Polymetallic ore beneficiation separation reagent as well as preparation method and application thereof

The prepared polymetallic ore beneficiation and separation agent utilizes the difference in coordination of metal ions on the mineral surface to achieve low-alkalinity separation of copper, sulfur, lead and zinc and efficient leaching of gold, solving the problem of large amounts of lime and high-alkalinity separation in the existing technology. solve difficult problems and improve the economy and environmental protection of the mineral processing process.

CN118744049AActive Publication Date: 2024-10-08BEIJING LAIRUNSI TECHNOLOGY CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410830334.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-10-08
Estimated Expiration
2044-06-25

AI Technical Summary

Technical Problem

In the existing mineral processing technology, there are problems in the recovery process of copper, lead, zinc and gold, such as large amounts of lime and difficulty in separation of high alkali, which leads to equipment scaling, ore body suppression and recovery rate decline, affecting economic benefits.

Method used

Through the mixing of intermediates prepared by catalytic reactions, a polymetallic ore beneficiation and separation agent is produced, which utilizes the differences in the coordination of metal ions on the surfaces of different minerals to target adsorption and increase the hydrophilicity of the minerals to achieve low-alkali separation of copper, sulfur, lead and zinc. and gold leaching, reducing the amount of lime.

Benefits of technology

It achieves low-alkalinity separation of copper, sulfur, lead and zinc and efficient leaching of gold. It has the advantages of green, low toxicity and environmental protection. It improves the concentrate quality and sorting effect, reduces the amount of lime, and solves the problem caused by traditional high-alkalinity separation. Equipment scaling and ore body inhibition problems.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of mineral separation, in particular to a polymetallic ore mineral separation agent and a preparation method and application thereof. The preparation method of the polymetallic ore beneficiation separation reagent comprises the steps that an N-containing compound, sodium hydroxide and sodium carbonate are mixed and then heated, a first catalytic reaction is conducted, and a first intermediate is obtained; the N-containing compound comprises at least one of urea, biuret and ammonium carbamate; a cyanamide compound and sodium hydroxide are mixed and then subjected to a second catalytic reaction in the chlorine atmosphere, and a second intermediate is obtained; the cyanamide compound comprises at least one of cyanamide, sodium dicyandiamide and calcium cyanamide; and the first intermediate and the second intermediate are mixed to obtain the polymetallic ore beneficiation separation reagent. The mineral separation agent prepared by the method can realize low-alkali separation of copper, sulfur, lead and zinc and leaching of gold, has the advantages of greenness, low toxicity and environmental protection, and is better in separation and leaching effects and higher in concentrate quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of mineral processing, and in particular to a multi-metal mineral processing and separation agent, and a preparation method and application thereof. Background Art

[0002] As the main non-ferrous metal resources, copper, lead, zinc and gold have received extensive attention for their development and utilization. At present, the recycling of copper, lead, zinc and gold generally has the problem of large amount of lime used and difficulty in high alkali separation, which is a common problem in the non-ferrous metal industry.

[0003] Among them, chalcopyrite in porphyry copper deposits is the main copper-containing mineral, often coexisting with pyrite. At present, high-alkali separation is mainly used to suppress pyrite in the copper-sulfur flotation separation process. The use of a large amount of lime can easily lead to a large amount of calcium ions in the flotation slurry, causing scaling of equipment or pipelines and increasing equipment failure rate. At the same time, the use of a large amount of lime will also suppress the associated molybdenum and rhenium metals in the ore body, reducing income.

[0004] Moreover, in polymetallic lead-zinc sulfide deposits, the inhibitors need to be carried out under strong alkaline conditions during the flotation separation of lead and zinc, resulting in a decrease in the lead recovery rate and a high lead content in the zinc concentrate.

[0005] In addition, in the process of gold ore leaching, cyanide is often used as a gold leaching agent, and a large amount of sodium cyanide needs to be added as a stabilizer to reduce the volatilization of sodium cyanide, which leads to calcium accumulation and blockage in the pipeline, affecting normal production.

[0006] Therefore, based on the characteristics of mineral crystal surfaces and the differences between atoms, and based on coordination chemistry, the saturated / unsaturated coordination structure of the reagent molecules and the mineral surface is analyzed through molecular orbital theory to modulate the electrochemical properties of the reagent π orbital and the mineral θ, and a new type of low-toxic, environmentally friendly and highly selective mineral processing and separation reagent is prepared to achieve low-alkali separation of copper, lead, zinc, gold and sulfur, and solve common problems in the non-ferrous metal industry, which is of great significance.

