Double-sided gas shielded welding method and application

Through the double-sided gas shielded welding method, the problems of low welding quality and low production efficiency in X-shaped groove gas shielded welding are solved, and the root cleaning treatment on the back side of the welding is realized, which improves the welding quality and production efficiency, reduces the cost and pollution, and significantly Improved welding results.

CN118744266APending Publication Date: 2024-10-08JIANGSU XCMG CONSTRUCTION MACHINERY RESEARCH INSTITUTE LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410843139.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

The existing X-shaped groove gas shielded welding method has the problems of low welding quality and production efficiency, high cost, and serious pollution. Especially during the weld root cleaning process, it is easy to increase the risk of cracking, material cost and energy consumption, and the workpiece is greatly deformed. .

Method used

The double-sided gas-shielded welding method is adopted, and by designing the independent groove angle of the X-shaped groove, the combination of joint points and the welding electrical parameters, the backside of the welding can be treated without root cleaning and the welding quality and production efficiency can be improved. Specific steps include plate bevel processing, pre-welding cleaning, point assembly, preheating and welding. Mixed gas protection is used during welding, and the welding current, voltage and welding speed are adjusted to ensure welding quality.

Benefits of technology

It achieves penetration of butt joints, reduces welding deformation, improves welding quality and production efficiency, reduces noise and dust pollution, reduces cost and energy consumption, and shortens the production cycle.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118744266A_ABST
    Figure CN118744266A_ABST
Patent Text Reader

Abstract

The invention provides a double-sided gas shielded welding method and a structural part. The method comprises the steps that plate groove machining, pre-welding cleaning, plate splicing point assembling, preheating and welding are sequentially conducted, in the plate groove machining process, a groove of a plate is machined into an X-shaped groove, the front face groove angle is alpha 1, the back face groove angle is alpha 2, when t-C is smaller than 2L, the groove angle alpha 1 and alpha 2 are independently selected from any angle ranging from 30 degrees to 45 degrees, and when t-C is larger than or equal to 2L, the groove angle alpha 1 and alpha 2 are independently selected from any angle ranging from 30 degrees to 45 degrees. The groove angles alpha 1 and alpha 2 respectively and independently meet the conditions that alpha i is larger than or equal to 2 * arctan (0.5 * (D-G) / L), t is the thickness of a welded plate, C is the truncated edge size, L is the dry elongation length of a welding wire, D is the outer diameter of a nozzle of a welding gun, G is a root gap designed during plate splicing point assembly, and the unit is mm. By means of the method, back gouging treatment is avoided while joint penetration welding is achieved, the welding deformation probability is reduced, and the production efficiency and the welding quality are both improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of welding technology, and in particular to a double-sided gas shielded welding method and application thereof. Background Art

[0002] Engineering machinery structural parts and building steel structures are mainly manufactured by welding, which requires a large amount of welding work and has high requirements for welding quality. The welding method used is mainly metal arc welding, commonly known as gas shielded welding. This method has high production efficiency and strong welding adaptability, and is widely used in the welding of structural steel materials with a thickness of more than 3mm.

[0003] In the design process of welding structures at key positions of important structural parts, butt joints with low stress concentration are often selected to meet the high requirements for welding technology and weld quality. Usually, in order to ensure the penetration, the welding of butt joints needs to be processed with grooves. Common groove forms include V-shaped, X-shaped, U-shaped, etc. Among them, the X-shaped groove is not only easy to process, but also has the advantages of small weld filling volume and strong anti-deformation ability, and has been widely used.

[0004] Currently, the gas shielded welding method for X-shaped grooves is to weld the front side first, then clean and grind the weld root from the back side (hereinafter referred to as "weld root cleaning"), and then weld from the back side, where carbon arc gouging or mechanical grinding are mainly used to clean the weld root. There are two problems with the above-mentioned gas shielded welding method for X-shaped grooves: first, the weld root cleaning operation will affect the subsequent welding quality. For example, the carbonization of the base material during the carbon arc gouging process will increase the risk of cracking. At the same time, the material cost, energy consumption, and production cycle required for root cleaning will increase, and there will be serious noise and dust pollution; second, the workpiece is often deformed too much after welding by the above-mentioned method, which affects the subsequent use.

[0005] In general, the X-groove gas shielded welding method in the prior art generally has the problems of low welding quality and production efficiency, high cost and pollution. Summary of the invention

[0006] The present application provides a double-sided gas shielded welding method and a structural part to improve welding efficiency.

[0007] The first aspect of the present application provides a double-sided gas shielded welding method, which includes plate groove processing, pre-welding cleaning, plate joint point assembly, preheating and welding in sequence. In the plate groove processing, the groove of the plate is processed into an X-shaped groove, the front groove angle of the X-shaped groove is α1, and the back groove angle is α2. When tC<2L, the groove angles α1 and α2 are independently selected from any angle between 30° and 45°. When tC≥2L, the groove angles α1 and α2 independently satisfy αi≥2*arctan(0.5*(DG) / L); wherein t is the thickness of the welding plate, in mm; C is the blunt edge size, in mm; L is the dry extension length of the welding wire, in mm; D is the outer diameter of the welding gun nozzle, in mm; and G is the root gap designed when the plate joint points are assembled, in mm.

