion, the more chances of hitting obstacles, and the better the filtering effect. Therefore, for the filter membrane for gas filtration, the pore size of its pore structure can often be appropriately larger to ensure the high load and high flux of the membrane. Therefore, even if the porous body on the first surface of the filter membrane and its vicinity shrinks to a certain extent, its load will not be significantly reduced. At the same time, after the porous body on the first surface and its vicinity shrinks to a certain extent, the relatively dense pore structure further enhances the interception capacity of the membrane, further ensuring that the membrane has high interception under the premise of high flux.

[0016] As the fermenter runs for a long time, the air pressure in the fermenter will gradually decrease, that is, the filtration driving force of the filter membrane will gradually decrease, and as the filter membrane is continuously intercepted, a certain filter cake will be formed inside the filter membrane, and this part of the filter cake narrows the passage for gas circulation in the membrane to a certain extent. The two will often cause the flux of the filter membrane to be significantly reduced through the action, and for the filter membrane of the present application, as the air pressure in the fermenter decreases, the originally contracted first surface of the filter membrane and the porous body near it will relax, further widen the passage of the filter membrane, and further ensure the flux and load of the filter membrane. And the flux improvement (airflow velocity) brought by the relaxation of the porous body will increase the motion inertia of impurity particles in the airflow, thereby increasing the possibility of inertial interception, so that the filter membrane has a good interception capacity. Further, due to the continuous interception of the filter membrane, the pore structure inside it becomes relatively smaller, even if the porous body on the first surface of the filter membrane and the porous body near it relax, the overall interception performance of the filter membrane will not be reduced too much, which further ensures the flux, load and interception of the filter membrane in the late fermentation period.

[0017] For another example, the filter membrane of the present application can be applied to the front-end filtration (liquid filtration) in the semiconductor field. For the filtration in the semiconductor field, the cleanliness of the filtrate is very important, and for the filter membrane that needs to be recycled, the cleaning of the filter membrane also needs to be taken seriously. For the filter membrane of the present application, since the filter membrane has a loose layer with a large thickness ratio, the loose layer with a large thickness ensures the high load of the filter membrane. Similarly, when the filter membrane is cleaned after the pressure is removed after the pressurized filtration, the membrane pores of the entire filter membrane will expand, making it easier to release the intercepted materials inside the filter membrane, that is, ensuring the high cleanliness of the filter membrane after cleaning, that is, ensuring the high retention of the filter membrane. Similarly, since there are fewer impurities remaining inside the filter membrane after cleaning, the recovery rate of the filter membrane flux is higher, and there is also a larger and more space inside the filter membrane to intercept the impurities in the filtrate, that is, ensuring the high flux and high load of the filter membrane.

[0018] In summary, the present application provides a UPE filter membrane with an appropriate thickness (60-140 μm), which ensures that the filter membrane as a whole has ideal self-supporting performance. Furthermore, the UPE filter membrane has a large-thickness loose area (accounting for at least 85% of the total thickness of the filter membrane) and a small-thickness dense area (accounting for no more than 15% of the thickness of the porous body). The special thickness ratios of the two support each other, greatly reducing the resistance of the filter membrane to the feed liquid, significantly improving the flux of the filter membrane, and the large-thickness loose area provides sufficient accommodation space for large particle impurities, significantly improving the load capacity of the filter membrane. Furthermore, the large-thickness and low-density loose area compensates for the loss of the retention capacity of the filter membrane of the present application, ensuring that the final filter membrane has only a small reduction (or even no reduction) in its ability to retain bacteria, and ultimately enables the UPE filter membrane of the present application to achieve high flux, high load and high retention effects under various working conditions.

[0019] Optionally, the complete bubbling point of the porous body is 0.16-0.24 MPa, and the porosity of the porous body is 60-85%.

[0020] By adopting the above technical scheme, the bubble point is an important performance characteristic of the membrane, and the level of the bubble point affects the application range of the UPE filter membrane; the test method of the bubble point is well known in the art, for example, the procedures of these tests are explained in detail in GB / T32361-2015, which is incorporated herein by reference. The test liquid used in the present invention is IPA (isopropyl alcohol); the bubble point is divided into an initial bubble point and a complete bubble point; first, take the UPE filter membrane (dry membrane) of this application and draw a gas flow-pressure diagram of the dry membrane. Subsequently, the UPE filter membrane is completely infiltrated with the test liquid, and the gas pressure on the membrane side is increased at a slow rate. The pressure when the gas passes through the liquid seal layer of the separation membrane and the first string of continuous bubbles appears is the initial bubble point. The "maximum pore size" of the filter membrane can be calculated from the initial bubble point pressure. The smaller the initial bubble point, the larger the "maximum pore size" inside the membrane. On the contrary, the larger the initial bubble point, the smaller the maximum pore size. At the same time, draw the gas flow-pressure diagram of the UPE filter membrane (wet membrane), and find the intersection between the wet membrane gas flow line and the dry membrane half flow line. The pressure at this time is the complete bubble point. The complete bubble point is used to characterize the "average pore size" inside the membrane. The larger the complete bubble point, the smaller the "average pore size". Conversely, the smaller the complete bubble point, the larger the "average pore size".

[0021] It can be understood that the bubble point is used to characterize the "smallest" pore size in the tortuous path of the filter membrane to a certain extent, the initial bubble point is used to characterize the maximum value of the "smallest" pore size in the tortuous path of the filter membrane to a certain extent, and the complete bubble point is used to characterize the average value of the "smallest" pore size in the tortuous path of the filter membrane to a certain extent. For the UPE filter membrane of this application, the pore size of the dense area is much smaller than the pore size of the loose area. Therefore, the "smallest" pore size in the tortuous path of the filter membrane often exists in the dense area. That is, the initial bubble point is used to characterize the maximum pore size in the dense area of ​​the UPE filter membrane, and the complete bubble point is used to characterize the "average pore size" in the dense area of ​​the UPE filter membrane.

[0022] The UPE filter membrane of the present application has a relatively ideal complete bubbling point, that is, the dense area of ​​the UPE filter membrane of the present application has an average pore size with a suitable pore size as a whole, which first ensures the efficient retention of bacteria by the filter membrane. At the same time, the dense area of ​​the small thickness of the filter membrane has an average pore size with a suitable pore size and the porous body as a whole has a relatively suitable porosity, which ensures the low resistance of the filter membrane as a whole to the feed liquid and further ensures the high flux of the filter membrane. In addition, the dense area of ​​the filter membrane has an average pore size with a suitable pore size, which further reduces the probability that the retained material (bacteria) will block the pore structure of the dense area and cause a significant attenuation of the filter membrane flux, that is, the high loading capacity of the filter membrane is ensured.