[0007] In view of this, the present invention is proposed. Summary of the invention

[0008] The first purpose of the present invention is to provide a method for preparing a polymetallic ore dressing and separation agent. After the first intermediate and the second intermediate obtained by the catalytic reaction are mixed and used, due to the difference in the coordination properties of metal ions on the surfaces of different minerals, the agent is targetedly adsorbed on the mineral surface. The -CN and -NH bonds in the molecular structure form bonds with low-spin iron ions, oxygen and other atoms and are dissolved in the form of stable -C / NHM (M is the target metal ion), so that defect sites are generated on the metal surface, which promotes the adsorption of hydrophilic groups such as -COOH bonds on the metal surface, thereby increasing the hydrophilicity of the mineral. The dressing and separation agent prepared by the method of the present invention can achieve low-alkali separation of copper, sulfur, lead and zinc and leaching of gold, and has the advantages of being green, low-toxic and environmentally friendly, and has better sorting and leaching effects and higher concentrate quality.

[0009] The second purpose of the present invention is to provide a polymetallic ore dressing and separation agent, which can achieve the separation of lead and zinc minerals after mixed flotation, the low-alkalinity separation of copper and sulfur minerals, and the leaching of gold ore, and has good separation effect, strong stability, and strong adaptability, solving the technical problem of large lime consumption caused by high-alkalinity separation in traditional ore dressing processes.

[0010] The third object of the present invention is to provide the application of the polymetallic ore dressing and separation agent in copper-sulfur flotation separation.

[0011] The fourth object of the present invention is to provide the application of the polymetallic ore dressing and separation agent in the flotation separation of lead and zinc.

[0012] The fifth object of the present invention is to provide the use of the polymetallic ore dressing and separation agent in gold ore leaching.

[0013] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0014] The present invention first provides a method for preparing a polymetallic ore separation agent, comprising the following steps:

[0015] (a), mixing a N-containing compound, sodium hydroxide and sodium carbonate and heating them to perform a first catalytic reaction to obtain a first intermediate; wherein the N-containing compound comprises at least one of urea, biuret and ammonium carbamate;

[0016] (b), mixing a cyanamide compound and sodium hydroxide and subjecting the mixture to a second catalytic reaction in a chlorine atmosphere to obtain a second intermediate; wherein the cyanamide compound comprises at least one of cyanamide, sodium dicyanamide and calcium cyanamide;

[0017] (c) After mixing the first intermediate and the second intermediate, the polymetallic ore dressing and separation agent is obtained.

[0018] Preferably, in step (a), the mass ratio of the N-containing compound, the sodium hydroxide and the sodium carbonate is 35-59:40-45:1-5.

[0019] Preferably, in step (a), the heating comprises: first reacting at room temperature for 1 to 2 hours under vacuum conditions, and then reacting at 100 to 200° C. for 1 to 3 hours.

[0020] Preferably, in step (a), the catalyst used in the first catalytic reaction includes at least one of a Pt / TiO2 catalyst, a Ru / TiO2 catalyst, and a Rh / TiO2 catalyst.

[0021] Preferably, in step (b), the mass ratio of the cyanamide compound to the sodium hydroxide is 5-7:1-2.

[0022] Preferably, in step (c), the mass ratio of the first intermediate to the second intermediate is 1-5:6-9.

[0023] The present invention further provides a polymetallic ore beneficiation and separation agent, which is prepared by the preparation method of the polymetallic ore beneficiation and separation agent.

[0024] The present invention further provides application of the polymetallic ore dressing and separation agent in copper-sulfur flotation separation.

[0025] Preferably, the copper-sulfur flotation separation method comprises the following steps: using the polymetallic ore dressing and separation agent as a pyrite flotation inhibitor and frother, mixing the polymetallic ore dressing and separation agent with copper-sulfur mixed flotation concentrate slurry, and then performing roughing, cleaning and scavenging to obtain copper concentrate and sulfur-containing tailings.

[0026] The present invention further provides the use of the polymetallic ore dressing and separation agent in lead and zinc flotation separation.

[0027] Preferably, the lead-zinc flotation separation method comprises the following steps: using the polymetallic ore dressing and separation agent as a flotation depressant, mixing the polymetallic ore dressing and separation agent with a lead-zinc-sulfur mixed flotation concentrate, a lead collector and a frother, and then performing roughing, cleaning and scavenging to obtain a lead concentrate and a zinc-sulfur tailings.