[0008] In any implementation manner of the first aspect, in the double-sided gas shielded welding method, the blunt edge dimension C is designed to be 0 to 1 mm.

[0009] In any embodiment of the first aspect, in the double-sided gas shielded welding method, the root gap G is designed to be 1 to 2 mm.

[0010] In any embodiment of the first aspect, in the double-sided gas shielded arc welding method, the blunt edge dimension C is 0 to 1 mm and the root gap G is 1 to 2 mm.

[0011] In any embodiment of the first aspect, the welding wire dry extension length L used for double-sided gas shielded welding is 15 to 20 mm.

[0012] In any embodiment of the first aspect, the outer diameter D of the welding gun nozzle used for double-sided gas shielded welding is 16 to 25 mm.

[0013] In any embodiment of the first aspect, the dry extension length L of the welding wire used for double-sided gas shielded welding is 15-20 mm and the outer diameter D of the welding gun nozzle is 16-25 mm.

[0014] In any embodiment of the first aspect, the pre-welding cleaning includes cleaning the groove surface and the plate surface within a range of 20 to 35 mm around the groove.

[0015] In any embodiment of the first aspect, the pre-welding cleaning method is mechanical grinding.

[0016] In any embodiment of the first aspect, the preheating temperature of the double-sided gas shielded welding in the preheating step is 100° C. to 200° C., and further, the groove surface of the plate and 35 to 42 mm around the groove can be preheated.

[0017] In any embodiment of the first aspect, the double-sided gas shielded welding step includes front root welding, back root welding, filling welding and cap welding performed in sequence.

[0018] In any embodiment of the first aspect, the welding speed of each pass in welding is 45 cm·min -1 ~50cm·min -1 .

[0019] In any embodiment of the first aspect, the interpass temperature of each pass in welding is 100°C to 300°C.

[0020] In any embodiment of the first aspect, the welding speed of each pass in welding is 45 cm·min -1 ~50cm·min -1 And the interlayer temperature is 100℃~300℃.

[0021] In any embodiment of the first aspect, the number of weld passes of the front bottom welding in the double-sided gas shielded welding method is 1, and one or more of the following conditions are met: (1) the welding current is 160 to 200 A; (2) the welding voltage is 18 to 21 V; (3) the welding line energy is 3.07 to 4.32 kJ·cm -1 .

[0022] In any embodiment of the first aspect, the number of weld passes of the back-end welding in the double-sided gas shielded welding method is 1, and one or more of the following conditions are met: (1) the welding current is 240 to 300 A; (2) the welding voltage is 24 to 29 V; (3) the welding line energy is 6.14 to 8.11 kJ·cm -1 .

[0023] In any embodiment of the first aspect, the filling welding in the double-sided gas shielded welding method includes alternating front filling welding and back filling welding, and the number of weld passes of the front filling welding and the back filling welding is multiple and independent.

[0024] In any embodiment of the first aspect, the welding conditions of each pass of the filling welding independently meet one or more of the following conditions: (1) the welding current is 240 to 300 A; (2) the welding voltage is 24 to 29 V; (3) the welding line energy is 6.14 to 8.11 kJ·cm -1 .

[0025] In any embodiment of the first aspect, the cap welding includes front cap welding and back cap welding, and the number of weld passes of the front cap welding and the back cap welding is multiple and independent.

[0026] In any embodiment of the first aspect, the welding conditions of each pass of the cap welding independently meet one or more of the following conditions: (1) the welding current is 210 to 280 A; (2) the welding voltage is 22 to 28 V; (3) the welding line energy is 4.93 to 6.62 kJ·cm -1 .

[0027] In any embodiment of the first aspect, a mixed gas is used as welding shielding gas during welding, and the mixed gas is selected from an inert gas and CO2.

[0028] In any embodiment of the first aspect, the welding shielding gas satisfies one or more of the following conditions: (1) the volume fraction of the inert gas in the welding shielding gas is 78% to 86%; (2) the volume fraction of CO2 in the welding shielding gas is 15% to 22%; (3) the flow rate of the welding shielding gas is 18 to 25 L / min.

[0029] A second aspect of the present application provides a structural member, comprising welded structural steel, wherein the welding is performed using the double-sided gas shielded welding method provided in the first aspect.

[0030] The double-sided gas shielded welding method provided in the present application can realize the back side of the welding without root cleaning through the design of the groove angle and the joint point group, the selection of welding electrical parameters and the adjustment of the welding sequence, so that the butt joint is welded through and the deformation of the workpiece after welding is reduced, thereby improving the welding quality and production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the specific embodiments of the present invention, the following will briefly introduce the drawings required for use in the specific embodiments. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work. In addition, in the following drawings, the contents of the drawings are not drawn according to the actual scale.

[0032] Figure 1 A schematic diagram of the X-shaped groove and welding gun nozzle of the butt joint is shown, wherein the plate thickness is t (unit: mm), the blunt edge size of the groove is C (unit: mm), the root gap when the plates are assembled is G (unit: mm), the outer diameter of the welding gun nozzle is D (unit: mm), the dry extension length of the welding wire is L (unit: mm), and the groove angles are α1 and α2 respectively.

[0033] Figure 2 A schematic diagram of welding passes of an X-shaped groove of a butt joint of a Q550 structural steel plate using the double-sided gas shielded welding method provided in Example 1 of the present application is shown.