[0023] If the complete bubble point of the porous body is too large (such as greater than 0.24MPa) and / or the porosity of the porous body is too low (such as less than 60%), it indicates to a certain extent that the overall density of the UPE filter membrane is relatively high, especially the pore structure in the dense area of ​​the filter membrane is relatively small and relatively few, the overall resistance of the filter membrane to the flow of the feed liquid is relatively high, and the flux of the filter membrane cannot be significantly improved. At the same time, the intercepted material (bacteria) is relatively easy to block the pore structure in the dense area, and the filter membrane load is relatively low. If the complete bubble point of the porous body is too small (such as less than 0.16MPa) and / or the porosity of the porous body is too high (such as greater than 85%), it indicates to a certain extent that the overall density of the UPE filter membrane is relatively low, especially the pore structure in the dense area of ​​the filter membrane is relatively large, which certainly means that the filter membrane as a whole has high flux and high load, but it also means that the high retention capacity of the filter membrane cannot be effectively guaranteed.

[0024] In summary, the dense area of ​​the filter membrane has an appropriate average pore size, and the porous body as a whole has a relatively suitable porosity, which further ensures the high retention, high flux and high loading capacity of UPE.

[0025] Optionally, the initial bubble point of the porous body is 0.14-0.20 MPa, and the ratio of the initial bubble point of the porous body to the complete bubble point of the porous body is 0.7-0.9.

[0026] By adopting the above technical scheme, as mentioned above, the UPE filter membrane of the present application has a suitable initial bubble point, which means that the dense area inside the UPE filter membrane of the present application has a maximum pore size with a suitable pore size. Furthermore, there is a suitable ratio between the initial bubble point and the complete bubble point of the porous body, that is, there is a suitable ratio between the maximum pore size inside the dense area of ​​the UPE filter membrane and the average pore size, which means that the overall pore size distribution of the dense area of ​​the UPE filter membrane of the present application is relatively uniform, further ensuring the high flux, high loading capacity and high retention of the UPE filter membrane of the present application.

[0027] If the initial bubble point of the porous body is too small (such as less than 0.14MPa) and / or the ratio between the initial bubble point of the porous body and the complete bubble point is too small (such as less than 0.7), it means that the maximum pore size of the dense zone of the UPE filter membrane of the present application is relatively large and the average pore size is relatively small, and the overall pore size distribution of the dense zone is uneven (there are a certain number of large and small pores). The presence of too many large pores will cause the filter membrane to lose its ability to retain bacteria to a certain extent, that is, the high retention of the filter membrane cannot be guaranteed, and too many small pores will cause the overall resistance of the filter membrane to the feed liquid to increase, so that the filter membrane cannot guarantee high flux, and the probability of small pores being blocked by bacteria is relatively high. Once the small pores are blocked, the flux of the filter membrane will also decay, that is, the high loading capacity of the filter membrane cannot be guaranteed.

[0028] Therefore, current researchers often hope that the pore size of the dense area (area used for interception) of the filter membrane is as uniform as possible. Different from conventional cognition, the ratio between the initial bubble point and the complete bubble point of the porous body of the UPE filter membrane of the present application is not greater than 0.9, that is, the UPE filter membrane of the present application still hopes that there are some large pores in the dense area. This may be because the average pore size of the dense area as a whole is relatively small. Therefore, the introduction of the dense area will inevitably bring about the problem of membrane flux attenuation to a certain extent. The presence of a part of large pores in the dense area makes up for the problem of membrane flux attenuation caused by the introduction of the dense area to a certain extent, that is, the high flux of the filter membrane of the present application is guaranteed. Although there are some large pores in the dense area, as mentioned above, the loose area with a specific large thickness and low density of the present application makes up for the bacterial interception of the filter membrane of the present application to a certain extent. Under the synergistic effect of the two, it is ensured that the final filter membrane has not only no reduction in bacterial interception capacity and flux, but even slightly improved.

[0029] Optionally, the porous body has a gram weight of 0.035-0.055 g /

[0030] By adopting the above technical scheme, the porous main body has suitable thickness and gram weight, further illustrating that the filter membrane of the present application has suitable pore structure as a whole, and then further ensuring that the filter membrane of the present application has higher flux, higher load and more efficient bacteria interception ability as a whole. This is because the gram weight and density (density of UPE) of the porous main body are known, and the theoretical volume of the porous basement membrane per unit area can be obtained by calculation (if the porous basement membrane is a completely dense object without any pore structure, the size of the three-dimensional space occupied by the porous basement membrane). At the same time, due to the actual thickness of the porous basement membrane, the actual volume of the loose area per unit area can be obtained by metering, and the difference between the actual volume and the theoretical volume is the volume of the pore structure in the porous basement membrane.

[0031] If the mass per unit area of ​​the porous body is too small (e.g., less than 0.035 g / That is, the mass of the membrane with a diameter of 47mm is less than 0.035g) and the thickness is too high (such as greater than 140μm). This shows that the UPE filter membrane is too loose as a whole, and the number of pore structures inside the loose area is too large and the volume is too large. On the one hand, the UPE filter membrane's ability to retain bacteria cannot be effectively guaranteed. On the other hand, the UPE filter membrane's overall pressure resistance is insufficient. Under the action of the liquid pressure, the probability of the overall pore structure of the filter membrane being deformed or even collapsed is relatively high. Once the pore structure of the filter membrane is deformed or even collapsed, the flux and load of the filter membrane will both be reduced. That is, the high load and high flux of the UPE filter membrane cannot be effectively guaranteed. If the mass of the porous body per unit area is too large (such as greater than 0.055g / That is, the mass of a membrane with a diameter of 47 mm is greater than 0.055 g) and the thickness is too small (such as less than 60 μm), which means that the loose area is too dense as a whole, and the flux and loading capacity of the filter membrane itself cannot be effectively guaranteed.

[0032] Optionally, the filtration coefficient T of the porous body is 4-14, and the filtration coefficient T is obtained as follows: T=a×b, wherein a is the thickness of the dense zone, and b is the ratio of the initial bubble point of the porous body to the complete bubble point of the porous body.