[0028] The present invention also provides application of the polymetallic ore dressing and separation agent in gold ore leaching.

[0029] Preferably, the method for leaching gold ore comprises the following steps: crushing, grinding and grading the raw gold ore to obtain coarse-grained minerals and fine-grained minerals; heaping the coarse-grained minerals to obtain a coarse-grained mineral pile; using the polymetallic ore dressing and separation agent as a leaching agent, heap leaching the coarse-grained mineral pile, and full-mud tank leaching the fine-grained minerals.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] (1) The polymetallic ore dressing and separation agent prepared by the preparation method of the polymetallic ore dressing and separation agent provided by the present invention has the advantages of different coordination properties of metal ions on the surfaces of different minerals, so that the agent is targetedly adsorbed on the surface of the mineral, and the -CN and -NH bonds in the molecular structure form bonds with low-spin iron ions, oxygen and other atoms and are dissolved in the form of stable -C / NHM (M is the target metal ion), so that defect sites are generated on the metal surface, which promotes the adsorption of hydrophilic groups such as -COOH bonds on the metal surface, thereby increasing the hydrophilicity of the mineral. The dressing and separation agent prepared by the method of the present invention can achieve low-alkali separation of copper, sulfur, lead and zinc and leaching of gold, and has the advantages of being green, low-toxic and environmentally friendly, and has better sorting and leaching effects and higher concentrate quality.

[0032] (2) The multi-metal ore dressing and separation agent provided by the present invention can achieve the separation of lead and zinc minerals after mixed flotation, the low-alkalinity separation of copper and sulfur minerals, and the leaching of gold ore, and has good separation effect, strong stability, and strong adaptability, solving the technical problem of large lime consumption caused by high alkalinity separation in the traditional ore dressing process.

[0033] (3) The polymetallic ore dressing and separation agent provided by the present invention can reduce the amount of lime used in the copper-sulfur separation process by more than 90%, thereby achieving low-toxic green flotation of lead-zinc sulfide minerals and green leaching of gold. DETAILED DESCRIPTION

[0034] The technical scheme of the present invention will be clearly and completely described below in conjunction with specific embodiments, but it will be appreciated by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work, all belong to the scope of protection of the present invention. If specific conditions are not indicated in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0035] If there is no special explanation, in the present invention, "the first aspect", "the second aspect", "the third aspect", "the fourth aspect", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "the first", "the second", "the third", "the fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.

[0036] If there is no special explanation, the "include" and "comprising" mentioned in the present invention represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may represent that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0037] If there is no special explanation, in the present invention, "one or more" or "at least one" refers to any one, any two or more of the listed items. Among them, "several" refers to any two or more of the listed items.

[0038] In a first aspect, the present invention provides a method for preparing a polymetallic ore separation agent, comprising the following steps:

[0039] (a), a N-containing compound, sodium hydroxide (for providing alkaline conditions) and sodium carbonate (for providing alkaline conditions) are mixed and heated, and a first catalytic reaction is carried out to obtain a first intermediate.

[0040] Wherein, the N-containing compound includes at least one of urea, biuret and ammonium carbamate.

[0041] The first intermediate includes: a substance containing -NH bond, -C=O bond, -NH2, and triuret.

[0042] (b) After uniformly mixing the cyanamide compound and sodium hydroxide, a second catalytic reaction is carried out under a chlorine atmosphere to obtain a second intermediate.

[0043] Among them, chlorine plays a protective role, and sodium hydroxide plays a role in adjusting pH.

[0044] Wherein, the cyanamide compound includes at least one of cyanamide, sodium dicyanamide and calcium cyanamide.

[0045] The second intermediate is mainly a cyanamide compound containing an alkali metal ion, which is mainly a -CN bond.

[0046] (c) After mixing the first intermediate and the second intermediate, the polymetallic ore dressing and separation agent is obtained.

[0047] Among them, the first intermediate and the second intermediate can synergistically enhance the interaction with metal ions, wherein the presence of -CN bonds and -NH bonds increases the water solubility of the agent, while increasing the interaction between the agent and metal ions, especially the -NH bonds, the coexistence with metal ions, and reduces the floatability of metal ions.

[0048] The polymetallic ore dressing and separation agent prepared by the method provided by the present invention performs targeted adsorption on the mineral surface due to the difference in the coordination properties of metal ions on the surfaces of different minerals. The -CN and -NH bonds in the molecular structure form bonds with low-spin iron ions, oxygen and other atoms and are dissolved in the form of stable -C / NHM (M is the target metal ion), so that defect sites are generated on the metal surface, which promotes the adsorption of hydrophilic groups such as -COOH bonds on the metal surface, thereby increasing the hydrophilicity of the mineral.