[0034] Figure 3A schematic diagram of the welding passes of the X-shaped groove of the butt joint of Q355 structural steel plate using the double-sided gas shielded welding method provided in Example 2 of the present application is shown, and the plate thickness is 50 mm.

[0035] Figure 4 A schematic diagram of the welding passes of the double-sided gas shielded welding method provided in Example 3 of the present application for the X-shaped groove of the butt joint of the Q1100 structural steel plate is shown, and the plate thickness is 16 mm.

[0036] Figure 5 A schematic diagram of welding passes of an X-shaped groove of a butt joint of a Q550 structural steel plate using the double-sided gas shielded welding method provided in Comparative Example 1 is shown, and the plate thickness is 25 mm.

[0037] Figure 6 A schematic diagram of the welding passes of the X-shaped groove of the butt joint of the Q355 structural steel plate using the double-sided gas shielded welding method provided in Comparative Example 2 is shown, and the plate thickness is 50 mm. DETAILED DESCRIPTION

[0038] The following embodiments further describe the implementation of the present application in detail. The detailed description of the following embodiments is used to illustrate the principle of the present application, but cannot be used to limit the scope of the present application, that is, the present application is not limited to the described embodiments.

[0039] If not otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0040] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0041] As analyzed in the background technology of this application, the gas shielded welding method of the X-shaped groove of the butt joint in the prior art generally requires the weld root cleaning, and the welding work is prone to deformation, so there are problems such as poor welding quality, high cost and serious pollution.

[0042] In the first embodiment of the present application, a double-sided gas shielded welding method is provided, which includes plate groove processing, pre-welding cleaning, plate joint point assembly, preheating and welding in sequence, wherein, during the plate groove processing, the plate groove is processed into an X-shaped groove, the front groove angle of the X-shaped groove is α1, and the back groove angle is α2; when tC<2L, the groove angles α1 and α2 are independently selected from any angle in the range of 30° to 45°, and when tC≥2L, the groove angles α1 and α2 are independently satisfied α≥2*arctan(0.5*(DG) / L). Wherein, t is the thickness of the welding plate, in mm; C is the blunt edge size, in mm; L is the dry extension length of the welding wire, in mm; D is the outer diameter of the welding gun nozzle, in mm; G is the root gap designed when the plate joint points are assembled, in mm.

[0043] In some embodiments, tC<2L is satisfied, and the groove angles α1 and α2 are each independently selected from any angle in the range of 30° to 45°, such as 30°, 32°, 35°, 41.5°, 43°, and 45°.

[0044] In some embodiments, tC≥2L is satisfied, and the groove angles α1 and α2 each independently satisfy α<180°, for example, α<170°, α<160°, α<150°, α<120°, α<90°, α<75°, α<60°.

[0045] The above-mentioned double-sided gas shielded welding method can achieve full penetration of the butt joint through the design of the groove angle, saving the back root cleaning process, thereby avoiding the cost, energy consumption and increased production cycle as well as noise and dust pollution caused by the root cleaning process; at the same time, the welding quality is reliable, the probability of welding deformation is reduced, and the production efficiency and welding quality are improved simultaneously.

[0046] Generally, the smaller the blunt edge size, the easier it is to weld through the root under the same welding conditions. In some embodiments, the blunt edge size C in the double-sided gas shielded welding method is 0-1 mm and / or the root gap G is 1-2 mm. On the basis of reserving a smaller blunt edge size, the root gap when the plate joints are assembled is adjusted to enhance the firmness of the welding.

[0047] The principle of selecting welding wire during welding in this application follows the conventional material selection rules in this field. For example, the welding wire model that matches the mechanical properties and brand of the plate is selected. When the plates are made of different materials, the one with lower tensile strength is selected as the basis.

[0048] In some embodiments of the first aspect of the present application, the dry extension length L of the welding wire in the double-sided gas shielded welding method is 15 to 20 mm. The dry extension length of the welding wire can be adjusted within the above range according to the conditions of the selected welding wire. In some embodiments, the dry extension length L of the welding wire can be selected as 15 mm, 16 mm, 17 mm, 18 mm, 19 mm or 20 mm. If the dry extension length of the welding wire is too short, the melting effect of the weld is difficult to control; on the contrary, if the dry extension length of the welding wire is too long, a large amount of gas protection is required to maintain the continuity of the arc, resulting in increased costs.

[0049] In some embodiments of the first aspect of the present application, in the double-sided gas shielded welding method, the welding gun nozzle diameter D is 16 to 25 mm. In some embodiments, the welding gun nozzle diameter D can be 16 mm, 22 mm or 25 mm. Generally, a larger nozzle diameter can provide more heat and droplet transfer, and the required gas flow rate is generally larger, so that the shielding gas can more fully cover the welding area.