[0033] By adopting the above technical scheme, as mentioned above, the ratio of the initial bubble point of the porous body to the complete bubble point of the porous body reflects the uniformity of the pore structure in the dense zone. Furthermore, while the pore structure in the dense zone of the porous body has a suitable uniformity, the porous body also has a suitable filtration coefficient, which further ensures the high flux, high loading capacity and high retention of the filter membrane.

[0034] If the thickness of the dense area of ​​the porous body is relatively small, the pore structure of the dense area of ​​the porous body needs to be relatively uniform (the ratio of the initial bubble point of the porous body to the complete bubble point of the porous body is relatively high, that is, there are as few large and small pores as possible). On the one hand, the thickness of the dense area is small, the resistance of the UPE filter membrane to the feed liquid as a whole is relatively small, and the flux of the filter membrane itself is high. Therefore, the dense area does not need large pores to compensate for the flux of the UPE filter membrane as a whole. On the other hand, the thickness of the dense area is small, and its ability to retain bacteria is relatively weak. If the pore structure of the dense area is uneven, the efficient retention of bacteria by the filter membrane as a whole may not be effectively guaranteed. On the contrary, if the thickness of the dense zone of the porous body is relatively large, even if there are some large pores in the dense zone, the filter membrane as a whole can still ensure relatively ideal bacterial retention performance under the auxiliary retention of the loose zone. At the same time, the thick dense zone has relatively large resistance to the feed liquid, resulting in the overall flux of the filter membrane is not high, and the probability of the dense zone being blocked is relatively high. Therefore, it is hoped that a part of large pores will be introduced into the dense zone to compensate for the overall flux and load loss of the filter membrane.

[0035] Optionally, along the thickness direction of the porous body, the loose area includes a first macroporous area, a support area, and a second macroporous area, a surface on one side of the first macroporous area is the first surface, and the second macroporous area is located between the support area and the dense area; the SEM average pore size of the support area is smaller than the SEM average pore size of the first macroporous area and the second macroporous area, and larger than the SEM average pore size of the dense area;

[0036] Optionally, the thickness of the support area accounts for 15-45% of the thickness of the porous body.

[0037] By adopting the above technical solution, the loose area includes a first large pore area, a supporting area and a second large pore area, and the average pore size of the supporting area is smaller than the average pore size of the first large pore area and the second large pore area, that is, along the thickness direction of the membrane, the pore size of the loose area first becomes smaller and then becomes larger.

[0038] Different from the typical V-shaped asymmetric membrane (typical V-shaped asymmetric membrane generally only includes a large pore area for retaining large particle impurities and a small pore area for retaining target retentate, and the pore size of the large pore area is continuously reduced along the membrane thickness direction), the UPE filter membrane of the present application introduces a support area with a relatively small pore size between the first large pore area and the second large pore area. Admittedly, the introduction of the support area increases the overall density of the filter membrane to a certain extent, which may cause a decrease in both the flux and the load of the filter membrane. However, the inventors of the present application unexpectedly found that the introduction of a support area of ​​suitable thickness not only did not reduce the overall flux and load of the UPE, but even slightly increased them, which was unexpected.

[0039] This may be because, when the filter membrane is used for bacterial filtration, a dead-end filtration method is generally used. During the filtration process, the applied pressure is the main driving force for filtration. Therefore, the filter membrane is subjected to a large pressure from the feed liquid. The first macroporous area (especially the first surface of the direct surface liquid pressure and the porous body in the vicinity thereof) is affected by the pressure of the feed liquid, and the possibility of deformation and collapse of its pore structure is relatively high. The UPE filter membrane of the present application introduces a support area of ​​suitable thickness between the first macroporous area and the second macroporous area (i.e., a porous body with relatively high density is introduced between the porous body with relatively low density). The introduction of the support area increases the pressure bearing performance of the entire loose area to a certain extent (increases the pressure bearing performance of the entire UPE filter membrane). On the one hand, this allows the filter membrane to work normally under higher environmental pressure, that is, even under a larger pressure, the first macroporous area (especially the first surface of the direct surface liquid pressure and the porous body in the vicinity thereof) is affected by the pressure of the feed liquid, and the possibility of deformation and collapse of its pore structure is relatively low. On the other hand, a higher environmental pressure also means a higher driving force for filtration, and the feed liquid as a whole has a higher flow rate. The combined effect of the two ensures that the UPE filter membrane of the present application has a relatively ideal flux as a whole.

[0040] At the same time, the support area with a relatively small average pore size further plays a pre-retention role. The pre-retention of the loose area includes two aspects. One is to intercept some impurity particles with relatively small particle sizes (which cannot be retained by the first large pore area and the second large pore area, and may block the dense area). That is, the setting of the support area further reduces the probability of the pore structure (flow channel) of the dense area being blocked, which further increases the load capacity of the filter membrane (the factors affecting the load capacity of the filter membrane not only consider the blockage of the loose area, but also the blockage of the dense area). The second is the pre-retention of the target interception (bacteria). The introduction of the support area further ensures the efficient retention of bacteria by the UPE filter membrane as a whole. At the same time, the introduction of the support area can reduce the pore size uniformity of the dense area to a certain extent, so that a part of large pores are introduced into the dense area, further ensuring the high flux and high load capacity of the filter membrane on the basis of ensuring the efficient retention of the filter membrane.

[0041] It is understandable that the thickness of the support area should not be too small (the thickness of the support area accounts for no less than 15% of the thickness of the porous body). If the thickness of the support area is too small, the support area cannot play a sufficient reinforcing effect on the loose area as a whole, the overall pressure bearing capacity of the filter membrane is relatively low, the flux and load of the filter membrane are not significantly improved, and the small thickness of the support area cannot play a sufficient pre-retention role, and the retention capacity of the filter membrane is not significantly improved. The thickness of the support area should not be too large (the thickness of the support area accounts for no more than 45% of the thickness of the porous body). A thick support area will excessively increase the overall density of the filter membrane, thereby excessively increasing the resistance of the filter membrane to the feed liquid, and the flux of the filter membrane will not be significantly improved. The thick support area also means that the overall retention space of the first large pore area and the second large pore area is relatively insufficient, and the load of the filter membrane cannot be fully guaranteed.

[0042] Optionally, the first macroporous region accounts for 15-40% of the thickness of the porous body.