[0049] The ore dressing and separation agent prepared by the method of the present invention can realize the low-alkali separation of copper, sulfur, lead and zinc and the leaching of gold, has the advantages of being green, low-toxic and environmentally friendly, and has better sorting and leaching effects and higher concentrate quality.

[0050] In some specific embodiments, in order to further improve the sorting and leaching effects of the polymetallic ore dressing and separation agent, in step (a), the mass ratio of the N-containing compound, the sodium hydroxide and the sodium carbonate is 35-59 (including but not limited to any one of 35, 40, 45, 50, 55, 59 or the range between any two): 40-45 (including but not limited to any one of 40, 41, 42, 43, 44, 45 or the range between any two): 1-5 (including but not limited to any one of 1, 2, 3, 4, 5 or the range between any two).

[0051] In some specific embodiments, in step (a), the heating comprises: first reacting at room temperature for 1 to 2 hours under vacuum conditions, and then reacting at 100 to 200° C. (including but not limited to any one of 100° C., 120° C., 130° C., 150° C., 160° C., 180° C., and 200° C. or any range between two thereof) for 1 to 3 hours. Wherein, room temperature refers to room temperature, for example, 20 to 30° C.

[0052] In some specific embodiments, in step (a), the catalyst used in the first catalytic reaction includes at least one of a Pt / TiO2 catalyst, a Ru / TiO2 catalyst, and a Rh / TiO2 catalyst.

[0053] In some specific embodiments, in order to further improve the sorting and leaching effects of polymetallic ore dressing and separation agents, in step (b), the mass ratio of the cyanamide compound to the sodium hydroxide is 5-7 (including but not limited to any one of 5, 5.3, 5.5, 5.8, 6, 6.2, 6.5, 6.8, 7 or the range between any two of them): 1-2 (including but not limited to any one of 1, 1.2, 1.5, 1.8, 2 or the range between any two of them).

[0054] In some specific embodiments, in order to further improve the sorting and leaching effects of the polymetallic ore dressing and separation agent, in step (c), the mass ratio of the first intermediate to the second intermediate is 1 to 5 (including but not limited to any one of 1, 2, 3, 4, 5 or a range between any two): 6 to 9 (including but not limited to any one of 6, 6.5, 7, 7.5, 8, 8.5, 9 or a range between any two).

[0055] In a second aspect, the present invention provides a polymetallic ore beneficiation and separation agent, which is prepared by the above-mentioned preparation method of the polymetallic ore beneficiation and separation agent.

[0056] The polymetallic ore dressing and separation agent can achieve the separation of lead and zinc minerals after mixed flotation, the low-alkalinity separation of copper and sulfur minerals, and the leaching of gold ore, and has good separation effect, strong stability and adaptability, solving the technical problem of large lime consumption caused by high-alkalinity separation in traditional ore dressing processes.

[0057] In some specific embodiments, the polymetallic ore dressing and separation agent provided by the present invention can reduce the amount of lime used in the copper-sulfur separation process by more than 90%, thereby achieving low-toxic green flotation of lead-zinc sulfide minerals and green leaching of gold.

[0058] In a third aspect, the present invention provides the use of the above-mentioned multi-metal ore dressing and separation agent in copper-sulfur flotation separation.

[0059] Due to the spin difference of iron atoms in chalcopyrite and pyrite, the iron in pyrite is in a low spin state and the iron in chalcopyrite is in a high spin state. At this time, the pyrite in the low spin state is more easily adsorbed by the multi-metal ore dressing and separation agent provided by the invention, so that the iron atoms in the pyrite in the low spin state are converted into iron ions in the high spin state. At this time, the Fe-S bond is broken, and vacancies are generated. The oxygen fills the gap, and the oxidation of the pyrite surface is realized, thereby reducing the floatability of the pyrite. Due to the high spin state of the iron ions on the surface of chalcopyrite, chalcopyrite is not easily oxidized, which increases the difference in floatability between pyrite and chalcopyrite, and realizes the efficient separation of pyrite and chalcopyrite.

[0060] In some specific embodiments, the copper-sulfur flotation separation method includes the following steps: using the polymetallic ore dressing and separation agent as a pyrite flotation inhibitor and frother, mixing the polymetallic ore dressing and separation agent with the copper-sulfur mixed flotation concentrate slurry, and then performing roughing, cleaning and scavenging to obtain copper concentrate and sulfur-containing tailings.