[0050] When designing the groove angle, on the one hand, it is necessary to meet the root penetration and welding gun accessibility, and on the other hand, it is necessary to make the deformation of the plate after welding as small as possible. According to the thickness of the plate to be welded, the specifications of the welding gun nozzle selected for gas shielded welding and other parameters, the appropriate groove angle and the blunt edge size of the plate are designed, and the plate is grooved. The following is an exemplary description of the groove selection. In some embodiments, when tC < 2L, the selection of the groove angle does not affect the accessibility of the welding gun. In order to achieve a better penetration effect, the groove angle can be selected in the range of 30° to 45° according to the size of the welding gun nozzle diameter D. In some embodiments, when D is 16mm, the groove angle is selected to be 30°; when D is 22mm, the groove angle is selected to be 40°; when D is 25mm, the groove angle is selected to be 45°.

[0051] In order to further improve the welding quality, in some embodiments, the pre-welding cleaning in the double-sided gas shielded welding method includes cleaning the groove surface and the plate surface within 20 to 35 mm around the groove; optionally, the pre-welding cleaning adopts mechanical grinding. In some embodiments, an angle grinder is used to grind the groove surface and the surface of the plate to be welded within 20 to 35 mm around the groove to remove rust, oil stains, primer, etc., and expose the metallic luster.

[0052] Before welding, the welding area of ​​the plate is preheated, and the preheating effect is monitored using a temperature testing device such as an infrared temperature measuring gun. Welding is started after the welding area of ​​the plate reaches the preheating temperature. The setting of the preheating temperature mainly depends on the chemical composition, mechanical properties and thickness of the plate. During the preheating process, the preheating temperature and time are adjusted according to the welding specifications and actual operating experience. In some embodiments, the preheating temperature in the double-sided gas shielded welding method is 100°C to 200°C; optionally, the groove surface of the plate and 35 to 42 mm around the groove are preheated. Preheating before welding within the above range is conducive to the escape of hydrogen atoms in the weld, thereby further reducing the risk of hardening, embrittlement and cold cracking of the heat-affected zone.

[0053] The method of preheating the plate before welding can be selected according to actual needs, and this application does not impose any special restrictions on this. For example, a box-type resistance furnace can be used to heat the plate as a whole, or a flame spray gun, infrared heater and other equipment can be used to heat the plate as a whole or locally. In some embodiments, the heating method of the preheating treatment before welding includes heating with an oxygen-acetylene flame (also referred to as an "oxygen-acetylene torch").

[0054] In some embodiments, welding in the double-sided gas shielded welding method includes front base welding, back base welding, filling welding and cap welding performed in sequence. Base welding is the first welding performed at the root of the joint. The present application designs the groove angle to ensure that the root is fully penetrated and well-formed during front base welding. Back base welding can be performed without root cleaning, laying a good foundation for subsequent welding. The main purpose of filling welding is to fill the gap between the root of the joint and the previous welding layer, increase the cross-sectional area and strength of the joint, and multi-layer and multi-pass welding can be used to gradually increase the size and strength of the joint. Cap welding is the welding layer directly exposed to the surface of the welded joint. The fewer defects such as cracks and pores generated during cap welding, the smoother and more uniform the weld surface.

[0055] As an important welding process parameter, welding speed directly affects welding quality and production efficiency. To further improve weld quality, the welding speed is set within a certain range. In some implementations, the welding speed of each pass is 45 cm / min. -1 ~50cm·min -1 . The welding conditions are adjusted according to the welded plates and the selected welding wire. The technicians in this field can control the welding speed within the above range. If the welding speed is too fast, it is difficult to control the generation of defects such as cracks and pores, and the weld formation quality is poor; on the contrary, if the welding speed is too slow, it may lead to insufficient weld pool temperature, poor weld penetration, and greater welding stress and deformation.

[0056] The interlayer temperature is the temperature that needs to be maintained when the next weld is made after a weld is completed during a multi-pass welding process. According to conventional operations in the field, the interlayer temperature should be equal to or slightly higher than the preheating temperature before welding. In some embodiments, the interlayer temperature of welding is 100°C to 300°C, thereby improving the strength of the weld formed by each weld combination. If the interlayer temperature is too high, it is easy to cause overheating and poor solidification at the weld, embrittlement of the microstructure in the weld area and surrounding areas, and deterioration of mechanical properties.

[0057] When welding the front bottom, the art can use conventional welding parameters as a reference to select corresponding welding parameters to avoid the root being not fully melted or burned through. In some embodiments, the number of weld passes for the front bottom welding is 1, and one or more of the following conditions are met: (1) the welding current is 160 to 200 A; (2) the welding voltage is 18 to 21 V; (3) the welding line energy is 3.07 to 4.32 kJ·cm -1 After the groove angle is determined, the corresponding welding parameters are selected from one or more of the above welding parameter ranges according to the properties of the welded materials to achieve full melting of the root and avoid burn-through caused by excessive melting.

[0058] When back-pass welding, appropriately increasing the welding electrical parameters is beneficial to the root remelting and penetration of the front-pass weld. In some embodiments, the welding electrical parameters can be increased by about 50% based on the conventional electrical parameters. In some embodiments, the number of welds for back-pass welding is 1, and one or more of the following conditions are met: (1) the welding current is 240 to 300A; (2) the welding voltage is 24 to 29V; (3) the welding line energy is 6.14 to 8.11 kJ·cm -1 .

[0059] The number of fill welding passes is related to the thickness of the plate, and the increase or decrease in the number of weld passes can be adjusted according to the thickness of the plate to be welded. The specific adjustment method can be referred to the conventional operation in the field, which will not be repeated here. In some embodiments, the fill welding includes alternating front fill welding and back fill welding, and the number of weld passes of the front fill welding and the back fill welding is multiple and independent.