[0043] By adopting the above technical solution, the first macroporous area of ​​suitable thickness can effectively filter out large particles in the feed liquid, the thickness of the first macroporous area is not too low (the first macroporous area accounts for no less than 15% of the thickness of the porous body), and the first macroporous area has enough space to intercept and accommodate large particles of impurities, thereby reducing the probability of large particles directly blocking the support area and the dense area, thereby extending the service life of the UPE filter membrane of the present application. Of course, the thickness of the first macroporous area cannot be too large (the first macroporous area accounts for no more than 40% of the thickness of the porous body), because the introduction of the relatively "loose" first macroporous area will inevitably lead to the loss of the mechanical properties (pressure resistance) of the entire filter membrane. If the thickness of the first macroporous area is too large, even if the filter membrane of the present application introduces a support area of ​​suitable thickness, it is not enough to ensure that the first macroporous area (especially the first surface and the porous body near the first surface) has sufficient pressure bearing performance. When the relatively high feed liquid pressure directly acts on the first macroporous area, the first macroporous area is easily deformed and compressed due to the pressure of the feed liquid, thereby reducing the flux and load of the UPE filter membrane.

[0044] In summary, the UPE filter membrane of the present application introduces a first large pore area and a support area of ​​appropriate thickness, and the synergistic effect of the two further ensures the overall flux and loading capacity of the filter membrane.

[0045] Optionally, the ratio of the thickness of the first macroporous region to the thickness of the second macroporous region is 1.2-2.

[0046] By adopting the above technical solution, compared with the second macroporous area, the first macroporous area is closer to the first surface (the feed liquid first passes through the first macroporous area, and then passes through the second macroporous area). Therefore, the first macroporous area is the key area to ensure high flux and high load of the filter membrane. The thickness of the first macroporous area is greater than that of the second macroporous area (the thickness ratio is greater than 1.2), ensuring that the first macroporous area as a whole has a larger dirt holding space. However, the first macroporous area cannot be too thick (the thickness ratio is less than 2). If the thickness of the first macroporous area is too thick and the second macroporous area is too thin, on the one hand, even if the filter membrane of the present application introduces a support area of ​​suitable thickness, it is not enough to ensure that the first macroporous area with a large thickness (especially the porous body near the first surface and the first surface) has sufficient pressure bearing performance. When the relatively high feed liquid pressure directly acts on the first macroporous area, the first macroporous area is easily deformed and compressed due to the pressure of the feed liquid, thereby reducing the flux and load of the UPE filter membrane. On the other hand, the second macroporous area with a small thickness cannot further fully play the role of pre-retention, and the overall load of the UPE filter membrane cannot be fully guaranteed.

[0047] Optionally, the hole area ratio of the cross section of the first macropore region is 50-70%.

[0048] By adopting the above technical solution, the number of holes in the first macroporous area is relatively large and the pore size is relatively large (the pore area ratio is greater than 50%). On the one hand, the low resistance of the UPE filter membrane to the feed liquid is guaranteed, and the high pressure bearing performance of the UPE filter membrane is matched to ensure the high flux of the filter membrane. On the other hand, it is guaranteed that the UPE filter membrane has enough space to effectively filter out large particles in the feed liquid, reduce the probability of large particles directly blocking the filter membrane, and ensure the service life of the UPE filter membrane. Of course, the pore area ratio of the first macroporous area is not the larger the better, because if the number of holes in the first macroporous area is too large and the pore size is too large (the pore area ratio is greater than 70%), it means that the first macroporous area is relatively "loose" as a whole. During filtration, the pressure of the feed liquid directly acts on the first macroporous area. The first macroporous area that is too "loose" is easy to deform and compress due to the pressure of the feed liquid, which will lead to a decrease in the flux and load of the entire membrane.

[0049] Optionally, the porous body also includes a mesopore zone, and the surface on one side of the mesopore zone is the first surface; the SEM average pore size of the mesopore zone is smaller than the SEM average pore size of the first macropore zone, and larger than the SEM average pore size of the dense zone; the mesopore zone accounts for 3%-12% of the thickness of the porous body.

[0050] By adopting the above technical solution, after the loose area is introduced into the mesoporous area, along the membrane thickness direction, the pore size of the loose area of ​​the filter membrane first becomes larger, then becomes smaller, and then becomes larger. It is generally believed that the pore size of the mesoporous area is relatively small compared to the first large pore area. Therefore, the pores in the mesoporous area are more easily blocked; at the same time, the introduction of the mesoporous area means the extension of the path of the tortuous passage inside the filter membrane, which will inevitably increase the resistance of the filter membrane to the feed liquid. Therefore, the introduction of the mesoporous area will lead to a decrease in both the overall flux and the loading capacity of the filter membrane. However, the inventors of the present application unexpectedly found that the flux and loading capacity of the filter membrane provided by the present application have been significantly improved when it is actually used (especially under high pressure), which is unexpected.

[0051] This may be because, when the filter membrane is used for bacterial filtration, a dead-end filtration method is generally used. During the filtration process, the external pressure is the main driving force for filtration. Therefore, the filter membrane is subjected to a large pressure from the liquid. For the filter membrane without the introduction of the mesoporous region, the first surface is the side close to the first macroporous region. Since the pore structure of the first macroporous region has a large pore size, under the action of the liquid pressure, the pore structure of the first macroporous region (especially for the porous body near the first surface) is prone to deformation, and even the collapse of the pore structure. Once the pore structure of the first macroporous region is deformed or collapsed, both the guiding capacity (flux) for the liquid and the pollutant holding capacity (load) will be greatly reduced.

[0052] After the mesopore area is introduced into the filter membrane, the first surface is the side close to the mesopore area. Since the average SEM pore size of the mesopore area is smaller than that of the first macropore area, that is, there are a large number of solid parts around the inlet hole to support the pore structure, the overall pressure resistance of the filter membrane is further improved under the synergistic effect of the loose area, so that the deformation degree of the pore structure on the first surface of the filter membrane is relatively small under high pressure environment (for example, 30Psi or even higher pressure environment), and large particles of impurities in the feed liquid can pass through the main inlet hole and smoothly enter the pre-filtration layer to be intercepted, thereby reducing the possibility of filter cake formation on the first surface of the filter membrane and ensuring the high load of the filter membrane. At the same time, the high-pressure environment also means that the feed liquid has a higher flow rate (higher feed liquid filtration driving force), the feed liquid flow rate is fast, and the deformation degree of the path of the feed liquid circulation is small, and the filter membrane has a high flux.