[0061] In some specific embodiments, the copper-sulfur mixed flotation concentrate slurry is pH adjusted. Preferably, the pH of the copper-sulfur mixed flotation concentrate slurry is first adjusted to 7-9 (including but not limited to any one of 7, 7.5, 8, 8.5, 9 or a range between any two of them), and then evenly mixed with the polymetallic ore dressing and separation agent.

[0062] In a fourth aspect, the present invention provides the use of the above-mentioned multi-metal ore dressing and separation agent in the flotation separation of lead and zinc.

[0063] Due to the difference of zinc or iron (sphalerite or brittle sulfide lead antimonite), the difference of iron also leads to the difference selection of reagent molecules. The iron in sphalerite / sphalerite is four-coordinated iron and is in a low-spin state. The iron in galena / brittle sulfide lead antimonite is in a high-spin state. At this time, the iron on the surface of the mineral is not easy to oxidize. After adding the polymetallic ore dressing and separation reagent provided by the present invention as an inhibitor, galena / brittle sulfide lead antimonite is not easy to be oxidized, or the oxidation rate is lower than that of sphalerite / sphalerite. At this time, the hydrophilicity of sphalerite / sphalerite is increased, and the floatability of sphalerite / sphalerite is reduced. In some specific embodiments, the lead-zinc flotation separation method comprises the following steps: using the polymetallic ore dressing and separation reagent as a flotation inhibitor, mixing the polymetallic ore dressing and separation reagent with lead-zinc-sulfur mixed flotation concentrate, lead collector and frother, and then performing roughing, concentrating and scavenging to obtain lead concentrate and zinc-sulfur tailings.

[0064] In some specific embodiments, the lead-zinc-sulfur mixed flotation concentrate is pH-adjusted. Preferably, the pH of the lead-zinc-sulfur mixed flotation concentrate is first adjusted to 8-11 (including but not limited to any one of 8, 8.5, 9, 9.5, 10, 10.5, 11 or a range between any two of them), and then evenly mixed with the polymetallic ore dressing and separation agent, the lead collector and the frother.

[0065] The lead collector includes any lead collector commonly used in the art, and the foaming agent includes any foaming agent commonly used in the art, which is not limited in the present invention.

[0066] In a fifth aspect, the present invention provides the use of the above-mentioned multi-metal ore dressing and separation agent in gold ore leaching.

[0067] Compared with conventional agents, the polymetallic ore dressing and separation agent provided by the present invention has the following advantages: low toxicity, small dosage, and selective adsorption with gold ore to form a -C / NH-Au complex, which is dissolved in an aqueous solution, so that the gold element in the ore undergoes a replacement reaction with the agent, thereby dissolving in the aqueous solution, thereby achieving the leaching selection of the gold element.

[0068] In some specific embodiments, the method for leaching gold ore includes the following steps: crushing, grinding and grading the raw gold ore to obtain coarse-grained minerals and fine-grained minerals; heaping the coarse-grained minerals to obtain a coarse-grained mineral pile; using the polymetallic ore dressing and separation agent as a leaching agent, heap leaching the coarse-grained mineral pile, and full-mud tank leaching the fine-grained minerals.

[0069] In some specific embodiments, after the classification process, the coarse-grained minerals with a particle size of +200 mesh and the fine-grained minerals with a particle size of -200 mesh are obtained.

[0070] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.

[0071] Example 1

[0072] The preparation method of the polymetallic ore separation agent provided in this embodiment comprises the following steps:

[0073] (1) Urea, sodium hydroxide and sodium carbonate in a mass ratio of 35:40:1 were uniformly mixed, and a small amount of Pt / TiO2 catalyst was added thereto (the mass ratio of Pt / TiO2 catalyst to the mixed material was 1:1.5). The mixture was first reacted under vacuum at room temperature (25°C) for 1 hour, and then heated to 180°C for a first catalytic reaction. After reacting for 2 hours, a first intermediate (triuret) was obtained.

[0074] (2) After cyanamide and sodium hydroxide are uniformly mixed in a mass ratio of 5 to 7:1 to 2, a second catalytic reaction is carried out in a chlorine atmosphere to obtain a second intermediate.

[0075] (3) The first intermediate and the second intermediate are uniformly mixed in a mass ratio of 5:6 to obtain a polymetallic ore dressing and separation agent.