[0060] The cap welding includes front cap welding and back cap welding, and the number of weld passes is also related to the thickness of the plate. The specific number of weld passes can be referred to the conventional operation in the field, which will not be repeated here. In some embodiments, the number of weld passes of the front cap welding and the back cap welding is multiple and independent.

[0061] When performing fill welding or cap welding, the selection of welding electrical parameters can also be fine-tuned appropriately with reference to the thickness of the plate to be welded. The welding electrical parameters of the back cap weld can be lower than those of the front cap weld to make the back excess height basically consistent with the front excess height as much as possible, thereby improving the welding appearance quality.

[0062] The welding conditions of each pass of the filling welding and the cap welding of the present application can be referenced by the corresponding conventional welding parameters. In some embodiments, the welding conditions of each pass of the filling welding independently meet one or more of the following conditions: (1) the welding current is 240 to 300A; (2) the welding voltage is 24 to 29V; (3) the welding line energy is 6.14 to 8.11 kJ·cm -1 .

[0063] In some embodiments, the welding conditions of each pass of the cap welding independently meet one or more of the following conditions: (1) the welding current is 210-280A; (2) the welding voltage is 22-28V; (3) the welding line energy is 4.93-6.62 kJ·cm -1 .

[0064] The above welding conditions are used to further improve the welding quality.

[0065] Welding shielding gases include single-component shielding gases and multi-component mixed shielding gases (for example, binary, ternary, and quaternary mixed gases). During the welding process, the shielding gas plays a role in protecting the molten pool and slag, isolating the molten weld from the air to avoid oxidation, and blocking impurities and moisture in the environment. The multi-component mixed gas has relative advantages in refining molten droplets, reducing spatter, and improving forming, which can further improve the welding quality. Depending on whether it reacts with the welding molten pool, the welding shielding gas can be divided into two categories: active gas and inert gas. In some embodiments, the double-sided gas shielded welding method of the present application uses a mixed gas as the welding shielding gas, and the mixed gas is selected from an inert gas and CO2. Commonly used inert gases include argon and helium, and the arc stability is good. CO2 is low in cost and easy to obtain, and is used as an active gas.

[0066] During welding, the welding shielding gas flow rate and the proportion of different gases can be selected according to the thickness, chemical composition, mechanical properties, etc. of the plate. In some embodiments, the welding shielding gas satisfies one or more of the following conditions: (1) the volume fraction of the inert gas in the welding shielding gas is 78% to 86%; (2) the volume fraction of CO2 in the welding shielding gas is 15% to 22%; (3) the flow rate of the welding shielding gas is 18 to 25 L / min. The use of the above-mentioned volume fraction of inert gas can improve the arc stability, and the use of the above-mentioned active gas can improve the welding efficiency and improve the droplet transition during the welding process.

[0067] In a second embodiment of the present application, a structural member is provided, comprising welded structural steel, wherein the welding is performed by the double-sided gas shielded welding method in the first embodiment of the present application. The structural member can be applied to engineering machinery and building construction, and the welding efficiency and welding quality of the structural member can be significantly improved by the double-sided gas shielded welding method in the first embodiment.

[0068] The beneficial effects of the present application will be further illustrated below in combination with examples and comparative examples, but the scope of the present invention is not limited to these examples.

[0069] Example 1

[0070] The double-sided gas shielded welding method provided in the present application is used to perform double-sided welding of the X-shaped groove of the butt joint of Q550 structural steel plates with a thickness t of 25 mm.

[0071] The welding power source is a MAG welding machine, the outer diameter D of the welding gun nozzle is 25 mm, and the dry extension length L of the welding wire is 18 mm.

[0072] The welding shielding gas is a binary mixed gas composed of 84% Ar + 16% CO2, and the welding shielding gas flow rate is 20L / min.

[0073] The welding wire is ER70-G solid wire with a wire diameter of 1.2 mm.

[0074] The specific steps of this embodiment are:

[0075] Step 1: Select the blunt edge size C as 0.5mm, tC<2L, and the groove angle as 45° to process the groove of the plate;

[0076] Step 2: Use an angle grinder to clean before welding, grind the groove surface and the surface of the parent material within 30mm around the groove to reveal the metallic luster;

[0077] Step 3: The Q550 structural steel plates to be welded are assembled and matched, and the root gap G is reserved to be 1mm;

[0078] Step 4: Preheating before welding: Based on the chemical composition, mechanical properties and thickness of the Q550 structural steel plate, the preheating temperature is set above 100°C, and the plate within 40mm around the groove surface is heated with an oxygen-acetylene flame, and the temperature is measured with an infrared temperature measuring gun. When the temperature of the area to be welded reaches above 100°C, stop heating;

[0079] Step 5: During welding, control the interlayer temperature to be between 100℃ and 300℃. According to the thickness of the plate and the groove angle, a total of 12 welds are required. Figure 2 The welding electrical parameters are shown in Table 1.