[0053] In a second aspect, the present application provides a method for preparing an asymmetric UPE filter membrane, using the following technical solution:

[0054] S1. preparing a casting solution, wherein the casting solution comprises a polyethylene resin and a solvent system, wherein the solvent system comprises a compound A and a compound B, wherein the compound A is a solvent for the polyethylene resin, and the compound B is a non-solvent for the polyethylene resin; in the casting solution, the solid content of the polyethylene resin is 10-20%; and in the solvent system, the content of the compound B is not less than 60%;

[0055] S2: melt extrusion, extruding the casting liquid to form a liquid film on the carrier;

[0056] S3: Phase separation solidification, cooling the liquid film, and forming a raw film after phase separation solidification; during the phase separation process, the temperature of one side of the liquid film is at least 40°C lower than the temperature of the other side;

[0057] S4: extraction, extracting the solvent system with an extraction liquid, so that the solvent system is removed from the raw membrane to obtain the original membrane, wherein the temperature of the extraction liquid is 0-40° C., the concentration of the extraction liquid is always not less than 95%, and during the extraction process, the raw membrane collapses and shrinks;

[0058] S5: heat setting, heat setting the original membrane to obtain a UPE filter membrane.

[0059] By adopting the above technical scheme, the present invention prepares UPE filter membrane based on thermally induced phase separation method. When preparing, the first step is to configure the casting liquid, and the material system of the casting liquid includes polyethylene resin and a corresponding solvent system. Wherein, the solvent system is composed of compound A and compound B, wherein compound A is a good solvent for polyethylene resin, and a good solvent means that when heated to the boiling point of compound A at most, compound A can completely dissolve the polyethylene resin to form a homogeneous solution; compound B is a non-solvent for polyethylene resin, and a non-solvent means that when heated to the boiling point of this compound at most, the compound cannot dissolve the polyethylene resin to form a homogeneous solution, and can only play a certain swelling role on the polyethylene resin. It can be understood that in this application, the solid content of polyethylene resin specifically refers to the ratio of the mass of polyethylene resin to the overall mass of casting liquid in the casting liquid. The content of compound B specifically refers to the ratio of the mass of compound B to the overall mass of the solvent system in the solvent system.

[0060] After the casting liquid is prepared, the second step is to extrude the uniform and stable casting liquid and form a liquid film on the carrier. Then the third step is to cool the liquid film and form a raw film after phase separation and solidification. During the phase separation process, the temperature on one side of the liquid film is at least 40°C lower than the temperature on the other side. It can be understood that the high temperature side of the liquid film specifically refers to the temperature on the carrier side of the liquid film, and the low temperature side of the liquid film specifically refers to the ambient temperature during the phase separation and solidification process of the liquid film. In the following text, the temperature difference between the two sides of the liquid film specifically refers to the difference between the temperature on the carrier side of the liquid film and the air side (environment) of the liquid film.

[0061] Generally speaking, there are at least two factors that affect the pore size of the liquid film after phase separation and solidification. The first is the driving force of phase separation and solidification. For the preparation of filter membranes by thermally induced phase separation, temperature is the driving force of phase separation and solidification of the liquid film. The lower the temperature, the faster the phase separation speed, and the smaller the membrane pores formed. In this application, there is a significant difference in temperature on both sides of the liquid film (the temperature on one side is at least 40°C lower than the temperature on the other side), ensuring that there is a relatively significant difference in the phase separation speed on both sides of the liquid film, thereby ensuring that the final film formation is an asymmetric membrane, the high-temperature side of the liquid film forms the loose area required by this application, and the low-temperature side of the liquid film forms the dense area of ​​this application. The second is the solid content of the liquid film. The higher the solid content of the liquid film, the smaller the pore size formed. Conversely, the lower the solid content of the liquid film, the larger the pore size formed.

[0062] Therefore, in general, in order to form a relatively dense membrane pore structure (dense area), researchers will choose to use a liquid membrane with a high solid content to ensure the density of the formed membrane pore structure. Different from the conventional membrane making process, the inventors of this application adopted a low solid content (10-20%) casting liquid system to prepare a UPE filter membrane with an ideal dense area structure, which was unexpected.

[0063] This may be because, in the casting liquid system of the present application, the content of film-forming substances (solid content) is relatively low, and the content of compound B (non-solvent) is not less than 60%, which makes the raw film after phase separation and solidification of the liquid film in a relatively "unstable" state. In the fourth extraction step, since the temperature of the extraction liquid is 0-40°C, the concentration of the extraction liquid is always not less than 95%. Under the relatively intense extraction environment, the liquid film collapses to a certain extent. At the same time, the pore structure formed by phase separation and solidification of the liquid film on the low-temperature side is relatively small. The synergistic effect of the two significantly reduces the pore size of the membrane, and its density is significantly improved.

[0064] Generally speaking, in the membrane making process, researchers hope to prepare a uniform and stable liquid membrane system, to form a raw membrane (semi-finished membrane) with a stable pore structure and not easy to collapse, and then to prepare a finished membrane (finished membrane) with a stable pore structure. In this application, a low solid content and high non-solvent content casting liquid system was selected, which is contrary to common sense. The instability of the raw membrane formed after phase separation and solidification is used to make the raw membrane collapse under the synergistic effect of the more intense extraction environment, thereby forming a denser dense area. It is understandable that since the solid content of the filter membrane of this application itself is relatively low, and the phase separation temperature on the other side of the liquid membrane is relatively high, its pore structure after phase separation and solidification is relatively large. Even if the liquid membrane collapses to a certain extent, its membrane pore structure is still relatively loose.

[0065] The fifth step is to heat-set the original membrane after the extraction. The role of heat setting is to eliminate the internal stress caused by the extraction on the one hand, and to finally set the membrane pores of the original membrane on the other hand to ensure that the membrane pores will not change basically, and obtain the UPE porous membrane with the required membrane pore structure.

[0066] Optionally, in step S3, the temperature difference T0 between the temperature of the liquid film and the ambient temperature is 150-200° C., and the thickness h of the liquid film is 100-240 μm.

[0067] Optionally, the phase separation coefficient D of the liquid film is 0.5-1.5°C / μm, wherein the phase separation coefficient D is obtained as follows: D=T0 / h.

[0068] By adopting the above technical scheme, in the phase solidification step, the temperature of the high-temperature side of the liquid film is at least 40°C higher than that of the low-temperature side, the liquid film also has a suitable thickness (100-240μm), and the temperature of the liquid film and the ambient temperature also have a suitable temperature difference (150-200°C). Under the joint action of the three, it is further guaranteed that the final formed UPE filter membrane forms an ideal structure.