[0076] Example 2

[0077] The preparation method of the polymetallic ore dressing and separation agent provided in this embodiment is basically the same as that in Example 1, except that in step (1), urea is replaced by an equal mass of biuret, and the first intermediate obtained is triuret.

[0078] Example 3

[0079] The preparation method of the polymetallic ore dressing and separation agent provided in this embodiment is basically the same as that in Example 1, except that in step (1), urea is replaced by an equal mass of ammonium carbamate, and the first intermediate obtained is triuret.

[0080] Example 4

[0081] The preparation method of the polymetallic ore dressing and separation agent provided in this embodiment is basically the same as that in Example 1, except that in step (1), the mass ratio of urea, sodium hydroxide and sodium carbonate is replaced with 58:45:3.

[0082] Example 5

[0083] The preparation method of the multi-metallic ore dressing and separation agent provided in this embodiment is basically the same as that in Example 1, except that in step (1), the catalyst is replaced with an equal mass of Ru / TiO2 catalyst, and the reaction is first carried out under vacuum and room temperature (25°C) for 2 hours, and then heated to 120°C for reaction for 3 hours.

[0084] Example 6

[0085] The preparation method of the polymetallic ore dressing and separation agent provided in this embodiment is basically the same as that in Example 1, except that in step (2), cyanamide is replaced by an equal mass of sodium dicyandiamide.

[0086] Example 7

[0087] The preparation method of the polymetallic ore dressing and separation agent provided in this embodiment is basically the same as that in Example 1, except that in step (2), cyanamide is replaced by an equal mass of calcium cyanamide.

[0088] Example 8

[0089] The preparation method of the polymetallic ore dressing and separation agent provided in this embodiment is basically the same as that in Embodiment 1, except that in step (3), the mass ratio of the first intermediate to the second intermediate is replaced with 1:9.

[0090] Example 9

[0091] The preparation method of the polymetallic ore dressing and separation agent provided in this embodiment is basically the same as that in Embodiment 1, except that in step (3), the mass ratio of the first intermediate to the second intermediate is replaced with 3:7.

[0092] Example 10

[0093] The polymetallic ore dressing and separation agents prepared in Example 1, Example 2, Example 3, and Example 4 were respectively used as pyrite flotation depressants and frothers for copper-sulfur flotation separation. The specific steps were as follows: the pH of the copper-sulfur mixed flotation concentrate slurry was adjusted to 9, and then the polymetallic ore dressing and separation agent (in an amount of 100 g / t) was added thereto and mixed evenly, and then roughing, concentrating, and scavenging were carried out to obtain copper concentrate and sulfur-containing tailings.

[0094] After testing, after copper-sulfur flotation separation was carried out using the polymetallic ore dressing and separation reagent obtained in Example 1, the grade of copper in the obtained copper concentrate was 23.09%, and the recovery rate of copper was 90.69%.

[0095] After copper-sulfur flotation separation was performed using the polymetallic ore dressing and separation reagent obtained in Example 2, the grade of copper in the obtained copper concentrate was 24.01%, and the recovery rate of copper was 91.06%.

[0096] After copper-sulfur flotation separation was performed using the polymetallic ore dressing and separation reagent obtained in Example 3, the grade of copper in the obtained copper concentrate was 22.98%, and the recovery rate of copper was 89.36%.

[0097] After copper-sulfur flotation separation was performed using the polymetallic ore dressing and separation reagent obtained in Example 4, the grade of copper in the obtained copper concentrate was 23.68%, and the recovery rate of copper was 91.23%.

[0098] Embodiment 11

[0099] The polymetallic ore dressing and separation reagents prepared in Example 1, Example 5, Example 6, and Example 7 were respectively used as flotation depressants for lead and zinc flotation separation. The specific steps were as follows: the pH of the lead, zinc, and sulfur mixed flotation concentrate was adjusted to 8, and then the polymetallic ore dressing and separation reagent (in an amount of 100 g / t), a lead collector (ethylthiocyanate and butyl xanthate in a mass ratio of 1:1, in an amount of 120 g / t) and a frother (pine oil, in an amount of 35 g / t) were added thereto and mixed evenly, and then roughing, concentrating, and scavenging were carried out to obtain lead concentrate and zinc-sulfur tailings.

[0100] After testing, after the polymetallic ore dressing and separation reagent obtained in Example 1 was used for lead and zinc flotation separation, the grade of lead element in the obtained lead concentrate was 23.58%, and the lead element recovery rate was 80.27%.