[0080] During welding, follow Figure 2 The welds 1 to 12 shown are welded in the order in which the 1st weld is the front base weld, which can make the root melt through; the 2nd weld is the back base weld, which can make the root of the front base weld remelt and weld through; after the front base welding, the back base welding is directly performed without root cleaning; the 3rd and 4th welds are the welding of the filling weld from the front, i.e., the front filling welding; the 5th and 6th welds are the welding of the filling weld from the back, i.e., the back filling welding; the 7th, 8th and 9th welds are the welding of the cover weld from the front, i.e., the front cover welding; the 10th, 11th and 12th welds are the welding of the cover weld from the back, i.e., the back cover welding.

[0081] Table 1

[0082]

[0083] The surface and internal nondestructive testing of the weld was carried out by visual inspection, magnetic particle inspection and ultrasonic inspection. No defects were found on the surface and inside of the weld area, and the root of the X-shaped groove was welded through. The three-coordinate measurement of the welding deformation of the joint showed that the warping deformation of the plates on the left and right sides was small, and the angle θ was less than 2°.

[0084] Example 2

[0085] The double-sided gas shielded welding method provided in the present application is used to perform double-sided welding of the X-shaped groove of the butt joint of Q355 structural steel plates with a thickness t of 50 mm.

[0086] The welding power source is a MAG welding machine, the outer diameter D of the welding gun nozzle is 25 mm, and the dry extension length L of the welding wire is 18 mm.

[0087] The welding shielding gas is a binary mixed gas composed of 84% Ar + 16% CO2, and the welding shielding gas flow rate is 22L / min.

[0088] The welding wire is ER50-6 solid wire with a wire diameter of 1.2mm.

[0089] The specific steps of this embodiment are:

[0090] Step 1: The blunt edge size C is selected as 0.5mm, tC>2L, according to the formula α≥2*arctan(0.5*(DG) / L), the minimum groove angle is 67.5°. For ease of processing, the groove angle is selected as 70°, and the groove of the plate is processed;

[0091] Step 2: Use an angle grinder to clean before welding, grind the groove surface and the surface of the parent material within 30mm around the groove to reveal the metallic luster;

[0092] Step 3: Assemble the Q355 structural steel plates to be welded, and reserve a root gap G of 1.5 mm;

[0093] Step 4: Preheating before welding: Based on the chemical composition, mechanical properties and thickness of the Q355 structural steel plate, the preheating temperature is set above 100°C, and the plate within 40mm around the groove surface is heated with an oxygen-acetylene flame, and the temperature is measured with an infrared temperature measuring gun. When the temperature of the area to be welded reaches above 100°C, stop heating;

[0094] Step 5: During welding, control the interlayer temperature to be between 100℃ and 300℃. According to the thickness of the plate and the groove angle, a total of 12 welds are required. Figure 3 The welding electrical parameters are shown in Table 2. During welding, Figure 3 The welds 1 to 72 shown are welded in the order of: the 1st weld is the front base weld, the 2nd weld is the back base weld, and root cleaning is not required; the 3rd to 56th welds are filling welds, the 57th to 64th welds are front cover welds, and the 65th to 72nd welds are back cover welds.

[0095] Table 2

[0096]

[0097]

[0098] The surface and internal nondestructive testing of the weld was carried out by visual inspection, magnetic particle inspection and ultrasonic inspection. No defects were found on the surface and inside of the weld area, and the root of the X-shaped groove was fully welded. The three-coordinate measurement of the welding deformation of the joint showed that the warping deformation of the plates on the left and right sides was small, and the angle θ was less than 3°.

[0099] Example 3

[0100] The double-sided gas shielded welding method provided in the present application is used to perform double-sided welding of the X-shaped groove of the butt joint of Q1100 structural steel plates with a thickness t of 16 mm.

[0101] The welding power source is a MAG welding machine, the outer diameter D of the welding gun nozzle is 25 mm, and the dry extension length L of the welding wire is 18 mm.

[0102] The welding shielding gas is a binary mixed gas composed of 84% Ar + 16% CO2, and the welding shielding gas flow rate is 20L / min.

[0103] The welding wire is ER90-G solid wire with a wire diameter of 1.2 mm.

[0104] The specific steps of this embodiment are:

[0105] Step 1: Select the blunt edge size C as 0.5mm, tC<2L, and the groove angle as 45° to process the groove of the plate;

[0106] Step 2: Use an angle grinder to clean before welding, grind the groove surface and the surface of the parent material within 30mm around the groove to reveal the metallic luster;

[0107] Step 3: The Q1100 structural steel plates to be welded are assembled and matched, and the root gap G is reserved to be 1mm;

[0108] Step 4: Preheating before welding: Based on the chemical composition, mechanical properties and thickness of the Q1100 structural steel plate, the preheating temperature is set above 150°C. The plate within 40mm of the groove surface and the surrounding area is heated with an oxygen-acetylene flame, and the temperature is measured with an infrared temperature measuring gun. When the temperature of the area to be welded reaches above 150°C, stop heating;

[0109] Step 5: During welding, control the interlayer temperature to be between 150℃ and 300℃. According to the thickness of the plate and the groove angle, a total of 4 welds are required. The number of welds is as follows: Figure 4 The welding electrical parameters are shown in Table 3.