[0069] Among them, due to the relatively thick thickness of the liquid film, the temperature transfer of the liquid film is relatively slow, that is, there is a relatively obvious temperature gradient along its thickness direction, thereby ensuring that there is a relatively obvious difference in the phase separation speed on both sides of the liquid film. During the phase separation solidification process, both sides of the liquid film are in direct contact with the environment. Due to the appropriate temperature difference between the temperature of the liquid film and the ambient temperature, under the driving force of temperature, the two sides of the liquid film are phase-separated and solidified, and the required dense and loose areas begin to be initially formed on both sides of the liquid film. However, the temperature of the liquid film is relatively high, and the phase separation speed inside the liquid film is relatively slow, that is, the pore size inside the final formed raw film is relatively large, and along the thickness direction of the raw film, the pore size of the raw film first becomes smaller and then becomes larger.

[0070] Furthermore, in the subsequent extraction step, since the pore size on both sides of the raw membrane is relatively small, while the internal pore size of the raw membrane is relatively large, under a more intense extraction environment, collapse also occurs inside the raw membrane. It can be understood that the larger the pore structure of the liquid membrane, the weaker its self-supporting performance, and the greater the degree of collapse of the region under a more intense extraction environment, that is, to ensure that the first large pore area, the support area and the second large pore area required by the present application are formed after the extraction is completed.

[0071] Optionally, in step S4, the raw membrane in the extraction process is pressurized at a multiple of 1.2-2 times.

[0072] By adopting the above technical solution, in general, during the membrane making process, it is often hoped that the extraction is relatively gentle, so that the pore structure between the raw membrane (semi-finished membrane) and the finished membrane remains basically unchanged. Different from conventional extraction methods, in the extraction process of this application, on the basis that the concentration of the extract is always not less than 95%, the raw membrane in the extraction process is further pressurized to further ensure that the raw membrane can be efficiently extracted, that is, to further ensure the collapse of the raw membrane, thereby further ensuring that the UPE filter membrane finally formed in this application has a dense area, a mesoporous layer and a loose area of ​​appropriate thickness. In this application, the pressurization multiple refers to the multiple of pressurization to atmospheric pressure. For example, a pressurization multiple of 1.5 means pressurization to 1.5 times the atmospheric pressure.

[0073] Optionally, the polyethylene resin is an ultra-high molecular weight polyethylene with a mass average molecular weight of more than 4 million; the compound A is at least one of paraffin oil, white oil, hydraulic oil, decalin, castor oil extract, and castor oil; and the compound B is at least one of dimethyl phthalate, dioctyl adipate, ethylene glycol diacetate, dimethyl carbonate, palm oil, and triacetin.

[0074] The present application can bring the following beneficial effects: the UPE filter membrane provided by the present application and the method for preparing the UPE filter membrane, for bacterial filtration, the UPE filter membrane of the present application can significantly improve the flux and load of the filter membrane while ensuring high interception efficiency, that is, for bacterial filtration, the UPE filter membrane of the present application has high load, high flux and high interception capacity. The preparation method provided by the present invention can conveniently, quickly and effectively prepare the above-mentioned sterilization filter membrane. BRIEF DESCRIPTION OF THE DRAWINGS

[0075] Figure 1 is a schematic diagram of a scanning electron microscope (SEM) of a cross section of the UPE filter membrane of Example 1, with a magnification of 500×;

[0076] Figure 2 is a schematic diagram of a scanning electron microscope (SEM) of a cross section of the UPE filter membrane of Example 4, with a magnification of 700×;

[0077] Figure 3 This is a schematic diagram of a scanning electron microscope (SEM) of a cross section of the UPE filter membrane of Comparative Example 1, with a magnification of 1000×. DETAILED DESCRIPTION

[0078] Example 1

[0079] Example 1 of the present application discloses an asymmetric UPE filter membrane, which is prepared by the following process steps:

[0080] S1: Casting liquid preparation, the casting liquid includes 12 parts of polyethylene resin (parts by weight), 20 parts of compound A (parts by weight) and 49 parts of compound B (parts by weight), wherein compound A is a solvent for polyethylene resin, specifically decalin, and compound B is a non-solvent for polyethylene resin, specifically dimethyl phthalate; in the casting liquid, the solid content of polyethylene resin is 14.8%, and the content of compound B is 71.0%; the polyethylene resin has a mass average molecular weight of 4.5 million;

[0081] S2: melt extrusion, the melt-mixed casting liquid is extruded through a die head, and the casting liquid forms a liquid film on the carrier, and the thickness of the liquid film h is 173 μm; the temperature difference T0 between the liquid film and the ambient temperature is 175°C; the phase separation coefficient D of the liquid film is 1.012°C / μm;

[0082] S3: Phase separation solidification, cooling the liquid film, and forming a raw film after phase separation solidification; during the phase separation solidification process, the temperature of one side of the liquid film is 60°C lower than the temperature of the other side;

[0083] S4: extraction, extracting the solvent system with an extraction liquid, so that the solvent system is removed from the raw membrane to obtain the original membrane. During the extraction process, the raw membrane collapses and shrinks; the temperature of the extraction liquid is 20° C., and the concentration of the extraction liquid is always not less than 95%; at the same time, the raw membrane during the extraction process is pressurized at a multiple of 1.6 times (1.6 times atmospheric pressure);

[0084] S5: heat setting, heat setting the original film to obtain a UPE porous film.

[0085] Example 2-Example 7

[0086] The difference between Example 2 to Example 7 and Example 1 is that the casting solution formula and various process parameters are different, see Table 1 and Table 2 for details.

[0087] It is particularly important to point out that in step S4 of Example 2, the raw membrane in the extraction process is pressurized by 2.5 times, while in step S4 of Example 5, the raw membrane in the extraction process is not pressurized.