[0101] After lead and zinc flotation separation was carried out using the polymetallic ore dressing and separation reagent obtained in Example 5, the grade of lead in the obtained lead concentrate was 20.28%, and the lead recovery rate was 78.39%.

[0102] After lead and zinc flotation separation was carried out using the polymetallic ore dressing and separation reagent obtained in Example 6, the grade of lead in the obtained lead concentrate was 21.36%, and the lead recovery rate was 79.95%.

[0103] After lead and zinc flotation separation was carried out using the polymetallic ore dressing and separation reagent obtained in Example 7, the grade of lead in the obtained lead concentrate was 23.98%, and the lead recovery rate was 81.87%.

[0104] Example 12

[0105] The polymetallic ore dressing and separation reagents prepared in Example 1, Example 8, and Example 9 were used to leach gold ore, and the specific steps were as follows: the gold ore was crushed, ground, and graded to obtain coarse-grained minerals with a particle size of +200 mesh and fine-grained minerals with a particle size of -200 mesh. The coarse-grained minerals were piled to obtain a coarse-grained mineral pile. The polymetallic ore dressing and separation reagents were used as leaching agents (the dosage was 1000 g / t, and the leaching time was 24 h), and the coarse-grained mineral pile was heap leached, and the fine-grained mineral was fully leached in a mud tank.

[0106] After testing, after the polymetallic ore dressing and separation reagent obtained in Example 1 was used to leach gold ore, the leaching rate of coarse-grained minerals was 97.68%, and the leaching rate of fine-grained minerals was 96.32%.

[0107] After gold ore was leached using the polymetallic ore dressing and separation reagent obtained in Example 8, the leaching rate of coarse-grained minerals was 98.57%, and the leaching rate of fine-grained minerals was 95.64%.

[0108] After gold ore was leached using the polymetallic ore dressing and separation reagent obtained in Example 9, the leaching rate of coarse-grained minerals was 98.61%, and the leaching rate of fine-grained minerals was 96.38%.

[0109] Comparative Example 1

[0110] The polymetallic ore dressing and separation agent provided in this comparative example is the first intermediate prepared in step (1) of Example 1.

[0111] According to the method of Example 10, the multi-metal ore dressing and separation reagent of this comparative example was used to carry out copper-sulfur flotation separation. After testing, the grade of copper element in the copper concentrate obtained in this comparative example was 20.18%, and the recovery rate of copper element was 85.69%.

[0112] According to the method of Example 11, the polymetallic ore dressing and separation reagent of this comparative example was used to carry out lead and zinc flotation separation. After testing, the lead grade in the copper concentrate obtained in this comparative example was 18.69%, and the lead recovery rate was 76.39%.

[0113] According to the method of Example 12, the polymetallic ore dressing and separation agent of this comparative example was used to leach gold ore. After testing, the leaching rate of the coarse-grained minerals of this comparative example was 95.12%, and the leaching rate of the fine-grained minerals was 94.32%.

[0114] Comparative Example 2

[0115] The polymetallic ore dressing and separation agent provided in this comparative example is the second intermediate prepared in step (2) of Example 1.

[0116] According to the method of Example 10, the multi-metal ore dressing and separation reagent of this comparative example was used to carry out copper-sulfur flotation separation. After testing, the grade of copper element in the copper concentrate obtained in this comparative example was 24.12%, and the recovery rate of copper element was 92.36%.

[0117] According to the method of Example 11, the polymetallic ore dressing and separation reagent of this comparative example was used to carry out lead and zinc flotation separation. After testing, the grade of lead element in the copper concentrate obtained in this comparative example was 22.91%, and the lead element recovery rate was 81.35%.

[0118] According to the method of Example 12, the polymetallic ore dressing and separation agent of this comparative example was used to leach gold ore. After testing, the leaching rate of the coarse-grained minerals of this comparative example was 96.69%, and the leaching rate of the fine-grained minerals was 95.39%.

[0119] Comparative Example 3

[0120] The preparation method of the polymetallic ore dressing and separation agent provided in this comparative example is basically the same as that in Example 1, except that in step (3), the mass ratio of the first intermediate to the second intermediate is replaced with 5:1.

[0121] According to the method of Example 10, the multi-metal ore dressing and separation reagent of this comparative example was used to carry out copper-sulfur flotation separation. After testing, the grade of copper element in the copper concentrate obtained in this comparative example was 21.98%, and the recovery rate of copper element was 82.36%.