[0110] During welding, follow Figure 4 The welds 1 to 4 shown are welded in the order in which the 1st weld is the front base weld, which can make the root melt through, the 2nd weld is the back base weld, which can make the root of the front base weld remelt and melt through, and the back base welding can be carried out directly after the front base welding without root cleaning, the 3rd weld is the filling (covering) weld welded from the front, and the 4th weld is the filling (covering) weld welded from the back.

[0111] Table 3

[0112]

[0113]

[0114] The surface and internal nondestructive testing of the weld was carried out by visual inspection, magnetic particle inspection and ultrasonic inspection. No defects were found on the surface and inside of the weld area, and the root of the X-shaped groove was fully welded. The three-coordinate measurement of the welding deformation of the joint showed that the warping deformation of the plates on the left and right sides was small, and the angle θ was less than 2°.

[0115] Comparative Example 1

[0116] In this comparative example, the double-sided gas shielded welding method is used to perform double-sided welding of the X-shaped groove of the butt joint of the Q550 structural steel plate with a thickness t of 25 mm.

[0117] The welding power source is a MAG welding machine, the outer diameter D of the welding gun nozzle is 25 mm, and the dry extension length L of the welding wire is 18 mm.

[0118] The welding shielding gas is a binary mixed gas composed of 84% Ar + 16% CO2, and the welding shielding gas flow rate is 20L / min.

[0119] The welding wire is ER70-G solid wire with a wire diameter of 1.2 mm.

[0120] The specific steps of this comparative example are:

[0121] Step 1: Select the blunt edge size C as 0.5mm, tC<2L, and the groove angle as 10° to process the groove of the plate;

[0122] Step 2: Use an angle grinder to clean before welding, grind the groove surface and the surface of the parent material within 30mm around the groove to reveal the metallic luster;

[0123] Step 3: The Q550 structural steel plates to be welded are assembled and matched, and the root gap G is reserved to be 1mm;

[0124] Step 4: Preheating before welding: Based on the chemical composition, mechanical properties and thickness of the Q550 structural steel plate, the preheating temperature is set above 100°C, and the plate within 40mm around the groove surface is heated with an oxygen-acetylene flame, and the temperature is measured with an infrared temperature measuring gun. When the temperature of the area to be welded reaches above 100°C, stop heating;

[0125] Step 5: During welding, control the interlayer temperature to be between 100℃ and 300℃. According to the thickness of the plate and the groove angle, a total of 4 welds are required, and the welding passes are as follows: Figure 5 The welding electrical parameters are shown in Table 4.

[0126] During welding, follow Figure 5 The welds 1 to 4 shown are welded in the order of, the 1st weld is the front base weld, due to the small groove angle, the flexibility and visibility of the welding wire are poor, resulting in poor penetration; the 2nd weld is the back base weld, due to the small groove angle, the flexibility and visibility of the welding wire are poor, resulting in poor penetration; the 3rd weld is the filling weld welded from the front, i.e., the front filling (capping) welding, and the 4th weld is the filling weld welded from the back, i.e., the back filling (capping) welding.

[0127] Table 4

[0128]

[0129] Visual inspection, magnetic particle inspection and ultrasonic inspection were used to conduct nondestructive testing on the surface and inside of the weld. No defects were found on the surface of the weld area, but there was incomplete penetration at the root of the X-shaped groove. The three-coordinate measurement of the welding deformation of the joint showed that the warping deformation of the plates on the left and right sides was small, and the angle θ was less than 1.5°.

[0130] Comparative Example 2

[0131] In this comparative example, double-sided gas shielded welding method is used to perform double-sided welding of the X-shaped groove of the butt joint of Q355 structural steel plate with a thickness t of 50 mm.

[0132] The welding power source is a MAG welding machine, the outer diameter D of the welding gun nozzle is 25 mm, and the dry extension length L of the welding wire is 18 mm.

[0133] The welding shielding gas is a binary mixed gas composed of 84% Ar + 16% CO2, and the welding shielding gas flow rate is 22L / min.

[0134] The welding wire is ER50-6 solid wire with a wire diameter of 1.2mm.

[0135] The specific steps of this comparative example are:

[0136] Step 1: Select the blunt edge size C as 0.5mm, tC>2L, and the groove angle as 50° to process the groove of the plate;

[0137] Step 2: Use an angle grinder to clean before welding, grind the groove surface and the surface of the parent material within 30mm around the groove to reveal the metallic luster;

[0138] Step 3: Assemble the Q355 structural steel plates to be welded, and reserve a root gap G of 1.5 mm;

[0139] Step 4: Preheating before welding: Based on the chemical composition, mechanical properties and thickness of the Q355 structural steel plate, the preheating temperature is set above 100°C, and the plate within 40mm around the groove surface is heated with an oxygen-acetylene flame, and the temperature is measured with an infrared temperature measuring gun. When the temperature of the area to be welded reaches above 100°C, stop heating;

[0140] Step 5: During welding, control the interlayer temperature to be between 100℃ and 300℃. According to the thickness of the plate and the groove angle, a total of 42 welds are required. Figure 6 The welding electrical parameters are shown in Table 5. Figure 6The welds 1 to 42 shown are welded in the order of: the first weld is a front base weld; since the welding wire cannot reach the root, the arc heat cannot melt the blunt edge, resulting in poor weld penetration; the second weld is a back base weld; since the welding wire cannot reach the root, the arc heat cannot melt the blunt edge, resulting in poor weld penetration; welds 3 to 30 are filling welds, welds 31 to 36 are front cover welds, and welds 37 to 42 are back cover welds.