[0088] Table 1 Casting solution formula of each embodiment

[0089]

[0090] Table 2 Process parameters of each embodiment

[0091]

[0092] Comparative Example 1

[0093] Comparative Example 1 of the present application discloses a symmetrical UPE filter membrane, which is prepared by the following process steps:

[0094] S1: casting liquid preparation, the casting liquid includes 14 parts of polyethylene resin (parts by weight), 23 parts of compound A (parts by weight) and 24 parts of compound B (parts by weight), wherein compound A is a solvent for polyethylene resin, specifically decalin, and compound B is a non-solvent for polyethylene resin, specifically dimethyl phthalate; in the casting liquid, the solid content of polyethylene resin is 23.0%, and the content of compound B is 51.1%;

[0095] S2: melt extrusion, the melt-mixed casting liquid is extruded through a die head, and the casting liquid forms a liquid film on the carrier, and the thickness of the liquid film h is 68 μm; the temperature difference T0 between the liquid film and the ambient temperature is 182°C; the phase separation coefficient D of the liquid film is 2.048°C / μm;

[0096] S3: Phase separation solidification, cooling the liquid film, and forming a raw film after phase separation solidification; during the phase separation solidification process, the temperature of one side of the liquid film is 20°C lower than the temperature of the other side;

[0097] S4: extraction, immersing the raw membrane in an extraction solution at 25°C for 24 hours to remove compound A and compound B;

[0098] S5: heat setting, heat setting the original film to obtain a UPE porous film.

[0099] Comparative Example 2

[0100] Comparative Example 2 of the present application discloses a V-shaped asymmetric UPE filter membrane, which is prepared by the following process steps:

[0101] S1: casting liquid preparation, the casting liquid includes 16 parts of polyethylene resin (parts by weight), 28 parts of compound A (parts by weight) and 58 parts of compound B (parts by weight), wherein compound A is a solvent for polyethylene resin, specifically decalin, and compound B is a non-solvent for polyethylene resin, specifically dimethyl phthalate; in the casting liquid, the solid content of polyethylene resin is 15.7%, and the content of compound B is 67.4%;

[0102] S2: melt extrusion, the melt-mixed casting liquid is extruded through a die head, and the casting liquid forms a liquid film on the carrier, and the thickness of the liquid film h is 87 μm; the temperature difference T0 between the liquid film and the ambient temperature is 160°C; the phase separation coefficient D of the liquid film is 2.069°C / μm;

[0103] S3: Phase separation solidification, cooling the liquid film, and forming a raw film after phase separation solidification; during the phase separation solidification process, the temperature of one side of the liquid film is 90°C lower than the temperature of the other side;

[0104] S4: extraction, extracting the solvent system with an extraction liquid, so that the solvent system is removed from the raw membrane to obtain the original membrane. During the extraction process, the raw membrane collapses and shrinks; the temperature of the extraction liquid is 20° C., and the concentration of the extraction liquid is always not less than 70% and not more than 80%; at the same time, the raw membrane during the extraction process is pressurized at a multiple of 1.1 times;

[0105] S5: heat setting, heat setting the original film to obtain a UPE porous film.

[0106] The detection methods are as follows:

[0107] PMI average pore size: The UPE filter membranes prepared in the embodiments and comparative examples were taken as samples, and the PMI average pore size of each sample was tested using a CFP-1J00AEX PMI pore size tester.

[0108] Retention performance test: The UPE filter membranes prepared in each embodiment and comparative example were used as samples for bacterial retention challenge experiments, wherein the detection method was based on the guidance document TR26 issued by PDA. During the test, 150 nm (0.15 μm) PSL particles were used to simulate the retention of bacteria, and the samples were subjected to a bacterial retention experiment according to the standard ASTM F838-2015 ae1 to test the LRV value of the filter membrane.

[0109] Flux test: The UPE filter membrane prepared in each embodiment and comparative example was taken as a sample for flux test. The filter membrane to be tested was cut into a circular membrane with a diameter of 47 mm. 50 mL of test liquid (water) was taken, and the temperature of the test liquid (water) was adjusted to 20°C. The filtration pressure was 0.03 MPa, and the time required for 50 mL of test liquid to pass through the filter membrane was measured (the higher the flux of the filter membrane, the shorter the time it takes for the test liquid to pass through the filter membrane).

[0110] Loading capacity test: The UPE filter membrane prepared in each embodiment and comparative example was taken as a sample for loading capacity test;

[0111] ①: Test solution preparation: prepare 2 portions of test solution, each portion of the preparation solution is 50 mL, the test solution is a PSL particle solution, wherein the particle size of the PSL particles is 150 nm, and the concentration of the PSL particle solution is 0.5 abs (absorbance is used to characterize the concentration);

[0112] ②: One-time filtration, cut the filter membrane to be tested into a circular membrane with a diameter of 47mm, take 50mL of the test liquid, and adjust the temperature of the test liquid to 20℃, the filtration pressure is 0.03Mpa, measure the time required for 50mL of the test liquid to pass through the filter membrane (complete one filtration), and record it as t1;

[0113] ③: Secondary filtration. After the first filtration is completed, take 50mL of test liquid and adjust the temperature of the test liquid to 20℃ and the filtration pressure to 0.03Mpa. Measure the time required for 50mL of test liquid to pass through the filter membrane (complete the secondary filtration) and record it as t2. The time difference △t between the first filtration and the second filtration (△t=t2-t1) is used to characterize the loading capacity of the UPE filter membrane. The smaller the time difference △t between the first filtration and the second filtration, the higher the loading capacity of the filter membrane.

[0114] The morphological parameters of the UPE filter membranes prepared in the embodiments and comparative examples are shown in Tables 2 and 3, and the performance parameters are shown in Table 4.

[0115] Table 2 Morphological parameters of the cross section of the UPE filter membranes prepared in the examples and comparative examples

[0116]

[0117] Table 3 Overall morphology parameters of the UPE membranes prepared in each embodiment and comparative example

[0118]

[0119] Table 4 Performance parameters of the UPE filter membranes prepared in the embodiments and comparative examples

[0120]

[0121] in conclusion

[0122] By comparing Example 1 and Comparative Example 1, it is not difficult to find that the flux and load of the UPE filter membrane of Comparative Example 1 are significantly lower than those of the UPE filter membrane of Example 1. This may be because, during the preparation process of the filter membrane of Comparative Example 1, the temperatures on both sides of the liquid membrane are basically close, and the phase separation speed is basically close. At the same time, the thickness of the liquid membrane is relatively small, and the heat transfer along the thickness direction of the liquid membrane is relatively fast, which ultimately leads to the overall phase separation speed of the liquid membrane of Comparative Example 1 being basically close, and then the final film formation is a filter membrane with a symmetrical structure. In order to ensure good retention of impurities in the feed liquid, the structurally symmetrical membrane should not have an overly large membrane pore structure, which will make the membrane have a relatively large resistance to the feed liquid, and the flux of the filter membrane is relatively low. Secondly, since the filter membrane is a symmetrical membrane, the area in the symmetrical membrane that retains small particle impurities will inevitably also retain a part of large particle impurities, that is, the symmetrical membrane is relatively easier to cause the concentrated retention of impurity particles, and once the large particle impurities block the relatively small membrane pores, the flux of the filter membrane will be greatly reduced.