[0122] According to the method of Example 11, the polymetallic ore dressing and separation reagent of this comparative example was used to carry out lead and zinc flotation separation. After testing, the grade of lead element in the copper concentrate obtained in this comparative example was 20.69, and the recovery rate of lead element was 78.69%.

[0123] According to the method of Example 12, the polymetallic ore dressing and separation agent of this comparative example was used to leach gold ore. After testing, the leaching rate of the coarse-grained minerals of this comparative example was 93.39%, and the leaching rate of the fine-grained minerals was 94.26%.

[0124] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.

Claims

1. A method for preparing a polymetallic ore separation agent, characterized in that: The steps include: (a), mixing a N-containing compound, sodium hydroxide and sodium carbonate and heating them to perform a first catalytic reaction to obtain a first intermediate; wherein the N-containing compound comprises at least one of urea, biuret and ammonium carbamate; (b), mixing a cyanamide compound and sodium hydroxide and subjecting the mixture to a second catalytic reaction in a chlorine atmosphere to obtain a second intermediate; wherein the cyanamide compound comprises at least one of cyanamide, sodium dicyanamide and calcium cyanamide; (c) After mixing the first intermediate and the second intermediate, the polymetallic ore dressing and separation agent is obtained.

2. The method for preparing a polymetallic ore separation agent according to claim 1, characterized in that: In step (a), at least one of the following conditions is met: (1) The mass ratio of the N-containing compound, the sodium hydroxide and the sodium carbonate is 35-59:40-45:1-5; (2) The heating comprises: first reacting at room temperature for 1 to 2 hours under vacuum conditions, and then reacting at 100 to 200° C. for 1 to 3 hours; (3) The catalyst used in the first catalytic reaction includes at least one of a Pt / TiO2 catalyst, a Ru / TiO2 catalyst, and a Rh / TiO2 catalyst.

3. The method for preparing a polymetallic ore separation agent according to claim 1, characterized in that: In step (b), the mass ratio of the cyanamide compound to the sodium hydroxide is 5-7:1-2.

4. The method for preparing a polymetallic ore dressing and separation agent according to claim 1, characterized in that: In step (c), the mass ratio of the first intermediate to the second intermediate is 1-5:6-9.

5. A polymetallic ore dressing and separation agent, characterized in that: The invention is prepared by the preparation method of the polymetallic ore dressing and separation agent according to any one of claims 1 to 4.

6. Use of the polymetallic ore dressing and separation agent as claimed in claim 5 in copper-sulfur flotation separation.

7. The use of the polymetallic ore dressing and separation agent in copper-sulfur flotation separation according to claim 6, characterized in that: The copper-sulfur flotation separation method comprises the following steps: using the polymetallic ore dressing and separation agent as a pyrite flotation inhibitor and frother, mixing the polymetallic ore dressing and separation agent with copper-sulfur mixed flotation concentrate slurry, and then performing roughing, concentrating and scavenging to obtain copper concentrate and sulfur-containing tailings.

8. Use of the polymetallic ore dressing and separation agent as claimed in claim 5 in lead and zinc flotation separation.

9. The use of the multi-metal ore dressing and separation reagent in lead and zinc flotation separation according to claim 8, characterized in that: The lead-zinc flotation separation method comprises the following steps: using the polymetallic ore dressing and separation agent as a flotation depressant, mixing the polymetallic ore dressing and separation agent with a lead-zinc-sulfur mixed flotation concentrate, a lead collector and a frother, and then performing roughing, cleaning and scavenging to obtain a lead concentrate and a zinc-sulfur tailings.

10. Use of the polymetallic ore separation agent as claimed in claim 5 in gold ore leaching; Preferably, the method for leaching gold ore comprises the following steps: The gold ore is crushed, ground and graded to obtain coarse-grained minerals and fine-grained minerals; the coarse-grained minerals are piled to obtain a coarse-grained mineral pile; the coarse-grained mineral pile is heap leached using the polymetallic ore dressing and separation agent as a leaching agent, and the fine-grained minerals are fully leached in a mud tank.

Citation Information

Patent Citations

  • Nuisanceless oredressing additive as well as preparation method and application thereof

    CN102121067A

  • Beneficiation reagent, synthesis method and method for comprehensively utilizing generated waste gases

    CN103409644A

  • Two-section synthesis method for beneficiation reagent

    CN105032622A

  • Gold and silver beneficiation agent, and preparation method and application thereof

    CN112522523A

  • Lead-zinc separation inhibitor and application method thereof

    CN117123373A