[0141] Table 5

[0142]

[0143]

[0144] Visual inspection, magnetic particle inspection and ultrasonic inspection were used in turn to conduct non-destructive testing on the surface and inside of the weld. No defects were found on the surface of the weld area, and the root of the internal X-shaped groove was found to be incomplete. The three-coordinate measurement of the welding deformation of the joint showed that the warping deformation of the plates on the left and right sides was small, and the angle θ was less than 3°.

[0145] It can be seen from the results of the above embodiments and comparative examples that the double-sided gas shielded welding method provided by the present application can achieve full penetration welding of the butt joint without back root cleaning through the design of the groove angle and the joint point group and the selection of welding electrical parameters and sequence, which significantly improves production efficiency and welding quality. In an actual operating environment, the double-sided gas shielded welding method provided by the present application is used for welding, and noise and dust pollution will also be smaller, reducing the harm of the processing environment to the human body. In addition, root cleaning is not only shortened The production cycle is also conducive to reducing energy consumption and costs.

[0146] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A double-sided gas shielded welding method, characterized in that: The double-sided gas shielded welding method includes the following steps: plate groove processing, pre-welding cleaning, plate point assembly, preheating and welding. In the plate groove processing, the plate groove is processed into an X-shaped groove, the front groove angle of the X-shaped groove is α1, and the back groove angle is α2. When tC<2L, the groove angles α1 and α2 are each independently selected from any angle in the range of 30° to 45°, and when tC≥2L, the groove angles α1 and α2 each independently satisfy αi≥2*arctan(0.5*(DG) / L); in, t is the thickness of the welding plate, in mm; C is the blunt edge size, in mm; L is the dry extension length of the welding wire, in mm; D is the outer diameter of the welding gun nozzle, in mm; G is the designed root gap when the plates are assembled, in mm.

2. The double-sided gas shielded welding method according to claim 1, characterized in that: The blunt edge dimension C is 0-1 mm and / or the root gap G is 1-2 mm.

3. The double-sided gas shielded welding method according to claim 1 or 2, characterized in that: The welding wire extension length L is 15-20 mm and / or the welding gun nozzle outer diameter D is 16-25 mm.

4. The double-sided gas shielded welding method according to claim 1, characterized in that: The cleaning before welding includes cleaning the groove surface and the plate surface within a range of 20 to 35 mm around the groove; optionally, the cleaning before welding is performed by mechanical grinding.

5. The double-sided gas shielded welding method according to claim 1, characterized in that: The preheating temperature is 100° C. to 200° C. Optionally, the groove surface of the plate and 35 to 42 mm around the groove are preheated.

6. The double-sided gas shielded welding method according to claim 5, characterized in that: The heating method of the preheating treatment includes heating with an oxygen-acetylene flame.

7. The double-sided gas shielded welding method according to any one of claims 1 to 6, characterized in that: The welding comprises: front bottom welding, back bottom welding, filling welding and cap welding performed in sequence.

8. The double-sided gas shielded welding method according to claim 7, characterized in that: The welding speed of each pass in the welding is 45 cm·min -1 ~50cm·min -1 And / or the interlayer temperature is 100°C to 300°C.

9. The double-sided gas shielded welding method according to claim 7, characterized in that: The number of weld passes of the front bottom welding is 1, and one or more of the following conditions are met: (1) The welding current is 160~200A; (2) The welding voltage is 18~21V.

10. The double-sided gas shielded welding method according to claim 7, characterized in that: The number of weld passes of the back-end welding is 1, and one or more of the following conditions are met: (1) The welding current is 240~300A; (2) The welding voltage is 24~29V.

11. The double-sided gas shielded welding method according to claim 7, characterized in that: The filling welding includes front filling welding and back filling welding which are performed alternately, and the number of weld passes of the front filling welding and the back filling welding is multiple and independent.

12. The double-sided gas shielded welding method according to claim 11, characterized in that: The welding conditions of each pass of the filling welding independently meet one or more of the following conditions: (1) The welding current is 240~300A; (2) The welding voltage is 24~29V.

13. The double-sided gas shielded welding method according to claim 7, characterized in that: The cap welding includes front cap welding and back cap welding, and the number of weld passes of the front cap welding and the back cap welding is multiple and independent.

14. The double-sided gas shielded welding method according to claim 13, characterized in that: The welding conditions of each pass of the cap welding independently meet one or more of the following conditions: (1) The welding current is 210~280A; (2) The welding voltage is 22~28V.

15. The double-sided gas shielded welding method according to claim 1, characterized in that: The welding uses a mixed gas as welding shielding gas, and the mixed gas is selected from an inert gas and CO2.

16. The double-sided gas shielded welding method according to claim 15, characterized in that: The welding shielding gas meets one or more of the following conditions: (1) The volume fraction of inert gas in welding shielding gas is 78% to 86%; (2) The volume fraction of CO2 in the welding shielding gas is 15% to 22%; (3) The flow rate of welding shielding gas is 18~25L / min.

17. A structural member comprising welded structural steel, characterized in that: The welding is carried out by the double-sided gas shielded welding method according to any one of claims 1 to 16.