[0123] By comparing Example 1 and Comparative Example 2, it is not difficult to find that the average pore size of the UPE membrane PMI of Comparative Example 2 is slightly larger than that of the membrane of Example 1, and the thickness of the dense area of ​​the membrane of Comparative Example 2 is much larger than that of the membrane of Example 1. However, the flux, loading capacity, and even the interception capacity of the membrane of Comparative Example 2 are slightly lower than those of the membrane of Example 1. This may be because the membrane of Example 1 has a large-thickness loose area. Although the pore size of the loose area is relatively large, the large-thickness loose area, through the continuous stacking of membrane pores and membrane pores in the membrane thickness direction, makes the loose area have a high interception effect. The result will be smaller than the size of its actual pore structure, that is, the loose area with large thickness and low density plays a part of the pre-retention role. Furthermore, with the continuous interception of the loose area (including the pre-retention of bacteria and the retention of large particle impurities), the pore size of the loose area continues to decrease, and the loose area's ability to retain bacteria is further improved. That is, although the thickness of the dense area of ​​the present application is relatively small, the loose area with large thickness and low density makes up for the loss of the retention capacity of the filter membrane of the present application, ensuring that the final filter membrane's ability to retain bacteria is not only not reduced, but even slightly improved.

[0124] The above is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.

Claims

1. An asymmetric UPE filter membrane comprising a porous body having a non-directional tortuous path therein, the porous body having a first surface for fluid inflow and a second surface for fluid outflow, characterized in that: The PMI average pore size of the UPE filter membrane is 0.08-0.7 μm; Along the thickness direction of the porous body, the porous body includes a loose area and a dense area, one side surface of the loose area is the first surface, one side surface of the dense area is the second surface, and the average pore size of the loose area is larger than the average pore size of the dense area. The thickness of the porous body is 60-140 μm; The thickness of the dense region accounts for no more than 15% of the thickness of the porous body.

2. The asymmetric UPE filter membrane according to claim 1, characterized in that: The complete bubble point of the porous body is 0.16-0.24 MPa, and the porosity of the porous body is 60-85%.

3. The asymmetric UPE filter membrane according to claim 1, characterized in that: The bubbling point of the porous body is 0.14-0.20 MPa, and the ratio of the bubbling point of the porous body to the complete bubbling point of the porous body is 0.7-0.

9.

4. The asymmetric UPE filter membrane according to claim 1, characterized in that: The porous body has a gram weight of 0.035-0.055 g / φ47 mm.

5. The asymmetric UPE filter membrane according to claim 1, characterized in that: The filtration coefficient T of the porous body is 4-14, and the filtration coefficient T is obtained as follows: T=a×b, wherein a is the thickness of the dense zone, and b is the ratio of the bubbling point of the porous body to the complete bubbling point of the porous body.

6. The asymmetric UPE filter membrane according to claim 1, characterized in that: Along the thickness direction of the porous body, the loose area includes a first macroporous area, a support area, and a second macroporous area, a surface on one side of the first macroporous area is the first surface, and the second macroporous area is located between the support area and the dense area; The SEM average pore size of the support area is smaller than the SEM average pore size of the first macropore area and the second macropore area, and larger than the SEM average pore size of the dense area; The thickness of the support area accounts for 15-45% of the thickness of the porous body.

7. The asymmetric UPE filter membrane according to claim 5, characterized in that: The first macroporous region accounts for 15-40% of the thickness of the porous body.

8. The asymmetric UPE filter membrane according to claim 5, characterized in that: The ratio of the thickness of the first macroporous region to the thickness of the second macroporous region is 1.2-2.

9. The asymmetric UPE filter membrane according to claim 5, characterized in that: The pore area ratio of the cross section of the first macropore region is 50-70%.

10. The asymmetric UPE filter membrane according to claim 1, characterized in that: The porous body further includes a mesoporous region, and a surface on one side of the mesoporous region is the first surface; The SEM average pore size of the mesopore region is smaller than the SEM average pore size of the first macropore region, and larger than the SEM average pore size of the dense region; The mesoporous region accounts for 3% to 12% of the thickness of the porous body.

11. A process for preparing the UPE filter membrane according to any one of claims 1 to 10, characterized in that: The process steps include: S1. Preparation of a casting solution, wherein the casting solution comprises a polyethylene resin, a compound A, and a compound B, wherein compound A is a solvent for the polyethylene resin and compound B is a non-solvent for the polyethylene resin; in the casting solution, the solid content of the polyethylene resin is 10-20%, and the content of compound B is not less than 60%; S2: melt extrusion, extruding the melt-mixed casting solution to form a liquid film on the carrier; S3: Phase separation solidification, cooling the liquid film, and forming a green film after phase separation solidification; during the phase separation process, the temperature of one side of the liquid film is at least 40°C lower than the temperature of the other side; S4: Extraction, extracting the solvent system with an extraction liquid to remove the solvent system from the green membrane to obtain the original membrane, wherein the temperature of the extraction liquid is 0-40°C, and the concentration of the extraction liquid is always not less than 95%. During the extraction process, the green membrane collapses and shrinks; S5: heat setting, heat setting the original membrane to obtain the UPE filter membrane.

12. The process for preparing an asymmetric UPE filter membrane according to claim 11, characterized in that: In step S3, the temperature difference T0 between the temperature of the liquid film and the ambient temperature is 150-200° C., and the thickness h of the liquid film is 100-240 μm.

13. The process for preparing an asymmetric UPE filter membrane according to claim 12, characterized in that: The phase separation coefficient D of the liquid film is 0.5-1.5°C / μm, wherein the phase separation coefficient D is obtained as follows: D=T0 / h.

14. The process for preparing an asymmetric UPE filter membrane according to claim 11, characterized in that: In step S4, the raw membrane in the extraction process is pressurized at a multiple of 1.2-2 times.

15. The process for preparing an asymmetric UPE filter membrane according to claim 11, characterized in that: The polyethylene resin is an ultra-high molecular weight polyethylene with a mass average molecular weight of more than 4 million; the compound A is at least one of paraffin oil, white oil, hydraulic oil, decalin, castor oil extract, and castor oil; and the compound B is at least one of dimethyl phthalate, dioctyl adipate, ethylene glycol diacetate, dimethyl carbonate, palm oil, and triacetin.